Method for recycling polybenzimidazole production waste liquid
By recycling waste liquid from polybenzimidazole production as a precipitant and washing liquid, the precipitation process was optimized, solving the waste liquid treatment problem, reducing production costs, and improving product quality.
Patent Information
- Application Number
- CN202310695243.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-12
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-06-12
AI Technical Summary
The waste liquid generated during the production of polybenzimidazole is complex and difficult to treat, which increases production costs and affects its industrialization process.
After precipitation and washing, the waste liquid generated during the production of polybenzimidazole is partially or completely recycled as a precipitant or washing liquid. Light components are then treated by distillation to reduce the consumption of precipitant and washing liquid and optimize the precipitation process.
It reduces the production cost of polybenzimidazole, improves product performance, reduces insoluble content, and enhances product quality.
Smart Images

Figure BDA0004281788390000051 
Figure BDA0004281788390000053 
Figure BDA0004281788390000061
Abstract
Description
Technical Field
[0001] This invention relates to the field of polybenzimidazole technology, and more specifically to a method for reusing waste liquid from polybenzimidazole production. Background Technology
[0002] Polybenzimidazole (PBI) is an aromatic heterocyclic polymer containing repeating benzimidazole structural units in its main chain. It is a high-performance engineering plastic with excellent high-temperature resistance, chemical stability, and mechanical properties. Its long-term service temperature can reach 375℃. It also exhibits excellent mechanical strength, flame retardancy, radiation stability, mechanical stability, electrical insulation, chemical stability, thermal stability, oxidation resistance, toughness, adhesion, and hygroscopicity. It can be used in extreme high-temperature, harsh chemical, and plasma environments, or in applications requiring high durability and abrasion resistance.
[0003] The synthesis of polybenzimidazole materials mainly involves two methods: melt polymerization and solution polymerization. Solution polymerization can prepare high-molecular-weight polybenzimidazoles and has a wider range of applicable monomers, making it advantageous for preparing functional polybenzimidazole materials. However, solution polymerization typically uses acidic solvents such as polyphosphoric acid and methanesulfonic acid, resulting in lower solid content and higher solvent consumption. Furthermore, post-polymerization processing and product purification and washing generate large amounts of complex waste liquid, which is difficult to treat and recycle, increasing the production cost of polybenzimidazole. Summary of the Invention
[0004] The purpose of this invention is to provide a method for reusing waste liquid from polybenzimidazole production. This method enables the waste liquid generated from solution polymerization to be reused, reducing the production cost of polybenzimidazole and promoting the industrialization of polybenzimidazole solution polymerization process.
[0005] To achieve the above objectives, the present invention provides a method for reusing waste liquid from the production of polybenzimidazole, the method comprising steps (1), (2) and (3A), or the method comprising steps (1), (2) and (3B):
[0006] (1) The reaction solution containing polybenzimidazole is contacted with a precipitant to precipitate, and the precipitate and the first waste liquid are obtained by solid-liquid separation.
[0007] (2) The precipitate is washed to obtain the second waste liquid;
[0008] (3A) The second waste liquid is returned to step (1) as at least part of the precipitant;
[0009] (3B) The light components obtained by distilling the first waste liquid and / or the second waste liquid; at least a portion of the light components are returned to step (1) as a precipitant; and / or, at least a portion of the light components are returned to step (2) as a washing liquid.
[0010] Through the above technical solution, the present invention can achieve the following beneficial effects:
[0011] (1) The present invention reduces the consumption of precipitant and / or washing liquid by recycling the first waste liquid generated during the precipitation process and / or the second waste liquid generated during the washing process, thereby reducing the production cost of polybenzimidazole.
[0012] (2) In a preferred embodiment, the present invention controls the diameter of a single bundle of polybenzimidazole-containing reaction liquid within a specific range by controlling the contact mode between the reaction liquid containing polybenzimidazole and the precipitant, thereby reducing the insoluble matter in the polybenzimidazole product and improving the product performance of polybenzimidazole. Detailed Implementation
[0013] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0014] In this invention, unless otherwise specified, the pressure is absolute pressure.
