High-temperature-resistant silicon-based aerogel and preparation method thereof
By introducing a nano-aluminum oxide layer on the surface of SiO₂ aerogel, the problem of SiO₂ aerogel being prone to sintering at high temperatures was solved, thereby improving high-temperature stability and thermal insulation performance, simplifying the preparation process and reducing costs.
Patent Information
- Application Number
- CN202411183023.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-08-27
AI Technical Summary
Existing SiO₂ aerogels are prone to sintering and collapse at high temperatures, leading to material shrinkage and reduced heat insulation performance. Existing improvement methods are complex and not applicable to large-size materials.
High-temperature resistant aluminum-modified SiO₂ aerogels were prepared by introducing a nanoscale aluminum oxide layer on the surface of SiO₂ aerogel using chemical liquid phase deposition and combined with hydrophobic treatment.
It significantly improves the high-temperature stability and thermal insulation performance of aerogels, simplifies the preparation process, reduces costs, and is suitable for large-size materials.
Smart Images

Figure CN119160901B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of silicon compounds, specifically relating to a high-temperature resistant silicon-based aerogel and its preparation method. Background Technology
[0002] SiO2 aerogel is the most well-developed aerogel system, characterized by its small, pearl-like constituent particles, fine three-dimensional framework, and high surface energy. Traditional SiO2 aerogels are generally considered to exhibit good thermal insulation performance in low-to-medium temperature applications below 600℃. However, in long-term use environments exceeding 600℃, the internal structure sintersects and collapses, resulting in significant material shrinkage and a substantial reduction in its thermal insulation effect, thus limiting its application in high-temperature environments. The temperature resistance of SiO2 aerogels can be improved through process optimization or methods such as doping and composites.
[0003] Patent CN109621849A discloses a method for preparing silica-coated alumina composite aerogel under normal pressure. The method involves immersing a pre-synthesized alumina wet gel in a mixed solution of silicon source and ethanol, then performing hydrophobic treatment in a modified solution of hexamethyldisiloxane and n-hexane, and finally drying it under normal pressure in an oven to prepare silica-coated alumina aerogel. The silica on the surface of alumina can inhibit the shrinkage of alumina aerogel under high temperature conditions, thereby improving the performance of the composite material in high temperature environments.
[0004] Patent CN115108809A discloses a method for preparing aluminum-modified silica sol using orthosilicate and inorganic aluminum source as co-precursors via a two-step acid-base catalysis process. This is followed by vacuum pressure impregnation of inorganic ceramic fiber preforms, and then supercritical drying with ethanol to obtain a modified silica aerogel heat-insulating composite material with a maximum service temperature of 1100℃. Similarly, Ceram.Int.,2022(48):15006-15016 describes a method for preparing aluminum-silica hybrid sol by adding a small amount of aluminum chloride to silicic acid, followed by gelation and surface modification, and then drying under normal pressure. The mechanism is as follows: Figure 1 As shown in the figure. These studies demonstrate that introducing Al into SiO2, especially forming a locally electronegative -Si-O-Al- structure on the particle surface, can generate electrostatic repulsion that inhibits the sintering of silicon oxide nanoparticles at high temperatures, thereby improving high-temperature stability.
[0005] Chemical vapor deposition (or infiltration) can form a controllable and uniform metal oxide heterostructure on the surface of a solid material skeleton, such as a nano-thickness layer composed of Al2O3, ZnO2, TiO2, carbon materials, etc. deposited on the surface of SiO2 aerogel. This can improve the temperature resistance of silica aerogel by inhibiting the movement of nanoparticles and enhancing the radiation effect (CN114804819B, Chem. Mater. 2021(33):5572-5583).
[0006] Zu et al. used chemical liquid phase deposition (CLD) to react the hydroxyl and alkoxy groups on the surface of Al2O3, ZrO2, and TiO2 wet gels with the hydroxyl groups on the surface of SiO2 sol to form a core-shell structured wet gel coated with SiO2 sol. After supercritical drying with ethanol, a composite aerogel was obtained. The advantages of introducing heterogeneous SiO2 onto the surface using CLD are enhanced structural and thermal stability of the aerogel, and suppression of crystal growth and phase transition.
