Aluminum foil cutting method and method for reducing radial color difference of aluminum foil roll end face

By spraying lubricant onto the surface of the disc cutter during the aluminum foil cutting process, the problem of light and dark color difference on the cut surface of the aluminum foil roll was solved, achieving uniformity of gloss on the cut surface and stability of product quality.

CN119116025BActive Publication Date: 2026-11-24江苏金域新能源科技有限公司
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311853286.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-29
Publication Date
2026-11-24
Estimated Expiration
2043-12-29

AI Technical Summary

Technical Problem

The existing aluminum foil rolls have a difference in light and dark color on the cut end face, which affects the product's aesthetics and quality stability.

Method used

During the aluminum foil cutting process, lubricant is sprayed onto the surface of the disc cutter through the first, second, or third nozzles onto the friction surface or non-friction surface to reduce blade wear and improve the uniformity of the cut surface gloss.

Benefits of technology

By reducing blade wear, we ensure uniform gloss on the cut surface of aluminum foil rolls, reduce radial color difference, and improve product appearance quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119116025B_ABST
    Figure CN119116025B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of battery foil technology, specifically relating to a method for cutting aluminum foil and a method for reducing radial color difference on the end face of an aluminum foil roll. The method includes feeding aluminum foil onto a cutting roller, where a rotating disc cutter cuts the aluminum foil; and spraying lubricating fluid onto the surface of the disc cutter. This application increases lubrication and reduces blade wear by spraying lubricating fluid onto the surface of the disc cutter during aluminum foil cutting. This results in minimal difference in blade wear between the early and later stages of cutting, leading to a smooth, low-roughness, and brighter appearance with no dark areas after specular reflection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of battery foil technology, specifically relating to an aluminum foil cutting method and a method for reducing radial color difference at the end face of an aluminum foil roll. Background Technology

[0002] The cut aluminum foil rolls obtained from the current process of unwinding, cutting, and rewinding exhibit significant differences in light and dark color on their end faces. For example... Figure 1 The central area 41 of the cut surface (4 end face) of the cut aluminum foil roll is light in color, while the outer area 42 of the cut surface (4 end face) is dark in color. This seriously affects the product's appearance and can easily lead customers to mistakenly believe that the products are from different batches or that the product quality is unstable, thus affecting product sales.

[0003] To address the above problems, this invention is proposed. Summary of the Invention

[0004] The first aspect of the present invention provides an aluminum foil cutting method, the method comprising feeding an aluminum foil 2 onto a cutting groove roller, cutting the aluminum foil 2 with a rotating disc cutter 1, and spraying lubricating liquid onto the surface of the disc cutter 1.

[0005] The grooved roller 3 refers to a roller with several parallel annular grooves engraved on its circumferential surface, and the aluminum foil 2 wraps around a portion of the roller's circumferential surface at a certain wrap angle. The structure of the grooved roller 3 is as follows: Figure 6 As shown.

[0006] Preferably, lubricant is sprayed through a first nozzle at the junction of the disc cutter 1 and the aluminum foil 2, and the distance between the first nozzle and the axis of rotation of the disc cutter 1 is greater than the radius of the disc cutter 1.

[0007] like Figure 2 , 4 Point P in equation 5 represents the position of the first nozzle.

[0008] Preferably, lubricating fluid is sprayed onto the friction surface 5 on the side of the disc cutter 1 through a second nozzle, wherein the annular surface of the disc cutter 1 that can contact the aluminum foil 2 during cutting is called the friction surface 5;

[0009] Alternatively, lubricant can be sprayed onto the non-friction surface portion of the side of the disc cutter 1 through a third nozzle.

[0010] More preferably, the second nozzle is located to the side of the disc cutter 1. There may be multiple second nozzles.

[0011] More preferably, projecting along the central axis of the disc cutter 1: the projection of the second nozzle is located on the friction surface 5 of the disc cutter 1. For example... Figure 2 Points Q1 and Q2 in the middle Figure 4 and Figure 5 Point Q2 in the diagram can be the position of the second nozzle. Figure 4 and Figure 5 The middle arrow indicates the direction of movement of aluminum foil 2.

