A method of forming a rear floor assembly reinforcement panel for an automobile

By employing steps such as substrate cutting, pressing, perforation, trimming, and shaping, the problems of discontinuous curved surface forming and insufficient stress release in the molding of automotive rear floor assembly reinforcement plates were solved, achieving high-quality reinforcement plate molding.

CN119115459BActive Publication Date: 2026-11-24CHONGQING DIGITAL DIE
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411259363.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2026-11-24
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

In existing methods for forming reinforcing plates for automotive rear floor assemblies, the continuity of curvature during curved surface forming is poor, large-angle arc cutting is difficult, and stress release is insufficient, resulting in poor processing quality.

Method used

The process involves steps such as substrate cutting, lamination, primary perforation, trimming, secondary trimming, curved surface shaping, secondary perforation, sprue trimming, and shaping. By reserving stress-relieving material plates and designing precise allowances, the continuity of curved surface forming and stress relief are ensured, avoiding the difficulties of trimming operations in narrow gaps.

Benefits of technology

This improves the molding quality of automotive rear floor assembly reinforcement plates, ensures the continuity of curved surface molding and sufficient stress release, avoids problems of poor processing quality, and achieves high-quality molding of irregular and curved automotive rear floor assembly reinforcement plates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119115459B_ABST
    Figure CN119115459B_ABST
Patent Text Reader

Abstract

This invention discloses a method for forming a reinforcing plate for an automotive rear floor assembly, comprising the following steps: S1, substrate cutting and pressing; S2, primary perforation and trimming, wherein a stress-relieving material plate is left between the trimmed areas of the substrate and the front and rear ends of the rear floor wing after pressing; S3, secondary trimming; S4, curved surface shaping; S5, secondary perforation; S6, trimming and opening of sprue material; S7, shaping and unloading: after grinding, polishing, settling, and inspection of the trimmed and perforated areas, the material is unloaded. This invention can solve the problems of poor continuity of curvature in curved surface forming, difficulty in operating large-angle arc cutting operations in narrow dimensions, and insufficient stress relief at the aforementioned processing areas, leading to poor processing quality in common automotive rear floor assembly reinforcing plate forming methods and processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of automotive parts manufacturing technology, specifically a method for forming a reinforcing plate for a rear floor assembly of an automobile. Background Technology

[0002] The rear floor assembly is an important component of the car body-in-white and forms the foundation of the entire vehicle. It supports the upper body, opening and closing components, other assemblies and related accessories, and the weight of the occupants. It also bears the loads, vibrations, impacts, and torques generated during the movement of the vehicle. Since the components of the car are distributed in different locations, the loads, vibrations, impacts, and torques generated in different locations of the rear floor are different. Therefore, the processing requirements for different areas of the rear floor are different during the automotive manufacturing process.

[0003] The molding of reinforcement plates for common automotive rear floor assemblies generally requires operations such as curved surface forming, hole opening, and sprue cutting. However, common molding methods and processes have problems such as poor continuity of curvature in curved surface forming, difficulty in operating large-angle arc cutting operations in narrow dimensions, and insufficient stress release at the above-mentioned processing points, resulting in poor processing quality. Summary of the Invention

[0004] The purpose of this invention is to provide a method for forming a reinforcing plate for an automotive rear floor assembly, in order to solve the problems of poor continuity of curvature in the forming process of common automotive rear floor assembly reinforcing plates, difficulties in the operation of cutting large-angle arcs in narrow dimensions, and insufficient stress release at the processing points, which lead to poor processing quality.

[0005] To achieve the above objectives, the present invention adopts the following technical solution: a method for forming a reinforcing plate for a car rear floor assembly, comprising the following steps:

[0006] S1. Substrate cutting and pressing: The sheet metal is cut into a substrate with a size larger than that of the rear floor assembly of the vehicle. The rear floor assembly of the vehicle is positioned on the substrate and the arc-shaped bottom surface of the rear floor wing plate is pressed with the substrate.

[0007] S2, One-time perforation and cutting: The first perforation area on the rear floor body on the inner side of the rear floor wing is perforated, and the second perforation area is perforated and shaped. The substrate after pressing is cut on the outer part of the rear floor wing, and the front and rear corners of both are cut. Stress relief material is left between the front and rear cuts.

