A two-component fluororesin-based anti-flash coating and a preparation method and application thereof
By designing a two-component fluoropolymer-based anti-flashover coating, the problems of easy aging of RTV coatings and the contradiction between hydrophobicity and anti-fouling performance are solved, achieving the effects of strong aging resistance, superhydrophobicity and high self-cleaning properties.
Patent Information
- Application Number
- CN202411294012.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-09-14
AI Technical Summary
Existing RTV coatings gradually lose their hydrophobic and antifouling properties after long-term use, easily forming large contact angle water droplets, increasing the risk of flashover, and the hydrophobicity and antifouling properties are contradictory.
A two-component fluoropolymer-based anti-flashover coating is adopted. By constructing a micro-nano rough structure through compounded fluoropolymers, multi-sized powder particles and additives, a coating with strong aging resistance, superhydrophobicity and high self-cleaning properties is designed.
It improves the coating's aging resistance and self-cleaning properties, reduces light energy absorption, enhances insulation performance, prevents the adhesion and accumulation of organic contaminants, and extends its effective service life.
Smart Images

Figure CN119119813B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of insulating and protective coatings for the power industry, and in particular relates to a two-component fluoropolymer-based anti-flashover coating, its preparation method, and its application. Background Technology
[0002] Room temperature vulcanized silicone rubber (RTV) and improved long-lasting PRTV (Persistent RTV) anti-pollution flashover coatings have been widely used in my country's power transmission and transformation projects since the early 1990s due to their advantages such as good hydrophobicity, hydrophobic migration, and the ability to be applied and molded on-site. They have played a good role in preventing pollution flashover accidents.
[0003] Analysis suggests that current RTV coatings have the following problems: (1) Due to the easy photoaging characteristics of silicone materials, their hydrophobic and antifouling properties gradually decrease after long-term use in the atmosphere, resulting in weak sustained effectiveness. The current effective period is mostly 5 to 8 years; (2) Due to the hydrophobic and oleophilic properties of silicone rubber coatings, the deposition of organic pollutants cannot be avoided. Under conditions of poor migration, large contact angle water droplets are easily formed on the surface, reducing insulation performance and increasing the probability of flashover; (3) The hydrophobicity of organic substances contradicts their antifouling properties, meaning that improving antifouling performance may reduce hydrophobicity and hydrophobic migration properties. Therefore, developing an antifouling flashover coating that simultaneously possesses strong aging resistance, superhydrophobicity, and high self-cleaning properties has significant scientific and application value. Summary of the Invention
[0004] To address the aforementioned problems, this invention provides a two-component fluoropolymer-based anti-flashover coating, its preparation method, and its application. The two-component fluoropolymer-based anti-flashover coating prepared by this invention constructs a micro-nano rough structure by compounding fluoropolymers, introducing multi-sized powder particles, and additives, thereby designing an anti-flashover coating with strong aging resistance, superhydrophobicity, and high self-cleaning properties.
[0005] Specifically, the technical solution of the present invention is as follows:
[0006] In a first aspect, the present invention provides a two-component fluoropolymer-based anti-flashover coating, comprising component A and component B; wherein component A comprises the following raw materials in parts by weight: 100 parts of fluoropolymer, 65-90 parts of filler, 10-15 parts of flame retardant, 1-3 parts of other additives, and 100 parts of dispersing solvent; and component B comprises 20-25 parts of curing agent.
[0007] Preferably, the fluororesin is a mixture of a copolymer of tetrafluoroethylene and alkyl vinyl esters and a copolymer of trifluorochloroethylene and alkyl vinyl esters.
[0008] Preferably, the filler comprises nano-sized silica, micron-sized silica, and nano-sized titanium dioxide;
[0009] The nano-sized silica has a particle size of 20–35 nm and its surface is treated with KH550 silane coupling agent; the micron-sized silica has a particle size of 2–5 μm and its surface is treated with KH550 silane coupling agent; and the nano-sized titanium dioxide has a particle size of 80–120 nm and its surface is treated with KH550 silane coupling agent.
[0010] Preferably, the flame retardant is selected from one or more of ammonium polyphosphate and alumina.
[0011] Preferably, the other additives include defoamers, leveling agents, wetting and dispersing agents, and adhesion promoters;
[0012] The defoamer is a mixture of BYK066 and BYK054; more preferably, the mass ratio of BYK066 to BYK054 is 1:1.
[0013] The leveling agent is BYK358N; the wetting and dispersing agent is BYK110; and the adhesion promoter is BYK4510.
[0014] Preferably, the dispersing solvent is a mixture of ethyl acetate and butyl acetate.
[0015] Preferably, the curing agent is a polyisocyanate curing agent; more preferably, the curing agent is selected from one or more of hexamethylene diisocyanate (HDI) and diphenylmethane diisocyanate (MDI).