[0012] Of course, the projection of the second nozzle may not be located on the disc cutter 1, but outside the disc cutter 1. For example, the second nozzle may be located on the oblique side of the disc cutter 1, in which case it is sufficient to ensure that the sprayed lubricant is on the friction surface 5 on the side of the disc cutter 1.

[0013] More preferably, the third nozzle is located to the side of the disc cutter 1. There may be multiple third nozzles.

[0014] More preferably, the projection along the central axis of the disc cutter 1: the projection of the third nozzle is located on the non-friction surface of the disc cutter 1. For example... Figure 2 Points R1 and R2 in the diagram can both be the positions of the third nozzle.

[0015] The friction surface 5 can be the annular blade portion of the disc cutter 1, or it can include the annular blade portion but be wider than the annular blade portion. Figure 2 This is a schematic diagram of the cutting process of aluminum foil 2 in this application, taking one side of a disc cutter 1 as an example. Figure 2 The direction of the middle arrow indicates the direction of the object's movement. The outer circle of the cutting roller 3 corresponds to the top of the cutting groove. The inner circle (dashed line) of the cutting roller 3 corresponds to the bottom of the cutting groove.

[0016] During cutting, aluminum foil 2 is conveyed by the groove roller 3, and the cutting edge of the disc cutter 1 is located in the groove of the groove roller 3, making contact with the aluminum foil 2 to cut it. M is the starting point of contact between the aluminum foil 2 and the disc cutter 1, and N is the ending point of contact. The annular surface swept by the arc MN of the disc cutter 1 as it rotates is the friction surface 5. The line connecting the axis A of the groove roller and the axis B of the disc cutter 1 intersects the groove roller 1 at point C. The circle formed with B as the center and BC as the radius is the non-friction surface of the disc cutter 1. The part of the disc cutter 1 surface excluding the non-friction surface is the friction surface 5. The friction surface 5 is annular.

[0017] Preferably, the lubricant comprises one or more of water, lubricating oil, rolling oil, or a mixture of water and oil.

[0018] Preferably, the water-oil mixture is an oil-in-water emulsion.

[0019] The second aspect of this application provides a method for reducing radial color difference at the end face of an aluminum foil roll, wherein the aluminum foil 2 is cut using the method described above, and then the cut aluminum foil 2 is wound up.

[0020] In this application, the end face of aluminum foil roll 4 specifically refers to the cut surface of the cut aluminum foil roll 4 obtained after the incoming aluminum foil has been unwound, cut, and rewound.

[0021] A third aspect of the invention relates to the use of an aluminum foil cutting method according to the first aspect of the invention for reducing radial color difference at the end face of an aluminum foil roll.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. Previous research has not addressed the color difference issue at the end faces of aluminum foil rolls. The applicant also encountered many setbacks in its attempts to solve this problem. For example, initially, it was assumed that the color difference stemmed from variations in the degree of oxidation on the cut surfaces, leading to extensive research into aluminum oxidation, all to no avail. Through in-depth research, the applicant discovered that the color difference between the cut surfaces of the aluminum foil rolls lies not in the inherent color difference, but in the difference in gloss. Therefore, strictly speaking, the lighter areas should be called bright areas, and the darker areas should be called dark areas. The difference in gloss arises from the varying degrees of wear on the cut surfaces. Bright areas are those produced during early cutting. Due to low blade wear and low blade temperature in the early stages, the cut surfaces are smooth with low roughness. Dark areas are those produced during later cutting. Due to high blade wear and higher blade temperature from prolonged friction, the cut surfaces are rough. Smooth cut surfaces primarily produce specular reflection, thus appearing brighter. Rough cut surfaces primarily produce diffuse reflection, thus appearing darker. Therefore, the cut surfaces of aluminum foil rolls appear to have color differences in shades to the naked eye, which should be more accurately described as light and dark color differences.

[0024] This application increases lubrication and reduces blade wear by spraying lubricant onto the surface of the disc cutter 1 during aluminum foil cutting. This results in minimal difference in blade wear between the early and later stages of cutting, leading to a smooth, low-roughness, and brighter appearance with no dark areas after specular reflection.

