Anticorrosive paint for outdoor metal members
By using modified calcium sulfate whiskers and water-based epoxy resin emulsions in anti-corrosion coatings, the problem of poor acid and alkali resistance of existing coatings has been solved, achieving high-efficiency anti-corrosion of outdoor metal components and enhancing the overall performance and applicability of the coatings.
Patent Information
- Application Number
- CN202411542619.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-31
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-10-31
AI Technical Summary
Existing anti-corrosion coatings have poor acid and alkali resistance and cannot meet the anti-corrosion requirements of outdoor metal components that are exposed to the natural environment for a long time.
Using modified calcium sulfate whiskers, waterborne epoxy resin emulsion, amino resin and other raw materials, the surface of calcium sulfate whiskers is modified to introduce active groups such as siloxy groups, acid anhydride groups, ester groups, fluorine groups, phenyl groups and other groups, thereby enhancing the interaction between the modified calcium sulfate whiskers and the raw materials and improving the impact strength, tensile strength, neutral salt spray resistance, acid resistance and alkali resistance of the coating film.
It improves the overall performance of anti-corrosion coatings, and the paint film exhibits excellent mechanical properties, adhesion and acid and alkali resistance, making it suitable for the protection of outdoor metal components such as stainless steel, aluminum alloy, galvanized sheet, copper sheet, copper alloy, and cast iron.
Smart Images

Figure BDA0005113121060000051 
Figure BDA0005113121060000061
Abstract
Description
Technical Field
[0001] This application relates to the field of water-based coatings technology, and more specifically, to an anti-corrosion coating for outdoor metal components. Background Technology
[0002] Outdoor metal components are exposed to the natural environment for extended periods, making them susceptible to corrosion from atmospheric, water, and chemical substances. This corrosion leads to decreased performance, shortened lifespan, and potential safety hazards. Among various anti-corrosion technologies for metal components, anti-corrosion coatings are one of the most effective methods to reduce or delay corrosion. Anti-corrosion coatings are widely used due to their advantages of easy application, strong adaptability, and low cost. Existing anti-corrosion coatings often use water-based epoxy resin emulsions as raw materials, with the addition of film-forming aids, catalysts, wetting agents, defoamers, leveling agents, and other additives. These raw materials are then mixed to obtain the anti-corrosion coating. While this type of coating exhibits good water resistance, its acid and alkali resistance is poor and requires further improvement. Summary of the Invention
[0003] To improve the acid and alkali resistance of anti-corrosion coatings, this application provides an anti-corrosion coating for outdoor metal components, employing the following technical solution: An anti-corrosion coating for outdoor metal components is mainly composed of the following raw materials in parts by weight: 90-110 parts of water-based epoxy resin emulsion, 9-11 parts of amino resin, 2-4 parts of film-forming aid, 0.3-0.8 parts of catalyst, 2-4 parts of modified calcium sulfate whiskers, 1-3 parts of organic bentonite, 1-2 parts of substrate wetting agent, 0.2-0.5 parts of adhesion promoter, 0.2-0.5 parts of anti-flash rust agent, 0.3-0.8 parts of defoamer, 0.3-0.8 parts of leveling agent, and 60-70 parts of deionized water; The modified calcium sulfate whiskers were obtained by treating calcium sulfate whiskers with 3-(methacryloyloxy)propyltrimethoxysilane, 2-methylene succinic anhydride, trifluoroethyl acrylate, and ethyl 4-acrylamidobenzoate.
[0004] The anti-corrosion coating for outdoor metal components disclosed in this application, through the synergistic effect of its raw materials, achieves a paint film with impact strength >70cm, tensile strength >5MPa, neutral salt spray resistance >55d, acid resistance >40d, and alkali resistance >45d. This demonstrates advantages such as strong mechanical properties, high adhesion, good acid and alkali resistance, and excellent anti-corrosion effect, meeting market demands. Furthermore, the paint film obtained by this anti-corrosion coating has a smooth, aesthetically pleasing, uniform appearance, facilitating application and making it suitable for the protection of outdoor metal components made of stainless steel, aluminum alloy, galvanized sheet, copper sheet, copper alloy, cast iron, and other materials, thus expanding its application range.