[0015] The present invention discloses a method for reusing waste liquid from the production of polybenzimidazole, the method comprising steps (1), (2) and (3A), or the method comprising steps (1), (2) and (3B):
[0016] (1) The reaction solution containing polybenzimidazole is contacted with a precipitant to precipitate, and the precipitate and the first waste liquid are obtained by solid-liquid separation.
[0017] (2) The precipitate is washed to obtain the second waste liquid;
[0018] (3A) The second waste liquid is returned to step (1) as at least part of the precipitant;
[0019] (3B) The light components obtained by distilling the first waste liquid and / or the second waste liquid; at least a portion of the light components are returned to step (1) as a precipitant; and / or, at least a portion of the light components are returned to step (2) as a washing liquid.
[0020] According to the present invention, when the alkalinity of the second waste liquid is low, it can be directly returned to step (1) as a precipitant. However, when the alkalinity of the second waste liquid is high, it can be mixed with freshly added precipitant as a partial precipitant before contacting the reaction solution containing polybenzimidazole for precipitation. Typically, the pH of the second waste liquid is 7-12. Therefore, preferably, in step (3A), at least a portion of the precipitant accounts for 50-100% by weight of the total amount of precipitant used in step (1).
[0021] The present invention can also distill and recycle the acidic waste liquid generated during the precipitation process and the alkaline waste liquid generated during the washing process. Preferably, in step (3B), the distillation of the first waste liquid and / or the second waste liquid includes: the first waste liquid and the second waste liquid are distilled separately; or, the first waste liquid and the second waste liquid are mixed to obtain a mixture, and then the mixture is distilled.
[0022] According to the present invention, preferably, the distillation process is carried out in a distillation column, which is a plate distillation column, preferably a sieve plate column with a pore size of 3 to 8 mm.
[0023] According to the present invention, preferably, the distillation process is carried out in a distillation column, which is filled with packing material. Preferably, the packing material is at least one of Raschig rings, Pall rings, stepped rings, arc-shaped saddle packing, spherical packing, corrugated packing, grid packing, and structured packing.
[0024] According to the present invention, preferably, the conditions of the distillation column include: an operating pressure of 0.0001-0.1 MPa; a top temperature of 10-100°C; and a bottom temperature of 50-200°C.
[0025] According to the present invention, preferably, the conditions for the first waste liquid to be separately distilled in the distillation column include: operating pressure of 0.0001-0.01 MPa; top temperature of 10-50°C; and bottom temperature of 50-200°C.
[0026] According to the present invention, preferably, the conditions for the second waste liquid to be separately distilled in the distillation column include: operating pressure of 0.005-0.1 MPa; top temperature of 30-100°C; and bottom temperature of 50-120°C.
[0027] According to the present invention, preferably, the conditions for the distillation column of the mixture include: operating pressure of 0.0005-0.1 MPa; top temperature of 10-100°C; and bottom temperature of 50-200°C.
[0028] In this invention, a light component is obtained at the top of the distillation column, and a concentrated liquid is obtained at the bottom of the column. The concentrated liquid is stored in a waste liquid tank or sent to a sewage treatment plant.
[0029] According to the present invention, preferably, the method further includes collecting the waste liquid in a waste liquid retention tank and then sending it into a distillation column for distillation.
[0030] According to the present invention, preferably, the light component obtained by distillation is cooled to 10-50°C and then returned to step (1) and / or step (2).
[0031] According to the present invention, preferably, in step (3B), at least a portion of the light components returned to step (1) accounts for 50-100% by weight of the total amount of precipitant used in step (1).
[0032] According to the present invention, preferably, in step (1), the total amount of precipitant used is in a weight ratio of 0.1-10:1 to the weight of the reaction solution containing polybenzimidazole.
[0033] According to the present invention, preferably, the reaction solution containing polybenzimidazole is brought into contact with the precipitant by controlling the diameter of a single bundle of reaction solution containing polybenzimidazole to be 0.1-2.5 cm (preferably 0.2-1.5 cm), and then gradually bringing it into contact with the precipitant.
