A method for the light-cured molding of high-strength fused quartz ceramics

By introducing SiC into fused silica powder, the over-curing problem in fused silica ceramic photopolymerization 3D printing was solved, improving molding accuracy and sintering density, and enhancing sample strength.

CN119118638BActive Publication Date: 2026-11-20NAT INST CORP OF ADDITIVE MFG XIAN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411258152.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2026-11-20
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

Traditional fused silica ceramic photopolymerization 3D printing suffers from over-curing, resulting in low precision of the molded parts, as well as low sintering density and poor strength.

Method used

By introducing silicon carbide (SiC) into fused silica powder, the high absorbance of SiC is used to reduce the curing depth, and SiO2 is generated at high temperature to connect the original SiO2 particles, thereby improving the sintering density.

Benefits of technology

The solidification depth of fused silica was reduced, which improved the molding accuracy and sintering density, and enhanced the strength of the sample.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005034710590000011
    Figure HDA0005034710590000011
  • Figure HDA0005034710590000012
    Figure HDA0005034710590000012
Patent Text Reader

Abstract

The application discloses a kind of high-strength fused quartz ceramic's light-cured forming preparation method, belong to light-cured forming technical field.It includes the following steps: fused quartz powder is blended with modifier one, modifier two, and mixed powder is prepared, then wet grinding is carried out, after drying, screening and then modified fused quartz powder is obtained;Prepolymer one, prepolymer two, resin monomer one, resin monomer two, photo initiator one, photo initiator two are mixed to prepare photosensitive resin system;Dispersing agent is added to photosensitive resin system and mixed uniformly, then modified fused quartz powder and SiC powder are mixed uniformly to prepare fused quartz ceramic light-cured slurry;Fused quartz ceramic light-cured slurry is printed, debinding treatment and sintering, and fused quartz ceramic is obtained;SiC powder dosage is 1wt%~5wt% of the mass of modified fused quartz powder.The preparation method can reduce the solidification depth of fused quartz, improve the forming precision, and at the same time improve the sintering density of fused quartz.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of photopolymerization molding technology, specifically relating to a photopolymerization molding preparation method for high-strength fused silica ceramics. Background Technology

[0002] Radar radomes are protective devices for aircraft radar antennas, integrating wave transmission, load-bearing, and temperature resistance. Fused silica ceramics possess advantages such as low coefficient of thermal expansion, good thermal shock resistance, and excellent dielectric properties, making them one of the main candidate materials for radar radomes in the defense and military industries. However, traditional fused silica radome manufacturing processes are time-consuming, technically demanding, and labor-intensive. Ceramic photopolymerization 3D printing technology, with its high molding efficiency, good molding accuracy, and high degree of model freedom, has become a boon for fused silica radome fabrication.

[0003] Ceramic photopolymerization 3D printing technology uses ceramic powder-photosensitive resin blends as raw materials. Following a designed 3D model, the ceramic green body is printed layer by layer using a photopolymerization 3D printing device. The green body is then degreased to remove organic components and sintered at high temperature to obtain the desired three-dimensional ceramic sample. However, due to the high light transmittance of fused silica, the single-layer curing depth is very high, which can lead to over-curing during printing, affecting the accuracy of the formed part. Furthermore, the sintering density of fused silica ceramics prepared by photopolymerization 3D printing is currently low, resulting in poor strength and limiting its application in practical production. Summary of the Invention

[0004] In order to overcome the shortcomings of the prior art, the present invention aims to provide a photopolymerization molding preparation method for high-strength fused silica ceramics, which can reduce the curing depth of fused silica, improve molding accuracy, and increase the sintering density of fused silica.

[0005] To achieve the above objectives, the present invention employs the following technical solution:

[0006] This invention provides a method for preparing high-strength fused silica ceramics by photopolymerization molding, comprising the following steps:

[0007] S1: Fused silica powder is mixed with modifier one and modifier two to obtain a mixed powder, which is then wet-milled, dried and sieved to obtain modified fused silica powder.

[0008] S2: A photosensitive resin system is prepared by mixing prepolymer 1, prepolymer 2, resin monomer 1, resin monomer 2, photoinitiator 1, and photoinitiator 2; a dispersant is added to the photosensitive resin system and mixed evenly, and then modified fused silica powder and SiC powder are added and mixed evenly to prepare a fused silica ceramic photocurable slurry.

[0009] S3: Print the fused silica ceramic photocurable slurry to obtain a fused silica ceramic green body;

[0010] S4: Degrease the fused silica ceramic green body to obtain a degreased fused silica part;

[0011] S5: Sinter the fused silica degreased parts to obtain fused silica ceramics;

[0012] Wherein, in S2, the amount of SiC powder used is 1wt% to 5wt% of the mass of the modified fused silica powder.

[0013] In one embodiment, in step S1, the first modifier is one or more of KH550, KH560, KH570, stearic acid, oleic acid, palmitic acid, and adipic acid; the amount of the first modifier is 1 wt% to 6 wt% of the mass of the modified fused silica powder.

[0014] The second modifier is one or more of polyethylene, polypropylene, polyacrylamide, polymaleic acid, polyethylene glycol, polyacrylic acid, and sodium polyacrylate; the amount of the second modifier is 1 wt% to 6 wt% of the mass of the modified fused silica powder.