[0008] S3, Secondary cutting: The stress relief material plate, the front cutting area and the back cutting area of ​​the rear floor wing plate and the base plate are cut respectively, and the stepped structure at the cutting area of ​​the front cutting area and the back cutting area is shaped.

[0009] S4. Surface shaping: The edges of the rear floor wing plate and the base plate are bent downwards in the lateral and axial directions in sequence;

[0010] S5. Secondary perforation: The first and second notches are cut out at both ends of the rear floor wing plate and the base plate axis, respectively. The rear floor body and the rear floor wing plate are perforated in the third perforation area and stamped in the countersunk hole area.

[0011] S6. Cutting and punching sprue material: Cut the sprue material between the sprue materials at the axis of the rear floor body with a third notch, and cut the sprue material. Punch the irregular hole in the fourth perforation area on the countersunk hole area.

[0012] S7. Shaping and unloading: After grinding, polishing, settling and inspecting the cut and perforated areas, the material is unloaded.

[0013] As a further description of the above technical solution:

[0014] The rear floor wing plate and the base plate are vertically positioned by a pressure rod, and the pressure roller at the end of the pressure rod is pressed onto the rear floor wing plate. The base plate is equipped with positioning posts on the edge of the rear floor wing plate.

[0015] As a further description of the above technical solution:

[0016] The thickness of the substrate is 1-2 mm. In step S2, a margin of 0.2-0.4 mm is left at the perforation of the first perforation area, and a margin of 0.2-0.3 mm is left at the perforation of the second perforation area.

[0017] As a further description of the above technical solution:

[0018] In step S2, a 0.2-0.5mm allowance is provided at the cutting points of the rear floor wing plate and the front end of the substrate, and a 0.6-0.7mm allowance is provided at the cutting corners of the two. A 0.3-0.7mm allowance is provided at the cutting points of the rear floor wing plate and the substrate, and a 1.2-1.4mm allowance is provided at the cutting corners of the two.

[0019] As a further description of the above technical solution:

[0020] Before cutting the front and rear cutting areas as described in step 3, several notches are cut at intervals along the axis at the rear end of the rear floor wing plate, with a margin of 0.3-0.6mm left at the cut points.

[0021] As a further description of the above technical solution:

[0022] In step 3, the cut edge of the stress-relieving material plate has a margin of 0.2-0.4mm, and the cut edge of the front cutting area has a margin of 0.3-0.5mm on the inner side and 1.2-1.4mm on the edge.

[0023] As a further description of the above technical solution:

[0024] After steps 2 and 5 are completed, the rear floor body is marked using a mold.

[0025] In summary, due to the adoption of the above technical solution, the present invention has the following beneficial effects compared with the prior art:

[0026] This invention ensures the continuity of curvature in the curved surface forming by step-by-step cutting of the curved edge of the pre-stress-relieving material plate. The straight sections (with angle changes greater than a set value) and curved sections (with angle changes greater than the set value) are precisely pre-set with allowances, further improving the quality of the curved surface forming. Precise allowance design is applied to the openings in the rear floor, ensuring stress release during the processing of the substrate, rear floor body, and wing plates. Cutting the sprue material inside the rear floor body involves first punching several notches, then cutting on one side, ensuring high-quality forming of the rear floor assembly clamping plate at the sprue material. This avoids operational difficulties caused by cutting in narrow gaps and poor processing quality due to insufficient stress release. The design of interspersing bending operations with the above operations ensures the forming quality of the reinforcing plate for irregularly shaped and curved automotive rear floor assemblies. Attached Figure Description

[0027] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0028] Figure 1 This document describes the material strip and product structure changes corresponding to a molding method for a reinforcing plate in an automotive rear floor assembly. Figure 1 .

[0029] Figure 2 This document describes the material strip and product structure changes corresponding to a molding method for a reinforcing plate in an automotive rear floor assembly. Figure 2 .

[0030] Legend:

[0031] 1. Rear floor body; 2. Rear floor wing plate; 3. Base plate; 4. First perforation area; 5. Stress relief material plate; 6. Front cutting area; 7. Rear cutting area; 8. Second perforation area; 9. First notch; 10. Second notch; 11. Countersunk hole area; 12. Third perforation area; 13. Third notch; 14. Fourth perforation area; 15. Sprue material. Detailed Implementation

[0032] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0033] In the description of this invention, it should be understood that the terms "upper", "lower", "front", "rear", "left", "right", "top", "bottom", "inner", "outer", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this invention.