[0034] In this invention, when the viscosity of the polybenzimidazole-containing reaction solution is low, the polybenzimidazole-containing reaction solution can gradually come into contact with the precipitant by gravity. When the viscosity of the polybenzimidazole-containing reaction solution is high, in order to ensure that the polybenzimidazole-containing reaction solution can be discharged smoothly, preferably, a certain pressure can be applied to the reaction vessel (polymerization vessel), for example, by using a pump or venting to apply a certain pressure to discharge the solution, thereby achieving the purpose of pressurization and thus enabling the polybenzimidazole-containing reaction solution to be discharged quickly.
[0035] According to the present invention, preferably, the precipitant is water and / or an alkaline aqueous solution. More preferably, the alkaline aqueous solution is at least one of an aqueous solution of an alkali metal hydroxide, an aqueous solution of an alkaline earth metal hydroxide, an aqueous solution of an alkali metal salt, an aqueous solution of an alkaline earth metal salt, and ammonia; even more preferably, at least one of ammonia, a saturated sodium carbonate aqueous solution, a potassium carbonate aqueous solution, a sodium bicarbonate aqueous solution, a potassium bicarbonate aqueous solution, a magnesium carbonate aqueous solution, a sodium hydroxide aqueous solution, and a potassium hydroxide aqueous solution.
[0036] According to the present invention, preferably, when the precipitant is an alkaline aqueous solution, the pH of the alkaline aqueous solution is ≤12.
[0037] According to the present invention, preferably, the reaction solution containing polybenzimidazole is obtained by: under polymerization reaction conditions, in an inactive atmosphere, polymerizing an aromatic component containing at least two groups of adjacent amino groups with an aromatic or aliphatic component containing at least two carboxyl groups to obtain a reaction solution containing polybenzimidazole.
[0038] According to the present invention, preferably, the aromatic component comprising at least two groups of ortho-amino groups is an aromatic tetraamine; more preferably, the aromatic tetraamine comprises 1-4 benzene rings; even more preferably, the aromatic tetraamine is selected from one or more of the following structures:
[0039]
[0040] Wherein, X is selected from oxygen atom, sulfur atom, carbonyl group, sulfonyl group, substituted or unsubstituted alkylene group, for example, -O-, -S-.
[0041] According to the present invention, preferably, the aromatic or aliphatic component containing at least two carboxyl groups has the structure shown in formula (1):
[0042]
[0043] Wherein, R is selected from aromatic rings, aromatic heterocycles, or hydrocarbon groups (e.g., alkane groups, cycloalkane groups, olefin groups, etc.); Y is hydrogen, aryl, or hydrocarbon group;
[0044] More preferably, the aromatic or aliphatic component containing at least two carboxyl groups is selected from one or more of the following structures:
[0045]
[0046] According to the present invention, preferably, the molar ratio of the aromatic component containing at least two groups of adjacent amino groups to the aromatic or aliphatic component containing at least two carboxyl groups is 1:0.8-1.2, more preferably 1:0.95-1.05.
[0047] According to the present invention, preferably, the polymerization reaction conditions include carrying out the polymerization reaction in the presence of a reaction medium, wherein the total molar amount of the aromatic component containing at least two groups of adjacent amino groups and the aromatic or aliphatic component containing at least two carboxyl groups is 1-160 mmol, preferably 2-100 mmol, relative to 100 g of the reaction medium.
[0048] According to the present invention, preferably, the reaction medium is a mixed solution of methanesulfonic acid and phosphorus pentoxide or polyphosphoric acid, wherein the mass ratio of methanesulfonic acid to phosphorus pentoxide is 6-16:1, more preferably 8-12:1.
[0049] According to the present invention, the polymerization conditions can be those commonly used in the art for solution polymerization. Preferably, the polymerization conditions include a temperature of 80-240°C and a time of 0.25-72 h. More preferably, the polymerization conditions include: first reacting at 100-160°C for 0.5-4 h, and then heating to 120-220°C for 1-24 h. Using the above polymerization conditions, functional polybenzimidazoles with higher molecular weights and fewer byproducts can be obtained.