[0015] In one embodiment, in step S2, the solid content of the fused silica ceramic photocurable slurry is 55 vol% to 65 vol%.

[0016] In one embodiment, in step S2, the particle size of both the modified fused silica powder and the fused silica powder is 1–5 μm; the particle size of the SiC powder is 200–500 nm.

[0017] In one embodiment, in S2, the first prepolymer is one or more of bisphenol A diglycidyl ether, brominated bisphenol F diglycidyl ether, polyurethane acrylate, and polyester acrylate; the second prepolymer is one or more of triethylene glycol divinyl ether, cyclohexyl-1,4-diethanol vinyl ether, and vinyl acetate; the first resin monomer is one or more of 1,6-hexanediol diacrylate, trimethylolpropane triacrylate, and pentaerythritol tetraacrylate; and the second resin monomer is one or more of isobornyl methacrylate, tripropylene glycol diacrylate, and pentaerythritol hexaacrylate.

[0018] In one embodiment, in S2, the ratio of prepolymer one, prepolymer two, resin monomer one, and resin monomer two is 1:3:8:8.

[0019] In one embodiment, in step S2, the first photoinitiator is one or two of 2,4,6-trimethylbenzoyl)diphenylphosphine oxide and phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide; the second photoinitiator is one or more of phenyldiazofluoroborate, diaryliodonium salt, triarylsulfonium salt and benzoin dimethyl ether.

[0020] In one embodiment, in step S2, the mass ratio of photoinitiator one to photoinitiator two is 1.5–2.5:0.5–1.5; the total amount of photoinitiator one and photoinitiator two is 1 wt%–5 wt% of the total mass of the photosensitive resin system.

[0021] In one embodiment, in S2, the dispersant is selected from Solsperse. TM 29000, Solsperse TM W210, Solsperse TM W75, Solsperse TM AC5160, Solsperse TM One or more of AC4380, the amount of dispersant is 2wt% to 8wt% of the mass of the modified fused silica powder.

[0022] In one embodiment, in step S3, the printing process is performed using a DLP photopolymerization device.

[0023] In step S4, the degreasing process is as follows:

[0024] Under an argon atmosphere, the maximum degreasing temperature is 650–800℃, the heating rate is 0.1–0.2℃ / min, the holding time is 120 min, and the furnace is cooled.

[0025] In step S5, the sintering process is as follows:

[0026] In an air environment, the sintering temperature is 1150℃~1400℃, the heating rate is 0.5~1℃ / min, the holding time is 120~180min, and the furnace is cooled.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] This invention provides a method for preparing high-strength fused silica ceramics using photopolymerization. By introducing silicon carbide (SiC) into fused silica powder, the method aims to reduce the curing depth and increase density. SiC particles, as a dark-colored ceramic powder, can be considered an inorganic dye. Through incorporation and blending, the absorbance of the ceramic slurry is increased, reducing ultraviolet light penetration and ultimately achieving the goal of reducing the curing depth. Simultaneously, SiC undergoes an oxidation reaction at high temperatures to generate SiO2 in situ. The newly generated SiO2 can connect the unsintered and dense original SiO2 particles in the matrix, thereby increasing the sintering density. In summary, this invention provides a method for preparing ceramics using photopolymerization by introducing SiC as an inorganic dye to reduce curing depth and increase sintering density. This method solves the technical problem of over-curing of fused silica during printing, which affects the accuracy of the formed parts, and addresses the technical problem of low sintering density and poor strength in fused silica ceramics prepared by current photopolymerization 3D printing.

[0029] In summary, compared with the existing ceramic preparation methods that commonly involve adding SiC to fused silica ceramic powder, this invention utilizes the high absorbance of SiC to solve the problem of high curing depth in the fused silica photopolymerization 3D printing process. Furthermore, through the in-situ generation of SiO2 by the oxidation behavior of SiC during atmospheric sintering, SiO2 particles are connected, thereby improving the sintering density of fused silica and increasing the sample strength. Attached Figure Description

[0030] Figure 1 This is a degreasing curve diagram of a fused silica part produced using photopolymerization molding technology in Embodiment 1 of the present invention;

[0031] Figure 2 This is a sintering curve of a fused silica part produced using photopolymerization molding technology in Embodiment 1 of the present invention. Detailed Implementation

[0032] To enable those skilled in the art to understand the features and effects of the present invention, the terms and expressions used in the specification and claims are explained and defined in general below. Unless otherwise specified, all technical and scientific terms used herein have the ordinary meaning understood by those skilled in the art regarding the present invention, and in case of conflict, the definitions in this specification shall prevail.

[0033] The theories or mechanisms described and disclosed herein, whether right or wrong, should not in any way limit the scope of the invention, that is, the contents of the invention can be implemented without being limited by any particular theory or mechanism.

[0034] In this document, all features defined by numerical ranges or percentage ranges, such as numerical values, quantities, contents, and concentrations, are for the sake of brevity and convenience only. Accordingly, descriptions of numerical ranges or percentage ranges should be considered as covering and specifically disclosing all possible sub-ranges and individual numerical values ​​(including integers and fractions) within those ranges.

