A drawing die and processing method suitable for high-strength high-carbon steel wire
By using a foamed steel die sleeve and a polycrystalline diamond die core, the problem of decreased plasticity caused by heat accumulation during the drawing process of high carbon steel wire was solved, achieving a drawing effect with high strength and high plasticity.
Patent Information
- Application Number
- CN202411301041.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-09-18
AI Technical Summary
The heat accumulation effect during the drawing process of high carbon steel wire leads to a sharp decrease in plasticity, resulting in high wire breakage and poor forming during production.
The drawing die, which uses a foam steel mold sleeve and a polycrystalline diamond mold core, achieves rapid heat dissipation and reduces the heat accumulation effect through a porous structure and cold-fit design.
It significantly improves the plasticity and strength of high-carbon steel wire, reduces heat accumulation during the drawing process, reduces defects and microcracks in high-carbon steel wire, and improves the drawing preparation effect.
Smart Images

Figure CN119114666B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of drawing die technology, and in particular to a drawing die and processing method suitable for high-strength, high-carbon steel wire. Background Technology
[0002] High-strength, low-weight cords can reduce the amount of steel wire used while ensuring the required strength of the tire, thereby reducing tire weight and fuel consumption.
[0003] The existing drawing technology for steel cord is wet drawing, which involves high-carbon steel wire being drawn through a drawing die under a certain drawing force in the presence of lubricating or cooling fluid. This technology is widely used, typically on a water tank drawing machine with multiple dies and multiple passes. The rapid aging and sharp decline in plasticity during the high-carbon steel wire drawing process are mainly due to the heat accumulation effect and the inability to quickly cool and diffuse the accumulated heat. This heat accumulation effect becomes more pronounced with increasing carbon equivalent. In the process of drawing high-strength, finer-diameter wires, the drawing of higher-strength wires generates more heat, and existing dies are insufficient to quickly transfer this heat to the lubricating fluid, which then carries it away. This results in a sharp decline in the wire's plasticity, accompanied by rapid age hardening, leading to extremely poor wire plasticity and causing high wire breakage and poor cord formation during production. Summary of the Invention
[0004] The present invention aims to provide a drawing die and processing method suitable for high-strength, high-carbon steel wire. The die uses foam steel, which has both good heat dissipation and strength, as the die sleeve, and artificial diamond (PCD), which has good thermal conductivity and high hardness and strength, as the die core. This creates a channel for the steel wire to generate heat and dissipate heat quickly, reducing the heat accumulation effect during the drawing of high-carbon steel wire, thereby solving the problems mentioned in the background art.
[0005] To achieve the above objectives, the present invention provides the following technical solution: A drawing die suitable for high-strength, high-carbon steel wire includes a die sleeve and a die core embedded in the die sleeve; the die sleeve is made of foamed steel and has a porous foam-like appearance; the die core is made of polycrystalline diamond and has a die hole at the center, which includes four parts: an inlet area, a working area, a sizing area, and an outlet area.
[0006] A further aspect of the present invention is that the die sleeve is made of No. 45 foam steel, and the internal morphology of the die sleeve is honeycomb-shaped with a three-dimensional interconnected pore pattern. The pore diameter is 300μm to 500μm and the porosity is 25% to 45%. During the drawing process, the lubricant enters the pores and flows to cool the die sleeve.
[0007] A further aspect of the present invention is that both the mold sleeve and the mold core are cylindrical in shape, and the mold sleeve and the mold core form a cold-fit interference fit.
[0008] A further aspect of the present invention is that the mold core inlet area functions as an entry point for high-carbon steel wire and an entry point for lubricating fluid.
[0009] A further aspect of the present invention is that the working area functions to radially compress the high-carbon steel wire with a lubricating film attached to its surface, thereby deforming the high-carbon steel wire.
[0010] A further aspect of the present invention is that the sizing zone functions to further stabilize the diameter of the high-carbon steel wire after compression deformation.
[0011] A further aspect of the present invention is that the function of the outlet area is to cool the high-carbon steel wire with a stable diameter after compression deformation using the lubricating fluid within the area.