[0025] 2. In one embodiment, the first nozzle is located in front of the cutting edge of the disc cutter 1 (e.g., Figure 2Point P is the position of the first nozzle. At this time, the first nozzle only sprays generally towards the cutting area, without targeting any specific area. However, as long as some of the lubricant from the first nozzle is sprayed onto the surface of the disc cutter 1, the lubricant on the disc cutter 1 will be thrown onto the friction surface 5 where the disc cutter 1 contacts the aluminum foil due to centrifugal force during the rotation of the disc cutter 1. During the cutting process, due to the lubricating effect of the lubricant, the wear of the blade on the friction surface 5 of the disc cutter 1 is reduced, but the disadvantage is that the utilization rate of the lubricant is low. The advantage is that, since the distance between adjacent annular cutting blades on the disc cutter 1 is narrow, placing the first nozzle in front of the blade of the disc cutter 1 is not limited by the narrow distance, and multiple first nozzles can be arranged side by side at the same time (see Figure 5 (The three P points).

[0026] 3. In a preferred embodiment, a second nozzle is provided, which can be provided even when the first nozzle is not present. The second nozzle is located on the side of the disc cutter (1) and sprays lubricant onto the friction surface 5 on the side of the disc cutter 1. Figure 2 Points Q1 and Q2 in the middle Figure 4 and Figure 5 Point Q2 in the diagram can be the location of the second nozzle. Although the position of the second nozzle is limited by the narrow spacing between adjacent annular cutting blades on the disc cutter 1, the lubricant sprayed from the second nozzle is highly targeted, being completely sprayed onto the friction surface 5 on the side of the disc cutter 1. Similarly, during the cutting process, the wear of the disc cutter 1's blade is reduced due to the lubricating effect of the lubricant. Furthermore, because the lubricant sprayed from the second nozzle is more concentrated, the lubricant utilization efficiency is higher at points Q1 and / or Q2 compared to point P, resulting in a better effect on reducing the wear of the disc cutter 1's blade.

[0027] Furthermore, since the second nozzle directly sprays the lubricant onto the friction surface 5 of the disc cutter 1, even if the sprayed lubricant droplets are very small (at which point the surface tension between the lubricant droplets and the disc cutter 1 is greater than the centrifugal force acting on the lubricant droplets, and the lubricant cannot be thrown out by the centrifugal force), it can still achieve a lubricating effect and effectively reduce the wear of the disc cutter 1's blade.

[0028] 4. In another alternative implementation: Lubricant is sprayed onto the non-friction surface portion of the side of the disc cutter 1 through a third nozzle. The third nozzle can also be provided independently without the first or second nozzle.

[0029] First, the lubricant can be water. The water is spread thinly on the friction surface 5 under the action of centrifugal force. The water evaporates after being heated to cool down the friction surface 5, which is heated by friction during the cutting process.

[0030] Secondly, the lubricant can also be a water-oil mixture or an oil-in-water emulsion. Under centrifugal force, the water is spread thinly onto the friction surface 5. The rapid evaporation of the water after heating significantly reduces the temperature of the friction surface 5. Simultaneously, before a section of the annular blade of the disc cutter 1 rotates to the cutting position, if the water phase has completely evaporated, the exposed oil phase begins to provide lubrication. Even if the water has not completely evaporated, it doesn't matter; both water and oil provide lubrication. Therefore, it can both cool the friction surface 5 and provide lubrication. This dual effect of cooling and lubrication further reduces blade wear. Attached Figure Description

[0031] Figure 1 This is a schematic diagram of the cut surface of an aluminum foil roll after cutting, as described in the prior art.

[0032] Figure 2 This is a schematic diagram of the cutting process of aluminum foil 2 in this application, taking a disc cutter 1 as an example.

[0033] Figure 3 This is a cross-sectional view of the aluminum foil 2 being cut in this application, using three disc cutters 1 as an example.

[0034] Figure 4 This is a top view of a portion of the structure of a disc cutter 1 cutting aluminum foil according to this application.

[0035] Figure 5 This is a top view of the partial structure of the three disc cutters 1 cutting aluminum foil according to this application.