[0035] In this article, unless otherwise specified, the terms “contains,” “includes,” “containing,” “has,” or similar terms cover the meanings of “composed of” and “mainly composed of”. For example, “A contains a” covers the meanings of “A contains a and others” and “A contains only a”.

[0036] For the sake of brevity, not all possible combinations of the technical features in each implementation scheme or embodiment are described herein. Therefore, as long as there is no contradiction in the combination of these technical features, the technical features in each implementation scheme or embodiment can be combined arbitrarily, and all possible combinations should be considered within the scope of this specification.

[0037] This invention provides a method for photopolymerization molding of high-strength fused silica ceramics, comprising the following steps:

[0038] S1. Powder modification: Fused silica powder is mixed with modifier one and modifier two to obtain a mixed powder, which is then dried and sieved to obtain modified fused silica powder.

[0039] S2. Preparation of fused silica ceramic photocurable slurry: The photosensitive resin system is composed of prepolymer I, prepolymer II, resin monomer I, resin monomer II, photoinitiator I, and photoinitiator II.

[0040] The dispersant is added to the photosensitive resin system and mixed evenly. Then, the modified fused silica powder and SiC powder obtained in step S1 are added and mixed evenly to obtain the fused silica ceramic photocurable slurry.

[0041] S3, Photopolymerization 3D Printing: The fused silica ceramic photopolymerization slurry obtained in step S2 is printed using a DLP photopolymerization device to obtain a fused silica ceramic green body.

[0042] S4. Green body degreasing: The fused silica ceramic green body obtained in step S3 is degreased according to the established process to obtain a degreased fused silica part.

[0043] S6. Sintering of fused silica ceramics: The fused silica degreased part obtained in step S4 is sintered according to the established process to obtain fused silica ceramics.

[0044] As a preferred option, the specific dosage of the above method is as follows:

[0045] In one embodiment, the wet milling is performed by adding alcohol, the wet milling time is 10-15 hours, and the mass ratio of alcohol to mixed powder is 1:1-1.5.

[0046] In one embodiment, the dispersant is added to the photosensitive resin system and mixed evenly, then homogenized using a homogenizer at a speed of 800 r / min to 1500 r / min for 30 to 60 seconds. The modified fused silica powder obtained in step S1 is added and mixed evenly with the SiC powder, then homogenized using a homogenizer at a speed of 1000 r / min to 2000 r / min for 1 to 3 minutes.

[0047] In one embodiment, the solid content of the fused silica ceramic photocurable slurry is 55 vol% to 65 vol%; the particle size of both the fused silica powder and the modified fused silica powder is 1 to 5 μm, and the particle size of the SiC powder is 200 to 500 nm; the amount of SiC powder used is 1 wt% to 5 wt% of the mass of the modified fused silica powder.

[0048] In one embodiment, the first modifier is selected from one or more of KH550, KH560, KH570, stearic acid, oleic acid, palmitic acid, and adipic acid, and the amount used is 1 wt% to 6 wt% of the mass of the modified fused silica powder; the second modifier is selected from one or more of polyethylene, polypropylene, polyacrylamide, polymaleic acid, polyethylene glycol, polyacrylic acid, and sodium polyacrylate, and the amount used is 1 wt% to 6 wt% of the mass of the modified fused silica powder.

[0049] In one embodiment, prepolymer one is selected from one or more of bisphenol A diglycidyl ether, brominated bisphenol F diglycidyl ether, polyurethane acrylate (PUA), and polyester acrylate (PEA); prepolymer two is selected from one or more of triethylene glycol divinyl ether, cyclohexyl-1,4-diethanol vinyl ether, and vinyl acetate; resin monomer one is selected from one or more of 1,6-hexanediol diacrylate (HDDA), trimethylolpropane triacrylate (TMPTA), and pentaerythritol tetraacrylate (PPTTA); resin monomer two is selected from one or more of isobornyl methacrylate (IBOMA), tripropylene glycol diacrylate (TPGDA), and dipentaerythritol hexaacrylate (DPHA). The ratio of prepolymer one, prepolymer two, resin monomer one, and resin monomer two is 1:3:8:8.

[0050] In one embodiment, the first photoinitiator is one or two of 2,4,6-trimethylbenzoyl)diphenylphosphine oxide (TPO) and phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (819); the second photoinitiator is one or more of phenyldiazofluoroborate, diaryliodonium salt, triaryl sulfide and benzoin dimethyl ether, and the ratio of the two photoinitiators is 1.5-2.5:0.5-1.5, and the total amount used is 1 wt% to 5 wt% of the total mass of the photosensitive resin system.

[0051] In one embodiment, the dispersant is selected from Solsperse. TM 29000, Solsperse TM W210, Solsperse TM W75, Solsperse TM AC5160, Solsperse TM One or more of AC4380, the amount of dispersant is 2wt% to 8wt% of the mass of the modified fused silica powder.

[0052] In one embodiment, the degreasing process is as follows: under an argon atmosphere, the maximum degreasing temperature is 650-800℃, the heating rate is 0.1-0.2℃ / min, the holding time is 120min, and the furnace is cooled.

