A multi-layered bi-phase graphite oxide nanoplatelet and a method of preparing the same
By controlling the reaction conditions, multilayer biphase graphite oxide was prepared, solving the problem of graphite's difficulty in dispersing in water and organic solvents. Stable dispersion and performance retention were achieved, providing a simple and low-cost solution.
Patent Information
- Application Number
- CN202411227229.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-09-03
AI Technical Summary
Graphite is difficult to disperse uniformly in water and organic solvents, which affects its use and application in many research fields.
By controlling the reaction temperature, time, and stirring speed, multilayer biphase graphite oxide was prepared, retaining the crystal structure of graphite and generating random and amorphous folded structures on the surface of the sheets, containing oxygen-containing groups such as hydroxyl and carboxyl groups, which enabled it to be stably dispersed in water and organic solvents.
Stable dispersion of graphite in water and organic solvents was achieved while retaining the excellent physical properties of graphite. The preparation method is simple, low-cost and highly efficient.
Smart Images

Figure CN119100383B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of graphene material preparation, specifically to a method for preparing multilayer biphase graphene oxide. Background Technology
[0002] Graphite is an allotrope of carbon, renowned for its layered structure and excellent electrical and thermal conductivity. Widely found in nature, graphite is commonly used as a lubricant, pencil lead, and battery electrode material. Furthermore, its unique physical properties make it important in high-tech fields. However, due to the lack of hydrophilic and oleophilic groups on its surface, graphite is difficult to disperse uniformly in water and organic solvents, significantly hindering its use and application in many research areas.
[0003] Graphene is a carbonaceous material with a two-dimensional periodic honeycomb lattice structure composed of six-membered carbon rings, typically existing in three states: zero-dimensional fullerenes, one-dimensional carbon nanotubes (CNTs), and three-dimensional graphite. Since its discovery in 2004, graphene has been the subject of extensive research. Monolithic graphene possesses the highest known tensile strength (130 GPa), the highest Young's modulus (1 TPa), and the highest carrier mobility (15000 cm⁻¹). 2 ·V -1 ·S -1 And the fastest heat transfer and conduction speed (thermal conductivity 5000 W·m) -1 ·K -1 ).
[0004] Graphene oxide is obtained by mechanical exfoliation after graphite is oxidized in a strong acid medium by a strong oxidizing agent. It is an important derivative of graphene and can also be considered an intermediate product in the process of preparing graphene from graphite via redox reactions. Unlike graphene, graphene oxide contains oxygen-containing functional groups in addition to carbon atoms, such as hydroxyl, carboxyl, epoxy, and carbonyl groups. The simultaneous presence of oxygen-containing functional groups and conjugated structures allows graphene oxide to form stable and homogeneous dispersions in water and some polar organic solvents. Due to the influence of the preparation process, graphene oxide contains some pores and defects on its surface, which causes its mechanical properties, thermal conductivity, and electrical conductivity to be much lower than the theoretical calculation values of graphene. Summary of the Invention
[0005] This invention provides a novel two-dimensional carbon material that can be uniformly dispersed in water and organic solvents while retaining the original crystalline structure and excellent physical properties of graphite, namely multilayer two-phase graphite oxide and its preparation method.
[0006] By controlling the reaction temperature and reaction time, this invention allows the middle region of the biphase graphite oxide to retain the complete crystalline structure of graphite, while generating random and amorphous folded structures on the surface of the sheets, containing oxygen-containing groups such as hydroxyl and carboxyl groups. This enables the multilayer biphase graphite oxide to be stably dispersed in water and organic solvents.