[0016] A second aspect of the present invention provides a method for preparing the above-mentioned two-component fluoropolymer-based anti-flashover coating, comprising the following steps:
[0017] S1. A filler is prepared by mixing nano-sized silica, micron-sized silica, and nano-sized titanium dioxide;
[0018] S2. Add the filler to the mixture of butyl acetate and ethyl acetate to obtain a dispersion;
[0019] S3. Add the copolymer resin of tetrafluoroethylene and alkyl vinyl ester and the copolymer resin of trifluorochloroethylene and alkyl vinyl ester to the dispersion, and then heat the reaction to obtain the fluororesin dispersion.
[0020] S4, mixed with fluoropolymer dispersion, flame retardant, defoamer, leveling agent, wetting and dispersing agent and adhesion promoter, yields component A of the two-component fluoropolymer-based anti-flashover coating;
[0021] S5. Mix component A of the two-component fluoropolymer-based anti-flashover coating with the curing agent to obtain the two-component fluoropolymer-based anti-flashover coating.
[0022] Preferably, in step S1, the weight ratio of the nano-sized silica, the micro-sized silica, and the nano-sized titanium dioxide is 25-35:30-40:10-15.
[0023] Preferably, in step S2, the mass ratio of ethyl acetate to butyl acetate is 3:7.
[0024] Preferably, in step S3, the viscosity of the copolymer resin of tetrafluoroethylene and alkyl vinyl ester is 5000-6000 mPa·s, accounting for 40%-60% of the mass ratio of fluororesin, and the viscosity of the copolymer resin of trifluorochloroethylene and alkyl vinyl ester is 5000-6000 mPa·s, accounting for 40%-60% of the mass ratio of fluororesin.
[0025] Preferably, in step S3, the temperature of the heating reaction is 95-115°C, and the heating reaction time is 0.5h-1.5h.
[0026] More preferably, the heating reaction temperature is 105°C and the heating reaction time is 1 hour.
[0027] In a third aspect, the present invention provides the application of the two-component fluoropolymer-based anti-flashover coating described in the first aspect on the surface of power equipment and insulators.
[0028] In a fourth aspect, the present invention provides a method for applying the two-component fluoropolymer-based anti-flashover coating described in the first aspect to power equipment, comprising the following steps:
[0029] (1) Clean and dry the surface of the power equipment;
[0030] (2) Mix component A and component B of the two-component fluoropolymer-based anti-flashover coating and then apply it to the surface of the power equipment.
[0031] (3) After the coating has fully cured, an effective protective coating is obtained.
[0032] Preferably, the coating method is selected from one of air spraying, airless spraying, and brushing;
[0033] Preferably, the curing time is 20 to 24 hours.
[0034] In a fifth aspect, the present invention provides a method for applying the two-component fluoropolymer-based anti-flashover coating described in the first aspect to the surface of an insulator, comprising the following steps:
[0035] (1) Clean and dry the surface of the insulator;
[0036] (2) Mix component A and component B of the two-component fluoropolymer-based anti-flashover coating and then apply it to the surface of the insulator;
[0037] (3) After the coating has fully cured, an effective protective coating is obtained.
[0038] Preferably, the coating method is selected from one of air spraying, airless spraying, and brushing.
[0039] Preferably, the curing time is 20 to 24 hours.
[0040] One or more embodiments of the present invention have at least the following beneficial effects:
[0041] (1) The two-component fluoropolymer-based anti-flashover coating prepared by the present invention uses perfluoropolymer as the base material. Based on the fact that the carbon chain of perfluoropolymer is helical and the CF bond energy is large, the carbon-carbon bond is protected and the surface bond is broken and aged. At the same time, the synergistic interaction between the added powder particles can lead to the improvement of the overall performance. For example, the introduction of silicon-oxygen bonds in the silica powder material improves the stability of the overall structure of the coating system. The micro-nano rough surface structure introduced by the powder material forms diffuse reflection of light and reduces the absorption of light energy. Moreover, the added powder materials are all non-combustible substances, which can improve the overall flame retardancy of the coating system on the one hand, and the porous hard structure formed by the inorganic filler during the combustion process is also conducive to preventing combustion.
[0042] (2) The nano-sized titanium dioxide added in this invention has an organic photocatalytic degradation effect. Together with the low surface energy resin and the micro-nano structure of each powder in the system, it achieves the high self-cleaning property of the coating on organic and inorganic substances, avoiding the adhesion and accumulation of organic pollutants during long-term outdoor use.
[0043] (3) The synergistic effect between the components in this invention constructs a surface micro-nano rough structure, which makes the coating surface superhydrophobic and easily removes surface dirt in rainy weather, achieving high self-cleaning performance. Attached Figure Description
[0044] Figure 1 This is a scanning electron microscope image of the two-component fluoropolymer-based anti-flashover coating prepared in Example 2 of the present invention. Detailed Implementation
[0045] It should be noted that the following detailed descriptions are exemplary and intended to provide further illustration of the invention. Unless otherwise specified, all technical and scientific terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.
