A method of preparing ssz-39 molecular sieve nanosheets
By controlling the water content and adding seed crystals to prepare monodisperse ultrathin SSZ-39 molecular sieve nanosheets, the problems of uneven crystal size and easy twinning growth in the existing technology are solved, and the catalytic and adsorption performance is improved.
Patent Information
- Application Number
- CN202411329028.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-09-24
AI Technical Summary
Existing methods for synthesizing SSZ-39 molecular sieves suffer from large and uneven crystal sizes, a tendency for twinning growth leading to agglomeration, and long micropores, which limit their efficiency in catalysis and adsorption.
Monodisperse ultrathin nanosheets were prepared by controlling the extremely low water content in the reaction system and adding SSZ-39 molecular sieve seed crystals, with the crystal thickness controlled to be below 30 nm.
The monodispersity and homogeneity of SSZ-39 molecular sieve were achieved, improving catalytic and adsorption performance and enhancing the adsorption selectivity of CO₂/N₂ and CO₂/CH₄ mixed gases.
Smart Images

Figure CN119143144B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of molecular sieves, specifically relating to a method for preparing SSZ-39 molecular sieve nanosheets. Background Technology
[0002] Boiling molecular sieves are a class of inorganic microporous materials with regular channel structures, widely used in gas adsorption and catalysis. When used as catalysts or adsorbents, the performance of molecular sieves is usually highly correlated with parameters such as crystal size, morphology, and aggregation state. Preparing ultrathin molecular sieve nanosheets (thickness below 100 nm) can significantly increase the specific surface area of molecular sieves and shorten the mass transfer path length within the crystal, thereby improving their performance in catalysis, adsorption, and other applications. SSZ-39 molecular sieve is an aluminosilicate with an AEI configuration, belonging to the orthorhombic crystal system. It is a typical eight-membered ring microporous molecular sieve with a three-dimensional channel structure distributed in […]. 100 ]、[ 110 ]and[ 001 Three directions, with a pore size of 3.8 Å. SSZ-39 molecular sieves have shown potential applications in gas adsorption and catalytic reactions. Zones et al. ( US-5958370 This report first describes the synthesis of SSZ-39 molecular sieve and its method: using a cyclic quaternary ammonium salt as a structure-directing agent, SSZ-39 was synthesized via transformation of USY molecular sieve, yielding a product with crystal sizes in the micrometer range. Existing literature largely follows the classic synthesis method published by Zones et al. Sano et al. used tetraethylphosphine hydroxide (TEPOH) as a structure-directing agent to prepare SSZ-39 molecular sieve via USY molecular sieve transformation. Chem. Lett. 2014, 43, 302-304 Its crystals have a cubic morphology of approximately 500 nm and exhibit obvious twinning. Patent CN202211679034.9 discloses a method for preparing nanoscale SSZ-39 molecular sieves, where crystallization is completed at a stirring speed of 50-300 rpm, and the synthesized SSZ-39 molecular sieves have a size of 100-600 nm. Xu et al. ( Microporous and Mesoporous Materials 312 (2021) 110736 SSZ-39 molecular sieve was synthesized by transcrystalline transformation of USY molecular sieve, yielding a plate-like SSZ-39 molecular sieve with a thickness of 200 nm. Xiao Fengshou et al. reported the successful synthesis of SSZ-39 molecular sieve using silica sol as the silicon source. ACS Appl. Mater. Interfaces 2019, 11, 23112-23117 However, the crystals agglomerate and grow, resulting in a very low yield.
[0003] The synthesis of existing SSZ-39 molecular sieves faces two main problems: firstly, the SSZ-39 crystals are large and non-uniform, with dimensions exceeding 200 nm in all three dimensions; secondly, SSZ-39 crystals are prone to twinning, leading to agglomeration and the formation of large particles. Consequently, the existing SSZ-39 molecular sieves have long micropores, restricting mass transfer and diffusion of guest molecules. This results in low efficiency when used as a catalyst, a tendency for carbon deposition, and slow adsorption rates and unsatisfactory adsorption effects when used for adsorption and separation. Summary of the Invention
[0004] To address the shortcomings of existing technologies for synthesizing SSZ-39 molecular sieves, this invention aims to provide a method for preparing monodisperse, ultrathin SSZ-39 molecular sieve nanosheet crystals. The key to achieving the synthesis of ultrathin SSZ-39 molecular sieves in this invention lies in removing moisture from the reaction system through evaporation and other means, controlling the water content in the sol to an extremely low level, and adding SSZ-39 molecular sieve as a seed crystal to induce synthesis. The preparation method provided by this invention is simple and can obtain ultrathin SSZ-39 molecular sieve nanosheets with good monodispersity and no twinning, with a thickness controllable to 30 nm. This significantly shortens the mass transfer channels within the crystal, effectively improving the catalytic and adsorption performance of the SSZ-39 molecular sieve.