[0005] Adding water-based epoxy resin emulsion and amino resin to the raw materials of anti-corrosion coatings gives the paint film excellent basic properties. Adding calcium sulfate whiskers and organic bentonite not only acts as fillers but also increases the bonding force and overall integrity between the raw materials, resulting in superior mechanical properties, adhesion, acid and alkali resistance, and anti-corrosion effects. Furthermore, the calcium sulfate whiskers are modified by introducing numerous active groups such as siloxy groups, acid anhydride groups, ester groups, fluorine groups, phenyl groups, and amide groups onto their surface. This enhances the interaction between the modified calcium sulfate whiskers and the raw materials, improving the performance of the modified calcium sulfate whiskers and increasing the paint film's impact strength, tensile strength, neutral salt spray resistance, acid resistance, and alkali resistance. This enhances the overall performance of the paint film, resulting in superior comprehensive performance of the anti-corrosion coating.
[0006] Optionally, the modified calcium sulfate whiskers are prepared using the following method: T1. Add calcium sulfate whiskers to ethanol and mix, then add 3-(methacryloyloxy)propyltrimethoxysilane and stir for 1-3 hours to obtain a premixed solution. T2. Mix the premixed solution, 2-methylene succinic anhydride, trifluoroethyl acrylate, and ethyl 4-acrylamidobenzoate, add peroxide, stir for 2-4 hours, filter, wash, and dry to obtain modified calcium sulfate whiskers.
[0007] Optionally, the weight ratio of the calcium sulfate whiskers, 3-(methacryloyloxy)propyltrimethoxysilane, 2-methylene succinic anhydride, trifluoroethyl acrylate, ethyl 4-acrylamidobenzoate, and peroxide is (9-11):(2-4):(0.5-1.5):(0.5-1.5):(0.5-1.5):(0.05-0.2).
[0008] By employing the above technical solution, 3-(methacryloyloxy)propyltrimethoxysilane is first grafted onto the surface of calcium sulfate whiskers using siloxy groups, introducing carbon-carbon double bonds. Then, 2-methylene succinic anhydride, trifluoroethyl acrylate, and ethyl 4-acrylamidobenzoate are grafted onto the surface of the calcium sulfate whiskers using a polymerization reaction. The preparation method of this application completes the grafting of calcium sulfate whiskers in steps, ensuring the grafting amount on the surface of the calcium sulfate whiskers, facilitating the preparation of calcium sulfate whiskers, enhancing the performance of the modified calcium sulfate whiskers, and improving the overall performance of the paint film.
[0009] Optionally, the peroxide is one or more of di-tert-butyl peroxide, tert-amyl peroxide neopentyl peroxide, benzoyl peroxide, benzoic acid peroxide, and tert-butyl peroxide.
[0010] By adopting the above technical solution, the peroxide is optimized, which facilitates the selection of peroxide. Moreover, di-tert-butyl peroxide, tert-amyl peroxide neopentyl ester, benzoyl peroxide, benzoic acid peroxide, and tert-butyl peroxide can all release free radicals and initiate and promote polymerization reactions, ensuring the smooth grafting of organic matter and also ensuring the stability and performance of the modified calcium sulfate whiskers.
[0011] Optionally, in the method for preparing modified calcium sulfate whiskers, the weight ratio of calcium sulfate whiskers to ethanol is (9-11):(80-120).
[0012] Optionally, the calcium sulfate whiskers have an average diameter of 1-3 μm and an average length of 20-50 μm.
[0013] By adopting the above technical solution, the average diameter and average length of calcium sulfate whiskers are optimized to ensure that the calcium sulfate whiskers have a good aspect ratio, thereby enhancing the effect of calcium sulfate whiskers on the mechanical properties and anti-corrosion performance of coatings. In several embodiments, the average diameter of the calcium sulfate whiskers is 2μm and the average length is 30μm. The average diameter can also be set to 1μm, 1.5μm, 2.5μm, or 3μm as needed, but is not limited to the listed values; other unlisted values within this range are also applicable. The average length can also be set to 20μm, 25μm, 35μm, 40μm, 45μm, or 50μm, but is not limited to the listed values; other unlisted values within this range are also applicable.
[0014] Optionally, the aqueous epoxy resin emulsion is EPIKOTE 3520-WY-55A; the amino resin is CYMEL325.
[0015] By adopting the above technical solutions, the waterborne epoxy resin emulsion and amino resin are optimized, which facilitates the selection of waterborne epoxy resin emulsion and amino resin, and ensures the stability and quality of the anti-corrosion coating performance.