[0036] Figure 6 This is a schematic diagram of the structure of the groove roller 3 in this application.

[0037] List of reference numerals in the attached diagram:

[0038] 1. Disc cutter; 11. Disc cutter blade; 12. Disc cutter body; 2. Aluminum foil; 3. Grooving roller; 4. Aluminum foil roll; 41. Central area; 42. Outer area; 5. Friction surface; A. Center of the side of the grooved roller; A-A'. Axis of the grooved roller; B. Center of the side of the disc cutter; B-B'. Axis of the disc cutter. Detailed Implementation

[0039] The present invention will be described below with reference to specific embodiments, but the implementation of the present invention is not limited thereto. Experimental methods not specifically described in the embodiments generally use conventional conditions and conditions described in the manual, or conditions recommended by the manufacturer. The general equipment, materials, reagents, etc., used are all commercially available unless otherwise specified. The raw materials required in the following embodiments and comparative examples are all commercially available.

[0040] The rolling oil was purchased from Jiangsu Yingji Lubrication Technology Co., Ltd., and its name is Stamping and Drawing Oil E-C20.

[0041] The automotive lubricant was purchased from Beijing Zhongrun Huayou Petrochemical Co., Ltd., model GL-5 85W-140.

[0042] Example 1

[0043] A method for reducing color difference on the cut surface of aluminum foil rolls, comprising the following steps:

[0044] The aluminum foil is fed onto the cutting roller, and the rotating disc cutter 1 cuts the aluminum foil 2.

[0045] At the same time, a lubricating fluid injection mechanism is used to spray lubricating fluid through a first nozzle onto the junction of the disc cutter 1 and the aluminum foil 2. The distance between the first nozzle and the axis of rotation of the disc cutter 1 is greater than the radius of the disc cutter 1.

[0046] The cut aluminum foil 2 is rolled up to obtain aluminum foil roll 4.

[0047] There is one disc cutter 1, which is used to cut the aluminum foil 2 in half.

[0048] The width of aluminum foil 2 is 1200mm. Each strip of aluminum foil after cutting is 600mm wide.

[0049] The minimum distance between the first nozzle and the edge of the disc cutter 1 is 30mm, such as Figure 2 and 4 As shown, the first nozzle is located at point P. The output pressure of the first nozzle is 0.11 MPa. There is one first nozzle.

[0050] The lubricant sprayed from the first nozzle is rolling oil.

[0051] Example 2

[0052] A method for reducing color difference on the cut surface of aluminum foil rolls, comprising the following steps:

[0053] The aluminum foil is fed onto the cutting roller, and the rotating disc cutter 1 cuts the aluminum foil 2.

[0054] At the same time, a lubricating fluid injection mechanism sprays lubricating fluid onto the friction surface 5 on the side of the disc cutter 1 through its second nozzle. The annular surface of the disc cutter 1 that can contact the aluminum foil 2 during cutting is called the friction surface 5.

[0055] Projecting along the central axis of the disc cutter 1: The projection of the second nozzle is located on the friction surface 5 of the disc cutter 1.

[0056] In this embodiment 2, the position of the second nozzle is... Figure 2At point Q2. There are two second nozzles. The distance between the second nozzle and the side of the disc cutter 1 is 20mm. The output pressure of the second nozzle is 0.11MPa. There is one disc cutter 1, used to cut the aluminum foil 2 in half. The width of the aluminum foil 2 is 1200mm. The width of each cut aluminum foil is 600mm. The lubricant is also rolling oil.

[0057] Example 3

[0058] A method for reducing color difference on the cut surface of aluminum foil rolls, comprising the following steps:

[0059] The aluminum foil is fed onto the cutting roller, and the rotating disc cutter 1 cuts the aluminum foil 2.

[0060] At the same time, a lubricating fluid injection mechanism sprays lubricating fluid onto the friction surface 5 on the side of the disc cutter 1 through its second nozzle. The annular surface of the disc cutter 1 that can contact the aluminum foil 2 during cutting is called the friction surface 5.

[0061] Projecting along the central axis of the disc cutter 1: The projection of the second nozzle is located on the friction surface 5 of the disc cutter 1.

