A method and system for manufacturing carbon fiber precursor

By adding a steam drawing machine and adjusting the coagulation bath parameters and drawing ratio, the carbon fiber precursor manufacturing method was optimized, solving the problem of low carbon fiber breaking strength and achieving efficient production of T700 grade carbon fiber precursor.

CN119145067BActive Publication Date: 2026-11-24JILIN TANGU CARBON FIBER CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411230055.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2026-11-24
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

The existing DMAC wet two-step process for manufacturing carbon fiber precursor has low breaking strength, and increasing the number of steam drawing machines or modifying the process route is costly and cannot effectively improve production efficiency.

Method used

By increasing the number of steam drawing machines, adjusting the temperature and DMAC concentration of the coagulation bath, and adjusting the drawing ratio of steam drawing and water washing, the manufacturing method of carbon fiber precursor is optimized, thereby improving the coagulation rate and strength of nascent fibers.

Benefits of technology

Without changing the process route, the strength of the nascent fiber was improved, enabling the produced carbon fiber precursor to reach the T700 level, reducing the breakage rate and the frequency of fuzzing, and lowering production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119145067B_ABST
    Figure CN119145067B_ABST
Patent Text Reader

Abstract

This invention discloses a method and system for manufacturing carbon fiber precursor. The spinning solution is ejected from a spinneret, drawn in a coagulation bath to obtain nascent fibers, followed by water washing, oiling, and drying. The fibers are then drawn through a steam drawing unit to obtain carbon fiber precursor. The steam drawing unit includes multiple parallel steam drawing machines. The number of nascent fiber spindles in the coagulation bath increases with the number of steam drawing machines. The temperature and / or DMAC concentration of the coagulation bath are adjusted accordingly based on the number of nascent fiber spindles. The beneficial effects of this invention are: by adjusting the coagulation bath temperature and DMAC concentration, the densification degree of the nascent fibers in the coagulation bath is improved, and the breaking strength of the nascent fibers is also improved, allowing the nascent fibers to withstand the greater drawing in the steam drawing unit, thereby obtaining carbon fiber precursor with higher strength and fewer fuzz.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of chemical fiber production, and specifically relates to a method and system for manufacturing carbon fiber precursor. Background Technology

[0002] Polyacrylonitrile (PAN)-based carbon fiber is a new material that developed rapidly in the 1960s. Due to its excellent properties such as light weight, high specific strength, high specific modulus, high temperature resistance, corrosion resistance, wear resistance, fatigue resistance, electrical conductivity, and thermal conductivity, it is widely used in military industries such as satellites, launch vehicles, tactical missiles, and spacecraft, and has become an indispensable material in the aerospace industry. High-quality carbon fiber precursors should possess characteristics such as high heat resistance, few pore structures, few surface defects, dense structure, and good tensile strength.

[0003] The traditional DMAC wet two-step process for manufacturing carbon fiber precursor uses only one steam drawing machine in the steam drawing process. While it offers high flexibility and production efficiency, the resulting carbon fiber filaments have a low breaking strength, below 4.5 GPA. To further improve the mechanical properties of the DMAC wet two-step process, the process route needs to be changed and the number of steam drawing machines increased, which incurs significant modification costs.

[0004] Furthermore, modifying the existing process is not feasible due to the limitations of the steam stretching machine's structure and dimensions on site, which prevent the installation of additional supporting equipment such as coagulation baths. If production capacity needs to be increased, a new factory building must be constructed, which is costly.

[0005] In addition, the tension of the nascent fibers near the steam drafting machine is too high, which can easily lead to production failures such as filament breakage if the spinning speed is not reduced. However, reducing the spinning speed will not effectively improve the production efficiency of the process, making this solution unsuitable for actual production.

[0006] In view of this, the present invention is proposed. Summary of the Invention

[0007] The technical problem to be solved by the present invention is to overcome the shortcomings of the prior art and provide a method for manufacturing carbon fiber precursor. By adjusting the operating parameters of the coagulation bath according to the increase of the steam drawing machine, the coagulation rate of the nascent fiber is accelerated and the strength of the nascent fiber is improved without changing the process route. This solves the problem that the performance of the nascent fiber decreases when the processing volume increases, and enables the produced carbon fiber precursor to reach the T700 level.

[0008] To solve the above-mentioned technical problems, the basic concept of the technical solution adopted by the present invention is: a method for manufacturing carbon fiber precursor, wherein the spinning solution is spun out by a spinneret, drawn in a coagulation bath to obtain nascent fibers, then washed and drawn with water, oiled, dried, and then drawn through a steam drawing unit to obtain carbon fiber precursor.

[0009] The steam drawing unit includes multiple parallel steam drawing machines. The number of nascent fibers in the coagulation bath increases with the number of steam drawing machines. The temperature and / or DMAC concentration of the coagulation bath are adjusted accordingly based on the change in the number of nascent fibers in the coagulation bath.

[0010] Furthermore, the coagulation bath is a multi-stage coagulation bath, with the temperature of each stage increasing as the number of nascent fiber spindles increases, and / or the DMAC concentration of each stage of the coagulation bath decreasing as the number of nascent fiber spindles increases.

[0011] Furthermore, with the number of steam stretching machines increased by n layers, the temperature of each coagulation bath was increased by (a*n) times, and the DMAC concentration of each coagulation bath was decreased by (b*n) times.

[0012] Among them, 2% ≤ a ≤ 8%, and 2% ≤ b ≤ 12%.

[0013] Furthermore, the temperature of the multi-stage solidification process is increased in stages, with the temperature of the first solidification bath between 50-70℃ and the temperature of the last solidification bath between 80-90℃.