[0053] In one embodiment, the sintering process is as follows: in an air environment, the sintering temperature is 1150℃~1400℃, the heating rate is 0.5~1℃ / min, the holding time is 120~180min, and the furnace is cooled.

[0054] The two core innovations of this invention are: first, the development of a photocurable fused silica slurry for 3D printing that uses SiC as a reinforcing phase and also functions as an inorganic dye; and second, the proposal of an innovative fused silica densification method, which is based on the oxidation reaction of SiC during sintering to generate SiO2 in situ, thereby effectively connecting the original SiO2 particles and achieving material densification.

[0055] The present invention will be further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Furthermore, it should be understood that after reading the teachings of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims.

[0056] The following examples use instruments and equipment conventional in the art. Experimental methods in the following examples, unless otherwise specified, are generally performed under conventional conditions or as recommended by the manufacturer. All raw materials used in the following examples are conventional commercially available products with specifications conventional in the art. In this specification and the following examples, unless otherwise specified, "%" refers to weight percentage, "parts" refers to parts by weight, and "ratio" refers to weight proportion.

[0057] Example 1:

[0058] 1) Powder modification: 2μm fused silica powder was mixed with 2.5wt% KH570 and 2wt% polyethylene glycol, and then wet-milled with alcohol for 12h. The mass ratio of alcohol to powder was 1:1. After drying and sieving, modified fused silica powder was obtained.

[0059] 2) Preparation of UV-curable slurry: The solid content of the UV-curable slurry is 65 vol%. The photosensitive resin system is composed of prepolymer bisphenol A diglycidyl ether, polyurethane acrylate (PUA), prepolymer dicyclohexyl-1,4-dimethylethanol vinyl ether, resin monomers 1,6-hexanediol diacrylate (HDDA), trimethylolpropane triacrylate (TMPTA), resin monomers di(tripropylene glycol diacrylate) (TPGDA), and photoinitiators 2,4,6-(trimethylbenzoyl)diphenylphosphine oxide (TPO) and diaryliodomonium salt. The ratio of prepolymer 1, prepolymer 2, resin monomer 1, and resin monomer 2 is 1:3:8:8, the ratio of photoinitiator 1 to photoinitiator 2 is 2:1, and the total amount of photoinitiator 1 and photoinitiator 2 is 2 wt% of the total mass of the photosensitive resin system. 4 wt% of dispersant Solsperse is added. TM Add 29000 to the photosensitive resin system, homogenize with a homogenizer at 1000 r / min for 30 s, then add the modified fused silica powder obtained in step 1) and 200 nm SiC powder. The amount of SiC powder is 5 wt% of the mass of the modified fused silica powder. Homogenize with a homogenizer at 2000 r / min for 2 min to obtain the fused silica ceramic photocurable slurry.

[0060] 3) Photopolymerization 3D printing: The fused silica photopolymerization slurry obtained in step 2) is printed using a DLP photopolymerization device to obtain fused silica ceramic green bodies.

[0061] 4) Degreasing of green billets: Under an argon atmosphere, the temperature is increased to 180℃ at a rate of 0.1℃ / min and held for 120 min. Then, the temperature is increased to 250℃ at a rate of 0.1℃ / min and held for 120 min. Next, the temperature is increased to 300℃ at a rate of 0.1℃ / min and held for 120 min. Then, the temperature is increased to 500℃ at a rate of 0.1℃ / min and held for 120 min. Next, the temperature is increased to 600℃ at a rate of 0.1℃ / min and held for 120 min. Finally, the temperature is increased to 700℃ at a rate of 0.2℃ / min and held for 120 min. The billets are then cooled in the furnace to complete the degreasing process.

[0062] 5) Ceramic sintering: Under air atmosphere, the temperature is raised to 600℃ at a rate of 0.5℃ / min and held for 180min. Then, the temperature is raised to 1300℃ at a rate of 1℃ / min and held for 180min. The mixture is then cooled in the furnace to obtain fused silica ceramic with a flexural strength of 48.7MPa.

[0063] This embodiment uses, as follows Figure 1 and Figure 2 The degreasing and sintering process curve shown is subjected to heat treatment.

[0064] Example 2:

[0065] 1) Powder modification: 3μm fused silica powder was mixed with 2wt% KH550 and 3wt% polyacrylamide, and then wet-milled with alcohol for 10h. The mass ratio of alcohol to powder was 1:1. After drying and sieving, modified fused silica powder was obtained.

[0066] 2) Preparation of UV-curable slurry: The solid content of the UV-curable slurry is 60 vol%. The photosensitive resin system is composed of prepolymer bisphenol A diglycidyl ether, prepolymer dicyclohexyl-1,4-dimethylethanol vinyl ether, resin monomer pentaerythritol tetraacrylate (PPTTA), resin monomer isobornyl dimethacrylate (IBOMA), dipropylene glycol diacrylate (TPGDA), and photoinitiators 2,4,6-(trimethylbenzoyl)diphenylphosphine oxide (TPO) and benzoin dimethyl ether. The ratio of prepolymer 1, prepolymer 2, resin monomer 1, and resin monomer 2 is 1:3:8:8, the ratio of photoinitiator 1 to photoinitiator 2 is 2.5:0.5, and the total amount of photoinitiator 1 and photoinitiator 2 is 5 wt% of the total mass of the photosensitive resin system. 2 wt% of dispersant Solsperse is added. TMW75 was added to the photosensitive resin system and homogenized for 45 seconds at 1000 r / min using a homogenizer. Then, the modified fused silica powder obtained in step 1) and 300 nm SiC powder were added. The amount of SiC powder was 3 wt% of the mass of the modified fused silica powder. The mixture was homogenized for 1 minute at 1800 r / min using a homogenizer to obtain the fused silica ceramic photocurable slurry.