[0007] The embodiments of the present invention provide the following preparation method: 1) Slowly add 1 part of graphite powder to 50 ml-200 ml of concentrated sulfuric acid. The size of the graphite powder is 200 mesh-500 mesh. The reaction temperature is controlled at -30℃~5℃, the reaction time is controlled at 3 h-6 h, and the stirring speed is controlled at 100 r-500 r / min. 2) Slowly add a number of parts of potassium permanganate powder to the solution that has reacted in step 1). The mass ratio of graphite to potassium permanganate is 1:1 to 1:6. The reaction temperature is controlled at -30℃ to 5℃, the reaction time is controlled at 3 h to 6 h, and the stirring speed is controlled at 100 r to 500 r / min. 3) Slowly add 60 ml to 200 ml of dilute sulfuric acid solution with a mass fraction of 10% to 30% to the solution that has reacted in step 2). The addition rate is 10 ml to 60 ml / h, the reaction temperature is controlled at -10℃ to 5℃, the reaction time is controlled at 1 h to 20 h, and the stirring speed is controlled at 100 r to 500 r / min. 4) Slowly add 150 ml-300 ml of deionized water dropwise to the solution that has reacted in step 3), at a rate of 10 ml-50 ml / h, while controlling the reaction temperature at -10℃ to 5℃, the reaction time at 3 h-30 h, and the stirring speed at 100 r-500 r / min. 5) Slowly add the solution obtained in step 4) to a 1500ml-2500ml ice-water mixing bath while stirring, and control the reaction temperature at 0℃; 6) Slowly add 5 g-20 g of hydrogen peroxide solution to the solution obtained in step 5) while stirring. Control the reaction temperature at 0℃-5℃, the stirring speed at 100 r-300 r / min, and the stirring time at 20 min-40 min to remove excess potassium permanganate that has not participated in the reaction until no more bubbles are generated. 7) Slowly add a 1%-10% dilute hydrochloric acid solution to the solution obtained in step 6), while stirring. Control the reaction temperature at 0℃-5℃, the stirring speed at 100 r-300 r / min, and the stirring time at 5 min-20 min. The mass ratio of potassium permanganate to hydrochloric acid is (2~10):1. 8) Seal and let the solution obtained in step 7) stand at a temperature of 2℃-10℃ for 3-10 days. 9) Discard the supernatant, wash repeatedly with water by centrifugation until the solution pH is above 5, and collect the centrifuged product; centrifuge at 5000-8000 rpm for 30 minutes; 10) The multilayer biphase graphene oxide solution obtained in 9) is placed at 3℃-10℃ and allowed to stand for subsequent material preparation.
[0008] The beneficial effects of this invention are as follows: (1) Through the two-phase design of graphite structure, it can be stably dispersed in water and organic solvents, while retaining the original crystal structure and excellent physical properties of graphite.
[0009] (2) The preparation method provided by the present invention is simple, low-cost, short-cycle and highly efficient. Attached Figure Description
[0010] Figure 1 This is a scanning electron microscope image of the biphase graphene oxide nanosheets from Example 1; Figure 2 It is the aqueous dispersion of biphase graphene oxide nanosheets from Example 1; Figure 3 This is the XRD pattern of the aqueous dispersion of biphase graphene oxide nanosheets in Example 1; Figure 4 These are Raman spectra of the biphase graphite sheet from Example 1 and the middle region of the graphite sheet after the surface layer has been removed; Figure 5 This is the aqueous dispersion of biphase graphene oxide nanosheets from Example 2; Figure 6 This is the XRD pattern of the aqueous dispersion of biphase graphene oxide nanosheets in Example 2; Figure 7 This is the aqueous dispersion of biphase graphene oxide nanosheets from Example 3; Figure 8 This is the XRD pattern of the aqueous dispersion of biphase graphene oxide nanosheets in Example 3; Figure 9 This is the aqueous dispersion of biphase graphene oxide nanosheets from Example 4; Figure 10 This is the XRD pattern of the aqueous dispersion of biphase graphene oxide nanosheets in Example 4; Figure 11 This is the aqueous dispersion of biphase graphene oxide nanosheets from Example 5; Figure 12 This is the XRD pattern of the aqueous dispersion of biphase graphene oxide nanosheets in Example 5. Detailed Implementation
[0011] Unless otherwise specified, the raw materials used in this invention are all conventional commercially available products. For example, the concentrated sulfuric acid is commercially available 98% concentrated sulfuric acid; the hydrogen peroxide has a mass fraction of 30%. Unless otherwise specified, the methods used in this invention are conventional methods in the art.
[0012] The embodiments of the present invention will be further described below with reference to several examples.
[0013] It should be understood that the described embodiments are merely some, not all, of the embodiments in this application. All other embodiments obtained by those skilled in the art based on the embodiments in this application without inventive effort are within the scope of protection of this application.