[0016] Optionally, the film-forming aid is one or more of the following: film-forming aid HY-12C, film-forming aid NX 795, film-forming aid DALPAD292, and film-forming aid OE 400.
[0017] By adopting the above technical solutions, the film-forming aids are optimized, facilitating their selection. Furthermore, these film-forming aids effectively improve the film-forming properties of anti-corrosion coatings, enhance the flexibility and weather resistance of the paint film, and ensure the acid and alkali resistance and anti-corrosion effect of the coatings.
[0018] Optionally, the catalyst is one or more of the following: catalyst CYCAT 4040, catalyst CYCAT 4045, catalyst CYCAT6020, and catalyst CYCAT 296-10.
[0019] By adopting the above technical solution, the catalyst can be optimized, facilitating catalyst selection. Furthermore, the catalyst can promote the reaction, increase the curing rate and film hardness of the anti-corrosion coating, and enhance its anti-corrosion performance.
[0020] Optionally, the substrate wetting agent is one or more of the following: substrate wetting agent TEGO 4100, substrate wetting agent TEGO 245, substrate wetting agent HY-408, and substrate wetting agent Dynol 607. The adhesion promoter is one or more of the following: adhesion promoter LD-157, adhesion promoter XH-168, adhesion promoter Z-6040, and adhesion promoter YB-201D.
[0021] By adopting the above technical solutions, the substrate wetting agent and adhesion promoter are optimized, facilitating their selection. Furthermore, the synergistic effect between the substrate wetting agent and adhesion promoter reduces the occurrence of paint film delamination and enhances the adhesion and durability of the paint film.
[0022] Optionally, the anti-flash embroidery agent is one or more of the following: anti-flash embroidery agent HX-1126, anti-flash embroidery agent THIF-3118, anti-flash embroidery agent CK34, and anti-flash embroidery agent R-726. The defoamer is one or more of the following: defoamer AKN-3801, defoamer TEGO 830, defoamer BYK 024, and defoamer HY-024; The leveling agent is one or more of the following: TEGO 410, BYK-333, BYK-310, and EFKA-FL3777.
[0023] By adopting the above technical solutions, the anti-rust agent, defoamer, and leveling agent are optimized, making their selection easier. Furthermore, the synergistic effect of these agents reduces rust formation on the paint film, maintaining a smooth, aesthetically pleasing, uniform appearance and improving overall paint film quality.
[0024] Optionally, a method for preparing an anti-corrosion coating for outdoor metal components includes the following steps: An anti-corrosion coating is obtained by mixing water-based epoxy resin emulsion, amino resin, film-forming aid, catalyst, modified calcium sulfate whiskers, organic bentonite, substrate wetting agent, adhesion promoter, anti-flash rust agent, defoamer, leveling agent, and deionized water.
[0025] In summary, this application has at least the following beneficial effects: 1. The anti-corrosion coating for outdoor metal components of this application incorporates modified calcium sulfate whiskers and organic bentonite into the raw materials. Utilizing the synergistic effect between these materials, the bonding strength and overall integrity of the raw materials are greatly enhanced. This not only results in a smooth, aesthetically pleasing, uniform, and uniform paint film appearance, but also enhances the film's mechanical properties, adhesion, acid and alkali resistance, and anti-corrosion effect. Furthermore, the paint film exhibits impact strength >70cm, tensile strength >5MPa, neutral salt spray resistance >55d, acid resistance >40d, and alkali resistance >45d, improving the overall performance of the paint film and ensuring the quality of the anti-corrosion coating. It is suitable for the protection of outdoor metal components made of stainless steel, aluminum alloy, galvanized sheet, copper sheet, copper alloy, cast iron, etc., meeting market demands.
[0026] 2. The method for preparing modified calcium sulfate whiskers in this application involves grafting 3-(methacryloyloxy)propyltrimethoxysilane onto the surface of calcium sulfate whiskers using siloxy groups, followed by a polymerization reaction to graft 2-methylene succinic anhydride, trifluoroethyl acrylate, and ethyl 4-acrylamidobenzoate onto the surface of the calcium sulfate whiskers. This preparation method is simple and convenient, and ensures the effectiveness of the modified calcium sulfate whiskers, improving the overall performance of the paint film. Detailed Implementation
[0027] To make this application easier to understand, the following detailed description will be provided with reference to embodiments. These embodiments are for illustrative purposes only and are not intended to limit the scope of application of this application. Unless otherwise specified, the raw materials or components used in this application can be obtained commercially or by conventional methods.