[0005] To achieve the above-mentioned objectives, the present invention provides the following technical solution: A method for preparing SSZ-39 molecular sieve nanosheets, the preparation process includes the following steps: (1) Mix the silicon source, aluminum source, USY molecular sieve, template agent (SDA), sodium hydroxide and water and stir evenly. Continue stirring and aging for 1~72 hours to obtain a gel. The molar ratio of its effective components is: SiO2 / Al2O3=5~200, Na2O / SiO2=0.05~0.5, SDA / SiO2=0.1~1.0, H2O / SiO2=4~100.
[0006] (2) Add SSZ-39 molecular sieve seed crystals to the gel in step (1), stir evenly, and evaporate the water in the gel at 40~90 ℃ until the H2O / SiO2 ratio reaches a certain value. Then grind and crush it to obtain dry gel.
[0007] (3) The dry gel from step (2) is placed in a reaction vessel and crystallized at 130~220 °C for 1~9 days. The reaction product is collected by centrifugation and washed until neutral, and then dried at 40~80 °C. Finally, the template agent is removed by calcination at 450~650 °C for 4~10 hours to obtain SSZ-39 molecular sieve nanosheets.
[0008] Preferably, the silicon source includes one or more of sodium silicate, silica powder, silica sol, solid silica gel, or tetraethyl orthosilicate.
[0009] Preferably, in step (1), the aluminum source includes one or more of sodium aluminate, aluminum hydroxide, metallic aluminum, boehmite, or aluminates.
[0010] Preferably, in step (1), the SiO2 / Al2O3 molar ratio of the USY molecular sieve is 5~120.
[0011] Preferably, in step (1), the SDA is hydroxide. N,N -Dimethyl-3,5-dimethylpiperidinium hydroxide, hydroxide N, N - One or more of diethyl-2,6-dimethylpiperidinium, tetraethylphosphine hydroxide, tetrapropylphosphine hydroxide, tetrabutylphosphine hydroxide, or tetraethylammonium hydroxide.
[0012] Preferably, in step (1), the effective component SiO2 in the gel is provided by USY molecular sieve and silicon source, and the molar ratio of the two is 0~9 based on SiO2 (silicon source) / SiO2 (USY).
[0013] Preferably, in step (2), the molecular sieve seed crystal is SSZ-39 molecular sieve. The molar ratio of the gel prepared is: SiO2 / Al2O3 = 10~200, Na2O / SiO2 = 0.05~0.5, SDA / SiO2 = 0.01~1.0, H2O / SiO2 = 10~200. The gel is crystallized at 130~220 ℃ for 1~4 days. The product is collected by centrifugation and washed until neutral, then dried at 40~80 ℃ and calcined at 550 ℃ for 10 hours to remove the template agent.
[0014] Preferably, in step (2), the mass of the added SSZ-39 molecular sieve seed crystals is 0.5~20 wt% of the total mass of SiO2 in the gel in step (1).
[0015] Preferably, in step (2), the dry gel has a molar ratio of H2O / SiO2 = 0.1~4.
[0016] This invention provides monodisperse SSZ-39 molecular sieve nanosheets prepared by the preparation method described above, with a crystal thickness of less than 200 nm. Preferably, the crystal thickness of the SSZ-39 molecular sieve nanosheets is 100 nm, and more preferably, the crystal thickness of the SSZ-39 molecular sieve nanosheets is 30 nm.
[0017] In another aspect, the present invention provides an adsorption and separation application of the monodisperse SSZ-39 molecular sieve nanosheets, which are used as adsorption materials for CO2 and can be used to separate mixtures such as CO2 / N2 and CO2 / CH4.
[0018] Compared with existing technologies, the advantages of this invention are as follows: By controlling the extremely low water content in the synthetic gel and using SSZ-39 molecular sieve as a seed crystal, this invention synthesizes monodisperse SSZ-39 molecular sieves with a nanosheet morphology, with a crystal thickness of less than 100 nm, preferably 30 nm. The SSZ-39 molecular sieve nanosheets synthesized by this invention have uniform size, good monodispersity, and no crystal aggregation. The specific surface area of the SSZ-39 molecular sieve nanosheets synthesized by this invention is as high as 773 m². 2 / g, with ideal adsorption solution theoretical selectivity (IAST) greater than 1000 and 130 for CO2 / N2 and CO2 / CH4 mixtures of 15 / 85 (v / v) and 15 / 85 (v / v) respectively, it is suitable for capturing CO2 in gases such as natural gas and flue gas, and can also be used as a catalyst material for catalytic reactions such as SCR and MTO. Attached Figure Description
[0019] Figure 1 The images show the XRD patterns of the SSZ-39 molecular sieve nanosheets synthesized in Examples 1-6 and Comparative Example 1.