[0014] The terminology used in the embodiments of this application is for the purpose of describing particular embodiments only and is not intended to be limiting of this application. The singular forms “a,” “the,” and “the” used in the embodiments of this application and the appended claims are also intended to include the plural forms unless the context clearly indicates otherwise. Example
[0015] 1) Slowly add 3g of graphite powder to 50ml of concentrated sulfuric acid. The size of the graphite powder is 200 mesh. The reaction temperature is controlled at -5℃, the reaction time is controlled at 3h, and the stirring speed is controlled at 100r / min. 2) Slowly add potassium permanganate powder to the solution that has reacted in step 1), with the mass ratio of graphite to potassium permanganate being 1:6, the reaction temperature being controlled at -5℃, the reaction time being controlled at 3 h, and the stirring speed being controlled at 100 r / min. 3) Slowly add 60 ml of 10% sulfuric acid solution to the solution that has reacted in step 2), at a rate of 10 ml / h, while controlling the reaction temperature at -5℃, the reaction time at 6 h, and the stirring speed at 100 r / min. 4) Slowly add 150 ml of deionized water dropwise to the solution that has reacted in step 3), at a rate of 10 ml / h, while controlling the reaction temperature at -5℃, the reaction time at 15 h, and the stirring speed at 100 r / min. 5) Slowly add the solution obtained in step 4) to a 1500ml ice-water mixing bath while stirring, and control the reaction temperature at 0℃; 6) Slowly add 5g of hydrogen peroxide solution to the solution obtained in step 5) while stirring. The reaction temperature is controlled at 0℃, the stirring speed is controlled at 100 r / min, and the stirring time is 20 min. 7) Slowly add 180g of a 1% dilute hydrochloric acid solution to the solution obtained in step 6), while stirring. The reaction temperature is controlled at 0℃, the stirring speed is controlled at 100 r / min, and the stirring time is 5 min. 8) Seal and let the solution obtained in step 7) stand at 2°C for 3 days; 9) Discard the supernatant, wash repeatedly with water by centrifugation until the solution pH is above 5, centrifuge at 5000 r / min for 30 min; 10) The multilayer biphase graphene oxide solution obtained in 9) was placed at 3°C and allowed to stand for subsequent material preparation.
[0016] 11) The thickness of the multilayer biphase graphene oxide nanosheets prepared in the experiment was 5-7 nm, such as Figure 2 As shown, its aqueous dispersion is uniform and stable.
[0017] according to Figure 3 The XRD pattern of this embodiment shows two characteristic peaks at 2Ɵ=9.96° and 2Ɵ=21.17°, corresponding to graphite interlayer spacings of 0.89 nm and 0.42 nm, respectively, which are close to the interlayer spacing of graphene oxide and graphite. This indicates that the biphase film contains two graphite structures with different degrees of oxidation.
[0018] Figure 4 The Raman spectra of the biphase graphite sheet and the central region of the graphite sheet after the surface layer has been removed are shown in this embodiment. Black represents the Raman spectrum of the biphase graphite sheet; the appearance of the 2D peak proves the presence of a graphite crystal structure within the graphite sheet. Red represents the Raman spectrum of the central region of the graphite sheet after the amorphous surface layer has been removed; after removing the surface layer, the G peak and 2D peak are significantly enhanced, proving that the central region of the biphase graphite sheet has an ordered graphite crystal structure. Therefore, the preparation method provided by this invention can successfully prepare multilayer biphase graphite oxide with an outer layer of graphene oxide and an inner layer of graphite. Example
[0019] 1) Slowly add 3g of graphite powder to 50ml of concentrated sulfuric acid. The size of the graphite powder is 200 mesh. The reaction temperature is controlled at -30℃, the reaction time is controlled at 3h, and the stirring speed is controlled at 100r / min. 2) Slowly add potassium permanganate powder to the solution that has reacted in step 1), with the mass ratio of graphite to potassium permanganate being 1:1, the reaction temperature being controlled at -30℃, the reaction time being controlled at 3 h, and the stirring speed being controlled at 100 r / min. 3) Slowly add 60 ml of 10% sulfuric acid solution to the solution that has reacted in step 2), at a rate of 60 ml / h, while controlling the reaction temperature at -10℃, the reaction time at 1 h, and the stirring speed at 100 r / min. 4) Slowly add 150 ml of deionized water dropwise to the solution that has reacted in step 3), at a rate of 10 ml / h, while controlling the reaction temperature at -10℃, the reaction time at 15 h, and the stirring speed at 100 r / min. 5) Slowly add the solution obtained in step 4) to a 1500ml ice-water mixing bath while stirring, and control the reaction temperature at 0℃; 6) Slowly add 5g of hydrogen peroxide solution to the solution obtained in step 5) while stirring. The reaction temperature is controlled at 0℃, the stirring speed is controlled at 100 r / min, and the stirring time is 20 min. 7) Slowly add 50g of 1% dilute hydrochloric acid solution dropwise to the solution obtained in step 6), while stirring. The reaction temperature is controlled at 0℃, the stirring speed is controlled at 100 r / min, and the stirring time is 5 min. 8) Seal and let the solution obtained in step 7) stand at 2°C for 3 days; 9) Discard the supernatant, wash repeatedly with water by centrifugation until the solution pH is above 5, centrifuge at 5000 r / min for 30 min; 10) The multilayer biphase graphene oxide solution obtained in 9) was placed at 3°C and allowed to stand for subsequent material preparation.