[0046] As mentioned above, the current RTV coatings have the following problems: (1) Due to the easy light aging characteristics of silicone materials, the hydrophobic and antifouling properties gradually decrease after long-term use in the atmosphere, and the continuous effective effect is not strong. The current effective period is mostly 5 to 8 years; (2) Due to the hydrophobic and oleophilic properties of silicone rubber coatings, the deposition of organic dirt cannot be avoided. Under the condition of poor migration, large contact angle water droplets are easily formed on the surface, which reduces the insulation performance and increases the probability of flashover; (3) The hydrophobicity of organic substances is contradictory to the antifouling performance, that is, while improving the antifouling performance, the hydrophobic performance and hydrophobic migration performance may be reduced.
[0047] Therefore, developing an anti-flashover coating that simultaneously possesses strong aging resistance, superhydrophobicity, and high self-cleaning properties is of significant scientific importance and application value.
[0048] In one specific embodiment of the present invention, a two-component fluoropolymer-based anti-flashover coating is provided, comprising component A and component B; wherein, component A comprises the following raw materials in parts by weight: 100 parts of fluoropolymer, 65-90 parts of filler, 10-15 parts of flame retardant, 1-3 parts of other additives, and 100 parts of dispersant; component B comprises 20-25 parts of curing agent.
[0049] In another specific embodiment of the present invention, the fluororesin is a mixture of a copolymer resin of tetrafluoroethylene and alkyl vinyl ester and a copolymer resin of trifluorochloroethylene and alkyl vinyl ester.
[0050] In another specific embodiment of the present invention, the filler includes nano-sized silica, micron-sized silica, and nano-sized titanium dioxide;
[0051] The nano-sized silica has a particle size of 20–35 nm and its surface is treated with KH550 silane coupling agent; the micron-sized silica has a particle size of 2–5 μm and its surface is treated with KH550 silane coupling agent; and the nano-sized titanium dioxide has a particle size of 80–120 nm and its surface is treated with KH550 silane coupling agent.
[0052] In another specific embodiment of the present invention, the flame retardant is selected from one or more of ammonium polyphosphate and alumina.
[0053] In another specific embodiment of the present invention, the other additives include defoamers, leveling agents, wetting and dispersing agents, and adhesion promoters;
[0054] The defoamer is a mixture of BYK066 and BYK054; more preferably, the ratio of BYK066 to BYK054 is 1:1.
[0055] The leveling agent is BYK358N; the wetting and dispersing agent is BYK110; and the adhesion promoter is BYK4510.
[0056] In another specific embodiment of the present invention, the dispersing solvent is a mixture of ethyl acetate and butyl acetate.
[0057] In another specific embodiment of the present invention, the curing agent is a polyisocyanate curing agent; more preferably, the curing agent is selected from one or more of hexamethylene diisocyanate (HDI) and diphenylmethane diisocyanate (MDI).
[0058] In another specific embodiment of the present invention, a method for preparing the above-mentioned two-component fluoropolymer-based anti-flashover coating is provided, comprising the following steps:
[0059] S1. A filler is prepared by mixing nano-sized silica, micron-sized silica, and nano-sized titanium dioxide;
[0060] S2. Add the filler to the mixture of butyl acetate and ethyl acetate to obtain a dispersion;
[0061] S3. Add the copolymer resin of tetrafluoroethylene and alkyl vinyl ester and the copolymer resin of trifluorochloroethylene and alkyl vinyl ester to the dispersion, and then heat the reaction to obtain the fluororesin dispersion.
[0062] S4, mixed with fluoropolymer dispersion, flame retardant, defoamer, leveling agent, wetting and dispersing agent and adhesion promoter, yields component A of the two-component fluoropolymer-based anti-flashover coating;
[0063] S5. Mix component A of the two-component fluoropolymer-based anti-flashover coating with the curing agent to obtain the two-component fluoropolymer-based anti-flashover coating.
[0064] In another specific embodiment of the present invention, in step S1, the weight ratio of the nano-sized silicon dioxide, the micron-sized silicon dioxide, and the nano-sized titanium dioxide is 25-35:30-40:10-15.
[0065] In another specific embodiment of the present invention, in step S2, the fractional ratio of ethyl acetate to butyl acetate is 3:7.
[0066] In another specific embodiment of the present invention, in step S3, the viscosity of the copolymer resin of tetrafluoroethylene and alkyl vinyl ester is 5000-6000 mPa·s, accounting for 40%-60% of the mass ratio of fluororesin, and the viscosity of the copolymer resin of trifluorochloroethylene and alkyl vinyl ester is 5000-6000 mPa·s, accounting for 40%-60% of the mass ratio of fluororesin.