[0020] Figure 2 Scanning electron microscope (SEM) images of SSZ-39 molecular sieve nanosheets synthesized in Examples 1-3 and Comparative Examples 1-2.
[0021] Figure 3 This is a transmission electron microscope image of the SSZ-39 molecular sieve nanosheets synthesized in Example 1.
[0022] Figure 4 The image shows the CO2, N2, and CH4 adsorption isotherms of the SSZ-39 molecular sieve nanosheets synthesized in Example 1.
[0023] Figure 5 The image shows the CO2 / N2 penetration curve of the SSZ-39 molecular sieve nanosheets synthesized in Example 1.
[0024] Figure 6 The image shows the CO2 / CH4 penetration curve of the SSZ-39 molecular sieve nanosheets synthesized in Example 1. Detailed Implementation
[0025] The present invention will be further described below with reference to specific embodiments to enable those skilled in the art to better understand the present invention. These specific embodiments are only used to explain the present invention and do not affect the scope of protection of the present invention. Example 1
[0026] (1) 2.08 g silica sol (40 wt%), 0.14 g aluminum hydroxide, 0.92 g USY molecular sieve (SiO2 / Al2O3 molar ratio of 15), 0.18 g NaOH, and 2.6 g hydroxide N,N- dimethyl- 3,5 A 25% dimethylpiperidine solution and 3.0 g deionized water were mixed and stirred for 1 hour to obtain a gel. The molar ratio of the effective components was: SiO2 / Al2O3=15, Na2O / SiO2=0.08, SDA / SiO2=0.5, H2O / SiO2=10, of which the ratio of SiO2 (silicon source) / SiO2 (USY) was 1.
[0027] (2) Mix 6.9 g silica sol, 0.05 g aluminum hydroxide, 1.0 g USY molecular sieve, 1.02 g NaOH, and 6.9 g aluminum hydroxide. N,N- dimethyl- 3,5 A 25% dimethylpiperidine solution and 4.4 g deionized water were mixed and stirred for 3 hours to obtain a seed crystal synthesis sol. This sol was then transferred to a reaction vessel and heated at 160 °C. The reaction was carried out at ℃ for 3 days. The product was collected by centrifugation and washed until neutral. It was then dried at 80℃ and calcined at 550℃ for 10 hours to remove the template agent, thus obtaining SSZ-39 molecular sieve seed crystals.
[0028] (3) Add 0.07 g of the SSZ-39 seed crystals prepared in step (2) (2% of the mass of SiO2 in the gel) to the gel in step (1), stir evenly, place in a 90 ℃ heater, heat to evaporate the water, calculate the H2O / SiO2 ratio by weighing its mass change, until the molar ratio of H2O / SiO2 is 0.1, grind the gel thoroughly to form a dry powder dry gel.
[0029] (4) The dry gel from step (3) was transferred to a reaction vessel and crystallized at 140 °C for 7 days. After the reaction was completed, the product was collected by centrifugation, washed with deionized water until neutral, and then dried in an oven at 60 °C. The dried product was then calcined at 450 °C for 10 h to obtain activated SSZ-39 molecular sieve nanosheets, which were labeled as NS-1.
[0030] XRD pattern of NS-1 is shown below. Figure 1 This indicates that it is a pure SSZ-39 molecular sieve. The SEM image of NS-1 is shown below. Figure 2 a) indicates that it has a nanosheet-like morphology, uniform size, with crystal dimensions of 300 nm in length and width and a thickness of 30 nm. The transmission electron microscope image of NS-1 is shown below. Figure 3 This shows that its maximum crystal surface area is (001)Crystal planes; their gas adsorption isotherms are as follows Figure 4 As shown, at 100 kPa, the adsorption ratios of CO2 / N2 and CO2 / CH4 are 11 and 5, respectively, and their specific surface area and micropore volume are 773 m². 2 / g and 0.31 m 3 / g. To further demonstrate the CO2 separation performance of the synthesized SSZ-39 molecular sieve nanosheets, the breakthrough curves for CO2 / N2 and CO2 / CH4 mixtures at 15 / 85 v / v were tested at room temperature, as shown in the figure. Figures 5-6 As shown, SSZ-39 molecular sieve nanosheets NS-1 exhibit excellent CO2 / N2 and CO2 / CH4 separation performance, and can be used for gas adsorption and separation. Example 2
[0031] The synthesis steps of SSZ-39 molecular sieve were the same as in Example 1, except that in step (1), the SiO2 / Al2O3 molar ratio of USY molecular sieve was 120, and the silicon source was tetraethoxysilane; the molar ratio of effective components in the gel was SiO2 / Al2O3=200, Na2O / SiO2=0.2, SDA / SiO2=0.1, and H2O / SiO2=100; in step (3), the mass of SSZ-39 seed crystals added was 20 wt% of the total mass of SiO2 in the gel, and the gel was evaporated until the molar ratio of H2O / SiO2 was 4; in step (4), the reaction temperature was 130 ℃, and the crystallization time was 9 days. The synthesized product was calcined at 650 ℃ for 4 h and labeled as NS-2.
