A red crystalline carbon nitride and a preparation method and application thereof
Red crystalline carbon nitride was synthesized by thermal polycondensation reaction of melamine, potassium thiocyanate and ammonium chloride, which solved the problems of low crystallinity and narrow light absorption range of carbon nitride and achieved efficient photocatalytic hydrogen production using sunlight.
Patent Information
- Application Number
- CN202411461646.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-18
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-10-18
AI Technical Summary
Existing carbon nitride photocatalysts have low crystallinity and narrow light absorption range, which limits their effectiveness in utilizing sunlight and their photocatalytic activity.
Red crystalline carbon nitride was synthesized via thermal polycondensation using melamine, potassium thiocyanate, and ammonium chloride as precursors, thereby improving crystallinity and expanding the photoresponse range.
It improves the crystallinity and visible light absorption range of crystalline carbon nitride, promotes the separation and transport of photogenerated carriers, and significantly enhances the photocatalytic hydrogen production activity.
Smart Images

Figure CN119100339B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of photocatalytic materials, specifically relating to a red crystalline carbon nitride, its preparation method, and its application. Background Technology
[0002] Graphitic carbon nitride (CN) is one of the most promising photocatalysts in the field of photocatalysis due to its suitable band structure, good optical properties, and excellent chemical stability. However, due to the kinetic problems in the high-temperature polymerization of traditional cyanamide-based carbon and nitrogen molecules, the synthesized carbon nitride has a low crystallinity and short-range disordered heptaazine-melon structure, which contains a large number of incompletely polymerized terminal amino groups. The hydrogen bonds formed between the amino groups greatly reduce the carrier transport efficiency between the heptaazine conjugated rings, thus limiting the photocatalytic activity of carbon nitride.
[0003] Furthermore, near-infrared light accounts for approximately 50% of the solar flux and possesses stronger tissue penetration and lower phototoxicity than ultraviolet-visible light. However, due to the compatibility issues between the high separation efficiency of photoexcited carriers and the narrow bandgap (0.5–1.8 eV), near-infrared light has rarely been effectively used in photocatalytic reactions to date. It is estimated that for industrial applications, the solar-to-hydrogen conversion efficiency needs to reach over 10%, corresponding to a photoresponse range of the semiconductor photocatalyst above 520 nm and an apparent quantum efficiency of 100%. Ordinary carbon nitride is pale yellow with a bandgap of 2.7 eV, absorbing only visible light below 460 nm; therefore, existing technologies require improvement and development. Summary of the Invention
[0004] To overcome the drawbacks of narrow light absorption range and low crystallinity of carbon nitride, this invention provides a red crystalline carbon nitride, its preparation method, and its application.
[0005] To achieve the above objectives, the technical solution of the present invention is as follows:
[0006] The first aspect of the present invention is a method for preparing red crystalline carbon nitride, comprising the following steps: mixing nitrogen-rich precursor melamine with molten salt potassium thiocyanate and ammonium chloride uniformly and then carrying out a thermal polycondensation reaction, followed by washing and drying to obtain red crystalline carbon nitride.
[0007] Furthermore, the conditions for the thermal polycondensation reaction are as follows: under an argon atmosphere, the temperature is raised to 400°C and held for 1 hour, and then the temperature is raised to 500-610°C and held for 1-2 hours.
[0008] Furthermore, the molar ratio of potassium thiocyanate to ammonium chloride is (4-2):1.
[0009] Furthermore, the mass ratio of melamine to potassium thiocyanate is (2-3):2.
[0010] Furthermore, the drying temperature is 60°C.
[0011] The second aspect of the present invention is red crystalline carbon nitride prepared by the preparation method described in the first aspect.
[0012] The third aspect of the present invention is the application of the red crystalline carbon nitride described in the second aspect as a photocatalyst.
[0013] Furthermore, it is applied to the photocatalytic water splitting reaction to produce hydrogen.