[0012] A method for processing drawing dies suitable for high-strength, high-carbon steel wire includes the following steps: Step 1: Clean and dry the un-drilled mold core. The cylindrical mold core has a diameter of 0.9 mm, a height of 0.9 mm, and a grain size of 0.5 μm. Cool it in liquid nitrogen for 1 hour. Step 2: Clean the machined mold sleeve and set it aside for use. The cylindrical mold sleeve has an outer diameter of 25mm and a height of 16mm. Step 3: Remove the un-drilled mold core cooled in liquid nitrogen, install it into the center of the mold sleeve to ensure concentricity, and fix it in place; Step 4: Preheat the un-drilled mold core to make it expand and generate a pre-tightening force against the inner wall of the mold sleeve; Step 5: Perform laser drilling on the center of the un-drilled mold core; Step 6: After drilling, the channel is machined and ground according to parameters such as the length-to-short axis ratio, entrance angle, and sizing zone length. Step 7: Polish the ground holes; Step 8: Perform parameter detection on the mold hole.
[0013] The beneficial effects of this invention are: This invention relates to a drawing die and processing method for high-strength, high-carbon steel wire. Compared with existing dies, this invention has a reasonable and simple structure, is easy to manufacture, has a long service life, and provides good cooling. The die improves heat dissipation efficiency and significantly reduces heat accumulation during the high-carbon steel wire drawing process. Furthermore, it reduces the risk of defects and microcrack propagation in the high-carbon steel wire, enabling the drawing of high-carbon steel wire with both high plasticity and high strength, while maintaining good surface quality. Attached Figure Description
[0014] Figure 1 This is an overall isometric view of the present invention.
[0015] Figure 2 for Figure 1A sectional view.
[0016] Figure 3 This is a comparison diagram of the plastic torsion performance of the conventional PCD mold and the experimental mold of the present invention in Example 1.
[0017] Figure 4 This is a comparison diagram of the plastic torsion performance of the conventional PCD mold and the experimental mold of the present invention in Example 1.
[0018] In the diagram: 1-mold sleeve, 2-mold core, 3-entry area, 4-working area, 5-sizing area, 6-exit area. Detailed Implementation
[0019] The present invention will be further explained below with reference to the accompanying drawings and specific embodiments.
[0020] like Figures 1-2 As shown, a drawing die suitable for high-strength, high-carbon steel wire includes a die sleeve 1 and a die core 2 embedded in the die sleeve 1; the die sleeve 1 is made of foam steel and has a porous foam appearance; the die core 2 is made of polycrystalline diamond and has a die hole at the center, which includes four parts: an inlet area 3, a working area 4, a sizing area 5, and an outlet area 6.
[0021] The die sleeve 1 is made of No. 45 foam steel. The internal shape of the die sleeve 1 is honeycomb-shaped, with a three-dimensional interconnected pore pattern. The pore diameter is 300μm to 500μm and the porosity is 25% to 45%. During the drawing process, the lubricant enters the pores of the die sleeve 1 and flows to cool the die sleeve 1.
[0022] Both the mold sleeve 1 and the mold core 2 are cylindrical in shape, and the mold sleeve 1 and the mold core 2 form a cold-fit interference fit.
[0023] The function of the inlet area 3 of the mold core 2 is to allow the high-carbon steel wire to enter and the lubricant to enter.
[0024] The function of working area 4 is to radially compress the high-carbon steel wire with a thin film of lubricating fluid on its surface, thereby deforming the high-carbon steel wire.
[0025] The function of sizing zone 5 is to further stabilize the diameter of the high-carbon steel wire after compression deformation.
[0026] The function of the export zone 6 is to cool the high-carbon steel wire with a stable diameter after compression deformation using the lubricating fluid in the zone.
[0027] A method for processing drawing dies suitable for high-strength, high-carbon steel wire includes the following steps: Step 1: Clean and dry the un-drilled mold core 2. The cylindrical mold core 2 has a diameter of 0.9 mm, a height of 0.9 mm, and a grain size of 0.5 μm. Cool it in liquid nitrogen for 1 hour. Step 2: Clean the machined mold sleeve 1 and set it aside for use. The cylindrical mold sleeve 1 has an outer diameter of 25mm and a height of 16mm. Step 3: Take out the un-drilled mold core 2 cooled in liquid nitrogen, install it into the center of the mold sleeve 1 to ensure concentricity and fix it; Step 4: Preheat the un-drilled mold core 2 to make it expand and generate a pre-tightening force against the inner wall of the mold sleeve 1; Step 5: Perform laser drilling on the center of the un-drilled mold core 2; Step 6: After drilling, the channel is machined and ground according to parameters such as the length-to-short axis ratio, entrance angle, and sizing zone length. Step 7: Polish the ground holes; Step 8: Perform parameter detection on the mold hole. Example 1
[0028] A 23-pass wet drawing method was used to draw 97C steel wire with a diameter of 1.44 mm to a diameter of 0.2 mm. The last six passes used the foamed steel die of this invention, while the remaining passes used a tungsten carbide die. The drawn wire strength was 4000 MPa, and the torsional parameters are shown in Table 1. The standard was implemented according to GB / T 239.1-2023 Part 1 Unidirectional Torsion Standard, and the torsional performance is as follows. Figure 3 As shown.