[0062] In this embodiment 3, the position of the second nozzle is... Figure 2 At point Q1. There are two second nozzles. The distance between the second nozzle and the side of the disc cutter 1 is 20mm. The output pressure of the second nozzle is 0.11MPa. There is one disc cutter 1, used to cut the aluminum foil 2 in half. The width of the aluminum foil 2 is 1200mm. The width of each cut aluminum foil is 600mm. The lubricant is also rolling oil.

[0063] Example 4

[0064] A method for reducing color difference on the cut surface of aluminum foil rolls, comprising the following steps:

[0065] The aluminum foil is fed onto the cutting roller, and the rotating disc cutter 1 cuts the aluminum foil 2.

[0066] At the same time, a lubricant injection mechanism is used to spray lubricant onto the non-friction surface of the side of the disc cutter 1 through its third nozzle;

[0067] The annular surface of the disc cutter 1 that can contact the aluminum foil 2 during cutting is called the friction surface.

[0068] Projection along the central axis of the disc cutter 1: The projection of the third nozzle is located on the non-friction surface of the disc cutter 1.

[0069] In this embodiment 4, the position of the third nozzle is... Figure 2 At point R2. There are two third nozzles. The distance between the third nozzle and the side of the disc cutter 1 is 20mm. The output pressure of the third nozzle is 0.105MPa. Due to the low output pressure, the droplets are large enough to be thrown onto the friction surface under centrifugal force. The lubricant is water. There is one disc cutter 1, used to cut the aluminum foil 2 in half. The width of the aluminum foil 2 is 1200mm. The width of each cut aluminum foil strip is 600mm.

[0070] Example 5

[0071] A method for reducing color difference on the cut surface of aluminum foil rolls, comprising the following steps:

[0072] The aluminum foil is fed onto the cutting roller, and the rotating disc cutter 1 cuts the aluminum foil.

[0073] At the same time, a lubricant injection mechanism is used to spray lubricant onto the non-friction surface of the side of the disc cutter 1 through its third nozzle;

[0074] The annular surface of the disc cutter 1 that can contact the aluminum foil during cutting is called the friction surface 5.

[0075] Projection along the central axis of the disc cutter 1: The projection of the third nozzle is located on the non-friction surface of the disc cutter 1.

[0076] In this embodiment 5, the position of the third nozzle is... Figure 2 At point R1. There are two third nozzles. The distance between the third nozzle and the side of the disc cutter 1 is 20mm. The output pressure of the third nozzle is 0.105MPa. Due to the low output pressure, the droplets are large enough to be thrown onto the friction surface under centrifugal force. The lubricant is water. There is one disc cutter 1, used to cut the aluminum foil in half. The width of the aluminum foil is 1200mm. After cutting, each strip of aluminum foil is 600mm wide.

[0077] Example 6

[0078] The only difference is that the lubricant sprayed by the third nozzle in Example 5 is replaced with a water-oil mixture instead of water. The water-oil mixture is prepared as follows: automotive lubricating oil and water are mixed at a mass ratio of 1:10 and vigorously stirred and emulsified to obtain an oil-in-water emulsion, which is then sprayed to obtain oil-in-water droplets.

[0079] Comparative Example 1

[0080] Compared with Example 1, no lubricant spraying mechanism is provided, and lubricant is not sprayed at the junction of the disc cutter 1 and the aluminum foil; other operations are the same.

[0081] Results test:

[0082] The gloss of the end face (i.e. the cut surface) of the aluminum foil rolls obtained after cutting in the above embodiments and comparative examples was tested.

[0083] The method is as follows: The gloss of the 60-degree cut surface of the obtained aluminum foil roll was measured using a CS-300S microporous gloss meter from Hangzhou Caipu Technology Co., Ltd. For each test sample, five locations were measured at the center of the cut surface, and the average value was taken as the gloss result for the center area. For each test sample, five locations were measured at the outer perimeter of the cut surface, and the average value was taken as the gloss result for the center area. Let the radius of the cut surface be R, and the circle be O. The center area of ​​the cut surface is then an inner circle with center O and a radius of 0.5R. The outer perimeter of the cut surface is the annular portion of the cut surface after removing this inner circle.