[0014] Furthermore, the DMAC concentration in the multi-stage coagulation bath is decreased in a stepwise manner, with the DMAC concentration in the first stage coagulation bath between 50% and 70%, and the DMAC concentration in the last stage coagulation bath between 10% and 30%.

[0015] Furthermore, coagulation drawing stretches the nascent fibers at a first drawing ratio, and steam drawing stretches the nascent fibers at a second drawing ratio.

[0016] The first draw ratio decreases as the number of layers in the steam drawing machine increases, while the second draw ratio increases as the number of layers in the steam drawing machine increases.

[0017] Furthermore, as the number of steam drawing machines increases by n layers, the first drawing ratio decreases by (c*n) times, and the second drawing ratio increases by (d*n) times.

[0018] Among them, 4% ≤ c ≤ 20%; 14% ≤ d ≤ 30%.

[0019] Furthermore, the nascent fibers are drawn with a third drawing ratio after washing, and the nascent fibers are drawn with a fourth drawing ratio after drying.

[0020] When the number of steam drawing machines increases by n layers, the third drawing ratio decreases by (e*n) times, and the fourth drawing ratio decreases by (f*n) times.

[0021] Among them, 5% ≤ e ≤ 7%; 4% ≤ f ≤ 9%;

[0022] Preferably, (1-c)*(1-e)*(1-f)*(1+d)=1.

[0023] A carbon fiber precursor manufacturing system employs the control method of a carbon fiber precursor manufacturing system as described above, wherein each layer of the steam drawing machine is provided with a threading channel for the nascent fibers to pass through.

[0024] The upstream and downstream of the threading channel are respectively provided with a first guide roller group and a second guide roller group. Each bundle of nascent fibers produced by the coagulation bath is guided by the first guide roller group to pass through the corresponding threading channel, and then extends downstream through the second guide roller group.

[0025] Furthermore, each guide roller group includes at least one guide roller and a support roller disposed near the corresponding threading channel, and the axis of each threading channel is tangent to the peripheral sidewall of the corresponding support roller.

[0026] The rotational speeds of all the branch rollers in the guide roller assembly are equal;

[0027] Preferably, each steam drawing machine is arranged vertically, and the support rollers of each guide roller group are arranged vertically, with the guide roller closest to the support roller being lower than the lowest support roller or higher than the highest support roller.

[0028] The vertical tangent of the guide roller near the threading channel coincides with the vertical tangent of the corresponding branch rollers away from the threading channel. Each raw yarn extends from the first side of the first guide roller to the second side of the corresponding branch roller.

[0029] After adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art: by adjusting the operating parameters of the coagulation bath according to the increase of the steam drawing machine, the coagulation rate of the nascent fiber is accelerated and the strength of the nascent fiber is improved without changing the process route, so that the produced carbon fiber precursor can reach the T700 level.

[0030] Furthermore, by adjusting the draw ratio of the coagulation bath and the steam drawing unit, while keeping the total tension of the manufacturing system constant, the speed of the nascent fibers in the coagulation bath is reduced, the soaking time in the coagulation bath is extended, and the strength of the nascent fibers is improved, thereby enabling the nascent fibers to withstand the tension during steam drawing and further reducing the fiber breakage rate.

[0031] Finally, by adding support rollers at the upstream and downstream of the steam drawing machine, the extension path of each bundle of nascent fibers is reasonably adjusted to prevent the nascent fibers from rubbing against the surface of the steam drawing machine.

[0032] At the same time, the present invention has a simple structure, significant effects, and is suitable for widespread use.

[0033] The specific embodiments of the present invention will now be described in further detail with reference to the accompanying drawings. Attached Figure Description

[0034] The accompanying drawings, as part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments and descriptions of the invention are used to explain the invention, but do not constitute an undue limitation of the invention. Obviously, the drawings described below are merely some embodiments, and those skilled in the art can obtain other drawings based on these drawings without creative effort. In the drawings:

[0035] Figure 1 This is a schematic diagram of the steam drawing unit in the present invention when using a three-layer steam drawing machine.

[0036] In the diagram: 1. First guide roller group; 2. Steam drawing machine; 201. Threading channel; 3. Second guide roller group; 4. Guide roller; 5. Support roller; 6. Nascent fiber.

[0037] It should be noted that these accompanying drawings and textual descriptions are not intended to limit the scope of the invention in any way, but rather to illustrate the concept of the invention to those skilled in the art by referring to specific embodiments. Detailed Implementation

[0038] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments will be clearly and completely described below with reference to the accompanying drawings. The following embodiments are used to illustrate the present invention, but are not intended to limit the scope of the present invention.

[0039] In the description of this invention, it should be noted that the terms "upper", "lower", "front", "rear", "left", "right", "vertical", "inner", "outer", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limiting this invention.

[0040] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.

[0041] like Figure 1 As shown in the embodiment of the present invention, a method for manufacturing carbon fiber precursor is introduced. The spinning solution is spun out through a spinneret, drawn in a coagulation bath to obtain nascent fiber 6, then washed and drawn again, oiled, dried, and then drawn through a steam drawing unit to obtain carbon fiber precursor. The steam drawing unit includes multiple parallel steam drawing machines 2. The number of spindles of nascent fiber 6 in the coagulation bath increases with the number of steam drawing machines 2. The temperature and / or DMAC concentration of the coagulation bath are adjusted accordingly based on the change in the number of spindles of nascent fiber 6 in the coagulation bath.

[0042] In embodiments of the present invention, the number of steam drawing machines 2 is increased by n layers, and n sets of spinnerets are correspondingly added to the coagulation bath.