[0067] 3) Photopolymerization 3D printing: The fused silica photopolymerization slurry obtained in step 2) is printed using a DLP photopolymerization device to obtain fused silica ceramic green bodies.

[0068] 4) Degreasing of green billets: Under an argon atmosphere, the temperature is increased to 220℃ at a rate of 0.1℃ / min and held for 120 min. Then, the temperature is increased to 280℃ at a rate of 0.1℃ / min and held for 120 min. Next, the temperature is increased to 340℃ at a rate of 0.1℃ / min and held for 120 min. Then, the temperature is increased to 520℃ at a rate of 0.1℃ / min and held for 120 min. Next, the temperature is increased to 600℃ at a rate of 0.1℃ / min and held for 120 min. Finally, the temperature is increased to 750℃ at a rate of 0.2℃ / min and held for 120 min. The billets are then cooled in the furnace to complete the degreasing process.

[0069] 5) Ceramic sintering: Under air atmosphere, the temperature is raised to 600℃ at a rate of 0.5℃ / min and held for 180min. Then, the temperature is raised to 1150℃ at a rate of 1℃ / min and held for 120min. The molten silica ceramic is cooled in the furnace to obtain a flexural strength of 40.6MPa.

[0070] Example 3:

[0071] 1) Powder modification: 5μm fused silica powder was mixed with 1wt% oleic acid and 3.5wt% polymaleic acid, and then wet-milled with alcohol for 15h. The mass ratio of alcohol to powder was 1:1.5. After drying and sieving, modified fused silica powder was obtained.

[0072] 2) Preparation of photocurable slurry: The solid content of the photocurable slurry is 58 vol%. The photosensitive resin system is composed of prepolymer bisphenol F diglycidyl ether bromide, prepolymer diethylene glycol divinyl ether, resin monomer 1,6-hexanediol diacrylate (HDDA), resin monomer isobornyl dimethacrylate (IBOMA), and photoinitiator phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (819) and photoinitiator di-triarylsulfonate. The ratio of prepolymer I, prepolymer II, resin monomer I, and resin monomer II is 1:3:8:8, the ratio of photoinitiator I to photoinitiator II is 1.5:1, and the total amount of photoinitiator I and photoinitiator II is 1 wt% of the total mass of the photosensitive resin system. 8 wt% of dispersant Solsperse is added. TM W210 was added to the photosensitive resin system and homogenized for 45 seconds at 1200 r / min using a homogenizer. Then, the modified fused silica powder obtained in step 1) and 200 nm SiC powder were added. The amount of SiC powder was 3 wt% of the mass of the modified fused silica powder. The mixture was homogenized for 1.5 minutes at 1500 r / min using a homogenizer to obtain the fused silica ceramic photocurable slurry.

[0073] 3) Photopolymerization 3D printing: The fused silica photopolymerization slurry obtained in step 2) is printed using a DLP photopolymerization device to obtain fused silica ceramic green bodies.

[0074] 4) Degreasing of green billets: Under an argon atmosphere, the temperature is increased to 200℃ at a rate of 0.1℃ / min and held for 120 min. Then, the temperature is increased to 300℃ at a rate of 0.1℃ / min and held for 120 min. Next, the temperature is increased to 380℃ at a rate of 0.1℃ / min and held for 120 min. Then, the temperature is increased to 550℃ at a rate of 0.1℃ / min and held for 120 min. Next, the temperature is increased to 600℃ at a rate of 0.1℃ / min and held for 120 min. Finally, the temperature is increased to 700℃ at a rate of 0.2℃ / min and held for 120 min. The billets are then cooled in the furnace to complete the degreasing process.

[0075] 5) Ceramic sintering: Under air atmosphere, the temperature is raised to 600℃ at a rate of 0.5℃ / min and held for 180min. Then, the temperature is raised to 1400℃ at a rate of 1℃ / min and held for 150min. The mixture is then cooled in the furnace to obtain fused silica ceramic with a flexural strength of 46.5MPa.

[0076] Example 4:

[0077] 1) Powder modification: 1μm fused silica powder was mixed with 3wt% palmitic acid and 3wt% sodium polyacrylate, and then wet-milled with alcohol for 11h. The mass ratio of alcohol to powder was 1:1. After drying and sieving, modified fused silica powder was obtained.