[0007] CN113716572A discloses a method for preparing an alumina-silica aerogel composite material. The method involves impregnating the prepared SiO2 gel in a prepared Al2O3 sol to obtain a silica-alumina composite wet gel. The -Al-O- bonds on the surface of the Al2O3 sol react with the Si-OH and Si-OR (R represents alkyl) bonds on the surface of the SiO2 wet gel to form an alumina gel on the surface of the SiO2 gel, thereby protecting the SiO2 aerogel network structure at high temperatures.
[0008] CN108467045A discloses a method for preparing self-hydrophobic aerogels of dual silicon source systems by chemical liquid phase deposition. The method involves placing the wet gel in an ethanol solution of partially hydrophilic polydimethyl silicone oil using chemical liquid phase deposition. The purpose is to deposit partially hydrophilic polydimethyl silicone oil on the surface of the wet gel to strengthen the skeletal structure. However, solvent replacement is still required before subsequent atmospheric pressure drying to achieve atmospheric pressure drying.
[0009] The main drawbacks of existing technologies that improve the temperature resistance of SiO2 aerogel by adding other types of metal oxides are as follows:
[0010] (1) Al is introduced into SiO2 gel by co-hydrolysis of single-molecule precursors. However, the hydrolysis rate of organic / inorganic aluminum salts (including aluminum isopropoxide, aluminum sec-butoxide, aluminum nitrate, aluminum chloride, aluminum sulfate, etc.) is extremely fast, making it difficult to match with the sol-gel time window of the silicon precursor. Chelating agents and fine adjustment of preparation parameters are required to prepare silicon-aluminum gel, which is a relatively complicated preparation process.
[0011] (2) The method of preparing silica-alumina aerogel by pre-forming silica sol and aluminum sol co-gel presents a challenge in controlling the co-gel time window because aluminum sol is difficult to maintain stably within the pH range of 4-9. If the gelation time is too fast, it is difficult to prepare engineering samples. In addition, this method has a long preparation time and complex process steps.
[0012] (3) By introducing Al2O3 sol into the pre-formed SiO2 gel, the matching problem of the time window of the co-hydrolysis-co-gel process of the SiO2 precursor can be avoided. However, due to the particle impregnation process, it is difficult to control the quality of the Al2O3 layer formed on the surface of the SiO2 framework, and there is also the drawback of blocking the nanopores.
[0013] (4) Chemical vapor deposition (ALD) can form high-quality alumina deposits on the surface of SiO2 aerogels, but current ALD equipment can only process samples with a size of centimeters, which is not suitable for large-sized aerogel materials used in industry. At the same time, ALD equipment and preparation processes are complex and require high standards for equipment and operators.
[0014] The three existing methods for introducing aluminum oxide into SiO2 wet gels—impregnated aluminum sol, impregnated aluminum precursor, and co-gelling of silicon-aluminum precursors—are prone to clogging of the three-dimensional interconnected channels in the gel, reducing the material's thermal insulation capacity. The water-rich channels in wet gels make the hydrolysis of the aluminum precursor uncontrollable, leading to self-condensation and making it difficult to achieve uniform grafting of aluminum oxide onto the SiO2 framework surface. Matching the hydrolysis and condensation conditions and time windows of silicon-aluminum precursors is difficult, requiring the addition of auxiliary materials and precise control of reaction conditions to achieve co-gelling, making the preparation process challenging. Summary of the Invention
[0015] The purpose of this invention is to propose a high-temperature resistant silicon-based aerogel and its preparation method. First, a SiO2 aerogel containing surface hydroxyl groups is prepared. Then, aluminum oxide is introduced onto the surface of the SiO2 framework using chemical liquid phase deposition (ALD). After hydrophobic treatment, a high-temperature resistant SiO2 aerogel coated with an aluminum oxide layer that can be stored for a long time is obtained, namely, aluminum-modified SiO2 aerogel.
[0016] The technical solution adopted in this invention is as follows:
[0017] A method for preparing a high-temperature resistant silicon-based aerogel includes the following steps:
[0018] (1) Add silicon precursor and acid catalyst to water for hydrolysis, then add alkaline catalyst for gelation to obtain SiO2 wet gel.