[0028] Preparation Example Preparation Example 1 A modified calcium sulfate whisker is prepared by the following method: T1. At a rotation speed of 400 r / min, add 10 g of calcium sulfate whiskers to 100 g of ethanol and stir for 5 min. Then add 3 g of 3-(methacryloyloxy)propyltrimethoxysilane and stir for 2 h to obtain a premix.
[0029] The calcium sulfate whiskers had an average diameter of 2 μm and an average length of 30 μm, and were selected from Jinan Xinquan Chemical Technology Co., Ltd.
[0030] T2. At a rotation speed of 400 r / min, 1 g of 2-methylene succinic anhydride, 1 g of trifluoroethyl acrylate, and 1 g of ethyl 4-acrylamidobenzoate were added to the premix obtained in step T1, and the mixture was stirred for 2 min. Then, 0.1 g of peroxide was added, and the mixture was stirred for 3 h. After that, the mixture was filtered, washed, and dried to obtain modified calcium sulfate whiskers.
[0031] The peroxide is di-tert-butyl peroxide.
[0032] Preparation Example 2 A modified calcium sulfate whisker is prepared by the following method: T1. At a rotation speed of 400 r / min, add 9 g of calcium sulfate whiskers to 80 g of ethanol and stir for 5 min. Then add 2 g of 3-(methacryloyloxy)propyltrimethoxysilane and stir for 1 h to obtain a premix.
[0033] The calcium sulfate whiskers had an average diameter of 2 μm and an average length of 30 μm, and were selected from Jinan Xinquan Chemical Technology Co., Ltd.
[0034] T2. At a rotation speed of 400 r / min, 1.5 g of 2-methylene succinic anhydride, 1.5 g of trifluoroethyl acrylate, and 0.5 g of ethyl 4-acrylamidobenzoate were added to the premix obtained in step T1, and the mixture was stirred for 2 min. Then, 0.2 g of peroxide was added, and the mixture was stirred for 2 h. After that, the mixture was filtered, washed, and dried to obtain modified calcium sulfate whiskers.
[0035] The peroxide is di-tert-butyl peroxide.
[0036] Preparation Example 3 A modified calcium sulfate whisker is prepared by the following method: T1. At a rotation speed of 400 r / min, 11 g of calcium sulfate whiskers were added to 120 g of ethanol and stirred for 5 min. Then, 4 g of 3-(methacryloyloxy)propyltrimethoxysilane was added and stirred for 3 h to obtain a premix.
[0037] The calcium sulfate whiskers had an average diameter of 2 μm and an average length of 30 μm, and were selected from Jinan Xinquan Chemical Technology Co., Ltd.
[0038] T2. At a rotation speed of 400 r / min, 0.5 g of 2-methylene succinic anhydride, 0.5 g of trifluoroethyl acrylate, and 1.5 g of ethyl 4-acrylamidobenzoate were added to the premix obtained in step T1, and the mixture was stirred for 2 min. Then, 0.05 g of peroxide was added, and the mixture was stirred for 4 h. After that, the mixture was filtered, washed, and dried to obtain modified calcium sulfate whiskers.
[0039] The peroxide is di-tert-butyl peroxide. Example
[0040] Table 1. Amount of each raw material used in anti-corrosion coatings (unit: ×10g) Example 1 A corrosion-resistant coating for outdoor metal components, the raw materials and their proportions are shown in Table 1.
[0041] Among them, the waterborne epoxy resin emulsion is EPIKOTE 3520-WY-55A; the amino resin is CYMEL325; the film-forming aid is HY-12C; the catalyst is CYCAT 4040; the organic bentonite is BENTONE SD-1; the substrate wetting agent is TEGO 4100; the adhesion promoter is LD-157; the anti-flash rust agent is HX-1126; the defoamer is AKN-3801; the leveling agent is TEGO 410; and the modified calcium sulfate whiskers are prepared using the method of Preparation Example 1.
[0042] A method for preparing an anti-corrosion coating for outdoor metal components includes the following steps: At a rotation speed of 800 rpm, deionized water and amino resin were added to an aqueous epoxy resin emulsion, and the mixture was stirred for 5 minutes. Then, film-forming aids, catalysts, substrate wetting agents, adhesion promoters, anti-flame rust agents, defoamers, and leveling agents were added, and the mixture was stirred for 5 minutes. Afterward, modified calcium sulfate whiskers and organobentonite were added, and the mixture was stirred for 10 minutes to obtain an anti-corrosion coating.