[0043] In embodiments of the present invention, the number of spinnerets increases with the increase of the number of steam drawing machines 2, and the number of spinnerets is controlled between 30 and 120.

[0044] In embodiments of the present invention, the coagulation bath is a multi-stage coagulation bath, wherein the temperature of each stage of the coagulation bath increases with the number of 6 spindles of nascent fibers, and / or the DMAC concentration of each stage of the coagulation bath decreases with the number of 6 spindles of nascent fibers.

[0045] In the embodiments of the present invention, the number of steam stretching machines 2 is increased by n layers, the temperature of each coagulation bath is increased by (a*n) times, and the DMAC concentration of each coagulation bath is reduced by (b*n) times; wherein, 2%≤a≤8%, 2%≤b≤12%.

[0046] In embodiments of the present invention, the temperature of multi-stage solidification is increased in a stepwise manner, with the temperature of the first-stage solidification bath between 50-70°C and the temperature of the last-stage solidification bath between 80-90°C.

[0047] In embodiments of the present invention, the DMAC concentration in the multi-stage coagulation bath decreases in a stepwise manner, with the DMAC concentration in the first-stage coagulation bath between 50% and 70%, and the DMAC concentration in the last-stage coagulation bath between 10% and 30%.

[0048] In embodiments of the present invention, solidification drawing stretches the original filament at a first drawing ratio, and steam drawing stretches the original filament at a second drawing ratio; the first drawing ratio and the second drawing ratio are adjusted according to the number of layers in the steam drawing machine 2.

[0049] In embodiments of the present invention, the first draw ratio decreases as the number of layers in the steam drawing machine 2 increases, and the second draw ratio increases as the number of layers in the steam drawing machine 2 increases.

[0050] In embodiments of the present invention, the number of steam drawing machines 2 is increased by n layers, the first drawing ratio is reduced by (c*n) times, and the second drawing ratio is increased by (d*n) times; 4%≤c≤20%; 14%≤d≤30%; preferably, 6%≤c≤16%; 19%≤d≤26%; more preferably, 8%≤c≤12%; 22%≤d≤24%.

[0051] In embodiments of the present invention, the nascent fiber 6 is drawn using a third drawing ratio after washing, and the nascent fiber 6 is drawn using a fourth drawing ratio after drying; the number of steam drawing machines 2 is increased by n layers, the third drawing ratio is reduced by (e*n) times, and the fourth drawing ratio is reduced by (f*n) times; wherein, 5%≤e≤7%; 4%≤f≤9%; (1-c)*(1+d)*(1-e)*(1-f)=1; preferably, 5.5%≤e≤6.3%; 6%≤f≤7%.

[0052] In embodiments of the present invention, during the oiling process, the length of the oiling immersion does not change with the increase in the number of steam stretching machines 2.

[0053] In the embodiments of the present invention, in the drying process, 10-30 steam hot rollers are used for drying, and the temperature of each steam hot roller increases in a stepwise manner.

[0054] In embodiments of the present invention, the temperature of each steam-heated roller in the drying process increases with the increase of the number of steam stretching machines 2; preferably, when the number of steam stretching machines 2 increases by n layers, the temperature of each steam-heated roller increases by (e*n) times; wherein, 4%≤e≤20%; preferably, e=15%.

[0055] In an embodiment of the present invention, the temperature of the first steam-heated roller is greater than or equal to 60°C and less than or equal to 90°C; the temperature of the last steam-heated roller is greater than or equal to 150°C and less than or equal to 175°C.

[0056] In an embodiment of the present invention, a carbon fiber precursor manufacturing system is also introduced, which adopts a carbon fiber precursor manufacturing method as described above. Each layer of steam drawing machine 2 is provided with a threading channel 201 for the nascent fibers 6 to pass through. A first guide roller group 1 and a second guide roller group 3 are respectively provided upstream and downstream of the threading channel 201. Each bundle of nascent fibers 6 produced by the coagulation bath is guided by the first guide roller group 1 to pass through the corresponding threading channel 201, and then extends downstream through the second guide roller group 3.

[0057] With the above settings, the nascent fibers 6 after oiling and drying are dispersed into the threading channel 201 of the corresponding steam drawing machine 2 by the first guide roller group 1, and then converged and extended downstream by the second guide roller 4, so that the nascent fibers 6 are arranged in an orderly manner, and the nascent fibers 6 are prevented from tangling and knotting during the dispersion and convergence process.

[0058] In embodiments of the present invention, each guide roller group includes at least one guide roller 4 and a support roller 5 disposed near the corresponding threading channel 201, and the axis of each threading channel 201 is tangent to the peripheral sidewall of the corresponding support roller 5; the rotational speed of each support roller 5 in the guide roller group is equal.

[0059] By setting the above settings and by setting the corresponding support rollers 5, the guide roller group is not increased by the same multiple as the number of steam drawing machines 2. This reduces the cost of the carbon fiber precursor manufacturing system while ensuring stable operation.

[0060] Furthermore, by making each support roller 5 tangent to the axis of the corresponding guide channel, the extension direction of the nascent fiber 6 extending downstream from the support roller 5 coincides with the axis of the threading channel 201, thereby making the nascent fiber 6 extend straight into the threading channel 201.

[0061] Finally, by making the rotational speed of each branch roller 5 of each guide roller group equal, the linear velocity and draw ratio of the nascent fiber 6 in each threading channel 201 are equal, thereby making the parameters of the carbon fiber precursor processed by each steam drawing machine 2 equal.

[0062] In embodiments of the present invention, each threading channel 201 is arranged in parallel to each other; preferably, each threading channel 201 is arranged horizontally.

[0063] In the embodiments of the present invention, the axis of each support roller 5 is perpendicular to the axis of the corresponding threading channel 201.