[0067] In another specific embodiment of the present invention, in step S3, the temperature of the heating reaction is 95-115°C, and the heating reaction time is 0.5h-1.5h.
[0068] In another specific embodiment of the present invention, the heating reaction temperature is 105°C and the heating reaction time is 1 hour.
[0069] In another specific embodiment of the present invention, the application of the above-mentioned two-component fluoropolymer-based anti-flashover coating on the surface of power equipment and insulators is provided.
[0070] In another specific embodiment of the present invention, a method for applying the above-mentioned two-component fluoropolymer-based anti-flashover coating to power equipment is provided, comprising the following steps:
[0071] (1) Clean and dry the surface of the power equipment;
[0072] (2) Mix component A and component B of the two-component fluoropolymer-based anti-flashover coating and then apply it to the surface of the power equipment.
[0073] (3) After the coating has fully cured, an effective protective coating is obtained.
[0074] In another specific embodiment of the present invention, the coating method is selected from one of air spraying, airless spraying, and brush coating;
[0075] In another specific embodiment of the present invention, the curing time is 20 to 24 hours.
[0076] In another specific embodiment of the present invention, a method for applying the above-mentioned two-component fluoropolymer-based anti-flashover coating to the surface of an insulator is provided, comprising the following steps:
[0077] (1) Clean and dry the surface of the insulator;
[0078] (2) Mix component A and component B of the two-component fluoropolymer-based anti-flashover coating and then apply it to the surface of the insulator;
[0079] (3) After the coating has fully cured, an effective protective coating is obtained.
[0080] In another specific embodiment of the present invention, the coating method is selected from one of air spraying, airless spraying, and brush coating.
[0081] In another specific embodiment of the present invention, the curing time is 20 to 24 hours.
[0082] The present invention will be further described in detail below with reference to specific embodiments. It should be noted that the specific embodiments are explanations of the present invention and not limitations thereof.
[0083] Example 1 This embodiment provides a two-component fluoropolymer-based anti-flashover coating and its preparation method.
[0084] Paint formulation:
[0085] Component A: 100 parts of fluororesin (50 parts of a copolymer of 5500 mP.S tetrafluoroethylene and alkyl vinyl ester and 50 parts of a copolymer of 5500 mP.S trifluorochloroethylene and alkyl vinyl ester), 65 parts of filler (25 parts of 35nm nano-sized silica, 30 parts of 3um micron-sized silica, and 10 parts of 100nm nano-sized titanium dioxide), 10 parts of flame retardant (5 parts of ammonium polyphosphate and 5 parts of alumina), 3 parts of other additives (0.6 parts of defoamer, 0.4 parts of leveling agent, 1 part of wetting and dispersing agent, and 1 part of adhesion promoter), and 100 parts of dispersing solvent;
[0086] Component B: 25 parts of curing agent.
[0087] The coating preparation method includes the following steps:
[0088] (1) Weigh the mixture of butyl acetate and ethyl acetate according to the proportion, and first stir and mix them evenly;
[0089] (2) Weigh out the nano-sized silica, micron-sized silica, and nano-sized titanium dioxide according to the proportions, and add them to the stirred (1) in sequence until they are completely wetted and there are no hard lumps.
[0090] (3) The prepared (2) was ground and dispersed using a nano-horizontal mill for 0.5 h;
[0091] (4) Continue stirring and dispersing the prepared (3) dispersion, then add 50 parts of 5500 mP.S tetrafluoroethylene and alkyl vinyl ester copolymer resin and 50 parts of 5500 mP.S trifluorochloroethylene and alkyl vinyl ester copolymer resin, and continue stirring and dispersing for 1 hour.
[0092] (5) Transfer the prepared (4) to a heated reaction vessel and heat and stir it at a temperature of 105℃ for 1 hour;
[0093] (6) Transfer the prepared (5) to room temperature drying conditions (humidity <50%), add flame retardant and other additives, continue to stir and disperse to room temperature, fill and seal for later use, and obtain component A of the two-component fluoropolymer-based anti-flashover coating;
[0094] (7) Mix component A and component B of the two-component fluoropolymer-based anti-flashover coating to obtain the two-component fluoropolymer-based anti-flashover coating.
[0095] Example 2This embodiment provides a two-component fluoropolymer-based anti-flashover coating and its preparation method.
