A method for manufacturing a bonded spray additive manufactured SKH-9 high speed steel part
By optimizing the process parameters and sintering temperature of binder jet additive manufacturing, the density and hardness problems of SKH-9 high-speed steel parts manufactured by binder jet additive manufacturing were solved, realizing the preparation of high-performance parts suitable for aerospace, automotive parts, medical and art design and other fields.
Patent Information
- Application Number
- CN202411550616.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-01
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-11-01
AI Technical Summary
Existing binder spraying additive manufacturing technology has problems such as low material properties, unoptimized process parameters, and low density of formed parts when preparing steel parts. In particular, the impact of binder decomposition and sintering processes on the densification of parts is unclear.
Using SKH-9 fine powder with a particle size of less than 17μm, the process parameters of binder spray additive manufacturing, including layer thickness, binder resolution, spraying voltage and leveling time, were optimized. Combined with low-temperature baking curing and high-temperature sintering, the maximum sintering temperature was limited to 1250-1270℃, and the sintering process was optimized to improve density and hardness.
SKH-9 high-speed steel parts with a density higher than 95% and a hardness greater than 540HV₃₀ were prepared. They have excellent performance, the process is simple and easy to implement, the overall cost is low, and they are suitable for widespread application.
Smart Images

Figure CN119159092B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for preparing SKH-9 high-speed steel parts, and more particularly to a method for preparing SKH-9 high-speed steel parts by binder spraying additive manufacturing. Background Technology
[0002] Additive manufacturing, commonly known as 3D printing, is an advanced green manufacturing technology that has many advantages over traditional machining methods, such as eliminating the need for tooling and molds, enabling the forming of complex parts, shortening processing cycles, and saving raw materials. It has already been applied in many fields, including aerospace, automotive parts, medical, and art design.
[0003] Additive manufacturing technology has many branches, and binder spraying is one that has developed rapidly in recent years. Compared with other additive manufacturing technologies, binder spraying additive manufacturing technology has advantages such as wide material adaptability, low equipment cost, fast forming speed, low thermal stress, and low overall cost. It is expected to achieve low-cost, high-efficiency mass production of complex parts and has broad development prospects. However, there are still some problems, such as the limited number of developed material systems, the need to optimize process parameters, and the relatively low performance of formed parts. Further research is needed to lay the foundation for the widespread application of this technology.
[0004] In existing binder spraying techniques for manufacturing steel parts, 420 stainless steel parts produced by binder spraying additive manufacturing exhibit good sintering performance at 1350℃. However, at lower sintering temperatures (1300℃), the density decreases, and at higher sintering temperatures, the tensile strength drops significantly. There are many reasons for the current low performance of metal parts manufactured using binder spraying additive manufacturing. On the one hand, the forming-densification mechanism of this manufacturing method needs further clarification, especially the impact of binder decomposition and escape processes on part densification, as well as the formation and growth of sintering necks between metal powder particles. On the other hand, process parameters during forming need optimization, such as the optimal combination of powder particle size distribution, layer thickness during powder spreading, and sintering temperature. Summary of the Invention
[0005] Purpose of the invention: The purpose of this invention is to disclose a method for preparing SKH-9 high-speed steel parts with high density and high hardness by binder spraying additive manufacturing.
[0006] Technical solution: This invention discloses a method for preparing SKH-9 high-speed steel parts by binder spraying additive manufacturing, comprising the following steps:
[0007] (1) Take SKH-9 fine powder with a particle size of less than 17μm and add it layer by layer by binder spraying additive manufacturing method to obtain green parts;
[0008] (2) Take the part obtained in step (1) and bake it in an oven at low temperature to obtain the cured SKH-9 high-speed steel part blank, thereby improving the strength of the green blank.
[0009] (3) Take the billet obtained in step (2), keep it warm and degrease it in a sintering furnace, and sinter it at a high temperature of 1250~1270℃ to obtain SKH-9 high-speed steel parts.
[0010] In step (1), the parameters of the adhesive spraying molding equipment are as follows: the maximum forming size range is 200mm×60mm×70mm, the nozzle has 1024 channels, and the total ink volume per spray is 30×10 -12 L, the sintering furnace used is a Tianjin Zhonghuan SK-Q06163 electric furnace.
[0011] In step (1), the adhesive spraying additive manufacturing uses the following forming parameters: layer thickness 55-65μm, adhesive resolution 800×800dpi, spraying voltage 55-60V, and leveling time 5000ms (extended to a range value); the forming parameters are further preferably 60μm, adhesive resolution 800×800dpi, spraying voltage 58V, and leveling time 5000ms.
[0012] In step (2), the low-temperature baking and curing process takes place at a temperature of 180-200°C for 2-3 hours.
[0013] In step (3), the heat preservation degreasing process parameters are as follows: heating from room temperature to 550-650℃ at a rate of 2-3℃ / min and holding for 6.5-7.5h for degreasing; the process parameters are further preferred to be heating from room temperature to 600℃ at a rate of 2℃ / min and holding for 7h for degreasing.