[0020] 11) The multilayer biphase graphene oxide nanosheets prepared in the experiment had a thickness of 40-50 nm and exhibited the following characteristics: Figure 5 The solution shown is homogeneous and stable.
[0021] like Figure 6 The XRD pattern of this embodiment shows two characteristic peaks at 2Ɵ=10.59° and 2Ɵ=21.53°, corresponding to graphite interlayer spacings of 0.86 nm and 0.41 nm, respectively, which are close to the interlayer spacing of graphene oxide and graphite. This indicates that the biphase film contains two graphite structures with different degrees of oxidation. Example
[0022] 1) Slowly add 3g of graphite powder to 200ml of concentrated sulfuric acid. The size of the graphite powder is 200 mesh. The reaction temperature is controlled at -30℃, the reaction time is controlled at 6 h, and the stirring speed is controlled at 500r / min. 2) Slowly add potassium permanganate powder to the solution that has reacted in step 1), with the mass ratio of graphite to potassium permanganate being 1:6, the reaction temperature being controlled at -30℃, the reaction time being controlled at 6 h, and the stirring speed being controlled at 500 r / min. 3) Slowly add 60 ml of 30% sulfuric acid solution to the solution that has reacted in step 2), at a rate of 30 ml / h, while controlling the reaction temperature at -10℃, the reaction time at 2 h, and the stirring speed at 500 r / min. 4) Slowly add 150 ml of deionized water dropwise to the solution that has reacted in step 3), at a rate of 30 ml / h, while controlling the reaction temperature at -10℃, the reaction time at 5 h, and the stirring speed at 500 r / min. 5) Slowly add the solution obtained in step 4) to a 2500ml ice-water mixing bath while stirring, and control the reaction temperature at 0℃; 6) Slowly add 20 g of hydrogen peroxide solution to the solution obtained in step 5) while stirring. The reaction temperature is controlled at 0℃, the stirring speed is controlled at 100 r / min, and the stirring time is 20 min. 7) Slowly add 100 g of 5% dilute hydrochloric acid solution dropwise to the solution obtained in step 6), while stirring. The reaction temperature is controlled at 0℃, the stirring speed is controlled at 300 r / min, and the stirring time is 5 min. 8) Seal and let the solution obtained in step 7) stand at 2°C for 10 days; 9) Discard the supernatant, wash repeatedly with water by centrifugation until the solution pH is above 5, centrifuge at 8000 r / min for 30 min; 10) The multilayer biphase graphene oxide solution obtained in 9) was placed at 3°C and allowed to stand for subsequent material preparation.
[0023] 11) The multilayer biphase graphene oxide nanosheets prepared in the experiment had a thickness of 20-30 nm and exhibited the following characteristics: Figure 7 The solution shown is homogeneous and stable.