[0096] Paint formulation:
[0097] Component A: 100 parts of fluororesin (50 parts of a copolymer of 5500 mP.S tetrafluoroethylene and alkyl vinyl esters and 50 parts of a copolymer of 5500 mP.S trifluorochloroethylene and alkyl vinyl esters), 70 parts of filler (25 parts of 35 nm nano-sized silica, 35 parts of 3 μm micron-sized silica, and 10 parts of 100 nm nano-sized titanium dioxide), 10 parts of flame retardant (5 parts of ammonium polyphosphate and 5 parts of alumina), 3 parts of other additives (0.6 parts of defoamer, 0.4 parts of leveling agent, 1 part of wetting and dispersing agent, and 1 part of adhesion promoter), and 100 parts of dispersing solvent;
[0098] Component B: 25 parts of curing agent.
[0099] The coating preparation method includes the following steps:
[0100] (1) Weigh the mixture of butyl acetate and ethyl acetate according to the proportion, and first stir and mix them evenly;
[0101] (2) Weigh out the nano-sized silica, micron-sized silica, and nano-sized titanium dioxide according to the proportions, and add them to the stirred (1) in sequence until they are completely wetted and there are no hard lumps.
[0102] (3) The prepared (2) was ground and dispersed using a nano-horizontal mill for 0.5 h;
[0103] (4) Continue stirring and dispersing the prepared (3) dispersion, then add 50 parts of 5500 mP.S tetrafluoroethylene and alkyl vinyl ester copolymer resin and 50 parts of 5500 mP.S trifluorochloroethylene and alkyl vinyl ester copolymer resin, and continue stirring and dispersing for 1 hour.
[0104] (5) Transfer the prepared (4) to a heated reaction vessel and heat and stir it at a temperature of 105℃ for 1 hour;
[0105] (6) Transfer the prepared (5) to room temperature drying conditions (humidity <50%), add flame retardant and other additives, continue to stir and disperse to room temperature, fill and seal for later use, and obtain component A of the two-component fluoropolymer-based anti-flashover coating;
[0106] (7) Mix component A and component B of the two-component fluoropolymer-based anti-flashover coating to obtain the two-component fluoropolymer-based anti-flashover coating.
[0107] Example 3 This embodiment provides a two-component fluoropolymer-based anti-flashover coating and its preparation method.
[0108] Paint formulation:
[0109] The components include: 100 parts of fluororesin (50 parts of a copolymer of 5500 mP.S tetrafluoroethylene and alkyl vinyl ester and 50 parts of a copolymer of 5500 mP.S trifluorochloroethylene and alkyl vinyl ester), 75 parts of filler (30 parts of 35nm nano-sized silica, 35 parts of 3um micron-sized silica, and 10 parts of 100nm nano-sized titanium dioxide), 10 parts of flame retardant (5 parts of ammonium polyphosphate and 5 parts of alumina), 3 parts of other additives (0.6 parts of defoamer, 0.4 parts of leveling agent, 1 part of wetting and dispersing agent, and 1 part of adhesion promoter), and 100 parts of dispersing solvent;
[0110] Component B: 25 parts of curing agent.
[0111] The coating preparation method includes the following steps:
[0112] (1) Weigh the mixture of butyl acetate and ethyl acetate according to the proportion, and first stir and mix them evenly;
[0113] (2) Weigh out the nano-sized silica, micron-sized silica, and nano-sized titanium dioxide according to the proportions, and add them to the stirred (1) in sequence until they are completely wetted and there are no hard lumps.
[0114] (3) The prepared (2) was ground and dispersed using a nano-horizontal mill for 0.5 h;
[0115] (4) Continue stirring and dispersing the prepared (3) dispersion, then add 50 parts of 5500 mP.S tetrafluoroethylene and alkyl vinyl ester copolymer resin and 50 parts of 5500 mP.S trifluorochloroethylene and alkyl vinyl ester copolymer resin, and continue stirring and dispersing for 1 hour.
[0116] (5) Transfer the prepared (4) to a heated reaction vessel and heat and stir it at a temperature of 105℃ for 1 hour;
[0117] (6) Transfer the prepared (5) to room temperature drying conditions (humidity <50%), add flame retardant and other additives, continue to stir and disperse to room temperature, fill and seal for later use, and obtain component A of the two-component fluoropolymer-based anti-flashover coating;
[0118] (7) Mix component A and component B of the two-component fluoropolymer-based anti-flashover coating to obtain the two-component fluoropolymer-based anti-flashover coating.
[0119] Example 4 This embodiment provides a two-component fluoropolymer-based anti-flashover coating and its preparation method.
[0120] Paint formulation:
[0121] Component A: 100 parts of fluororesin (50 parts of a copolymer of 5500 mP.S tetrafluoroethylene and alkyl vinyl esters and 50 parts of a copolymer of 5500 mP.S trifluorochloroethylene and alkyl vinyl esters), 80 parts of filler (30 parts of 35 nm nano-sized silica, 35 parts of 3 μm micron-sized silica, and 15 parts of 100 nm nano-sized titanium dioxide), 10 parts of flame retardant (5 parts of ammonium polyphosphate and 5 parts of alumina), 3 parts of other additives (0.6 parts of defoamer, 0.4 parts of leveling agent, 1 part of wetting and dispersing agent, and 1 part of adhesion promoter), and 100 parts of dispersing solvent;
[0122] Component B: 25 parts of curing agent.
