Preparation method of high-performance core-sheath type composite industrial yarn

By using a composite spinning technology with a shaped spinneret as the sheath and a high-strength material as the core in high-performance fiber materials, the problem of insufficient interfacial friction in traditional sheath-core structures has been solved, achieving a complementary advantage of high strength and functionality, and meeting the performance requirements of high-end industrial fields.

CN119194634BActive Publication Date: 2026-11-24ZHEJIANG GUXIANDAO POLYESTER DOPE DYED YARN CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411445953.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-10-16
Publication Date
2026-11-24
Estimated Expiration
2044-10-16

Smart Images

  • Figure CN119194634B_ABST
    Figure CN119194634B_ABST
Patent Text Reader

Abstract

This application provides a method for preparing high-performance core-sheath composite industrial yarn, belonging to the field of high-performance textile materials technology. A functional polymer material is used as the sheath material, and a high-strength material is used as the core material. After pre-crystallization, the sheath and core materials are dried to a moisture content ≤100ppm and then separately fed into a screw extruder for melt extrusion. The melt corresponding to the sheath material and the melt corresponding to the core material are respectively introduced into the inner and outer layers of the spinning nozzle through a composite spinning assembly. The spinneret of the composite spinning assembly is a shaped spinneret. After spinning, drawing, cooling and solidification, stretching and heat setting, and winding, a core-sheath composite industrial yarn is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to a method for preparing high-performance core-sheath composite industrial yarn, belonging to the field of high-performance textile materials technology. Background Technology

[0002] In the chemical fiber industry, chemical fibers with high strength, high modulus, high temperature resistance, chemical resistance, and weather resistance are collectively referred to as high-performance fibers. In addition to the above mechanical properties, in order to give high-performance fibers better performance, the composition of materials and structures such as composites and core-sheaths are also improved. Two or more polymer spinning solutions are fed into the same spinning assembly and extruded through the same spinneret to obtain composite fibers. During the composite process, different spinnerets can be set to form core-sheath or parallel structures.

[0003] With the rapid development of industrial technology, the demand for high-performance fiber materials is increasing. Common core-sheath composite industrial yarns often improve upon material composition. Examples include: concentric core-sheath composite structures with polyester or polyamide as the sheath and in-situ polymerized graphene polyester or wear-resistant polyamide containing nano-inorganic minerals as the core, imparting anti-pilling properties; core-sheath structures with blended modified polymers as the sheath and polyester as the core, imparting easy dyeing and crimping properties under normal pressure; and polyester-polyamide block copolymers with polyamide as the sheath, polyester as the core, and unsaturated groups dispersed between the sheath and core, and so on. This circular interface facilitates mass production of spinning components and control of the spinning process. However, for applications, as we know, the friction of a circular surface is relatively low, leading to poor core-sheath bonding and performance. Some literature has modified the core-sheath structure to an island-type structure to improve peelability, but it still maintains a circular interface. Traditional high-performance fiber materials with this structure can no longer meet the stringent requirements of high-end industrial fields in terms of strength, wear resistance, and thermal stability. Summary of the Invention

[0004] In view of this, this application provides a method for preparing high-performance core-sheath composite industrial yarn, which not only enables the composite of multiple fibers, but also endows the composite industrial yarn with a core-sheath structure. This core-sheath structure has excellent interfacial bonding force, thereby giving the finished composite industrial yarn higher strength.

[0005] Specifically, this application is implemented through the following scheme:

[0006] A method for preparing a high-performance core-sheath composite industrial filament, using a functional polymer material as the sheath material and a high-strength material as the core material, wherein the sheath material and the core material are treated by the following steps:

[0007] Step 1: After the skin material and core material are pre-crystallized, they are dried until the water content is ≤100ppm;

[0008] Step two: The skin layer material and the core layer material are fed into a screw extruder for melt extrusion.

[0009] The die pressure of the screw extruder corresponding to the skin material is 70–81 bar.