[0029] Example 2
[0030] A 23-pass wet drawing method was used to draw 92C steel wire with a diameter of 1.48 mm to a diameter of 0.2 mm. The last six passes used the foamed steel die of this invention, while the remaining passes used tungsten carbide dies. The drawn steel wire had a strength of 4100 MPa. The torsional parameters are shown in Table 2. The standard conforms to GB / T 239.1-2023 Part 1 Unidirectional Torsion Standard, and the torsional performance is as follows. Figure 4 As shown.
[0031]
[0032] The above embodiments are only for illustrating the technical concept and features of the present invention, and are intended to enable those skilled in the art to understand the content of the present invention and implement it accordingly. They should not be construed as limiting the scope of protection of the present invention. All equivalent transformations or modifications made in accordance with the spirit and essence of the present invention should be covered within the scope of protection of the present invention.
Claims
1. A drawing die suitable for high-strength, high-carbon steel wire, characterized in that: The mold includes a mold sleeve (1) and a mold core (2) embedded in the mold sleeve (1); the mold sleeve (1) is made of foam steel and has a porous foam appearance; the mold core (2) is made of polycrystalline diamond and has a mold hole at the center, which includes an inlet area (3), a working area (4), a sizing area (5), and an outlet area (6); the mold sleeve (1) is made of No. 45 foam steel and has a honeycomb pore shape inside, distributed in a three-dimensional pore through-hole shape, with a pore diameter of 300μm to 500μm and a porosity of 25% to 45%. During the drawing process, the lubricant enters the pores of the mold sleeve (1) and flows to cool the mold sleeve (1).
2. The drawing die for high-strength, high-carbon steel wire as described in claim 1, characterized in that: The mold sleeve (1) and the mold core (2) are both cylindrical in shape, and the mold sleeve (1) and the mold core (2) form a cold-fit interference fit.
3. The drawing die for high-strength, high-carbon steel wire as described in claim 1, characterized in that: The function of the entrance area (3) of the mold core (2) is to allow high carbon steel wire to enter and lubricant to enter.
4. A drawing die suitable for high-strength, high-carbon steel wire as described in claim 1, characterized in that: The function of the working area (4) is to radially compress the high carbon steel wire with a lubricating film attached to its surface, thereby deforming the high carbon steel wire.
5. A drawing die suitable for high-strength, high-carbon steel wire as described in claim 1, characterized in that: The function of the sizing zone (5) is to further stabilize the diameter of the high-carbon steel wire after compression deformation.
6. A drawing die suitable for high-strength, high-carbon steel wire as described in claim 1, characterized in that: The function of the outlet area (6) is to cool the high-carbon steel wire with a stable diameter after compression deformation with lubricating fluid in the area.
7. A method for processing a drawing die for high-strength, high-carbon steel wire as described in any one of claims 1-6, characterized in that... Includes the following steps: Step 1: Clean and dry the un-drilled mold core (2). The cylindrical mold core (2) has a diameter of 0.9 mm, a height of 0.9 mm, and a grain size of 0.5 μm. Place it in liquid nitrogen and cool for 1 hour. Step 2: Clean the machined mold sleeve (1) and set it aside for use. The cylindrical mold sleeve (1) has an outer diameter of 25mm and a height of 16mm. Step 3: Take out the un-drilled mold core (2) cooled in liquid nitrogen, install it into the center of the mold sleeve (1) to ensure concentricity and fix it; Step 4: Preheat the un-drilled mold core (2) to make it expand and generate a pre-tightening force against the inner wall of the mold sleeve (1); Step 5: Perform laser drilling on the center of the un-drilled mold core (2); Step 6: After drilling, the channel is machined and ground according to the length-to-short axis ratio, entrance angle, and sizing belt length parameters. Step 7: Polish the ground holes; Step 8: Perform parameter detection on the mold hole.
Citation Information
Patent Citations
Large-aperture die for wire drawing
CN212525477U
Ceramic drawing die and manufacture thereof
JP1992305309A