[0019] (2) The SiO2 wet gel is dried to obtain SiO2 aerogel, which is then placed in a container and an aluminum precursor organic solution that reacts with the hydroxyl and alkoxy groups on the surface of the SiO2 aerogel is added to carry out a chemical liquid phase deposition reaction to deposit a nano-thick aluminum oxide layer on the surface of the SiO2 aerogel to obtain a high-temperature resistant aluminum modified SiO2 aerogel.
[0020] (3) Dry the aluminum-modified SiO2 aerogel in a ventilated environment, and then perform gas-phase hydrophobicity or liquid-phase hydrophobicity to obtain high-temperature resistant aluminum-modified SiO2 aerogel.
[0021] Further, in step (1), the solid content of SiO2 in the SiO2 wet gel (i.e., the proportion of SiO2 to the total mass of water + silicon precursor) is 15% to 30%, and the amount of silicon precursor added is determined according to this solid content.
[0022] Further, in step (1), the silicon precursor is selected from either an organosilicon source or an inorganic silicon source. The organosilicon source is one of methyl orthosilicate, ethyl orthosilicate, polyethyl orthosilicate Si-40, methyl(ethyl)trimethoxysilane, methyl(ethyl)triethoxysilane, dimethyl(ethyl)dimethoxysilane, dimethyl(ethyl)diethoxysilane, vinyltrimethoxysilane, and phenyltrimethoxysilane. The inorganic silicon source is one of sodium silicate, silicic acid, and silica sol.
[0023] Furthermore, in step (1), for organosilicon sources that are immiscible with water, a phase separation inhibitor is added simultaneously or in advance, such as cationic surfactants like ethanol, hexadecyltrimethylammonium bromide, and hexadecyltrimethylammonium chloride, or nonionic surfactants like F123 and polyethylene glycol. The amount of the phase separation inhibitor is 1% to 5% of the total mass of the silicon precursor and water.
[0024] Furthermore, in step (1), the acid catalyst is selected from one of the small molecule acids such as nitric acid, hydrochloric acid, sulfuric acid, phosphoric acid, oxalic acid, acetic acid, citric acid, maleic acid, and hydrofluoric acid. After the acid catalyst is added, the pH of the solution is between 2 and 7.5, and the hydrolysis time is between 0.5 and 24 hours.
[0025] Furthermore, in step (1), the alkaline catalyst is one of the water-soluble small-molecule organic quaternary ammonium bases such as ammonia, NH4F, tetramethyl(ethyl)ammonium hydroxide, and tetramethyl(ethyl)ammonium fluoride, and the amount of alkaline catalyst used is 0.01% to 3% of the total mass of silicon precursor and water.
[0026] Furthermore, in step (1), the gelation conditions are aging at 40–200°C for 24–96 hours.
[0027] Furthermore, in step (2), the drying method is atmospheric pressure drying, supercritical drying or freeze drying. Among them, silicon precursors containing non-hydrolyzable organic groups are selected for atmospheric pressure drying, while other silicon precursors are aged, replaced with ethanol, and then subjected to supercritical drying or freeze drying.
[0028] Furthermore, in step (2), the SiO2 aerogel dried at normal pressure is calcined at 350-500℃ for 0.5-2h to remove surface alkyl groups.
[0029] Furthermore, in step (2), the aluminum precursor is one of aluminum isopropoxide, aluminum sec-butoxide, aluminum hydroxide, aluminum chloride, aluminum nitrate, aluminum sulfate, and sodium aluminate.
[0030] Furthermore, in step (2), the organic solvent used in the organic solution of the aluminum precursor is one of n-hexane, cyclohexane, n-heptane, pentane, ethanol, and isopropanol. The mass ratio of the aluminum precursor to the volume of the organic solvent is 1 g / (50-400 mL). The mass ratio of the dried, non-hydrophobic SiO2 aerogel to the aluminum precursor is 1:(0.01-0.2).
[0031] Furthermore, in step (2), the temperature of the chemical liquid phase deposition reaction is room temperature to 90°C, and the reaction time is 0.5 to 9 hours. When the reaction temperature is higher than that of the organic solvent volatilization, a condensation reflux device is configured to dissolve the aluminum precursor and make the SiO2 aerogel below the surface of the organic solvent.