[0014] In step (3), the high-temperature sintering process parameters are as follows: heating to 950-1000℃ at a rate of 5-6℃ / min and holding for 1.5-2h for initial sintering; then heating to 1250-1270℃ at a rate of 5-6℃ / min and holding for 4-5h; finally cooling to room temperature at a rate of 9-11℃ / min; the process parameters are further preferably as follows: heating to 1000℃ at a rate of 5℃ / min and holding for 1.5h for initial sintering; then heating to 1250-1270℃ at a rate of 5℃ / min and holding for 4h; finally cooling to room temperature at a rate of 10℃ / min.
[0015] This invention also discloses SKH-9 high-speed steel parts prepared by the above-mentioned method, wherein the parts have a density higher than 95% and a hardness greater than 540 HV. 30 .
[0016] Invention Principle: The method for preparing SKH-9 high-speed steel parts by binder spraying additive manufacturing of the present invention obtains high-performance shaped parts by optimizing process parameters. This is mainly due to the following points: (1) The method uses fine powder with a particle size distribution range of 0-17μm. Finer powder has a larger specific surface area, higher surface activity during sintering, and is easier to densify; (2) The forming parameters of binder spraying additive manufacturing have been repeatedly optimized to make the initial blank dense and uniform under the condition of using as little binder as possible, laying the foundation for subsequent sintering; (3) The method strictly limits the sintering process, especially the maximum sintering temperature. The sintering process fully considers the influencing factors such as material composition, melting point, and sintering atmosphere. It is a sintering process specifically formulated for SKH-9 material. Under specific process conditions, the SKH-9 fine powder with special particle size is effectively activated, and high-performance high-speed steel parts are obtained through synergistic enhancement.
[0017] Beneficial Effects: Compared with the prior art, the present invention has the following significant advantages: The method for preparing SKH-9 high-speed steel parts by binder spraying additive manufacturing of the present invention has a simple process, is easy to implement, has low overall cost, is easy to promote, and the SKH-9 high-speed steel parts obtained have excellent performance, a dense overall structure, high roundness, and a density of over 95%; the hardness is greater than 540 HV. 30 It has great application prospects in actual manufacturing. Attached Figure Description
[0018] Figure 1 The surface morphology of the SKH-9 high-speed steel samples after low-temperature baking and curing (bottom) and after high-temperature sintering at 1250℃ (top) in Example 1 is shown.
[0019] Figure 2 The metallographic structure of the SKH-9 high-speed steel sample after high-temperature sintering at 1250℃ in Example 1;
[0020] Figure 3 The surface morphology of the sample deformed at a sintering temperature of 1350℃ is shown in Comparative Example 1. Detailed Implementation
[0021] The technical solution of the present invention will be further described below with reference to the embodiments. The test materials used in the embodiments can all be purchased through conventional means.
[0022] Example 1
[0023] The method for preparing SKH-9 high-speed steel parts by binder spraying additive manufacturing of the present invention includes the following steps:
[0024] (1) SKH-9 fine powder with a particle size range of 0-17μm was used to accumulate layers by binder spraying additive manufacturing to obtain green parts. The forming parameters used in binder spraying additive manufacturing were: layer thickness 65μm, binder resolution 800×800dpi, spraying voltage 55V, and leveling time 5000ms.
[0025] (2) The green body is cured by low-temperature baking in an oven at 180°C for 2 hours to improve its strength.
[0026] (3) The cured SKH-9 high-speed steel parts blanks are degreased and sintered at high temperature in a sintering furnace. The specific process parameters for high-temperature sintering are as follows: the temperature is increased from room temperature to 600℃ at a rate of 2℃ / min and held for 7 hours for degreasing; then the temperature is increased to 1000℃ at a rate of 5℃ / min and held for 1.5 hours for initial sintering; then the temperature is increased to 1250℃ at a rate of 5℃ / min and held for 4 hours; finally, the temperature is cooled to room temperature at a rate of 10℃ / min to obtain SKH-9 high-speed steel parts.
[0027] In this embodiment, the appearance photos of the SKH-9 high-speed steel samples after curing at 180℃ and sintering at 1250℃ are as follows: Figure 1 As shown in the image, the sintered sample exhibits a bright metallic luster. Compared to the green sample, its three dimensions have shrunk, but no significant deformation has been observed. Metallographic photographs of the sintered sample are shown below. Figure 2 As shown, the tissue is generally dense with a small number of pores and exhibits high roundness. Testing revealed a density of 95.68% and a microhardness of 542 HV. 30 The material exhibits good performance. This indicates that the forming, curing, and sintering process is appropriate, resulting in a material with excellent properties.
[0028] Example 2
[0029] The method for preparing SKH-9 high-speed steel parts by binder spraying additive manufacturing of the present invention includes the following steps:
[0030] (1) SKH-9 fine powder with a particle size range of 0-17μm was used to accumulate layers by binder spraying additive manufacturing to obtain green parts. The forming parameters used in binder spraying additive manufacturing were: layer thickness 55μm, binder resolution 800×800dpi, spraying voltage 60V, and leveling time 5000ms.