[0064] In an embodiment of the present invention, each bundle of nascent fibers 6 is wound onto the corresponding support roller 5 via the guide roller 4 of the first guide roller group 1, and extends to the corresponding threading channel 201, and then wound onto the corresponding support roller 5 of the second guide roller 4 via each threading channel 201, and extends to the guide roller 4 of the second guide roller group 3.

[0065] In the embodiments of the present invention, each steam drawing machine 2 is arranged vertically, and each guide roller group's support roller 5 is arranged vertically. The guide roller 4 closest to the support roller 5 is lower than the lowest support roller 5 or higher than the highest support roller 5. The vertical tangent of the guide roller 4 near the threading channel 201 coincides with the vertical tangent of the corresponding support roller 5 away from the threading channel 201. Each raw yarn extends from the first side of the first guide roller 4 to the second side of the corresponding support roller 5.

[0066] Specifically, each branch roller 5 is higher than the corresponding guide roller 4, and the horizontal tangent of the upper side wall of each branch roller 5 coincides with the axis of the corresponding threading channel 201; or, each branch roller 5 is lower than the corresponding guide roller 4, and the horizontal tangent of the lower side wall of each branch roller 5 coincides with the axis of the corresponding threading channel 201.

[0067] With the above configuration, each bundle of nascent fibers 6 extends vertically from the guide roller 4 of the first guide roller group 1, and when it reaches the corresponding support roller 5, it bends 90 degrees horizontally around the circumferential side of the support roller 5 before extending horizontally into the corresponding threading channel 201. Then, each carbon fiber filament processed by the steam drawing machine 2 extends downstream horizontally from the corresponding threading channel 201, and bends 90 degrees vertically around the corresponding support roller 5 of the second guide roller group 3 before converging on the guide roller 4 and extending downstream. This makes the distribution of nascent fibers 6 more reasonable, avoiding the entanglement of nascent fibers 6 or the breakage caused by excessive friction between nascent fibers 6 and the surface of the steam drawing machine 2.

[0068] Example 1

[0069] (1) After the prepared spinning solution is sprayed out through the spinneret, it enters the multi-stage coagulation bath process to obtain nascent fiber 6.

[0070] The first stage coagulation bath has a DMAC concentration of 70% and a temperature of 50℃; the last stage coagulation bath has a DMAC concentration of 30% and a temperature of 80℃; and the first draw ratio of the coagulation bath is 2.

[0071] (2) After being washed, stretched, oiled, and dried, the nascent fiber 6 extends into the steam stretching unit;

[0072] The third stretching ratio of the water washing stretching is 1.8, the oiling immersion length of the oiling process is 1.5 meters, and the fourth stretching ratio of the drying process is 1.2; the temperature of the first steam hot roller is 80℃, and the temperature of the last steam hot roller is 170℃.

[0073] (3) The dried nascent fibers 6 are guided to a steam drawing unit with two layers of steam drawing machines 2. Each bundle of nascent fibers 6 is drawn by the corresponding steam drawing machine 2 to obtain carbon fiber precursor.

[0074] The second draw ratio of the steam drawing unit is 1.9;

[0075] The total draw ratio of the carbon fiber precursor manufacturing system is 10, the breakage rate is 63%, and the fuzzing frequency is 65%.

[0076] It should be noted that the fiber breakage rate refers to the proportion of carbon fiber precursor fibers that break during processing, which is a key indicator for evaluating the performance of carbon fiber precursor fibers. In addition, the fuzz occurrence frequency is the number of fuzz balls that appear per meter of manufactured carbon fiber precursor fibers. The frequency of fuzz ball occurrence is related to the performance of carbon fiber precursor fibers and the process. A decrease in the fuzz ball occurrence frequency can indicate that the performance of carbon fiber precursor fibers has been improved and the process has been effectively optimized.

[0077] Example 2

[0078] (1) After the prepared spinning solution is sprayed out through the spinneret, it enters the multi-stage coagulation bath process to obtain nascent fiber 6.

[0079] The first stage coagulation bath has a DMAC concentration of 50% and a temperature of 50℃; the last stage coagulation bath has a DMAC concentration of 10% and a temperature of 80℃; the first draw ratio of the coagulation bath is 2.4.

[0080] (2) After being washed, stretched, oiled, and dried, the nascent fiber 6 extends into the steam stretching unit;

[0081] The third stretching ratio of the water washing stretching is 1.8, the upstream immersion length of the oiling process is 1.5 meters, and the fourth stretching ratio of the drying process is 1.2; the temperature of the first steam hot roller is 85℃, and the temperature of the last steam hot roller is 170℃.

[0082] (3) The dried nascent fibers 6 are guided to the steam drawing unit with 3 layers of steam drawing machine 2. Each bundle of nascent fibers 6 is drawn by the corresponding steam drawing machine 2 to obtain carbon fiber precursor.

[0083] The second draw ratio of the steam drawing unit is 1.9;

[0084] The total draw ratio of the carbon fiber precursor manufacturing system is 10, the breakage rate is 70%, and the fuzzing frequency is 70%.

[0085] Example 3

[0086] (1) After the prepared spinning solution is sprayed out through the spinneret, it enters the multi-stage coagulation bath process to obtain nascent fiber 6.

[0087] The first stage coagulation bath has a DMAC concentration of 70% and a temperature of 70℃; the last stage coagulation bath has a DMAC concentration of 30% and a temperature of 90℃; the first draw ratio of the coagulation bath is 2.4.