[0014] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0015] (1) This invention proposes a simple bottom-up strategy for synthesizing crystalline carbon nitride. This method uses melamine as a nitrogen-rich precursor source and ammonium thiocyanate, synthesized from potassium thiocyanate and ammonium chloride during high-temperature thermal polycondensation, as another precursor source, ultimately producing red crystalline carbon nitride. This preparation method uses inexpensive raw materials, is simple and easy to operate, has low requirements for production equipment, and is easy to industrialize.
[0016] (2) The method for preparing red crystalline carbon nitride provided by the present invention can improve the crystallinity of crystalline carbon nitride, promote the separation and transport of photogenerated carriers, and significantly improve the photocatalytic hydrogen production activity.
[0017] (3) This invention solves the drawbacks of narrow visible light response range and low crystallinity of carbon nitride, and can maximize the use of sunlight to achieve high visible light chemical decomposition of water to produce hydrogen, thus realizing the efficient use of sunlight. Attached Figure Description
[0018] Figure 1 The X-ray diffraction patterns of the red crystalline carbon nitride prepared in Comparative Example 1 and Examples 1-4 are shown, where the horizontal axis 2θ is the diffraction angle (degree) and the vertical axis Intensity is the intensity (au).
[0019] Figure 2 The X-ray diffraction patterns of the red crystalline carbon nitride prepared in Comparative Example 2 and Examples 5-6 are shown, where the horizontal axis 2θ is the diffraction angle (degree) and the vertical axis Intensity is the intensity (au).
[0020] Figure 3 The UV-Vis diffuse reflectance spectra of the red crystalline carbon nitride prepared in Comparative Example 1 and Examples 1-4 are shown, where the horizontal axis represents wavelength (nm) and the vertical axis represents intensity (au).
[0021] Figure 4 The UV-Vis diffuse reflectance spectra of the red crystalline carbon nitride prepared in Comparative Examples 1, 2 and 5-6 are shown, where the horizontal axis represents wavelength (nm) and the vertical axis represents intensity (au).
[0022] Figure 5 The graph shows the photocatalytic hydrogen production performance of the red crystalline carbon nitride prepared in Comparative Example 1 and Examples 1-4 under light irradiation with a wavelength greater than 510 nm. The horizontal axis, H2 Production, represents the hydrogen production rate (mmol·g). -1 ·h -1 The vertical axis represents each sample.
[0023] Figure 6 The graph shows the photocatalytic hydrogen production performance of the red crystalline carbon nitride prepared in Comparative Examples 1-2 and Examples 1-6 under light irradiation with a wavelength greater than 420 nm. The horizontal axis, H2 Production, represents the hydrogen production rate (mmol·g). -1 ·h -1 The vertical axis represents each sample. Detailed Implementation
[0024] To facilitate understanding of the present invention, a more comprehensive description will be given below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a thorough and complete understanding of the disclosure of the present invention.
[0025] Example 1:
[0026] A method for preparing red crystalline carbon nitride, the specific steps of which are as follows:
[0027] (1) First, weigh out an excess of potassium thiocyanate and dry it in a vacuum drying oven at 140°C for 2 hours.
[0028] (2) Weigh 3g of melamine, 2g of potassium thiocyanate dried in step (1) and 0.546g of ammonium chloride and grind them in an agate mortar until they are evenly mixed.
[0029] (3) Place the sample from step (2) in a ceramic boat, wrap it with aluminum foil, and place it in a tube furnace. Under the protection of an argon atmosphere with a flow rate of 20 mL / min, heat it to 400℃ at a rate of 10℃ / min and hold it for 1 hour. Then continue to heat it to 550℃ at a rate of 10℃ / min and hold it for 2 hours. Cool it to room temperature with the furnace.
[0030] (4) The sample from step (3) is thoroughly washed with deionized water to remove the remaining metal salts and then dried in an oven at 60°C.
[0031] Example 2:
[0032] A method for preparing red crystalline carbon nitride, the specific steps of which are as follows:
[0033] (1) First, weigh out an excess of potassium thiocyanate and dry it in a vacuum drying oven at 140°C for 2 hours.