[0123] The coating preparation method includes the following steps:
[0124] (1) Weigh the mixture of butyl acetate and ethyl acetate according to the proportion, and first stir and mix them evenly;
[0125] (2) Weigh out the nano-sized silica, micron-sized silica, and nano-sized titanium dioxide according to the proportions, and add them to the stirred (1) in sequence until they are completely wetted and there are no hard lumps.
[0126] (3) The prepared (2) was ground and dispersed using a nano-horizontal mill for 0.5 h;
[0127] (4) Continue stirring and dispersing the prepared (3) dispersion, then add 50 parts of 5500 mP.S tetrafluoroethylene and alkyl vinyl ester copolymer resin and 50 parts of 5500 mP.S trifluorochloroethylene and alkyl vinyl ester copolymer resin, and continue stirring and dispersing for 1 hour.
[0128] (5) Transfer the prepared (4) to a heated reaction vessel and heat and stir it at a temperature of 105℃ for 1 hour;
[0129] (6) Transfer the prepared (5) to room temperature drying conditions (humidity <50%), add flame retardant and other additives, continue to stir and disperse to room temperature, fill and seal for later use, and obtain component A of the two-component fluoropolymer-based anti-flashover coating;
[0130] (7) Mix component A and component B of the two-component fluoropolymer-based anti-flashover coating to obtain the two-component fluoropolymer-based anti-flashover coating.
[0131] Example 5 This embodiment provides a two-component fluoropolymer-based anti-flashover coating and its preparation method.
[0132] Paint formulation:
[0133] Component A: 100 parts of fluororesin (50 parts of a copolymer of 5500 mP.S tetrafluoroethylene and alkyl vinyl esters and 50 parts of a copolymer of 5500 mP.S trifluorochloroethylene and alkyl vinyl esters), 85 parts of filler (35 parts of 35 nm nano-sized silica, 35 parts of 3 μm micron-sized silica, and 15 parts of 100 nm nano-sized titanium dioxide), 10 parts of flame retardant (5 parts of ammonium polyphosphate and 5 parts of alumina), 3 parts of other additives (0.6 parts of defoamer, 0.4 parts of leveling agent, 1 part of wetting and dispersing agent, and 1 part of adhesion promoter), and 100 parts of dispersing solvent;
[0134] Component B: 25 parts of curing agent.
[0135] The coating preparation method includes the following steps:
[0136] (1) Weigh the mixture of butyl acetate and ethyl acetate according to the proportion, and first stir and mix them evenly;
[0137] (2) Weigh out the nano-sized silica, micron-sized silica, and nano-sized titanium dioxide according to the proportions, and add them to the stirred (1) in sequence until they are completely wetted and there are no hard lumps.
[0138] (3) The prepared (2) was ground and dispersed using a nano-horizontal mill for 0.5 h;
[0139] (4) Continue stirring and dispersing the prepared (3) dispersion, then add 50 parts of 5500 mP.S tetrafluoroethylene and alkyl vinyl ester copolymer resin and 50 parts of 5500 mP.S trifluorochloroethylene and alkyl vinyl ester copolymer resin, and continue stirring and dispersing for 1 hour.
[0140] (5) Transfer the prepared (4) to a heated reaction vessel and heat and stir it at a temperature of 105℃ for 1 hour;
[0141] (6) Transfer the prepared (5) to room temperature drying conditions (humidity <50%), add flame retardant and other additives, continue to stir and disperse to room temperature, fill and seal for later use, and obtain component A of the two-component fluoropolymer-based anti-flashover coating;
[0142] (7) Mix component A and component B of the two-component fluoropolymer-based anti-flashover coating to obtain the two-component fluoropolymer-based anti-flashover coating.
[0143] Example 6 This embodiment provides a two-component fluoropolymer-based anti-flashover coating and its preparation method.
[0144] Paint formulation:
[0145] Component A: 100 parts of fluororesin (50 parts of a copolymer of 5500 mP.S tetrafluoroethylene and alkyl vinyl esters and 50 parts of a copolymer of 5500 mP.S trifluorochloroethylene and alkyl vinyl esters), 90 parts of filler (35 parts of 35 nm nano-sized silica, 40 parts of 3 μm micron-sized silica, and 15 parts of 100 nm nano-sized titanium dioxide), 10 parts of flame retardant (5 parts of ammonium polyphosphate and 5 parts of alumina), 3 parts of other additives (0.6 parts of defoamer, 0.4 parts of leveling agent, 1 part of wetting and dispersing agent, and 1 part of adhesion promoter), and 100 parts of dispersing solvent;
[0146] Component B: 25 parts of curing agent.