[0088] (2) After being washed, stretched, oiled, and dried, the nascent fiber 6 extends into the steam stretching unit;

[0089] The third stretching ratio of the water washing stretching is 1.8, the upstream immersion length of the oiling process is 1.5, and the fourth stretching ratio of the drying process is 1.2; the temperature of the first steam hot roller is 90℃, and the temperature of the last steam hot roller is 165℃.

[0090] (3) The dried nascent fibers 6 are guided to the steam drawing unit with 3 layers of steam drawing machine 2. Each bundle of nascent fibers 6 is drawn by the corresponding steam drawing machine 2 to obtain carbon fiber precursor.

[0091] The second draw ratio of the steam drawing unit is 1.9;

[0092] The carbon fiber precursor manufacturing system has a total draw ratio of 10, a breakage rate of 80%, and a fuzzing frequency of 70%.

[0093] Example 4

[0094] (1) After the prepared spinning solution is sprayed out through the spinneret, it enters the multi-stage coagulation bath process to obtain nascent fiber 6.

[0095] The first stage coagulation bath has a DMAC concentration of 50% and a temperature of 70℃; the last stage coagulation bath has a DMAC concentration of 10% and a temperature of 90℃; the first draw ratio of the coagulation bath is 2.4.

[0096] (2) After being washed, stretched, oiled, and dried, the nascent fiber 6 extends into the steam stretching unit;

[0097] The third stretching ratio of the water washing stretching is 1.8, the upstream immersion length of the oiling process is 1.5 meters, and the fourth stretching ratio of the drying process is 1.2; the temperature of the first steam hot roller is 85℃, and the temperature of the last steam hot roller is 170℃.

[0098] (3) The dried nascent fibers 6 are guided to a steam drawing unit with two layers of steam drawing machines 2. Each bundle of nascent fibers 6 is drawn by the corresponding steam drawing machine 2 to obtain carbon fiber precursor.

[0099] The second draw ratio of the steam drawing unit is 1.9;

[0100] The total draw ratio of the carbon fiber precursor manufacturing system is 10, the breakage rate is 60%, and the fuzzing frequency is 30%.

[0101] Example 5

[0102] (1) After the prepared spinning solution is sprayed out through the spinneret, it enters the multi-stage coagulation bath process to obtain nascent fiber 6.

[0103] The first stage coagulation bath has a DMAC concentration of 50% and a temperature of 70℃; the last stage coagulation bath has a DMAC concentration of 10% and a temperature of 90℃; the first draw ratio of the coagulation bath is 2.5.

[0104] (2) After being washed, stretched, oiled, and dried, the nascent fiber 6 extends into the steam stretching unit;

[0105] The third stretching ratio of the water washing stretching is 1.7, the upstream immersion length of the oiling process is 1.5, and the fourth stretching ratio of the drying process is 1.15; the temperature of the first steam hot roller is 85°C, and the temperature of the last steam hot roller is 170°C.

[0106] (3) The dried nascent fibers 6 are guided to the steam drawing unit with 3 layers of steam drawing machine 2. Each bundle of nascent fibers 6 is drawn by the corresponding steam drawing machine 2 to obtain carbon fiber precursor.

[0107] The second draw ratio of the steam drawing unit is 2.3;

[0108] The carbon fiber precursor manufacturing system has a total draw ratio of 10, a breakage rate of 55%, and a fuzzing frequency of 25%.

[0109] Example 6

[0110] (1) After the prepared spinning solution is sprayed out through the spinneret, it enters the multi-stage coagulation bath process to obtain nascent fiber 6.

[0111] The first stage coagulation bath has a DMAC concentration of 60% and a temperature of 60℃; the last stage coagulation bath has a DMAC concentration of 10% and a temperature of 90℃; and the first draw ratio of the coagulation bath is 2.

[0112] (2) After being washed, stretched, oiled, and dried, the nascent fiber 6 extends into the steam stretching unit;

[0113] The third stretching ratio of the water washing stretching is 1.58, the upstream immersion length of the oiling process is 2, and the fourth stretching ratio of the drying process is 1.07; the temperature of the first steam hot roller is 95°C, and the temperature of the last steam hot roller is 165°C.

[0114] (3) The dried nascent fibers 6 are guided to the steam drawing unit with 4 layers of steam drawing machine 2. Each bundle of nascent fibers 6 is drawn by the corresponding steam drawing machine 2 to obtain carbon fiber filaments.

[0115] The second draw ratio of the steam drawing unit is 2.9;

[0116] The carbon fiber precursor manufacturing system has a total draw ratio of 10, a breakage rate of 15%, and a fuzzing frequency of 10%.

[0117] Comparing Examples 3 and 4, this invention shows that when the number of layers in the steam drawing machine increases, reducing the DMAC concentration in the coagulation bath can effectively reduce the fiber breakage rate of the carbon fiber precursor manufacturing system. Comparing Examples 2 and 4, this invention shows that when the number of layers in the steam drawing machine increases, adjusting the temperature of the coagulation bath can effectively reduce the fiber breakage rate of the carbon fiber precursor manufacturing system. Comparing Examples 4 and 5, this invention shows that when the number of layers in the steam drawing machine increases, adjusting the draw ratio of each process can effectively reduce the fiber breakage rate of the carbon fiber precursor manufacturing system. Comparing Examples 1, 7, 8, and 9, it can be concluded that when the number of layers in the steam drawing machine increases, correspondingly adjusting the DMAC concentration, temperature, and the first and second draw ratios in the coagulation bath can ensure that the fiber breakage rate of the carbon fiber precursor manufacturing system does not increase, or even decreases.

[0118] Comparative Example 1

[0119] The difference between Comparative Example 1 and the above embodiment is that the steam drawing unit is equipped with only one layer of steam drawing machine 2, and the values ​​of DMAC concentration, temperature and first drawing ratio and second drawing ratio are adjusted to the optimal values ​​respectively.