[0043] Example 2 An anti-corrosion coating for outdoor metal components differs from that in Example 1 in that the raw material ratio of the anti-corrosion coating is different, and the raw material ratio is shown in Table 1.
[0044] Example 3 An anti-corrosion coating for outdoor metal components differs from that in Example 1 in that the raw material ratio of the anti-corrosion coating is different, and the raw material ratio is shown in Table 1.
[0045] Example 4 An anti-corrosion coating for outdoor metal components differs from Example 1 in that the modified calcium sulfate whiskers in the raw materials of the anti-corrosion coating are from a different source, and the modified calcium sulfate whiskers are prepared using the method of Preparation Example 2.
[0046] Example 5 An anti-corrosion coating for outdoor metal components differs from that in Example 1 in that the modified calcium sulfate whiskers in the raw materials of the anti-corrosion coating are from a different source, and the modified calcium sulfate whiskers are prepared using the method of Preparation Example 3.
[0047] Comparative Example Comparative Example 1 An anti-corrosion coating for outdoor metal components differs from that in Example 1 in that an equal amount of water-based epoxy resin emulsion replaces modified calcium sulfate whiskers and organic bentonite in the raw materials of the anti-corrosion coating.
[0048] Comparative Example 2 An anti-corrosion coating for outdoor metal components differs from Example 1 in that, in the raw materials of the anti-corrosion coating, an equal amount of calcium sulfate whiskers replaces modified calcium sulfate whiskers and organic bentonite.
[0049] Comparative Example 3 An anti-corrosion coating for outdoor metal components differs from Example 1 in that an equal amount of organic bentonite is used to replace the modified calcium sulfate whiskers in the raw materials of the anti-corrosion coating.
[0050] Comparative Example 4 An anti-corrosion coating for outdoor metal components differs from that in Example 1 in that an equal amount of calcium sulfate whiskers are used to replace modified calcium sulfate whiskers in the raw materials of the anti-corrosion coating.
[0051] Comparative Example 5 An anti-corrosion coating for outdoor metal components differs from that in Example 1 in that, in the preparation method of modified calcium sulfate whiskers, an equal amount of 2-methylene succinic anhydride replaces trifluoroethyl acrylate and ethyl 4-acrylamidobenzoate.
[0052] Comparative Example 6 An anti-corrosion coating for outdoor metal components differs from that in Example 1 in that, in the preparation method of modified calcium sulfate whiskers, an equal amount of trifluoroethyl acrylate is used instead of ethyl 4-acrylamidobenzoate.
[0053] Comparative Example 7 An anti-corrosion coating for outdoor metal components differs from that in Example 1 in that, in the preparation method of modified calcium sulfate whiskers, an equal amount of ethyl 4-acrylamidobenzoate is used instead of ethyl trifluoroacrylate in the raw materials of the anti-corrosion coating.
[0054] Performance testing The anti-corrosion coatings obtained in Examples 1-5 and Comparative Examples 1-7 were taken as samples, and the following performance tests were performed on the samples. The test results are shown in Table 2.
[0055] In accordance with GB / T1732-2020 "Test Method for Impact Resistance of Coating Film", the impact resistance of the sample is tested, and the greater the impact resistance, the better the mechanical properties of the coating film.
[0056] According to GB / T5210-2006 "Paints and Varnishes - Pull-off Adhesion Test", the pull-off strength of the samples is tested, and the greater the pull-off strength, the better the adhesion of the paint film.
[0057] The neutral salt spray resistance of the samples was tested in accordance with GB / T1771-2007 "Determination of resistance to neutral salt spray in paints and varnishes".
[0058] According to GB / T9274-1988 "Determination of resistance to liquid media for paints and varnishes", the acid resistance and alkali resistance of the samples were tested.
[0059] The acid-resistant liquid medium used is a 5% hydrochloric acid aqueous solution at a temperature of 23°C; the alkali-resistant liquid medium used is a 5% sodium hydroxide aqueous solution at a temperature of 23°C.