[0078] 2) Preparation of UV-curable slurry: The solid content of the UV-curable slurry is 55 vol%. The photosensitive resin system is composed of prepolymer bromopolyester acrylate (PEA), prepolymer vinyl diacetate, resin monomer trimethylolpropane triacrylate (TMPTA), resin monomer dipentaerythritol hexaacrylate (DPHA), and photoinitiators phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide (819) and diphenyl diazofluoroborate. The ratio of prepolymer I, prepolymer II, resin monomer I, and resin monomer II is 1:3:8:8, the ratio of photoinitiator I to photoinitiator II is 2.5:1.5, and the total amount of photoinitiator I and photoinitiator II is 3 wt% of the total mass of the photosensitive resin system. 5 wt% of dispersant Solsperse is added. TM AC5160 was added to the photosensitive resin system and homogenized for 60 seconds at 1000 r / min using a homogenizer. Then, the modified fused silica powder obtained in step 1) and 500 nm SiC powder were added. The amount of SiC powder was 1 wt% of the mass of the modified fused silica powder. The mixture was homogenized for 1 minute at 1500 r / min using a homogenizer to obtain the fused silica ceramic photocurable slurry.

[0079] 3) Photopolymerization 3D printing: The fused silica photopolymerization slurry obtained in step 2) is printed using a DLP photopolymerization device to obtain fused silica ceramic green bodies.

[0080] 4) Degreasing of green billets: Under an argon atmosphere, the temperature is increased to 215℃ at a rate of 0.1℃ / min and held for 120 min. Then, the temperature is increased to 320℃ at a rate of 0.1℃ / min and held for 120 min. Next, the temperature is increased to 380℃ at a rate of 0.1℃ / min and held for 120 min. Then, the temperature is increased to 450℃ at a rate of 0.1℃ / min and held for 120 min. Next, the temperature is increased to 650℃ at a rate of 0.1℃ / min and held for 120 min. Finally, the temperature is increased to 800℃ at a rate of 0.2℃ / min and held for 120 min. The billets are then cooled in the furnace to complete the degreasing process.

[0081] 5) Ceramic sintering: Under air atmosphere, the temperature is raised to 600℃ at a rate of 0.5℃ / min and held for 180min. Then, the temperature is raised to 1150℃ at a rate of 1℃ / min and held for 180min. The mixture is then cooled in the furnace to obtain fused silica ceramic with a flexural strength of 38.6MPa.

[0082] Example 5:

[0083] 1) Powder modification: 2μm fused silica powder was blended with 1wt% stearic acid and 1wt% polyethylene, and then wet-milled with alcohol for 12h. The mass ratio of alcohol to powder was 1:1. After drying and sieving, modified fused silica powder was obtained.

[0084] 2) Preparation of UV-curable slurry: The solid content of the UV-curable slurry is 65 vol%. The photosensitive resin system is composed of prepolymer bisphenol A diglycidyl ether, polyurethane acrylate (PUA), prepolymer dicyclohexyl-1,4-dimethylethanol vinyl ether, resin monomers 1,6-hexanediol diacrylate (HDDA), trimethylolpropane triacrylate (TMPTA), resin monomers di(tripropylene glycol diacrylate) (TPGDA), and photoinitiators 2,4,6-(trimethylbenzoyl)diphenylphosphine oxide (TPO) and diaryliodomonium salt. The ratio of prepolymer 1, prepolymer 2, resin monomer 1, and resin monomer 2 is 1:3:8:8, the ratio of photoinitiator 1 to photoinitiator 2 is 2:1, and the total amount of photoinitiator 1 and photoinitiator 2 is 2 wt% of the total mass of the photosensitive resin system. 4 wt% of dispersant Solsperse is added. TM AC4380 was added to the photosensitive resin system and homogenized for 30 seconds at 1000 r / min using a homogenizer. Then, the modified fused silica powder obtained in step 1) and 200 nm SiC powder were added. The amount of SiC powder was 5 wt% of the mass of the modified fused silica powder. The mixture was homogenized for 2 minutes at 2000 r / min using a homogenizer to obtain the fused silica ceramic photocurable slurry.

[0085] 3) Photopolymerization 3D printing: The fused silica photopolymerization slurry obtained in step 2) is printed using a DLP photopolymerization device to obtain fused silica ceramic green bodies.

[0086] 4) Degreasing of green billets: Under an argon atmosphere, the temperature is increased to 180℃ at a rate of 0.1℃ / min and held for 120 min. Then, the temperature is increased to 250℃ at a rate of 0.1℃ / min and held for 120 min. Next, the temperature is increased to 300℃ at a rate of 0.1℃ / min and held for 120 min. Then, the temperature is increased to 500℃ at a rate of 0.1℃ / min and held for 120 min. Next, the temperature is increased to 600℃ at a rate of 0.1℃ / min and held for 120 min. Finally, the temperature is increased to 700℃ at a rate of 0.2℃ / min and held for 120 min. The billets are then cooled in the furnace to complete the degreasing process.

[0087] 5) Ceramic sintering: Under air atmosphere, the temperature is raised to 600℃ at a rate of 0.5℃ / min and held for 180 min. Then, the temperature is raised to 1300℃ at a rate of 1℃ / min and held for 180 min. The mixture is then cooled in the furnace to obtain fused silica ceramic with a flexural strength of 48.7 MPa.