[0120] (1) After the prepared spinning solution is sprayed out through 32 sets of spinnerets, it enters the multi-stage coagulation bath process to obtain nascent fiber 6.

[0121] The first stage coagulation bath has a DMAC concentration of 60% and a temperature of 60℃; the last stage coagulation bath has a DMAC concentration of 10% and a temperature of 85℃; and the first draw ratio of the coagulation bath is 2.5.

[0122] (2) After being washed, stretched, oiled, and dried, the nascent fiber 6 extends into the steam stretching unit;

[0123] The third stretching ratio of the water washing stretching is 1.9, the upstream immersion length of the oiling process is 2, and the fourth stretching ratio of the drying process is 1.33; the temperature of the first steam hot roller is 95°C, and the temperature of the last steam hot roller is 170°C.

[0124] (3) The dried nascent fibers 6 are guided to a steam drawing unit with a steam drawing machine 2. Each bundle of nascent fibers 6 is drawn by the steam drawing machine 2 to obtain carbon fiber filaments.

[0125] The second draw ratio of the steam drawing unit is 1.5;

[0126] The total draw ratio of the carbon fiber precursor manufacturing system is 10, the breakage rate is 8%, and the fuzzing frequency is 5%.

[0127] By comparing the fiber breakage rates of the carbon fiber precursor manufacturing systems in Comparative Example 1 and Examples 2, 5 and 6, it can be seen that when the number of layers in the steam drawing machine 2 of the steam drawing unit increases, by adjusting the DMAC concentration, temperature and the drawing ratio of each process, the fiber breakage rate and the frequency of fuzz formation can remain unchanged or even be lower.

[0128] Comparative Example 2

[0129] The difference between Comparative Example 2 and the above embodiment is that the steam drawing unit has three layers of steam drawing machines 2, and the values ​​of DMAC concentration, temperature, and the first and second drawing ratios are the same as those in Comparative Example 1. 10%

[0130] (1) After the prepared spinning solution is sprayed out through the spinneret, it enters a multi-stage coagulation bath, water washing and stretching, oiling, and drying to obtain nascent fiber 6.

[0131] The first stage coagulation bath has a DMAC concentration of 70% and a temperature of 50℃; the last stage coagulation bath has a DMAC concentration of 30% and a temperature of 80℃; and the first draw ratio of the coagulation bath is 2.4.

[0132] (2) After being washed, stretched, oiled, and dried, the nascent fiber 6 extends into the steam stretching unit;

[0133] The third stretching ratio of the water washing stretching is 1.8, the upstream immersion length of the oiling process is 1.5 meters, and the fourth stretching ratio of the drying process is 1.2; the temperature of the first steam hot roller is 80℃, and the temperature of the last steam hot roller is 170℃.

[0134] (3) The dried nascent fibers 6 are guided to the steam drawing unit with 3 layers of steam drawing machine 2. Each bundle of nascent fibers 6 is drawn by the steam drawing machine 2 to obtain carbon fiber precursor.

[0135] The second draw ratio of the steam drawing unit is 1.9;

[0136] The total draw ratio of the carbon fiber precursor manufacturing system is 10, the breakage rate is 67%, and the frequency of fuzz formation is 68%.

[0137] By comparing the fiber breakage rates of the carbon fiber precursor manufacturing systems of Comparative Example 2 and Example 1, it was found that if the number of layers of the steam drawing machine 2 is increased while other operating parameters of the carbon fiber precursor manufacturing system remain unchanged, the fiber breakage rate of the carbon fiber precursor manufacturing system will increase and the frequency of fuzzing will also increase, making it unsuitable for actual production.

[0138] Experimental Example 1

[0139] In this experimental example, 3k carbon fiber precursor was prepared using the preparation method of Example 1. A spinneret with 32 spinneret holes and a spinneret size of 3000 was used, the spinning speed was controlled at 22m / min, the spinning speed of the carbon fiber preparation system was 10m, and the number of spindles of the carbon fiber precursor was 40.

[0140] Experiment Example 2

[0141] In this experimental example, 3k carbon fiber precursor was prepared using the preparation method of Example 1. A spinneret with a spinneret hole size of 3000 was used, the spinning speed was controlled at 23m / min, the spinning speed of the carbon fiber preparation system was 10m, and the number of spindles of the carbon fiber precursor was 40.

[0142] Experimental Example 3

[0143] In this experimental example, 3k carbon fiber precursor was prepared using the preparation method of Example 1. A spinneret with a spinneret hole size of 3000 was used, the spinning speed was controlled at 24m / min, the spinning speed of the carbon fiber preparation system was 10, and the number of spindles of the carbon fiber precursor was 40.

[0144] Experiment Example 4

[0145] In this experimental example, 3k carbon fiber precursor was prepared using the preparation method of Example 1. A spinneret with a spinneret hole size of 3000 was used, the spinneret speed was controlled at 25m / min, the spinning speed of the carbon fiber preparation system was 10, and the number of spindles of the carbon fiber precursor was 40.

[0146] Experimental Example 5

[0147] In this experimental example, 6k carbon fiber precursor was prepared using the preparation method of Example 1. A spinneret with a spinneret hole size of 6000 was used, the spinning speed was controlled at 22m / min, the spinning speed of the carbon fiber preparation system was 10m, and the number of spindles for the carbon fiber precursor was 40.

[0148] Experimental Example 6

[0149] In this experimental example, 6k carbon fiber precursor was prepared using the preparation method of Example 1. A spinneret with a spinneret hole size of 6000 was used, the spinning speed was controlled at 23m / min, the spinning speed of the carbon fiber preparation system was 24, and the number of spindles of the carbon fiber precursor was 40.