[0147] The coating preparation method includes the following steps:
[0148] (1) Weigh the mixture of butyl acetate and ethyl acetate according to the proportion, and first stir and mix them evenly;
[0149] (2) Weigh out the nano-sized silica, micron-sized silica, and nano-sized titanium dioxide according to the proportions, and add them to the stirred (1) in sequence until they are completely wetted and there are no hard lumps.
[0150] (3) The prepared (2) was ground and dispersed using a nano-horizontal mill for 0.5 h;
[0151] (4) Continue stirring and dispersing the prepared (3) dispersion, then add 50 parts of 5500 mP.S tetrafluoroethylene and alkyl vinyl ester copolymer resin and 50 parts of 5500 mP.S trifluorochloroethylene and alkyl vinyl ester copolymer resin, and continue stirring and dispersing for 1 hour.
[0152] (5) Transfer the prepared (4) to a heated reaction vessel and heat and stir it at a temperature of 105℃ for 1 hour;
[0153] (6) Transfer the prepared (5) to room temperature drying conditions (humidity <50%), add flame retardant and other additives, continue to stir and disperse to room temperature, fill and seal for later use, and obtain component A of the two-component fluoropolymer-based anti-flashover coating;
[0154] (7) Mix component A and component B of the two-component fluoropolymer-based anti-flashover coating to obtain the two-component fluoropolymer-based anti-flashover coating.
[0155] Comparative Example 1 :
[0156] Unlike Example 1, no nano-silica is added in step (2).
[0157] Comparative Example 2 :
[0158] The difference from Example 2 is that nano-silica and micron-silica are not added in step (2).
[0159] Comparative Example 3 :
[0160] The difference from Example 3 is that nano-titanium dioxide is not added in step (2).
[0161] Comparative Example 4 :
[0162] The difference from Example 1 is that component A contains 65 parts of filler (25 parts of 35nm nano-silica, 30 parts of 3um micron-silica, and 10 parts of micron-titanium dioxide).
[0163] Comparative Example 5 :
[0164] The difference from Example 4 is that no flame retardant is added in step (6).
[0165] Comparative Example 6 :
[0166] The difference from Example 5 is that no other auxiliary agents are added in step (6).
[0167] Comparative Example 7 :
[0168] The difference from Example 6 is that the fluororesin described in step (4) only includes a copolymer resin of tetrafluoroethylene and alkyl vinyl ester.
[0169] Experimental Example 1 :
[0170] This example provides the coating preparation and performance testing of the two-component fluororesin-based anti-pollution flashover coating prepared in Examples 1 to 6 and Comparative Examples 1 to 6.
[0171] Coating preparation method: Prepare insulators with clean and dry surfaces, thoroughly mix the above-mentioned coating component A and component B, apply the mixture to the insulator surface by air spraying, and cure and maintain it at room temperature (25°C, 50%<RH<85%) for 24 hours to obtain a 200μm protective coating.
[0172] Performance testing: The hydrophobic angle and rolling angle are tested using the static water contact angle method; the flame retardant rating is tested using the vertical burning method; the aging resistance is tested using 340nm wavelength ultraviolet light irradiation, and the time of discoloration, peeling, and shedding is observed every 24 hours; the self-cleaning property is tested using the glass bead method; the adhesion is tested using the circle cutting method.
[0173] The specific performance parameters are shown in Table 1 and Table 2:
[0174] Table 1 Performance test results of the examples
[0175] Example 1 2 3 4 5 6 Hydrophobic angle / ° 140 145 152 156 160 163 Roll angle / ° 9 9 7 7 3 3 Flame retardant rating FV-0 FV-0 FV-0 FV-0 FV-0 FV-0 Aging resistance 1500 1500 1500 1500 1500 1500 Self-cleaning 2 2 2 1 1 1 Adhesion 1 1 1 2 2 2
[0176] Table 2 shows the performance test results of the comparative examples.
[0177] Comparative Example 1 2 3 4 5 6 7 Hydrophobic angle / ° 128 110 135 130 149 157 148 Roll angle / ° >20 >30 >15 >15 12 4 10 Flame retardant rating FV-1 FV-2 FV-1 FV-1 FV-2 FV-1 FV-2 Aging resistance 1300 1100 1000 1000 1450 1400 1380 Self-cleaning 3 3 3 3 1 2 3 Adhesion 1 1 1 2 2 2 3
[0178] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A two-component fluoropolymer-based anti-flashover coating, comprising component A and component B; wherein, Component A contains the following raw materials by weight: 100 parts of fluororesin, 65-90 parts of filler, 10-15 parts of flame retardant, 1-3 parts of other additives, and 100 parts of dispersion solvent; Component B contains 20-25 parts of curing agent. The fluororesin is a mixture of a copolymer of tetrafluoroethylene and alkyl vinyl esters and a copolymer of trifluorochloroethylene and alkyl vinyl esters; the filler includes nano-sized silica, micron-sized silica, and nano-sized titanium dioxide; the flame retardant is selected from one or more of ammonium polyphosphate and alumina; the other additives include defoamers, leveling agents, wetting and dispersing agents, and adhesion promoters.