[0050] According to the present invention, in order to make the reactants more fully contacted and improve the uniformity of the polymerization reaction, preferably, the polymerization is carried out under stirring, and the linear speed of the stirring is 0.05-1.0 m / s, more preferably 0.1-0.5 m / s.
[0051] According to the present invention, preferably, the washing includes alkaline washing and water washing. During the alkaline washing process, an alkaline solution can be used to wash the precipitate. More preferably, the alkaline solution is selected from at least one of aqueous solutions of alkali metal hydroxides, aqueous solutions of alkaline earth metal hydroxides, aqueous solutions of alkali metal salts, aqueous solutions of alkaline earth metal salts, and ammonia; further preferably, it is selected from at least one of ammonia, aqueous solutions of sodium carbonate, aqueous solutions of potassium carbonate, aqueous solutions of sodium bicarbonate, aqueous solutions of potassium bicarbonate, aqueous solutions of magnesium carbonate, aqueous solutions of sodium hydroxide, and aqueous solutions of potassium hydroxide.
[0052] According to the present invention, preferably, the alkaline solution used in the washing process has a mass fraction of 0.1-60 wt%.
[0053] In this invention, there is no particular limitation on the number of washes, and the alkaline solution can be used for 1-2 washes. Preferably, the amount of alkaline solution used during the washing process is such that the pH of the waste liquid generated from the last alkaline solution wash is 7-8.
[0054] In this invention, the number of water washes can be 1-3 times. Preferably, the amount of water used during the washing process is such that the pH of the waste liquid generated from the final water wash is 7-8.
[0055] According to the present invention, in order to better remove ions or acids adsorbed on the polymer surface, the method preferably further includes pulverizing the precipitate after washing with alkaline solution and then washing it with water. Pulverizing followed by washing with water can further remove residual acidic solvents.
[0056] According to the present invention, preferably, the method further includes drying the precipitate after washing with water at a temperature of 60-100°C; more preferably, the drying is carried out under a non-reactive atmosphere of 0.01-0.1 MPa.
[0057] In this invention, the inactive atmosphere used in the polymerization and drying processes is not particularly limited and can be any inactive atmosphere commonly used in the art. The inactive atmosphere can be provided by an inert gas and / or nitrogen; the inert gas can be at least one of helium, neon, argon, krypton, xenon and radon.
[0058] The present invention will be described in detail below through embodiments. In the following embodiments,
[0059] All raw materials used are commercially available products.
[0060] Example 1
[0061] (1) The reaction medium (methanesulfonic acid and phosphorus pentoxide) and the reaction monomers 3,3-diaminobenzidine (0.2 mol) and 4,4-dicarboxylic acid diphenyl ether (0.2 mol) were fed into the polymerization reactor through the feed pipeline. Under N2 atmosphere, the stirring linear speed was 0.31 m / s, and the mixture was stirred at 120℃ for 40 min. The temperature was then raised to 140℃ and the reaction was continued for 2 h to obtain a viscous polymerization reaction solution. The total weight of methanesulfonic acid and phosphorus pentoxide was 1.5 kg, and the weight ratio of methanesulfonic acid to phosphorus pentoxide was 10:1.
[0062] A precipitant (water, 2.4 kg) is added from the top of the settling vessel. The feed diameter and number of feed streams of the viscous polymerization reaction solution are then controlled via a top feed controller, allowing it to gradually contact the precipitant in the settling vessel to form precipitate and waste liquid. Specifically, the diameter of a single stream of polymerization reaction solution contacting the water is controlled to be 1.0 cm-1.5 cm, and the number of feed streams is one. Settling is carried out under stirring conditions, with a stirring linear velocity of 0.2 m / s in the settling vessel. The upper waste liquid after settling is discharged from the side outlet of the settling vessel and enters the first waste liquid storage tank, which is designated as the first waste liquid.