[0032] Furthermore, the thickness of the aluminum oxide layer in step (2) is 2–15 nm.
[0033] A high-temperature resistant silicon-based aerogel is an aluminum-modified SiO2 aerogel prepared by the above preparation method.
[0034] The beneficial effects achieved by this invention are as follows:
[0035] 1. When using supercritical drying or freeze-drying, the surface of the dried SiO2 aerogel is rich in hydroxyl groups (-OH) and some alkoxy groups (-OR). When using atmospheric pressure drying, removing the surface alkyl groups after high-temperature calcination of the dried SiO2 aerogel yields even more surface hydroxyl groups. Then, a nano-thick layer of aluminum oxide is uniformly grafted onto the surface of the hydroxyl-rich SiO2 aerogel by hydrolysis of the surface hydroxyl groups and a small amount of alkoxy groups using a small-molecule aluminum precursor. This strengthens the framework structure without significantly affecting pore connectivity or porosity, ensuring the material's low thermal conductivity and improving the temperature resistance of the SiO2 aerogel.
[0036] 2. Compared with chemical vapor deposition, this invention only requires a simple and controllable chemical liquid phase deposition treatment between hydrophobic surfaces to improve the temperature resistance of the substrate. It does not require a complex vacuum system and gas intake system, is simple to operate, has relatively mild reaction conditions, low cost, and is easy to promote in industry.
[0037] 3. In this invention, chemical liquid phase deposition is performed on the obtained dry aerogel to introduce aluminum oxide with higher temperature resistance, which not only strengthens the skeleton, but also inhibits neck sintering by utilizing the electronegative Si-O-Al bonds formed at the interface through repulsion.
[0038] 4. This invention uses a low-polarity, low-surface-tension, and highly volatile organic solvent. After the chemical liquid-phase deposition reaction is completed, the organic solvent fills the aerogel channels. Due to the low polarity, low surface tension, and high volatility of the organic solvent, a high-temperature resistant aluminum-modified SiO2 aerogel that can be stored for a long time can be obtained by simple ventilation drying and gas-phase hydrophobic or liquid-phase hydrophobic treatment. Attached Figure Description
[0039] Figure 1 This is a schematic diagram illustrating the mechanism by which Al doping improves the temperature resistance of SiO2 aerogel in existing technologies.
[0040] Figure 2 This is a flowchart of the preparation of high-temperature resistant silicon-based aerogel in the example. Detailed Implementation
[0041] To make the various technical features, advantages, or effects of the present invention more apparent and understandable, a detailed description is provided below in conjunction with the accompanying drawings.
[0042] The following three embodiments provide the operational steps for preparing high-temperature resistant silicon-based aerogels, and the preparation process is as follows: Figure 2 As shown, the Al-modified high-temperature resistant SiO2 aerogel obtained is the high-temperature resistant aluminum-modified SiO2 aerogel in the above technical solution, both referring to the high-temperature resistant silicon-based aerogel to be prepared in this invention. In the examples, the shrinkage rate and specific surface area before and after calcination were measured after the aerogel was prepared. A pair of proportions are also given below as a comparison. These proportions lack key steps in the preparation method of this invention, and the relevant parameters of the prepared aerogels were also measured.
[0043] Example 1:
[0044] Take 100g of deionized water, add tetraethyl orthosilicate to achieve a SiO2 solid content of 20%, add 2g of 1mol / L HNO3 solution, stir and hydrolyze for 1h, then add 2g of 1mol / L ammonia water and stir thoroughly. After gelation, age at 120℃ for 3 days. The aged wet gel is replaced with ethanol three times over 2 days to obtain an alcohol gel, which is then subjected to supercritical drying. After drying, place 2g of SiO2 aerogel in a container equipped with a reflux condenser, add aluminum isopropoxide and hexane solution (0.15g aluminum isopropoxide and 50mL hexane solution). React at 80℃ for 1.5h in a reflux condenser to deposit a nano-thick layer of aluminum oxide on the surface of the SiO2 aerogel particles. After the solution cools to room temperature, remove the Al-modified SiO2 aerogel, air dry it, and perform vapor-phase hydrophobic treatment with hexamethyldisiloxane to obtain an Al-modified high-temperature resistant SiO2 aerogel that can be stored for a long time.