[0024] like Figure 8 The XRD pattern of this embodiment shows two characteristic peaks at 2Ɵ=9.84° and 2Ɵ=20.12°, corresponding to graphite interlayer spacings of 0.9 nm and 0.44 nm, respectively, which are close to the interlayer spacing of graphene oxide and graphite. This indicates that the biphase film contains two graphite structures with different degrees of oxidation. Example
[0025] 1) Slowly add 3g of graphite powder to 200ml of concentrated sulfuric acid. The size of the graphite powder is 500 mesh. The reaction temperature is controlled at 5℃, the reaction time is controlled at 3h, and the stirring speed is controlled at 500r / min. 2) Slowly add potassium permanganate powder to the solution that has reacted in step 1), with the mass ratio of graphite to potassium permanganate being 1:6, the reaction temperature being controlled at 5℃, the reaction time being controlled at 3 h, and the stirring speed being controlled at 500 r / min. 3) Slowly add 200 ml of 10% sulfuric acid solution to the solution that has reacted in step 2), at a rate of 10 ml / h, while controlling the reaction temperature at 5℃, the reaction time at 20 h, and the stirring speed at 100 r / min. 4) Slowly add 300 ml of deionized water dropwise to the solution that has reacted in step 3), at a rate of 10 ml / h, while controlling the reaction temperature at 5℃, the reaction time at 30 h, and the stirring speed at 100 r / min. 5) Slowly add the solution obtained in step 4) to a 1500ml ice-water mixing bath while stirring, and control the reaction temperature at 0℃; 6) Slowly add 5g of hydrogen peroxide solution to the solution obtained in step 5) while stirring. The reaction temperature is controlled at 0℃, the stirring speed is controlled at 100 r / min, and the stirring time is 20 min. 7) Slowly add 50g of 1% dilute hydrochloric acid solution dropwise to the solution obtained in step 6), while stirring. The reaction temperature is controlled at 5℃, the stirring speed is controlled at 100 r / min, and the stirring time is 20 min. 8) Seal and let the solution obtained in step 7) stand at 10°C for 10 days; 9) Discard the supernatant, repeatedly wash with water by centrifugation until the solution pH is above 5, centrifuge at 5000 r / min for 5 h; 10) The multilayer biphase graphene oxide solution obtained in 9) was placed at 8°C and allowed to stand for subsequent material preparation, exhibiting the following appearance. Figure 9 The solution shown is homogeneous and stable.
[0026] like Figure 10 The XRD pattern of this embodiment shows two characteristic peaks at 2Ɵ=10.11° and 2Ɵ=20.58°, corresponding to graphite interlayer spacings of 0.88 nm and 0.43 nm, respectively, which are close to the interlayer spacing of graphene oxide and graphite. This indicates that the biphase film contains two graphite structures with different degrees of oxidation. Example
[0027] 1) Slowly add 3g of graphite powder to 200ml of concentrated sulfuric acid. The size of the graphite powder is 200 mesh. The reaction temperature is controlled at -20℃, the reaction time is controlled at 4h, and the stirring speed is controlled at 500r / min. 2) Slowly add potassium permanganate powder to the solution that has reacted in step 1), with the mass ratio of graphite to potassium permanganate being 1:5, the reaction temperature being controlled at -20℃, the reaction time being controlled at 4 h, and the stirring speed being controlled at 500 r / min. 3) Slowly add 150 ml of dilute sulfuric acid solution with a mass fraction of 10%-30% to the solution that has reacted in step 2), at a dropping rate of 50 ml / h, while controlling the reaction temperature at -10℃, the reaction time at 3 h, and the stirring speed at 500 r / min. 4) Slowly add 300 ml of deionized water dropwise to the solution that has reacted in step 3), at a rate of 50 ml / h, while controlling the reaction temperature at -10℃, the reaction time at 3 h, and the stirring speed at 500 r / min. 5) Slowly add the solution obtained in step 4) to a 2000ml ice-water mixing bath while stirring, and control the reaction temperature at 0℃; 6) Slowly add 20 g of hydrogen peroxide solution to the solution obtained in step 5) while stirring. The reaction temperature is controlled at 5℃, the stirring speed is controlled at 300 r / min, and the stirring time is 40 min. 7) Slowly add 50g of 10% dilute hydrochloric acid solution dropwise to the solution obtained in step 6), while stirring. The reaction temperature is controlled at 2℃, the stirring speed is controlled at 200 r / min, and the stirring time is 20 min. 8) Seal and let the solution obtained in step 7) stand at 2°C for 3 days; 9) Discard the supernatant, wash repeatedly with water by centrifugation until the solution pH is above 5, centrifuge at 8000 r / min for 30 min; 10) The multilayer biphase graphene oxide solution obtained in 9) was placed at 10°C and allowed to stand for subsequent material preparation, exhibiting the following appearance: Figure 11 The solution shown is homogeneous and stable.