2. The two-component fluoropolymer-based anti-flashover coating as described in claim 1, characterized in that, The nano-sized silica has a particle size of 20-35 nm and its surface is treated with KH550 silane coupling agent; the micron-sized silica has a particle size of 2-5 μm and its surface is treated with KH550 silane coupling agent; the nano-sized titanium dioxide has a particle size of 80-120 nm and its surface is treated with KH550 silane coupling agent. The defoamer is a mixture of BYK066 and BYK054; the ratio of BYK066 to BYK054 is 1:1; the leveling agent is BYK358N; the wetting and dispersing agent is BYK110; and the adhesion promoter is BYK4510.
3. The two-component fluoropolymer-based anti-flashover coating as described in claim 1, characterized in that, The dispersing solvent is a mixture of ethyl acetate and butyl acetate; the curing agent is a polyisocyanate curing agent.
4. The two-component fluoropolymer-based anti-flashover coating as described in claim 3, characterized in that, The curing agent is selected from one or more of hexamethylene diisocyanate (HDI) and diphenylmethane diisocyanate (MDI).
5. A method for preparing a two-component fluoropolymer-based anti-flashover coating according to any one of claims 1 to 4, characterized in that, Includes the following steps: S1. A filler is prepared by mixing nano-sized silica, micron-sized silica, and nano-sized titanium dioxide; S2. Add the filler to the mixture of butyl acetate and ethyl acetate to obtain a dispersion; S3. Add the copolymer resin of tetrafluoroethylene and alkyl vinyl ester and the copolymer resin of trifluorochloroethylene and alkyl vinyl ester to the dispersion, and then heat the reaction to obtain the fluororesin dispersion. S4, mixed with fluoropolymer dispersion, flame retardant, defoamer, leveling agent, wetting and dispersing agent and adhesion promoter, yields component A of the two-component fluoropolymer-based anti-flashover coating; S5. Mix component A of the two-component fluoropolymer-based anti-flashover coating with the curing agent to obtain the two-component fluoropolymer-based anti-flashover coating.
6. The preparation method according to claim 5, characterized in that, In step S1, the weight ratio of the nano-sized silica, micron-sized silica, and nano-sized titanium dioxide is 25~35:30~40:10~15. In step S2, the fractional ratio of ethyl acetate to butyl acetate is 3:7; In step S3, the viscosity of the copolymer resin of tetrafluoroethylene and alkyl vinyl ester is 5000~6000 mPa·s, accounting for 40%~60% of the mass ratio of fluororesin, and the viscosity of the copolymer resin of trifluorochloroethylene and alkyl vinyl ester is 5000~6000 mPa·s, accounting for 40%~60% of the mass ratio of fluororesin.
7. The preparation method according to claim 5, characterized in that, In step S3, the temperature of the heating reaction is 95-115℃, and the heating reaction time is 0.5 h-1.5 h.
8. The preparation method according to claim 7, characterized in that, In step S3, the heating reaction temperature is 105°C and the heating reaction time is 1 h.
9. The application of the two-component fluoropolymer-based anti-flashover coating according to any one of claims 1 to 4 on the surface of power equipment and insulators.
10. A method of applying the two-component fluoropolymer-based anti-flashover coating according to any one of claims 1 to 4 to power equipment, comprising the following steps: (1) Clean and dry the surface of the power equipment; (2) Mix component A and component B of the two-component fluoropolymer-based anti-flashover coating and then apply it to the surface of the power equipment; (3) After the coating has fully cured, an effective protective coating is obtained; The coating method is selected from one of air spraying, airless spraying, and brushing; The curing time is 20~24 h.
11. A method for applying the two-component fluoropolymer-based anti-flashover coating according to any one of claims 1 to 4 to the surface of an insulator, comprising the following steps: (1) Clean and dry the surface of the insulator; (2) Mix component A and component B of the two-component fluoropolymer-based anti-flashover coating and then apply it to the surface of the insulator; (3) After the coating has fully cured, an effective protective coating is obtained; The coating method is selected from one of air spraying, airless spraying, and brushing. The curing time is 20~24 h.
Citation Information
Patent Citations
Super-hydrophobic conformal coating, and preparation method and application method thereof
CN107446424A
Super-hydrophobic high-self-cleaning solvent-free silicone rubber anti-pollution flashover coating as well as preparation method and application thereof