[0045] Al-modified high-temperature resistant SiO2 aerogel was heat-treated at 800℃, and its shrinkage rate was measured to be 2.4%. The specific surface area distribution before and after calcination was 542.5 m². 2 / g and 493.4m 2 / g, the thermal conductivity before and after the test is 0.022W / m / k and 0.023W / m / k respectively.
[0046] Example 2:
[0047] 100g of deionized water was added to tetraethyl orthosilicate with a SiO2 solid content of 27%, followed by 2g of 1mol / L HNO3 solution. The mixture was stirred and hydrolyzed for 1 hour to obtain a silica sol. Then, 3g of 1mol / L ammonia was added, and the mixture was vigorously mixed. The gel was allowed to stand and aged at 60℃ for 4 days. The aged gel was replaced three times with ethanol over two days to obtain an alcohol gel, which was then subjected to supercritical drying. After drying, 2g of SiO2 aerogel was placed in a container equipped with a reflux condenser, and an aluminum isopropoxide cyclohexane solution was added (0.3g of aluminum isopropoxide and 60mL of hexane solution). The reaction was carried out at 90℃ for 1 hour in a heated reflux condenser, depositing a nano-thick layer of aluminum oxide on the surface of the SiO2 aerogel particles. After the solution cooled to room temperature, the Al-modified SiO2 aerogel was removed, dried, and subjected to vapor-phase hydrophobic treatment with hexamethyldisiloxane to obtain a long-term storage-grade Al-modified high-temperature resistant SiO2 aerogel.
[0048] Al-modified high-temperature resistant SiO2 aerogel was heat-treated at 1000℃, and its shrinkage rate was measured to be 3.3%. The specific surface area distribution before and after calcination was 320.2 m². 2 / g and 290.6m 2 / g, the thermal conductivity before and after the test is 0.026W / m / k and 0.027W / m / k respectively.
[0049] Example 3:
[0050] Take 100g of deionized water, add 4g of hexadecyltrimethylammonium bromide and 0.2g of citric acid, and add methyltriethoxysilane according to a SiO2 solid content of 23% (the percentage of water + silicon precursor by mass). Stir vigorously for 4 hours to hydrolyze, then add 0.3g of 1mol / L NH4F solution, stir for 20 minutes, allow the gel to stand, and age at 180℃ for 1.5 days. The aged gel is then directly dried under normal pressure for 4 days, followed by gradient drying at 60℃ and 120℃ for 6 hours each. Immediately afterward, calcination is performed at 450℃ for half an hour to remove surface alkyl groups. Place 3g of alkyl-free aerogel in a container equipped with a reflux condenser, add 0.4g of aluminum sec-butoxide and 120mL of n-heptane solution. React at 90℃ for 2 hours in a reflux condenser to deposit a nano-thick layer of aluminum oxide on the surface of the SiO2 aerogel particles. After the solution cooled to room temperature, the Al-modified SiO2 aerogel was removed, dried, and hydrophobically treated with hexamethyldisiloxane to obtain an Al-modified high-temperature resistant SiO2 aerogel that could be stored for a long time.
[0051] Al-modified high-temperature resistant SiO2 aerogel was heat-treated at 900℃, and its shrinkage rate was measured to be 3.6%. The specific surface area distribution before and after calcination was 280.7 m². 2 / g and 227.8m 2 / g, the thermal conductivity before and after the test is 0.033W / m / k and 0.034W / m / k respectively.
[0052] Example 4:
[0053] Take 100g of deionized water, add 3g of hexadecyltrimethylammonium chloride and 0.3g of acetic acid, and add methyltrimethoxysilane according to a SiO2 solid content of 15%. Stir vigorously for 24h to hydrolyze. Add 0.5g of 1mol / L NH3·H2O solution, stir for 15min, allow the gel to stand, and age at 150℃ for 4 days. The aged gel is then directly dried under normal pressure for 3 days, followed by gradient drying at 60℃ and 150℃ for 5h each. Immediately afterward, calcine at 350℃ for two hours to remove surface alkyl groups. Place 2g of alkyl-free aerogel in a sealed container, add aluminum isopropoxide cyclohexane solution (0.2g by mass) and n-heptane solution (60mL by mass), and react at 30℃ for 8h to deposit a nano-thick aluminum oxide layer on the surface of the SiO2 aerogel particles. After the solution cooled to room temperature, the Al-modified SiO2 aerogel was removed, dried, and hydrophobically treated with hexamethyldisiloxane to obtain an Al-modified high-temperature resistant SiO2 aerogel that could be stored for a long time.