[0150] Experimental Example 7

[0151] In this experimental example, 6k carbon fiber precursor was prepared using the preparation method of Example 1. A spinneret with a spinneret hole size of 6000 was used, the spinning speed was controlled at 24m / min, the spinning speed of the carbon fiber preparation system was 10, and the number of spindles for the carbon fiber precursor was 40.

[0152] Experimental Example 8

[0153] In this experimental example, 6k carbon fiber precursor was prepared using the preparation method of Example 1. A spinneret with a spinneret hole size of 6000 was used, the spinning speed was controlled at 25m / min, the spinning speed of the carbon fiber preparation system was 10m, and the number of spindles for the carbon fiber precursor was 40.

[0154] Experimental Example 9

[0155] In this experimental example, 12k carbon fiber precursor was prepared using the preparation method of Example 1. A spinneret with a spinneret hole size of 12000 was used, the spinneret speed was controlled at 22m / min, the spinning speed of the carbon fiber preparation system was 9, and the number of spindles of the carbon fiber precursor was 40.

[0156] Experimental Example 10

[0157] In this experimental example, 12k carbon fiber precursor was prepared using the preparation method of Example 1. A spinneret with a spinneret hole size of 12000 was used, the spinneret speed was controlled at 23m / min, the spinning speed of the carbon fiber preparation system was 9, and the number of spindles of the carbon fiber precursor was 40.

[0158] Experimental Example 11

[0159] In this experimental example, 12k carbon fiber precursor was prepared using the preparation method of Example 1. A spinneret with a spinneret hole size of 12000 was used, the spinning speed was controlled at 15m / min, the spinning speed of the carbon fiber preparation system was 9, and the number of spindles of the carbon fiber precursor was 40.

[0160] Experimental Example 12

[0161] In this experimental example, 12k carbon fiber precursor was prepared using the preparation method of Example 1. A spinneret with a spinneret hole size of 12000 was used, the spinning speed was controlled at 20m / min, the spinning speed of the carbon fiber preparation system was 9, and the number of spindles of the carbon fiber precursor was 40.

[0162] Experimental Example 13

[0163] In this experimental example, 24k carbon fiber precursor was prepared using the preparation method of Example 1. A spinneret with a spinneret hole size of 24000 was used, the spinneret speed was controlled at 22m / min, the spinning speed of the carbon fiber preparation system was 8, and the number of spindles of the carbon fiber precursor was 40.

[0164] Experimental Example 14

[0165] In this experimental example, 24k carbon fiber precursor was prepared using the preparation method of Example 1. A spinneret with a spinneret hole size of 24000 was used, the spinning speed was controlled at 23m / min, the spinning speed of the carbon fiber preparation system was 8, and the number of spindles of the carbon fiber precursor was 40.

[0166] Experimental Example 15

[0167] In this experimental example, 24k carbon fiber precursor was prepared using the preparation method of Example 1. A spinneret with a spinneret hole size of 24000 was used, the spinneret speed was controlled at 24m / min, the spinning speed of the carbon fiber preparation system was 8, and the number of spindles of the carbon fiber precursor was 32.

[0168] Experimental Example 16

[0169] In this experimental example, 24k carbon fiber precursor was prepared using the preparation method of Example 1. A spinneret with a spinneret hole size of 24000 was used, the spinneret speed was controlled at 20m / min, the spinning speed of the carbon fiber preparation system was 8, and the number of spindles of the carbon fiber precursor was 32.

[0170] Experimental Example 17

[0171] In this experimental example, 25k carbon fiber precursor was prepared using the preparation method of Example 1. A spinneret with a spinneret hole size of 25000 was used, the spinning speed was controlled at 22m / min, the spinning speed of the carbon fiber preparation system was 8, and the number of spindles of the carbon fiber precursor was 32.

[0172] Experimental Example 18

[0173] In this experimental example, 25k carbon fiber precursor was prepared using the preparation method of Example 1. A spinneret with a spinneret hole size of 25000 was used, the spinning speed was controlled at 23m / min, the spinning speed of the carbon fiber preparation system was 8, and the number of spindles of the carbon fiber precursor was 32.

[0174] Experimental Example 19

[0175] In this experimental example, 25k carbon fiber precursor was prepared using the preparation method of Example 1. A spinneret with a spinneret hole size of 25000 was used, the spinning speed was controlled at 24m / min, the spinning speed of the carbon fiber preparation system was 8, and the number of spindles of the carbon fiber precursor was 32.

[0176] Experimental Example 20

[0177] In this experimental example, 25k carbon fiber precursor was prepared using the preparation method of Example 1. A spinneret with a spinneret hole size of 25000 was used, the spinning speed was controlled at 25m / min, the spinning speed of the carbon fiber preparation system was 8, and the number of spindles of the carbon fiber precursor was 32.

[0178] Experimental Example 21

[0179] In this experimental example, 35k carbon fiber precursor was prepared using the preparation method of Example 1. A spinneret with a spinneret hole size of 35000 was used, the spinning speed was controlled at 22m / min, the spinning speed of the carbon fiber preparation system was 6, and the number of spindles for the carbon fiber precursor was 24.

[0180] Experiment Example 22

[0181] In this experimental example, 35k carbon fiber precursor was prepared using the preparation method of Example 1. A spinneret with a spinneret hole size of 35000 was used, the spinning speed was controlled at 23m / min, the spinning speed of the carbon fiber preparation system was 6, and the number of spindles of the carbon fiber precursor was 24.