[0031] (2) The green body is cured by low-temperature baking in an oven at 200°C for 3 hours to improve its strength.
[0032] (3) The cured SKH-9 high-speed steel parts blanks are degreased and sintered at high temperature in a sintering furnace. The specific process parameters for high-temperature sintering are as follows: the temperature is increased from room temperature to 600℃ at a rate of 2℃ / min and held for 7 hours for degreasing; then the temperature is increased to 1000℃ at a rate of 5℃ / min and held for 1.5 hours for initial sintering; then the temperature is increased to 1270℃ at a rate of 5℃ / min and held for 4 hours; finally, the temperature is cooled to room temperature at a rate of 10℃ / min to obtain SKH-9 high-speed steel parts.
[0033] According to tests, the density of the SKH-9 high-speed steel sample cured at 200℃ and sintered at 1270℃ in this embodiment was 96.73%, and the microhardness was 568 HV. 30 The performance is good, indicating that the forming, curing, and sintering process is appropriate.
[0034] Comparative Example 1
[0035] A method for preparing SKH-9 high-speed steel parts, compared with Example 2, Comparative Example 1 changes the maximum sintering temperature in step (3), including the following steps:
[0036] (1) SKH-9 fine powder with a particle size range of 0-17μm was used to accumulate layers by binder spraying additive manufacturing to obtain green parts. The forming parameters used in binder spraying additive manufacturing were: layer thickness 60μm, binder resolution 800×800dpi, spraying voltage 58V, and leveling time 5000ms.
[0037] (2) The green body is cured by low-temperature baking in an oven at 200°C to improve its strength;
[0038] (3) The cured SKH-9 high-speed steel part blanks are degreased and sintered at high temperature in a sintering furnace. The specific process parameters for high-temperature sintering are as follows: the temperature is increased from room temperature to 600℃ at a rate of 2℃ / min and held for 7h for degreasing; then the temperature is increased to 1000℃ at a rate of 5℃ / min and held for 1.5h for initial sintering; then the temperature is increased to 1350℃ at a rate of 5℃ / min and held for 4h; finally, the temperature is cooled to room temperature at a rate of 10℃ / min to obtain the formed part.
[0039] like Figure 3 As shown, after sintering, the sample surface had a higher gloss, but it also exhibited significant deformation, changing from a square shape to an approximately drum-shaped or spherical shape. This indicates that excessively high sintering temperatures can have a significant adverse effect on the sample morphology, damaging the part's shape and rendering it unusable.
[0040] By comparing the examples and comparative examples, the binder-spraying additive manufacturing method for SKH-9 high-speed steel parts of the present invention, under the conditions of a low-temperature curing temperature of 180-200°C and a maximum sintering temperature of 1250-1270°C, can obtain high-performance SKH-9 high-speed steel parts with a density >95% and a microhardness >540 HV. 30 It has good performance, and the process is simple, easy to implement, has low overall cost, is easy to promote, and has great application prospects.
Claims
1. A method for preparing SKH-9 high-speed steel binder spray additive manufacturing based on a specific sintering temperature, characterized in that, Includes the following steps: (1) Take SKH-9 fine powder with a particle size of less than 17 μm and obtain green parts by binder spraying additive manufacturing method; (2) Take the parts obtained in step (1) and bake them in an oven at a low temperature. The low temperature baking and curing temperature is 180~200 ℃ and the time is 2-3 h to obtain the cured SKH-9 high-speed steel parts blank. (3) Take the blank obtained in step (2), keep it warm and degrease it in a sintering furnace, and sinter it at high temperature. The specific process parameters of the high temperature sintering are as follows: heat up from room temperature to 600 ℃ at a rate of 2 ℃ / min, keep it warm for 7 h to degrease; then heat up to 1000 ℃ at a rate of 5 ℃ / min, keep it warm for 1.5 h for initial sintering; then heat up to 1250 ℃ at a rate of 5 ℃ / min, keep it warm for 4 h; finally cool it to room temperature at a rate of 10 ℃ / min to obtain SKH-9 high-speed steel parts.
2. The preparation method according to claim 1, characterized in that, In step (1), the forming parameters used in the adhesive spraying additive manufacturing are: layer thickness 55~65 μm, adhesive resolution 800×800 dpi, spraying voltage 55-60 V, and leveling time 5000 ms.
3. The preparation method according to claim 1, characterized in that, In step (1), the parameters of the adhesive spraying molding equipment used are: the maximum forming size range is 200 mm × 60 mm × 70 mm, and the total amount of ink sprayed per stroke is 30 × 10 mm. -12 L.
4. The preparation method according to claim 1, characterized in that, In step (3), the heat preservation degreasing process parameters are as follows: the temperature is increased from room temperature to 550-650 ℃ at a rate of 2-3 ℃ / min, and the temperature is maintained for 6.5-7.5 h for degreasing.
5. An SKH-9 high-speed steel part prepared by the method of claim 1, characterized in that, The part has a density higher than 95% and a hardness greater than 540 HV. 30 .
Citation Information
Patent Citations
Green body sintering process based on binder jet printing
CN115722685A