[0032] XRD pattern of NS-2 is shown below. Figure 1 This indicates that it is a pure SSZ-39 molecular sieve. The SEM image of NS-2 is shown below. Figure 2 b indicates that its size is uniform, with a length and width of 700 nm and a thickness of 100 nm. Example 3
[0033] The synthesis steps of SSZ-39 molecular sieve are the same as in Example 1, except that the template agent in step (1) is hydroxide. N,N- Diethyl-2,6-dimethylpiperidine solution (55%), sodium aluminate as the aluminum source, the molar ratio of SiO2 / Al2O3 in USY molecular sieve was 5, gel aging for 72 hours, the molar ratio of effective components in the gel was SiO2 / Al2O3=30, Na2O / SiO2=0.05, SDA / SiO2=1.0, H2O / SiO2=10; in step (3), SSZ-39 seed crystals were added at a mass of 0.5 wt% of the total mass of SiO2 in the gel, and the water was evaporated at 40 ℃ until the molar ratio of H2O / SiO2 in the dry gel was 1.4; in step (4), the reaction temperature was 160 ℃ and the crystallization time was 5 days. The synthesized product was calcined at 550 ℃ for 6 h and labeled as NS-3.
[0034] XRD pattern of NS-3 is shown below. Figure 1 This indicates that it is a pure SSZ-39 molecular sieve. The SEM image of NS-2 is shown below. Figure 2 c indicates that its size is uniform, with a length and width of 600 nm and a thickness of 70 nm. Example 4
[0035] The synthesis steps of SSZ-39 nanosheets were the same as in Example 1, except that no other silicon and aluminum sources were added during gel preparation in step (1). Only USY molecular sieve was added to provide silicon and aluminum sources, and the molar ratio of SiO2 (silicon source) / SiO2 (USY) was 0. The product was dried in an oven at 60 °C, and the dried product was calcined at 650 °C for 4 h. The product was labeled as NS-4.
[0036] XRD pattern of NS-4 is shown below. Figure 1 This indicates that it is a pure SSZ-39 molecular sieve. Its dimensions are uniform, with crystal length and width of 400 nm and a thickness of 30 nm. Example 5
[0037] The synthesis steps of SSZ-39 nanosheets are the same as in Example 1, except that in step (1), the template agent is hydroxide. N,N -Diethyl-2,6-dimethylpiperidinium, the molar ratio of effective components in the gel is SiO2 / Al2O3=5, Na2O / SiO2=0.5, SDA / SiO2=0.08, H2O / SiO2=4, and the molar ratio of SiO2 (silicon source) / SiO2 (USY) is 9; in step (4), the crystallization temperature is 220 ℃ and the synthesis time is 1 day. The product is labeled as NS-5.
[0038] XRD pattern of NS-5 is shown below. Figure 1 This indicates that it is a pure SSZ-39 molecular sieve. Its dimensions are uniform, with crystal length and width of 300 nm and a thickness of 30 nm. Example 6
[0039] The synthesis steps of SSZ-39 nanosheets are the same as in Example 1, except that the molar ratio of H2O / SiO2 in the dry gel in step (3) is 0.5; the crystallization synthesis temperature of the dry gel in step (4) is 180℃, and the reaction time is 3 days. The product is labeled as NS-6.
[0040] XRD pattern of NS-6 is shown below. Figure 1 This indicates that it is a pure SSZ-39 molecular sieve. Its dimensions are uniform, with crystal length and width of 400 nm and a thickness of 50 nm. Comparative Example 1
[0041] The synthesis steps of SSZ-39 molecular sieve are the same as those in Example 1, except that SSZ-39 molecular sieve seed crystals are not added in step (3); in step (4), the reaction temperature is 140 ℃ and the crystallization time is 9 days. The synthesized product is labeled as NS-7.