[0060] Table 2 Detection Results Testing items Impact resistance strength (cm) Tensile strength (MPa) Neutral salt spray resistance / (d) Acid resistance / (d) Alkali resistance / (d) Example 1 75 5.9 60 45 52 Example 2 73 5.7 58 44 50 Example 3 72 5.8 57 43 51 Example 4 73 5.8 59 43 51 Example 5 74 5.7 57 44 50 Comparative Example 1 43 4.7 34 23 28 Comparative Example 2 58 4.4 46 34 38 Comparative Example 3 55 5.1 43 32 36 Comparative Example 4 62 4.9 49 37 41 Comparative Example 5 65 5.2 51 38 44 Comparative Example 6 69 5.6 54 40 45 Comparative Example 7 68 5.6 55 41 46 As can be seen from Table 2, the anti-corrosion coating obtained by this application has high impact strength and tensile strength, with an impact strength of 72-75 cm and a tensile strength of 5.7-5.9 MPa, demonstrating high mechanical properties and adhesion. It also has high resistance to neutral salt spray, acid and alkali, with a neutral salt spray resistance of 57-60 days, an acid resistance of 43-45 days, and an alkali resistance of 50-52 days, demonstrating high acid and alkali resistance and anti-corrosion effect, which can meet market demand.
[0061] Comparative Examples 1-4 were compared. Comparative Example 1's anti-corrosion coating did not contain calcium sulfate whiskers or organic bentonite; Comparative Example 2's anti-corrosion coating contained calcium sulfate whiskers; and Comparative Example 3's anti-corrosion coating contained organic bentonite. This shows that adding organic bentonite alone to the anti-corrosion coating can improve tensile strength, but adding calcium sulfate whiskers alone actually reduces tensile strength. Furthermore, adding either organic bentonite or calcium sulfate whiskers alone can increase impact strength, acid and alkali resistance, and anti-corrosion effect. Combining this with Comparative Example 4, the anti-corrosion coating in Comparative Example 4 contained calcium sulfate whiskers and organic bentonite. This shows that further, adding both organic bentonite and calcium sulfate whiskers to the anti-corrosion coating, and utilizing their synergistic effect, can significantly improve impact strength, neutral salt spray resistance, acid resistance, and alkali resistance without affecting tensile strength.
[0062] Comparative Examples 4 and 5 were compared. Comparative Example 4's anticorrosion coating raw materials included calcium sulfate whiskers; Comparative Example 5's anticorrosion coating raw materials included calcium sulfate whiskers treated with 3-(methacryloyloxy)propyltrimethoxysilane and 2-methylenesuccinic anhydride. This shows that modifying calcium sulfate whiskers improves the compatibility between the whiskers and the raw materials, significantly enhances paint film adhesion, and also improves the mechanical properties, acid and alkali resistance, and anticorrosion effect of the paint film. In conjunction with Comparative Examples 6-7 and Example 1, the raw materials of the anti-corrosion coating of Comparative Example 6 were supplemented with calcium sulfate whiskers treated with 3-(methacryloyloxy)propyltrimethoxysilane, 2-methylene succinic anhydride, and trifluoroethyl acrylate; the raw materials of the anti-corrosion coating of Comparative Example 7 were supplemented with calcium sulfate whiskers treated with 3-(methacryloyloxy)propyltrimethoxysilane, 2-methylene succinic anhydride, and ethyl 4-acrylamidobenzoate; and the raw materials of the anti-corrosion coating of Example 1 were supplemented with calcium sulfate whiskers treated with 3-(methacryloyloxy)propyltrimethoxysilane, 2-methylene succinic anhydride, trifluoroethyl acrylate, and ethyl 4-acrylamidobenzoate. This demonstrates that further grafting of 3-(methacryloyloxy)propyltrimethoxysilane and 2-methylene succinic anhydride onto calcium sulfate whiskers, along with the simultaneous grafting of trifluoroethyl acrylate and 4-acrylamidoethyl benzoate, and utilizing their synergistic effect, can further improve the performance of modified calcium sulfate whiskers. This enhances impact resistance, tensile strength, neutral salt spray resistance, acid resistance, and alkali resistance, thereby strengthening the overall performance of the coating film and resulting in superior comprehensive performance and effectiveness of the anti-corrosion coating.