[0034] (2) Weigh 3g of melamine, 2g of potassium thiocyanate dried in step (1) and 0.546g of ammonium chloride and grind them in an agate mortar until they are evenly mixed.
[0035] (3) Place the sample from step (2) in a ceramic boat, wrap it with aluminum foil, and place it in a tube furnace. Under the protection of an argon atmosphere with a flow rate of 20 mL / min, heat it to 400°C at a rate of 10°C / min and hold it for 1 hour. Then continue to heat it to 575°C at a rate of 10°C / min and hold it for 2 hours. Cool it to room temperature with the furnace.
[0036] (4) The sample from step (3) is thoroughly washed with deionized water to remove the remaining metal salts and then dried in an oven at 60°C.
[0037] Example 3:
[0038] A method for preparing red crystalline carbon nitride, the specific steps of which are as follows:
[0039] (1) First, weigh out an excess of potassium thiocyanate and dry it in a vacuum drying oven at 140°C for 2 hours.
[0040] (2) Weigh 3g of melamine, 2g of potassium thiocyanate dried in step (1) and 0.546g of ammonium chloride and grind them in an agate mortar until they are evenly mixed.
[0041] (3) Place the sample from step (2) in a ceramic boat, wrap it with aluminum foil, and place it in a tube furnace. Under the protection of an argon atmosphere with a flow rate of 20 mL / min, heat it to 400℃ at a rate of 10℃ / min and hold it for 1 hour. Then continue to heat it to 600℃ at a rate of 10℃ / min and hold it for 2 hours. Cool it to room temperature with the furnace.
[0042] (4) The sample from step (3) is thoroughly washed with deionized water to remove the remaining metal salts and then dried in an oven at 60°C.
[0043] Example 4:
[0044] A method for preparing red crystalline carbon nitride, the specific steps of which are as follows:
[0045] (1) First, weigh out an excess of potassium thiocyanate and dry it in a vacuum drying oven at 140°C for 2 hours.
[0046] (2) Weigh 3g of melamine, 2g of potassium thiocyanate dried in step (1) and 0.546g of ammonium chloride and grind them in an agate mortar until they are evenly mixed.
[0047] (3) Place the sample from step (2) in a ceramic boat, wrap it with aluminum foil, and place it in a tube furnace. Under the protection of an argon atmosphere with a flow rate of 20 mL / min, heat it to 400℃ at a rate of 10℃ / min and hold it for 1 hour. Then continue to heat it to 610℃ at a rate of 10℃ / min and hold it for 2 hours. Cool it to room temperature with the furnace.
[0048] (4) The sample from step (3) is thoroughly washed with deionized water to remove the remaining metal salts and then dried in an oven at 60°C.
[0049] Example 5:
[0050] A method for preparing red crystalline carbon nitride, the specific steps of which are as follows:
[0051] (1) First, weigh out an excess of potassium thiocyanate and dry it in a vacuum drying oven at 140°C for 2 hours.
[0052] (2) Weigh 2g of melamine, 2g of potassium thiocyanate dried in step (1) and 0.27g of ammonium chloride and grind them evenly in an agate mortar.
[0053] (3) Place the sample from step (2) in a ceramic boat, wrap it with aluminum foil, and place it in a tube furnace. Under the protection of an argon atmosphere with a flow rate of 20 mL / min, heat it to 400°C at a rate of 10°C / min and hold it for 1 hour. Then continue to heat it to 500°C at a rate of 10°C / min and hold it for 1 hour. Cool it to room temperature with the furnace.
[0054] (4) The sample from step (3) is thoroughly washed with deionized water to remove the remaining metal salts and then dried in an oven at 60°C.
[0055] Example 6:
[0056] A method for preparing red crystalline carbon nitride, the specific steps of which are as follows:
[0057] (1) First, weigh out an excess of potassium thiocyanate and dry it in a vacuum drying oven at 140°C for 2 hours.
[0058] (2) Weigh 2g of melamine, 2g of potassium thiocyanate dried in step (1) and 0.55g of ammonium chloride and grind them in an agate mortar until they are evenly mixed.