[0034] Example 1:

[0035] Please see Figure 1-2 This invention provides a technical solution: a method for forming a reinforcing plate for a car rear floor assembly, comprising the following steps:

[0036] S1. Substrate cutting and pressing: The sheet metal is cut into a substrate 3 with a size larger than that of the rear floor assembly of the automobile. The rear floor assembly of the automobile is positioned on the substrate 3 and the arc-shaped bottom surface of the rear floor wing 2 is pressed with the substrate 3.

[0037] S2, One-time perforation and cutting: The first perforation area 4 on the rear floor body 1 on the inner side of the rear floor wing plate 2 is perforated, and the second perforation area 8 is perforated and shaped. The substrate 3 after pressing is cut on the outer part of the rear floor wing plate 2, and the front and rear corners of the two are cut. A stress relief material plate 5 is left between the front and rear cuts.

[0038] S3, Secondary cutting: The stress relief material plate 5, the front cutting area 6 and the rear cutting area 7 of the rear floor wing plate 2 and the base plate 3 are cut respectively, and the stepped structure at the cutting points of the front cutting area 6 and the rear cutting area 7 is shaped.

[0039] S4. Surface shaping: The edges of the rear floor wing plate 2 and the base plate 3 are bent downwards in the lateral and axial directions in sequence.

[0040] S5. Secondary perforation: The first notch 9 and the second notch 10 are cut at both ends of the axis of the rear floor wing plate 2 and the base plate 3 respectively. The rear floor body 1 and the rear floor wing plate 2 are perforated in the third perforation area 12 and stamped in the countersunk hole area 11 respectively.

[0041] S6. Cutting and punching sprue material: Cutting the sprue material 15 between the sprue material 15 on the axis of the rear floor body 1 with the third notch 13, cutting the sprue material 15, and punching irregular holes in the fourth perforation area 14 on the countersunk hole area 11.

[0042] S7. Shaping and unloading: After grinding, polishing, settling and inspecting the cut and perforated areas, the material is unloaded.

[0043] The rear floor wing plate 2 and the base plate 3 are vertically positioned by a pressure rod. The pressure roller at the end of the pressure rod is pressed onto the rear floor wing plate 2. The base plate 3 is equipped with positioning posts on the edge of the rear floor wing plate 2.

[0044] The thickness of the substrate 3 is 1-2 mm. In step S2, a margin of 0.2-0.4 mm is left at the perforation of the first perforation area 4, and a margin of 0.2-0.3 mm is left at the perforation of the second perforation area 8.

[0045] In step S2, a 0.2-0.5mm allowance is provided at the cutting points of the rear floor wing plate 2 and the base plate 3, and a 0.6-0.7mm allowance is provided at the cutting corners of the two. A 0.3-0.7mm allowance is provided at the cutting points of the rear floor wing plate 2 and the base plate 3, and a 1.2-1.4mm allowance is provided at the cutting corners of the two.

[0046] Before cutting in the front cutting area 6 and the rear cutting area 7 in step 3, several notches are cut at intervals at the axis of the rear end of the rear floor wing plate 2, with a margin of 0.3-0.6mm left at the cut of the notches.

[0047] In step 3, the stress-relieving material plate 5 has a 0.2-0.4mm allowance at the cut end, and the front cutting area 6 has 0.3-0.5mm allowance on the inner side and 1.2-1.4mm allowance on the edge.

[0048] After steps 2 and 5 are completed, the rear floor body 1 is marked using a mold.

[0049] Example 2:

[0050] Based on the above embodiment 1, preferably, the thickness of the substrate 3 is 1.2mm, and a 0.3mm allowance is left at the perforation of the first perforation area 4.