[0088] Example 6:

[0089] 1) Powder modification: 3μm fused silica powder was blended with 6wt% adipic acid and 6wt% polypropylene, and then wet-milled with alcohol for 10h. The mass ratio of alcohol to powder was 1:1. After drying and sieving, modified fused silica powder was obtained.

[0090] 2) Preparation of UV-curable slurry: The solid content of the UV-curable slurry is 60 vol%. The photosensitive resin system is composed of prepolymer bisphenol A diglycidyl ether, prepolymer dicyclohexyl-1,4-dimethylethanol vinyl ether, resin monomer pentaerythritol tetraacrylate (PPTTA), resin monomer isobornyl dimethacrylate (IBOMA), dipropylene glycol diacrylate (TPGDA), and photoinitiators 2,4,6-(trimethylbenzoyl)diphenylphosphine oxide (TPO) and benzoin dimethyl ether. The ratio of prepolymer 1, prepolymer 2, resin monomer 1, and resin monomer 2 is 1:3:8:8, the ratio of photoinitiator 1 to photoinitiator 2 is 2.5:0.5, and the total amount of photoinitiator 1 and photoinitiator 2 is 5 wt% of the total mass of the photosensitive resin system. 2 wt% of dispersant Solsperse is added. TM W75 was added to the photosensitive resin system and homogenized for 45 seconds at 1000 r / min using a homogenizer. Then, the modified fused silica powder obtained in step 1) and 300 nm SiC powder were added. The amount of SiC powder was 3 wt% of the mass of the modified fused silica powder. The mixture was homogenized for 1 minute at 1800 r / min using a homogenizer to obtain the fused silica ceramic photocurable slurry.

[0091] 3) Photopolymerization 3D printing: The fused silica photopolymerization slurry obtained in step 2) is printed using a DLP photopolymerization device to obtain fused silica ceramic green bodies.

[0092] 4) Degreasing of green billets: Under an argon atmosphere, the temperature is increased to 220℃ at a rate of 0.1℃ / min and held for 120 min. Then, the temperature is increased to 280℃ at a rate of 0.1℃ / min and held for 120 min. Next, the temperature is increased to 340℃ at a rate of 0.1℃ / min and held for 120 min. Then, the temperature is increased to 520℃ at a rate of 0.1℃ / min and held for 120 min. Next, the temperature is increased to 600℃ at a rate of 0.1℃ / min and held for 120 min. Finally, the temperature is increased to 750℃ at a rate of 0.2℃ / min and held for 120 min. The billets are then cooled in the furnace to complete the degreasing process.

[0093] 5) Ceramic sintering: Under air atmosphere, the temperature is raised to 600℃ at a rate of 0.5℃ / min and held for 180min. Then, the temperature is raised to 1150℃ at a rate of 1℃ / min and held for 120min. The molten silica ceramic is cooled in the furnace to obtain a flexural strength of 40.6MPa.

[0094] Comparative Example 1:

[0095] 1) Powder modification: 2μm fused silica powder was mixed with 2.5wt% KH570 and 2wt% polyethylene glycol, and then wet-milled with alcohol for 12h. The mass ratio of alcohol to powder was 1:1. After drying and sieving, modified fused silica powder was obtained.

[0096] 2) Preparation of UV-curable slurry: The solid content of the UV-curable slurry is 65 vol%. The photosensitive resin system is composed of prepolymer bisphenol A diglycidyl ether, polyurethane acrylate (PUA), prepolymer dicyclohexyl-1,4-dimethylethanol vinyl ether, resin monomers 1,6-hexanediol diacrylate (HDDA), trimethylolpropane triacrylate (TMPTA), resin monomers di(tripropylene glycol diacrylate) (TPGDA), and photoinitiators 2,4,6-(trimethylbenzoyl)diphenylphosphine oxide (TPO) and diaryl iodomonium salt. The ratio of prepolymer 1, prepolymer 2, resin monomer 1, and resin monomer 2 is 1:3:8:8, the ratio of photoinitiator 1 to photoinitiator 2 is 2:1, and the total amount of photoinitiator 1 and photoinitiator 2 is 2 wt% of the total mass of the photosensitive resin system. 4 wt% of dispersant Solsperse is added. TM Add 29000 to the photosensitive resin system, homogenize with a homogenizer at 1000 r / min for 30 s, then add the modified fused silica powder obtained in step 1) and 200 nm SiC powder, with the SiC powder amount being 6 wt%, and homogenize with a homogenizer at 2000 r / min for 2 min to obtain the fused silica ceramic photocurable slurry.

[0097] 3) Photopolymerization 3D printing: The fused silica photopolymerization slurry obtained in step 2) is printed using a DLP photopolymerization device to obtain fused silica ceramic green bodies.

[0098] 4) Degreasing of green billets: Under an argon atmosphere, the temperature is increased to 180℃ at a rate of 0.1℃ / min and held for 120 min. Then, the temperature is increased to 250℃ at a rate of 0.1℃ / min and held for 120 min. Next, the temperature is increased to 300℃ at a rate of 0.1℃ / min and held for 120 min. Then, the temperature is increased to 500℃ at a rate of 0.1℃ / min and held for 120 min. Next, the temperature is increased to 600℃ at a rate of 0.1℃ / min and held for 120 min. Finally, the temperature is increased to 700℃ at a rate of 0.2℃ / min and cooled with the furnace to complete the degreasing process.