[0059] (3) Place the sample from step (2) in a ceramic boat, wrap it with aluminum foil, and place it in a tube furnace. Under the protection of an argon atmosphere with a flow rate of 20 mL / min, heat it to 400°C at a rate of 10°C / min and hold it for 1 hour. Then continue to heat it to 500°C at a rate of 10°C / min and hold it for 1 hour. Cool it to room temperature with the furnace.
[0060] (4) The sample from step (3) is thoroughly washed with deionized water to remove the remaining metal salts and then dried in an oven at 60°C.
[0061] Comparative Example 1:
[0062] A method for preparing red crystalline carbon nitride, the specific steps of which are as follows:
[0063] (1) Weigh 3g of melamine, place it in a porcelain boat, and wrap it with aluminum foil.
[0064] (2) Place the ceramic boat from step (1) into a tube furnace, and heat it to 400°C at a rate of 10°C / min under an argon atmosphere with a flow rate of 20 mL / min and hold for 1 hour. Then continue heating it to 600°C at a rate of 10°C / min and hold for 1 hour. Then cool it to room temperature with the furnace.
[0065] (3) Grind the sample from step (2) into powder in an agate mortar.
[0066] Comparative Example 2:
[0067] A method for preparing red crystalline carbon nitride, the specific steps of which are as follows:
[0068] (1) First, weigh out an excess of potassium thiocyanate and dry it in a vacuum drying oven at 140°C for 2 hours.
[0069] (2) Weigh 2g of melamine and 2g of potassium thiocyanate dried in step (1) and grind them in an agate mortar until they are evenly mixed.
[0070] (3) Place the sample from step (2) in a ceramic boat, wrap it with aluminum foil, and place it in a tube furnace. Under the protection of an argon atmosphere with a flow rate of 20 mL / min, heat it to 400°C at a rate of 10°C / min and hold it for 1 hour. Then continue to heat it to 500°C at a rate of 10°C / min and hold it for 1 hour. Cool it to room temperature with the furnace.
[0071] (4) The sample from step (3) is thoroughly washed with deionized water to remove the remaining metal salts and then dried in an oven at 60°C.
[0072] Structural characterization:
[0073] Figure 1The X-ray diffraction patterns of Comparative Example 1 and Examples 1-4 are shown. Comparative Example 1 has two typical diffraction peaks at 12.7° and 27.7°, which represent the repeating heptaazine unit (100) crystal plane in the carbon nitride plane and the interlayer stacked (002) crystal plane of the conjugated aromatic system, respectively. In Examples 1-4, the diffraction peak of the (100) crystal plane shifts to the left by 8°, which means that the heptaazine skeleton in the plane is more complete. The diffraction peak of the (002) crystal plane shifts to the right by 28.2°, which corresponds to the interlayer spacing being reduced to 3.16 nm, indicating that the method successfully synthesized crystalline carbon nitride.
[0074] Figure 2 The X-ray diffraction patterns of Comparative Example 2 and Examples 5-6 are shown. The diffraction patterns of the three samples are similar, all showing a crystalline carbon nitride structure. As can be seen from the figure, compared with Comparative Example 2, the intensity of the diffraction peaks on the (100) and (002) crystal planes of Examples 5 and 6 is significantly increased, indicating that the crystalline carbon nitride synthesized by this method has a higher degree of crystallinity.
[0075] Figure 3 The images show the UV-Vis diffuse reflectance spectra of Comparative Example 1 and Examples 1-4. The absorption edge of Comparative Example 1 is 464 nm, while the absorption edges of Examples 1-4 all show a significant red shift, corresponding to sp... 2 The intrinsic π→π* electron transitions of hybrid C and N, and the emergence of a prominent new absorption band between 449 and 800 m, are due to the n→π* electron transitions of lone pairs of electrons in the edge N atoms of the heptaazine framework. This significantly increases the photoresponse range of Examples 1 to 4.