[0084] The results are shown in Table 1.

[0085] Table 1 proves:

[0086] 1. Compared to Comparative Example 1, where the gloss level of the central area is relatively high while the gloss level of the peripheral area is very low, in Examples 1-6, the gloss levels of both the central and peripheral areas are high (above 450 GU) and not significantly different (the gloss difference between the central and peripheral areas is less than 50 GU). This indicates that spraying lubricant onto the disc cutter 1 can reduce the radial color difference on the end face of the aluminum foil roll 4 and improve the end face gloss.

[0087] 2. The gloss levels of both the central and peripheral regions in Examples 2 and 3 are greater than those in Example 1. The gloss difference between the central and peripheral regions in Examples 2 and 3 is also smaller than that in Example 1. This indicates that spraying lubricating oil onto the friction surface 5 of the disc cutter 1, rather than spraying lubricating fluid onto the interface between the disc cutter 1 and the aluminum foil, can further improve the gloss level of the cut surface of the aluminum foil roll 4 and reduce the radial color difference at the end face.

[0088] 3. The gloss levels of both the central and peripheral regions in Examples 4 and 5 are greater than those in Example 1. The gloss difference between the central and peripheral regions in Examples 4 and 5 is also smaller than that in Example 1. This indicates that, compared to spraying lubricant at the interface between the disc cutter 1 and the aluminum foil, spraying water on the non-friction surface of the disc cutter 1 to cool it down can further improve the gloss level of the cut surface of the aluminum foil roll 4 and reduce the radial color difference at the end face.

[0089] 4. The gloss of both the central and peripheral regions of Example 6 is greater than that of Example 5. The gloss difference between the central and peripheral regions of Example 6 is also smaller than that of Example 5. This indicates that replacing water with a water-oil mixture in the lubricant sprayed on the non-friction surface of the disc cutter 1 can further increase the cooling and lubrication effect on the disc cutter, further improve the gloss of the cut surface of the aluminum foil roll 4, and reduce the radial color difference at the end face.

[0090] Table 1

[0091]

[0092]

Claims

1. A method for cutting aluminum foil, the method comprising feeding aluminum foil (2) onto a cutting groove roller, and a rotating disc cutter (1) cutting the aluminum foil (2); characterized in that, Lubricating fluid is sprayed onto the surface of the disc cutter (1); The lubricant comprises a water-oil mixture, wherein the water-oil mixture is an oil-in-water emulsion. During the cutting process, a lubricant spraying mechanism sprays the lubricant through a third nozzle onto the non-friction surface of the side of the disc cutter (1); Among them, the part of the annular surface of the disc cutter (1) that can contact the aluminum foil (2) during cutting is called the friction surface (5), and the non-friction surface is the part of the side of the disc cutter (1) other than the friction surface (5); Projecting along the central axis of the disc cutter (1), the projection of the third nozzle is located on the non-friction surface of the disc cutter (1), the number of the third nozzles is 2, the distance of the third nozzle from the side of the disc cutter (1) is 20mm, and the output pressure of the third nozzle is 0.105MPa; The lubricant is an oil-in-water emulsion obtained by mixing automotive lubricating oil and water at a mass ratio of 1:10 and then vigorously stirring and emulsifying it. The sprayed lubricating fluid droplets are thrown from the non-friction surface onto the friction surface (5) by the centrifugal force generated by the rotation of the disc cutter (1). The aqueous phase of the water-in-oil emulsion evaporates upon heating to cool the friction surface (5), and the oil phase lubricates the friction surface (5).

2. A method for reducing radial color difference at the end face of an aluminum foil roll, characterized in that, After cutting the aluminum foil (2) using the method described in claim 1, the cut aluminum foil (2) is then wound up.

3. The aluminum foil cutting method according to claim 1 is used to reduce the radial color difference at the end face of an aluminum foil roll.

Citation Information

Patent Citations

  • Method and apparatus of slitting film

    CN102152334A

  • Separate lubrication and cooling for machining processes

    CN1119424A

  • Multifunctional slitting equipment for aluminum foil

    CN115196403A