[0063] (2) Add 2.67 kg of potassium carbonate solution (10 wt%) to the top of the sedimentation tank to wash the precipitate. The resulting waste liquid (pH 7-8) is discharged through the pipeline on the side wall of the sedimentation tank and sent to the second waste liquid storage tank. The neutralized product is fed into the pulverizer from the bottom outlet and then sent to the treatment tank. Add water (2.4 kg) to the top inlet of the treatment tank to continue washing until neutral. The waste liquid after washing is discharged from the side wall to the second waste liquid storage tank. The washed product enters the dryer and is dried in a nitrogen atmosphere at 0.01 MPa and 80°C to obtain the product. The waste liquid in the second waste liquid storage tank is used as the second waste liquid.
[0064] (3) The first waste liquid and the second waste liquid are mixed to obtain a mixture, which is then fed into a distillation column. The distillation column is a 5mm aperture sieve plate column, and the conditions of the distillation column include: operating pressure of 0.01MPa; top temperature of 50℃; and bottom temperature of 90℃. The light component obtained at the top of the column is cooled to 30℃ and then returned to the settling vessel for recycling as a precipitant. The heavy component (concentrate) obtained at the bottom of the column is sent to a third waste liquid tank for storage. The distillation efficiency of the distillation column is 90%: 90% of the waste liquid can be recycled through distillation in the distillation column.
[0065] Example 2
[0066] The system and method of Example 1 were implemented, except that the diameter of the single-bundle polymerization reaction solution in contact with water was controlled to be 0.3 cm-0.5 cm. The first waste liquid, after distillation, was returned to the settling tank as a precipitant for recycling. The distillation conditions for the first waste liquid included: operating pressure of 0.001 MPa; top temperature of 10°C; and bottom temperature of 110°C. A light component was obtained at the top of the column and was returned to the settling tank as a precipitant for recycling. The second waste liquid, after distillation, was returned to the treatment tank as a washing liquid for recycling. The distillation conditions for the second waste liquid included: operating pressure of 0.01 MPa; top temperature of 50°C; and bottom temperature of 90°C. A light component was obtained at the top of the column, cooled to 30°C, and then returned to the treatment tank as a washing liquid for recycling.
[0067] Example 3
[0068] The system and method of Example 1 are implemented, except that after the second waste liquid reaches the waste liquid storage tank, it is directly returned to the settling vessel for recycling as a settling agent. The first waste liquid is sent to a distillation column, and the operating conditions of the distillation column include: operating pressure of 0.0001 MPa; top temperature of 10°C; and bottom temperature of 70°C. The light component obtained at the top of the column is returned to the treatment vessel for recycling as washing water. The heavy component (concentrate) obtained at the bottom of the column is sent to a third waste liquid tank for storage.
[0069] Example 4
[0070] The system and method of Example 1 were implemented, except that the diameter of the single-bundle polymerization reaction solution in contact with water was controlled to be 0.7 cm-1.0 cm.
[0071] Example 5
[0072] The system and method of Example 1 were implemented, except that the diameter of the single-bundle polymerization reaction solution in contact with water was controlled to be 2 cm-2.5 cm.
[0073] Comparative Example 1
[0074] The procedure is carried out according to the method in Example 1, except that the first and second waste liquids are not treated and are not recycled.
[0075] Comparative Example 2
[0076] The method and system of Comparative Example 1 are followed, except that the discharge diameter is not controlled (>3cm).
[0077] Test case
[0078] (1) The intrinsic viscosity (reflecting molecular weight) of polybenzimidazole was obtained by the Ubbelohde viscosity test: PBI powder was dissolved in concentrated sulfuric acid (98 wt%) to prepare a sulfuric acid solution with a concentration of 0.6 g / dL. The sulfuric acid solution was added to an Ubbelohde viscometer with a capillary inner diameter of 1.0–1.1 mm and stabilized in a constant temperature water bath at 25 °C for 30 min. The outflow time of the solution was recorded as t1, the outflow time of the concentrated sulfuric acid was recorded as t0, and the concentration of the polymer solution was recorded as C. The intrinsic viscosity of PBI was calculated according to Equations 1 and 2.
[0079] Increased specific viscosity
[0080] Intrinsic viscosity
[0081] (2) Insoluble content of polybenzimidazole solution: Add 0.2g of polybenzimidazole product and 9.8g of dimethyl sulfoxide (DMSO) to a flask, dissolve at 80℃ for 12 hours, centrifuge, separate the clear upper layer, weigh the mass of the residual filter residue, and the percentage of the residual filter residue to the total mass of the solution is the insoluble content.