[0076] Figure 4 The UV-Vis diffuse reflectance spectra of Comparative Examples 1-2 and Examples 5-6 are shown. Compared with Comparative Example 1, the absorption edges of Examples 5-6 and the Comparative Examples are significantly red-shifted, and a prominent new absorption band appears near 500 nm. This is due to the n→π* electronic transition of lone pair electrons in the edge N atoms of the heptaazine framework, which significantly increases the light response range of Examples 5-6.
[0077] Photocatalysis test:
[0078] The photocatalytic performance of the photocatalyst was evaluated using water splitting for hydrogen production as an example. First, 100 mg of the catalyst was dispersed in a quartz reactor containing 90 mL of deionized water and sonicated for 10 min. Then, 10 mL of triethanolamine was added as a sacrificial agent, followed by the addition of a chloroplatinic acid aqueous solution and a xenon lamp irradiation system to support 3.0 wt% Pt nanoparticles as a co-catalyst. An offline hydrogen production system was used, irradiated with a 300 W xenon lamp equipped with a UVCUT-420 nm or UVCUT-510 nm filter. 1 mL of gas was extracted every 1 h and injected into a gas chromatograph equipped with a thermal conductivity detector to determine the hydrogen content. The hourly hydrogen production rate was calculated based on a hydrogen standard curve. Figure 5 The graphs show the photocatalytic hydrogen production performance of Comparative Example 1 and Examples 1-4 under visible light irradiation with a wavelength greater than 510 nm. It can be seen that the photocatalytic hydrogen production rates of Examples 1-4 are all improved to varying degrees, with the photocatalytic hydrogen production rate of Example 3 being 7.1 times that of Comparative Example 1. Figure 6 The photocatalytic activities of Comparative Examples 1-2 and Examples 1-6 under visible light irradiation with wavelengths greater than 420 nm were compared. The photocatalytic hydrogen production activities of Examples 1-6 were all higher than those of Comparative Examples 1 and 2. Among them, the photocatalytic activity of Example 6 was the highest, which was 12.2 times that of Comparative Example 1.
[0079] The results of the examples show that the present invention synthesizes red crystalline carbon nitride using the molten salt method. The synthesized crystalline carbon nitride has higher crystallinity and a wider visible light absorption range, which solves the drawback of low visible light utilization of carbon nitride, promotes the separation and transport of photogenerated carriers, and has better photocatalytic hydrogen production activity.
[0080] The above description is only for better explaining the embodiments of the present invention and is not intended to limit them. Any modifications or equivalent substitutions that do not depart from the spirit and scope of the present invention shall fall within the scope of the present invention.
Claims
1. A method for preparing red crystalline carbon nitride, characterized in that, The process includes the following steps: melamine, a nitrogen-rich precursor, is mixed evenly with molten potassium thiocyanate and ammonium chloride, and then subjected to a thermal polycondensation reaction. After washing and drying, red crystalline carbon nitride is obtained. The conditions for the thermal polycondensation reaction are as follows: under an argon atmosphere, the temperature is raised to 400°C and held for 1 hour, and then the temperature is raised to 500~610°C and held for 1~2 hours. The molar ratio of potassium thiocyanate to ammonium chloride is (4~2):1; The mass ratio of melamine to potassium thiocyanate is (2~3):
2.
2. The method for preparing red crystalline carbon nitride according to claim 1, characterized in that, The potassium thiocyanate was pre-dried in a vacuum drying oven at 140°C for 2 hours.
3. The method for preparing red crystalline carbon nitride according to claim 1, characterized in that, The thermal polycondensation reaction was carried out in a tube furnace. The sample was placed in a ceramic boat and wrapped with aluminum foil. Under an argon atmosphere with a flow rate of 20 mL / min, it was heated to 400°C at a rate of 10°C / min and held for 1 hour. Then, it was heated to 500–610°C at a rate of 10°C / min and held for 1–2 hours. The sample was then cooled to room temperature in the furnace.
4. The method for preparing red crystalline carbon nitride according to claim 1, characterized in that, The drying temperature is 60°C.