[0054] Al-modified high-temperature resistant SiO2 aerogel was heat-treated at 700℃, and its shrinkage rate was measured to be 0.8%. The specific surface area distribution before and after calcination was 330.2 m². 2 / g and 315.6m 2 / g, the thermal conductivity before and after the test is 0.031W / m / k and 0.031W / m / k respectively.
[0055] Comparative Example 1:
[0056] Take 100g of deionized water, add tetraethyl orthosilicate with a SiO2 solid content of 20% (the percentage of water + silicon precursor by total mass), add 2g of 1mol / L HNO3 solution, stir and hydrolyze for 1h, then add 1.5g of 1mol / L ammonia solution and stir thoroughly. After gelation, age at 120℃ for 3 days. The aged wet gel is replaced with ethanol three times over 2 days to obtain an alcohol gel, which is then subjected to supercritical drying. Hydrophobic treatment with hexamethyldisiloxane yields a SiO2 aerogel suitable for long-term storage.
[0057] The SiO2 aerogel was heat-treated at 800℃, and its shrinkage rate was measured to be 22%. The specific surface area distribution before and after calcination was 632.5 m². 2 / g and 63.4m 2 / g, the thermal conductivity before and after the test is 0.021W / m / k and 0.058W / m / k respectively.
[0058] Comparative Example 2:
[0059] Take 100g of deionized water, add 3g of hexadecyltrimethylammonium chloride and 0.3g of acetic acid, and add methyltrimethoxysilane according to a SiO2 solid content of 15%. Stir vigorously for 24h to hydrolyze, then add 0.5g of 1mol / L NH3·H2O solution, stir for 15min, allow the gel to stand, and age at 150℃ for 4 days. The aged gel is then directly dried under normal pressure for 3 days, followed by gradient drying at 60℃ and 150℃ for 5h each time, and then hydrophobically treated with hexamethyldisiloxane to obtain a high-temperature resistant SiO2 aerogel suitable for long-term storage.
[0060] The SiO2 aerogel was heat-treated at 700℃, and its shrinkage rate was measured to be 19%. The specific surface area distribution before and after calcination was 330.2 m². 2 / g and 315.6m 2 / g, the thermal conductivity before and after the test is 0.031W / m / k and 0.057W / m / k respectively.
[0061] The test data for the above embodiments and comparative examples are shown in Table 1 below.
[0062] Table 1. Summary of Test Data for Examples and Comparative Examples
[0063]
[0064] The comparison of the test data in Table 1 above shows that introducing aluminum oxide onto the aerogel surface by chemical liquid phase deposition significantly improves the temperature resistance of the material. After high-temperature treatment, the shrinkage rate is greatly controlled (within 5%), and the specific surface area is well preserved, indicating that the pore structure is supported and protected. The aerogel structure is maintained at high temperatures, which helps to effectively suppress high-temperature gas phase heat transfer and play a role in high-temperature heat insulation.
[0065] Although the present invention has been disclosed above with reference to embodiments, it is not intended to limit the present invention. Appropriate modifications or equivalent substitutions made by those skilled in the art to the technical solutions of the present invention should be covered within the protection scope of the present invention, which is defined by the claims.
Claims
1. A method for preparing a high-temperature resistant silicon-based aerogel, characterized in that, Includes the following steps: (1) Add silicon precursor and acid catalyst to water for hydrolysis, then add base catalyst for gelation to obtain SiO2 wet gel; (2) The SiO2 wet gel is dried to obtain SiO2 aerogel, which is then placed in a container and an aluminum precursor organic solution that reacts with the hydroxyl and alkoxy groups on the surface of the SiO2 aerogel is added to carry out a chemical liquid phase deposition reaction to deposit a nano-thick aluminum oxide layer on the surface of the SiO2 aerogel to obtain a high-temperature resistant aluminum modified SiO2 aerogel. (3) Dry the aluminum-modified SiO2 aerogel in a ventilated environment, and then perform gas-phase hydrophobicity or liquid-phase hydrophobicity to obtain high-temperature resistant aluminum-modified SiO2 aerogel.