[0042] XRD pattern of NS-7 can be found Figure 1 This indicates that it is a pure SSZ-39 molecular sieve. Its SEM image is shown below. Figure 2 As shown in d, the product has non-uniform dimensions, with crystal length and width dimensions of 1~2 μm and a thickness of 300 nm. Figure 2 d). Comparative Example 2
[0043] The synthesis steps of SSZ-39 molecular sieve are the same as in Example 1, except that in step (3), the molar ratio of H2O / SiO2 in the gel is 5.0. The synthesized product is labeled as NS-8.
[0044] SEM images of NS-8 are shown below. Figure 2 e. Impurities were observed in the product in the figure, and the crystal size of SSZ-39 molecular sieve was about 5 μm, and the crystal thickness was greater than 500 nm.
Claims
1. A method for preparing SSZ-39 molecular sieve nanosheets, characterized in that, The preparation process includes the following steps: (1) Mix silicon source, aluminum source, USY molecular sieve, template agent (SDA), sodium hydroxide and water and stir evenly. Continue stirring and aging for 1~72 hours to obtain gel. The molar ratio of its effective components is: SiO2 / Al2O3=5~200, Na2O / SiO2=0.05~0.5, SDA / SiO2=0.1~1.0, H2O / SiO2=4~100; (2) Add SSZ-39 molecular sieve seed crystals to the gel in step (1), stir evenly, and then place at 40~90 o Evaporate the water in the gel at C until the H2O / SiO2 ratio reaches H2O / SiO2=0.1~4, then grind and pulverize it to obtain dry gel; (3) The dry gel from step (2) is placed in a reaction vessel and crystallized at 130~220 °C for 1~9 days. The reaction product is collected by centrifugation and washed until neutral, and then dried at 40~80 °C. Finally, the template agent is removed by calcination at 450~650 °C for 4~10 hours to obtain SSZ-39 molecular sieve nanosheets, wherein the crystal thickness of the SSZ-39 molecular sieve nanosheets is less than 100 nm.
2. The method for preparing SSZ-39 molecular sieve nanosheets according to claim 1, characterized in that, In step (1), the silicon source includes one or more of sodium silicate, silica powder, silica sol, solid silica gel or tetraethyl orthosilicate.
3. The method for preparing SSZ-39 molecular sieve nanosheets according to claim 1, characterized in that, In step (1), the aluminum source includes one or more of sodium aluminate, aluminum hydroxide, metallic aluminum, boehmite, or aluminates.
4. The method for preparing SSZ-39 molecular sieve nanosheets according to claim 1, characterized in that, In step (1), the SiO2 / Al2O3 molar ratio of the USY molecular sieve is 5~120.
5. The method for preparing SSZ-39 molecular sieve nanosheets according to claim 1, characterized in that, In step (1), the SDA is hydroxide. N,N -Dimethyl-3,5-dimethylpiperidinium hydroxide, hydroxide N,N - One or more of diethyl-2,6-dimethylpiperidinium, tetraethylphosphine hydroxide, tetrapropylphosphine hydroxide, tetrabutylphosphine hydroxide, or tetraethylammonium hydroxide.
6. The method for preparing SSZ-39 molecular sieve nanosheets according to claim 1, characterized in that, In step (1), the effective component SiO2 in the gel is provided by USY molecular sieve and silicon source. The molar ratio of the two is calculated based on SiO2, and the ratio of SiO2 provided by silicon source to SiO2 provided by USY molecular sieve is 0~9.
7. The method for preparing SSZ-39 molecular sieve nanosheets according to claim 1, characterized in that, In step (2), the molecular sieve seed crystal is SSZ-39 molecular sieve; the molar ratio of the gel preparation is: SiO2 / Al2O3=10~200, Na2O / SiO2=0.05~0.5, SDA / SiO2=0.01~1.0, H2O / SiO2=10~200; the gel is crystallized at 130~220 ℃ for 1~4 days, the product is collected by centrifugation and washed until neutral, then dried at 40~80 ℃, and then dried at 550 ℃. o Remove the template agent by calcining at C for 10 hours.
8. The method for preparing SSZ-39 molecular sieve nanosheets according to claim 1, characterized in that, In step (2), the mass of the added SSZ-39 molecular sieve seed crystals is 0.5~20 wt% of the total mass of SiO2 in the gel in step (1).
Citation Information
Patent Citations
Preparation method and application of nanoscale SSZ-39 molecular sieve
CN116199236A
Zeolite SSZ-39
US5958370A
A method for rapidly synthesizing an AEI molecular sieve through microwave heating
CN107285333A
Method of solid-phase synthesis of AEI molecular sieve and catalyst
CN107285334A