[0082] The intrinsic viscosity, insoluble content, and total water consumption after five reactions of the final product are shown in Table 1.
[0083] Table 1
[0084]
[0085] Note: Water saving percentage refers to the amount of water saved compared to the control group where the waste liquid is not recycled.
[0086] As can be seen from the results in Table 1, the method of the present invention can not only reduce water consumption, but also save costs (waste liquid disposal costs are huge).
[0087] Examples 1-4, which employ the preferred embodiments of the present invention to control the slow contact between the viscous mixed solution containing the polymer product and the precipitant, have lower insoluble content, better solubility of the polybenzimidazole product, and significantly better product quality (significantly lower insoluble content).
[0088] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A method for reusing waste liquid from the production of polybenzimidazole, characterized in that, The method includes steps (1), (2) and (3): (1) The reaction solution containing polybenzimidazole is contacted with a precipitant to precipitate, and the precipitate and the first waste liquid are obtained by solid-liquid separation; (2) The precipitate is washed to obtain the second waste liquid; (3) The light components obtained by distilling the first waste liquid and / or the second waste liquid; at least a portion of the light components are returned to step (1) as a precipitant; and / or, at least a portion of the light components are returned to step (2) as a washing liquid, wherein the at least portion of the light components returned to step (1) accounts for 50-100% by weight of the total amount of precipitant used in step (1). The distillation process is carried out in a distillation column, the conditions of which include: operating pressure of 0.0001-0.1 MPa; top temperature of 10-100℃; bottom temperature of 50-200℃. The reaction solution containing polybenzimidazole is brought into contact with the precipitant by controlling the diameter of a single bundle of reaction solution containing polybenzimidazole to be 0.3-1.5 cm, and then gradually bringing it into contact with the precipitant. The precipitant is an aqueous and / or alkaline aqueous solution; the total amount of precipitant used is in a weight ratio of 10-0.1:1 to the weight of the reaction solution containing polybenzimidazole. The reaction solution containing polybenzimidazole is obtained by polymerizing 3,3-diaminobenzidine and 4,4-dicarboxylic acid diphenyl ether under polymerization conditions and in an inactive atmosphere. The polymerization conditions include: first reacting at 100-160℃ for 0.5-4h, and then heating to 120-220℃ for 1-24h.
2. The method according to claim 1, wherein, In step (3), the distillation of the first waste liquid and / or the second waste liquid includes: the first waste liquid and the second waste liquid are distilled separately; or, the first waste liquid and the second waste liquid are mixed to obtain a mixture, and then the mixture is distilled.
3. The method according to claim 2, wherein, The distillation process is carried out in a distillation column filled with packing material; And / or, the distillation process is carried out in a distillation column, which is a plate distillation column.
4. The method according to claim 3, wherein, The packing material is at least one of Raschig rings, Pall rings, step rings, arc saddle-shaped saddle packing, spherical packing, corrugated packing, grid packing, and structured packing.
5. The method according to claim 3, wherein, The distillation column is a sieve plate column with a pore size of 3-8 mm.
6. The method according to claim 2, wherein, The conditions for the first waste liquid to be separately distilled in a distillation column include: operating pressure of 0.0001-0.01 MPa; top temperature of 10-50℃; bottom temperature of 50-200℃. And / or, the conditions for the second waste liquid to be separately distilled in the column include: operating pressure of 0.005-0.1 MPa; top temperature of 30-100℃; bottom temperature of 50-120℃; And / or, the conditions for the distillation column of the mixture include: operating pressure of 0.0005-0.1 MPa; top temperature of 10-100℃; bottom temperature of 50-200℃.
7. The method according to claim 1, wherein, The light components obtained from distillation are cooled to 10-50°C and then returned to step (1) and / or step (2).
8. The method according to claim 1, wherein, The washing process includes alkaline washing and water washing.
Citation Information
Patent Citations
Preparation method of aromatic polybenzimidazole
CN102863620A
Waste alkali solution recycling method
CN105000742A