[0063] It should be noted that the embodiments described above are only for explaining this application and do not constitute any limitation on this application. This application has been described with reference to typical embodiments, but it should be understood that the terms used therein are descriptive and explanatory terms, not limiting terms. Modifications can be made to this application within the scope of the claims, and revisions can be made to the invention without departing from the scope and spirit of this application. Although the application described herein relates to specific methods, materials, and embodiments, it does not mean that this application is limited to the specific examples disclosed herein; on the contrary, this application can be extended to all other methods and applications with the same function.
Claims
1. An anti-corrosion coating for outdoor metal components, characterized in that: It is mainly made of the following raw materials in parts by weight: 90-110 parts of water-based epoxy resin emulsion, 9-11 parts of amino resin, 2-4 parts of film-forming aid, 0.3-0.8 parts of catalyst, 2-4 parts of modified calcium sulfate whiskers, 1-3 parts of organic bentonite, 1-2 parts of substrate wetting agent, 0.2-0.5 parts of adhesion promoter, 0.2-0.5 parts of anti-flash rust agent, 0.3-0.8 parts of defoamer, 0.3-0.8 parts of leveling agent, and 60-70 parts of deionized water; The modified calcium sulfate whiskers are prepared by the following method: T1, calcium sulfate whiskers are added to ethanol and mixed, then 3-(methacryloyloxy)propyltrimethoxysilane is added and stirred for 1-3 hours to obtain a premixed solution; T2. Mix the premixed solution, 2-methylene succinic anhydride, trifluoroethyl acrylate, and ethyl 4-acrylamidobenzoate, add peroxide, stir for 2-4 hours, filter, wash, and dry to obtain modified calcium sulfate whiskers. The weight ratio of the calcium sulfate whiskers, 3-(methacryloyloxy)propyltrimethoxysilane, 2-methylene succinic anhydride, trifluoroethyl acrylate, ethyl 4-acrylamidobenzoate, and peroxide is (9-11):(2-4):(0.5-1.5):(0.5-1.5):(0.5-1.5):(0.05-0.2).
2. The anti-corrosion coating for outdoor metal components according to claim 1, characterized in that: The peroxide is one or more of di-tert-butyl peroxide, tert-pentyl peroxide neopentyl ester, benzoyl peroxide, benzoic acid peroxide, and tert-butyl peroxide.
3. The anti-corrosion coating for outdoor metal components according to claim 2, characterized in that: The average diameter of the calcium sulfate whiskers is 1-3 μm and the average length is 20-50 μm.
4. The anti-corrosion coating for outdoor metal components according to claim 1, characterized in that: The aqueous epoxy resin emulsion is EPIKOTE 3520-WY-55A; the amino resin is CYMEL325.
5. The anti-corrosion coating for outdoor metal components according to claim 1, characterized in that: The film-forming aid is one or more of the following: film-forming aid HY-12C, film-forming aid NX 795, film-forming aid DALPAD 292, and film-forming aid OE 400.
6. The anti-corrosion coating for outdoor metal components according to claim 1, characterized in that: The catalyst is one or more of the following: catalyst CYCAT 4040, catalyst CYCAT 4045, catalyst CYCAT 6020, and catalyst CYCAT 296-10.
7. The anti-corrosion coating for outdoor metal components according to claim 1, characterized in that: The substrate wetting agent is one or more of the following: substrate wetting agent TEGO 4100, substrate wetting agent TEGO 245, substrate wetting agent HY-408, and substrate wetting agent Dynol 607; the adhesion promoter is one or more of the following: adhesion promoter LD-157, adhesion promoter XH-168, adhesion promoter Z-6040, and adhesion promoter YB-201D.
8. The anti-corrosion coating for outdoor metal components according to claim 1, characterized in that: The anti-flash embroidery agent is one or more of the following: anti-flash embroidery agent HX-1126, anti-flash embroidery agent THIF-3118, anti-flash embroidery agent CK34, and anti-flash embroidery agent R-726; the defoamer is one or more of the following: defoamer AKN-3801, defoamer TEGO 830, defoamer BYK 024, and defoamer HY-024; the leveling agent is one or more of the following: leveling agent TEGO 410, leveling agent BYK-333, leveling agent BYK-310, and leveling agent EFKA-FL3777.
Citation Information
Patent Citations
Modified calcium sulphate crystal whisker as well as preparation method and application thereof
CN108003386A
Aqueous epoxy zinc-enriched paint and preparation method therefor
CN110643260A
Concrete for prefabricated part as well as preparation method and application of concrete
CN118324470A