[0099] 5) Ceramic sintering: Under air atmosphere, the temperature was increased to 600℃ at a rate of 0.5℃ / min and held for 180 min, then increased to 1200℃ at a rate of 1℃ / min and held for 180 min. The mixture was then cooled in the furnace to obtain fused silica ceramic with a flexural strength of 28.6 MPa. When the SiC powder addition was 6 wt%, unoxidized SiC particles were present, leading to a decrease in flexural strength.

[0100] This invention provides a method for preparing high-strength fused silica ceramics by photocuring. It utilizes the high light absorption rate of SiC powder, treating it as an inorganic dye to reduce the curing depth of the slurry. At the same time, it utilizes the in-situ oxidation reaction of SiC at high temperature to generate SiO2, thereby connecting the original SiO2 particles and promoting sintering densification.

[0101] The above content is only for illustrating the technical concept of the present invention and should not be construed as limiting the scope of protection of the present invention. Any modifications made to the technical solution based on the technical concept proposed in this invention shall fall within the scope of protection of the claims of this invention.

Claims

1. A method for preparing high-strength fused silica ceramic by photopolymerization molding, characterized in that, Includes the following steps: S1: Fused silica powder is mixed with modifier one and modifier two to obtain a mixed powder, which is then wet-milled, dried, and sieved to obtain modified fused silica powder; in S1, modifier one is one or more of KH550, KH560, KH570, stearic acid, oleic acid, palmitic acid, and adipic acid; the amount of modifier one is 1 wt% to 6 wt% of the mass of the modified fused silica powder; modifier two is one or more of polyethylene, polypropylene, polyacrylamide, polymaleic acid, polyethylene glycol, polyacrylic acid, and sodium polyacrylate; the amount of modifier two is 1 wt% to 6 wt% of the mass of the modified fused silica powder. S2: A photosensitive resin system is prepared by mixing prepolymer 1, prepolymer 2, resin monomer 1, resin monomer 2, photoinitiator 1, and photoinitiator 2; a dispersant is added to the photosensitive resin system and mixed evenly, and then modified fused silica powder and SiC powder are added and mixed evenly to prepare a fused silica ceramic photocurable slurry; the particle size of the SiC powder is 200~500 nm; the ratio of prepolymer 1, prepolymer 2, resin monomer 1, and resin monomer 2 is 1:3:8:

8. In step S2, prepolymer one is one or more of bisphenol A diglycidyl ether, brominated bisphenol F diglycidyl ether, polyurethane acrylate, and polyester acrylate; prepolymer two is one or more of triethylene glycol divinyl ether and cyclohexyl-1,4-diethanol vinyl ether; resin monomer one is one or more of 1,6-hexanediol diacrylate, trimethylolpropane triacrylate, and pentaerythritol tetraacrylate; and resin monomer two is one or more of isobornyl methacrylate, tripropylene glycol diacrylate, and pentaerythritol hexaacrylate. In step S2, the first photoinitiator is one or two of 2,4,6-(trimethylbenzoyl)diphenylphosphine oxide and phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide; the second photoinitiator is one or more of phenyl diazofluoroborate, diaryliodonium salt, triaryl sulfide and benzoin dimethyl ether. In step S2, the mass ratio of photoinitiator one to photoinitiator two is 1.5~2.5:0.5~1.5; the total amount of photoinitiator one and photoinitiator two is 1 wt%~5 wt% of the total mass of the photosensitive resin system. S3: Print the fused silica ceramic photocurable slurry to obtain a fused silica ceramic green body; S4: The fused silica ceramic green body is degreased to obtain a degreased fused silica part; the degreasing process is as follows: under an argon atmosphere, the maximum degreasing temperature is 650~800℃, the heating rate is 0.1~0.2℃ / min, the holding time is 120min, and the part is cooled with the furnace. S5: Sinter the fused silica degreased part to obtain fused silica ceramic; the sintering process is as follows: in an air environment, the sintering temperature is 1150℃~1400℃, the heating rate is 0.5~1℃ / min, the holding time is 120~180min, and the furnace is cooled. In S2, the SiC powder content is 1 wt% to 5 wt% of the mass of the modified fused silica powder.

2. The method for preparing high-strength fused silica ceramic by photopolymerization according to claim 1, characterized in that, In step S2, the solid content of the fused silica ceramic photocurable slurry is 55 vol% to 65 vol%.

3. The method for preparing high-strength fused silica ceramic by photopolymerization according to claim 1, characterized in that, In step S2, the particle size of both the modified fused silica powder and the fused silica powder is 1~5 μm.

4. The method for preparing high-strength fused silica ceramic by photopolymerization according to claim 1, characterized in that, In S2, the dispersant is selected from Solsperse. TM 29000, Solsperse TM W210, Solsperse TM W75, Solsperse TM AC5160, Solsperse TM One or more of AC4380, the amount of dispersant is 2 wt% to 8 wt% of the mass of the modified fused silica powder.