2. The preparation method according to claim 1, characterized in that, In step (1), the solid content of SiO2 in the SiO2 wet gel is 15%~30%, and the amount of silicon precursor added is determined according to this solid content.
3. The preparation method according to claim 1, characterized in that, In step (1), the silicon precursor is selected from either an organosilicon source or an inorganic silicon source. The organosilicon source is one of methyl orthosilicate, ethyl orthosilicate, polyethyl orthosilicate Si-40, methyltrimethoxysilane, ethyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, dimethyldimethoxysilane, diethyldimethoxysilane, dimethyldiethoxysilane, diethyldiethoxysilane, vinyltrimethoxysilane, or phenyltrimethoxysilane. The inorganic silicon source is one of sodium silicate, silicic acid, or silica sol. For organosilicon sources that are immiscible with water, a phase separation inhibitor is added simultaneously or in advance. The phase separation inhibitor is a cationic surfactant or a nonionic surfactant, and the amount of the phase separation inhibitor is 1% to 5% of the total mass of the silicon precursor and water.
4. The preparation method according to claim 1, characterized in that, In step (1), the acid catalyst is selected from one of nitric acid, hydrochloric acid, sulfuric acid, phosphoric acid, oxalic acid, acetic acid, citric acid, maleic acid, and hydrofluoric acid. After the acid catalyst is added, the pH of the solution is between 2 and 7.5, and the hydrolysis time is 0.5 to 24 hours. The alkaline catalyst is one of ammonia, NH4F, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetramethylammonium fluoride, and tetraethylammonium fluoride. The amount of alkaline catalyst used is 0.01% to 3% of the total mass of silicon precursor and water.
5. The preparation method according to claim 1, characterized in that, In step (1), the gelation conditions are aging at 40~200℃ for 24~96h.
6. The preparation method according to claim 1, characterized in that, In step (2), the drying method is atmospheric pressure drying, supercritical drying or freeze drying. Silicon precursors containing non-hydrolyzable organic groups are selected for atmospheric pressure drying, while other silicon precursors are aged and replaced with ethanol, and then subjected to supercritical drying or freeze drying. The SiO2 aerogel after atmospheric pressure drying is calcined at 350~500℃ for 0.5~2h to remove surface alkyl groups.
7. The preparation method according to claim 1, characterized in that, In step (2), the aluminum precursor is one of aluminum isopropoxide, aluminum sec-butoxide, aluminum hydroxide, aluminum chloride, aluminum nitrate, aluminum sulfate, and sodium aluminate; the organic solvent used in the organic solution of the aluminum precursor is one of n-hexane, cyclohexane, n-heptane, pentane, ethanol, and isopropanol; the mass ratio of the aluminum precursor to the volume of the organic solvent is 1 g / (50~400 mL); and the mass ratio of the dried, non-hydrophobic SiO2 aerogel to the aluminum precursor is 1:(0.01~0.2).
8. The preparation method according to claim 1, characterized in that, In step (2), the temperature of the chemical liquid phase deposition reaction is room temperature to 90°C, and the reaction time is 0.5 to 9 hours. When the reaction temperature is higher than that of the organic solvent volatilization, a condensation reflux device is configured to dissolve the aluminum precursor and make the SiO2 aerogel below the surface of the organic solvent.
9. The preparation method according to claim 1, characterized in that, In step (2), the thickness of the aluminum oxide layer is 2~15nm.
Citation Information
Patent Citations
Method of preparing double-silicon source system self-hydrophobic aerogel by chemical liquid phase deposition
CN108467045A
Ordinary pressure preparation method for aluminium oxide composite aerogel rapped by silicon dioxide
CN109621849A
Preparation method of high-temperature-resistant modified silicon oxide aerogel heat-insulation composite material
CN115108809A
Preparation method of aluminum oxide-silicon oxide aerogel composite material
CN113716572A