[0051] In summary, due to the adoption of the above technical solution, the method for forming a reinforcing plate for a car rear floor assembly in this embodiment has the following advantages compared to the prior art:

[0052] This invention ensures the continuity of curvature in the curved surface forming by step-by-step cutting of the curved edge of the pre-stress-relieving material plate. The straight sections (with angle changes greater than a set value) and curved sections (with angle changes greater than the set value) are precisely pre-set with allowances, further improving the quality of the curved surface forming. Precise allowance design is applied to the openings in the rear floor, ensuring stress release during the processing of the substrate, rear floor body, and wing plates. Cutting the sprue material inside the rear floor body involves first punching several notches, then cutting on one side, ensuring high-quality forming of the rear floor assembly clamping plate at the sprue material. This avoids operational difficulties caused by cutting in narrow gaps and poor processing quality due to insufficient stress release. The design of interspersing bending operations with the above operations ensures the forming quality of the reinforcing plate for irregularly shaped and curved automotive rear floor assemblies.

[0053] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.

Claims

1. A method for forming a reinforcing plate for a car rear floor assembly, characterized in that, Includes the following steps: S1. Substrate cutting and pressing: The sheet metal is cut into a substrate with a size larger than that of the rear floor assembly of the vehicle. The rear floor assembly of the vehicle is positioned on the substrate and the arc-shaped bottom surface of the rear floor wing plate is pressed with the substrate. S2, One-time perforation and cutting: The first perforation area on the rear floor body on the inner side of the rear floor wing is perforated, and the second perforation area is perforated and shaped. The substrate after pressing is cut on the outer part of the rear floor wing, and the front and rear corners of both are cut. Stress relief material is left between the front and rear cuts. S3, Secondary cutting: The stress relief material plate, the front cutting area and the back cutting area of ​​the rear floor wing plate and the base plate are cut respectively, and the stepped structure at the cutting area of ​​the front cutting area and the back cutting area is shaped. S4. Surface shaping: The edges of the rear floor wing plate and the base plate are bent downwards in the lateral and axial directions in sequence; S5. Secondary perforation: The first and second notches are cut out at both ends of the rear floor wing plate and the base plate axis, respectively. The rear floor body and the rear floor wing plate are perforated in the third perforation area and stamped in the countersunk hole area. S6. Cutting and punching sprue material: Cut the sprue material between the sprue materials at the axis of the rear floor body with a third notch, and cut the sprue material. Punch the irregular hole in the fourth perforation area on the countersunk hole area. S7. Shaping and unloading: After grinding, polishing, settling and inspecting the cut and perforated areas, the material is unloaded.

2. The method for forming a reinforcing plate for a vehicle rear floor assembly according to claim 1, characterized in that, The rear floor wing plate and the base plate are vertically positioned by a pressure rod, and the pressure roller at the end of the pressure rod is pressed onto the rear floor wing plate. The base plate is equipped with positioning posts on the edge of the rear floor wing plate.

3. The method for forming a reinforcing plate for a vehicle rear floor assembly according to claim 1, characterized in that, The thickness of the substrate is 1-2 mm. In step S2, a 0.2-0.4 mm margin is left at the perforation of the first perforation area, and a 0.2-0.3 mm margin is left at the perforation of the second perforation area.

4. The method for forming a reinforcing plate for a vehicle rear floor assembly according to claim 1, characterized in that, In step S2, a 0.2-0.5mm allowance is provided at the cutting points of the rear floor wing plate and the front end of the substrate, and a 0.6-0.7mm allowance is provided at the cutting corners of the two. A 0.3-0.7mm allowance is provided at the cutting points of the rear floor wing plate and the substrate, and a 1.2-1.4mm allowance is provided at the cutting corners of the two.

5. The method for forming a reinforcing plate for a vehicle rear floor assembly according to claim 1, characterized in that, Before cutting the front and rear cutting areas as described in step 3, several notches are cut at intervals along the axis at the rear end of the rear floor wing plate, with a margin of 0.3-0.6mm left at the cut points.

6. The method for forming a reinforcing plate for a vehicle rear floor assembly according to claim 1, characterized in that, In step 3, the cut edge of the stress-relieving material plate has a margin of 0.2-0.4mm, and the cut edge of the front cutting area has a margin of 0.3-0.5mm on the inner side and 1.2-1.4mm on the edge.

7. The method for forming a reinforcing plate for a vehicle rear floor assembly according to claim 1, characterized in that, After steps 2 and 5 are completed, the rear floor body is marked using a mold.

Citation Information

Patent Citations

  • Sheet metal forming technology of front floor threshold girder of automobile

    CN103624144A