[0028] like Figure 12 The XRD pattern of this embodiment shows two characteristic peaks at 2Ɵ=10.25° and 2Ɵ=22.15°, corresponding to graphite interlayer spacings of 0.86 nm and 0.4 nm, respectively, which are close to the interlayer spacing of graphene oxide and graphite. This indicates that the biphase film contains two graphite structures with different degrees of oxidation.
[0029] The above embodiments describe in detail the structure, features, and effects of the present invention. The above description is only a preferred embodiment of the present invention. Any changes made in accordance with the concept of the present invention, or equivalent embodiments modified to have equivalent changes, shall still fall within the scope of protection of the present invention if they do not exceed the scope covered by the specification.
[0030] Although embodiments of the invention have been disclosed for illustrative purposes, those skilled in the art will understand that various substitutions, variations, and modifications are possible without departing from the spirit and scope of the invention and the appended claims. Therefore, the scope of the invention is not limited to the contents disclosed in the embodiments.
Claims
1. A method for preparing multilayer biphase graphene oxide nanosheets, characterized in that, Includes the following steps: 1) Add graphite powder to 50 ml-200 ml of concentrated sulfuric acid. The size of the graphite powder is 200 mesh-500 mesh. Control the reaction temperature and reaction time, and control the stirring speed at 100 r-500 r / min. 2) Add potassium permanganate powder, control the reaction temperature and reaction time, and control the stirring speed at 100r-500r / min; 3) Add 60 ml to 200 ml of dilute sulfuric acid solution at a rate of 10 ml to 60 ml / h, control the reaction temperature at -10℃ to 5℃, control the reaction time at 1 h to 20 h, and control the stirring speed at 100 r to 500 r / min. 4) Add 150 ml-300 ml of deionized water dropwise at a rate of 10 ml-50 ml / h, control the reaction temperature at -10℃ to 5℃, control the reaction time at 3 h-30 h, and control the stirring speed at 100 r-500 r / min. 5) Add the solution obtained in step 4) to a 1500 ml-2500 ml ice-water mixing bath while stirring, and control the reaction temperature at 0℃. 6) Add hydrogen peroxide solution dropwise to remove excess potassium permanganate that has not participated in the reaction until no more bubbles are produced; 7) Add dilute hydrochloric acid solution dropwise while stirring. Control the reaction temperature at 0℃-5℃, the stirring speed at 100 r-300 r / min, and the stirring time at 5 min-20 min. The mass ratio of potassium permanganate to hydrochloric acid is 2:1-10:
1. 8) Seal and let the solution obtained in step 7) stand at a temperature of 2℃-10℃ for 3-10 days. 9) Discard the supernatant, and repeatedly centrifuge and wash at a speed of 5000-8000 r / min until the pH value of the solution is above 5; collect the centrifuged product, which is a multilayer biphase graphene oxide nanosheet; The surface layer of the multilayer biphase graphene oxide nanosheet is a graphene oxide structure, exhibiting a random and amorphous folded structure, while the middle region of the graphite sheet after the surface layer is peeled off is a graphite crystal phase structure.
2. The preparation method according to claim 1, characterized in that, The mass ratio of graphite to potassium permanganate in steps 1) and 2) is 1:1 to 1:
6.
3. The preparation method according to claim 1, characterized in that, The reaction temperature in step 1) is controlled at -30℃ to 5℃, and the reaction time is controlled at 3 h to 6 h.
4. The preparation method according to claim 1, characterized in that, The reaction temperature in step 2) is controlled at -30℃ to 5℃, and the reaction time is controlled at 3 h to 6 h.
5. The preparation method according to claim 1, characterized in that, The mass fraction of the dilute sulfuric acid mentioned in step 3) is between 10% and 30%.
6. The preparation method according to claim 1, characterized in that, The hydrogen peroxide mentioned in step 6) has a mass of 5 g-20 g.
7. The preparation method according to claim 1, characterized in that, The mass fraction of the dilute hydrochloric acid mentioned in step 7) is 1%-10%.
Citation Information
Patent Citations
Method for preparing edge graphene oxide nanosheets in batches
CN117985702A