[0182] Experimental Example 23

[0183] In this experimental example, 35k carbon fiber precursor was prepared using the preparation method of Example 1. A spinneret with a spinneret hole size of 35000 was used, the spinning speed was controlled at 24m / min, the spinning speed of the carbon fiber preparation system was 6, and the number of spindles for the carbon fiber precursor was 24.

[0184] Experimental Example 24

[0185] In this experimental example, 35k carbon fiber precursor was prepared using the preparation method of Example 1. The spinneret with a certain number of spinneret holes was used, the spinning speed was controlled at 25m / min, the spinning speed of the carbon fiber preparation system was a certain value, and the number of spindles for the carbon fiber precursor was 24.

[0186] The properties of the carbon fiber precursors in Examples 1-24 were tested in this invention, specifically including nominal fineness, linear density, breaking strength, fineness cv value, elongation at break, oil content, DMAC content, and modulus. The results are shown in Table 1 below:

[0187] Table 1

[0188]

[0189]

[0190] As shown in the table above, the CV values ​​of the linear density of the 1-35k carbon fiber precursor produced using the embodiments of the present invention are all less than or equal to 10% over a length of 1m. This means that the carbon fiber precursor produced in the present invention has good linear density stability, high product uniformity and stability, which is beneficial for large-scale production.

[0191] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-described technical content to create equivalent embodiments without departing from the scope of the present invention. The implementation schemes in the above embodiments can be further combined or replaced. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.

Claims

1. A method for manufacturing carbon fiber precursor, wherein the spinning solution is spun out through a spinneret, drawn through a coagulation bath to obtain nascent fiber, then washed and drawn with water, oiled, dried, and drawn through a steam drawing unit to obtain carbon fiber precursor. Its features are, The steam drawing unit includes multiple parallel steam drawing machines. The number of spindles of nascent fibers in the coagulation bath increases with the number of steam drawing machines. The temperature and / or DMAC concentration of the coagulation bath are adjusted accordingly based on the change in the number of nascent fibers in the coagulation bath. Each layer of the steam drawing machine is equipped with a threading channel for the nascent fibers to pass through; a first guide roller group and a second guide roller group are respectively set up upstream and downstream of the threading channel. Each bundle of nascent fibers produced by the coagulation bath is guided by the first guide roller group to pass through the corresponding threading channel, and then extends downstream through the second guide roller group. Each guide roller group includes at least one guide roller and a support roller located near the corresponding threading channel. The axis of each threading channel is tangent to the peripheral sidewall of the corresponding support roller. The rotational speeds of all support rollers in the guide roller group are equal. Each bundle of nascent fibers extends vertically from the guide rollers of the first guide roller group, and when it extends to the corresponding support roller, it bends 90 degrees horizontally around the circumferential side of the support roller, and then extends horizontally into the corresponding threading channel. The coagulation drawing uses the first drawing ratio to draw the nascent fiber, and the steam drawing uses the second drawing ratio to draw the nascent fiber; when the number of steam drawing machines increases by n layers, the first drawing ratio decreases by (c*n) times, and the second drawing ratio increases by (d*n) times. The nascent fibers are drawn using the third drawing ratio after washing and the fourth drawing ratio after drying. When the number of steam drawing machines increases by n layers, the third drawing ratio decreases by (e*n) times, and the fourth drawing ratio decreases by (f*n) times. The total draw ratio is 10, and c, e, f, and d satisfy the following relationship: (1-c)*(1-e)*(1-f)*(1+d)=1; where 4%≤c≤20%; 14%≤d≤30%; 5%≤e≤7%; 4%≤f≤9%; This manufacturing method is applicable to the production of carbon fiber precursors ranging from 1 to 35 kJ. The linear density CV value of the produced carbon fiber precursors is ≤10% over a length of 1 meter. The breakage rate and the frequency of fuzzing are consistent with, or even lower than, those when only a single-layer steam drawing machine is used.

2. The method for manufacturing carbon fiber precursor according to claim 1, characterized in that, The coagulation bath is a multi-stage coagulation bath, with the temperature of each stage increasing as the number of nascent fiber spindles increases, and / or the DMAC concentration of each stage of the coagulation bath decreasing as the number of nascent fiber spindles increases.

3. The method for manufacturing carbon fiber precursor according to claim 2, characterized in that, The temperature of the multi-stage solidification is increased in a stepwise manner, with the temperature of the first stage solidification bath between 50-70℃ and the temperature of the last stage solidification bath between 80-90℃.

4. The method for manufacturing carbon fiber precursor according to claim 2, characterized in that, The DMAC concentration in the multi-stage coagulation bath is decreased in a stepwise manner, with the DMAC concentration in the first stage coagulation bath between 50% and 70%, and the DMAC concentration in the last stage coagulation bath between 10% and 30%.

5. A system for manufacturing carbon fiber precursor, characterized in that, The control method of the carbon fiber precursor manufacturing system according to any one of claims 1-4 is adopted.

6. The carbon fiber precursor manufacturing system according to claim 5, characterized in that, Each steam drawing machine (2) is arranged vertically, and each guide roller group's support roller (5) is arranged vertically. The guide roller (4) closest to the support roller (5) is lower than the lowest support roller (5) or higher than the highest support roller (5). The vertical tangent of the guide roller (4) near the threading channel (201) coincides with the vertical tangent of each corresponding branch roller (5) away from the threading channel (201), and each raw yarn extends from the first side of the first guide roller (4) to the second side of the corresponding branch roller (5).

Citation Information

Patent Citations

  • Preparation method of 25k carbon fiber and carbon fiber

    CN114606602A

  • Preparation method of 24-50k carbon fiber precursor, carbon fiber precursor and carbon fiber

    CN115506049A

  • Carbon fiber precursor steam drafting device

    CN210458441U