[0010] The core material corresponds to a die pressure of 80–84 bar in the screw extruder;

[0011] Step 3: The melt corresponding to the skin material and the melt corresponding to the core material are respectively introduced into the inner and outer layers of the spinning nozzle through the composite spinning assembly. The spinneret of the composite spinning assembly is a special-shaped spinneret. The spinning is drawn, cooled and solidified, stretched and heat-set, and wound to obtain the skin-core type composite industrial yarn.

[0012] This application employs a unique bicomponent core-sheath composite structure design. The sheath and core materials are composed of different polymers. The functional polymers emphasize functionality, such as abrasion resistance, UV resistance, and processability, while the high-strength materials utilize conventional polyester PET, prioritizing high strength, high modulus, and excellent thermal stability. This structural design not only achieves complementary advantages in material properties but also, combined with melt extrusion using shaped spinnerets and composite spinning, produces shaped core-sheath industrial yarns. This effectively increases the interfacial contact area between the sheath and core, enhancing the cohesion between the two components. Thus, while ensuring fiber strength, it endows the composite fiber with specific functionalities, such as abrasion resistance, flexibility, and compatibility with other materials.

[0013] Furthermore, as a preferred option:

[0014] The pre-crystallization temperature of the core material is 90–120°C, and the drying temperature is 110–140°C.

[0015] The parameters of each drafting roller in the spinning process are set as follows:

[0016] The first pair of rollers, GR1+2, has a roller speed of 400–600 m / min.

[0017] The second pair of rollers, GR3+4, has a roller speed of 420–620 m / min and a roller temperature of 80–100 °C.

[0018] The third pair of rollers, GR5+6, has a roller speed of 1800–2000 m / min and a roller temperature of 90–110℃.

[0019] The fourth pair of rollers, GR7+8, has a roller speed of 2700–2900 m / min and a roller temperature of 120–240℃.

[0020] The fifth pair of rollers, GR9+10, has a roller speed of 2650–2850 m / min and a roller temperature of 140–160 °C.

[0021] The draw ratio, which is the ratio of the highest roll speed to the lowest roll speed, is 4.5 to 7.5.

[0022] To ensure the performance of the core-sheath composite industrial filament fiber, the parameters of each drafting roller in the spinning and stretching process are as follows: the roller speed of GR1+2 is 420–560 m / min (preferably 460–480 m / min), and the draft ratio is 5.5–6.5 times; that is, the roller speed of GR7+8 is 2750–2900 m / min. The roller temperature of GR7+8 is 230–240℃.

[0023] The cooling process employs side-blowing cooling for curing and molding, with the side-blowing wind speed set to 0.5–2.0 m / s and the temperature set to 20–40°C.

[0024] The composite spinning assembly includes a main chamber and a secondary chamber. The heat transfer systems of the main chamber and the secondary chamber are independent of each other and are separated by an insulation board. The melt corresponding to the skin material and the melt corresponding to the core material are introduced into the inner and outer layers of the spinning nozzle through the main chamber and the secondary chamber, respectively. The composite spinning chamber adopts the composite chamber structure composed of the main chamber and the secondary chamber. The two chambers are insulated and supplied with samples using independent heat transfer systems at different temperatures, and are separated by an insulation board to reduce heat transfer between the main chamber and the secondary chamber, thereby ensuring the uniformity of the two melt components.

[0025] To achieve a good interface bonding between the core and sheath structure and improve fiber performance, a core-sheath spinneret assembly with a special cross-section is selected. The cross-section of the composite spinning assembly is serrated or cross-shaped. In this way, the two components of melt reach the spinning assembly through the main and auxiliary spinning boxes, and under the action of the specially constructed spinneret assembly, a core-sheath composite fiber with a special interface is formed.

[0026] The above scheme does not require a fixed combination of skin and core materials; they can be freely combined to obtain composite industrial yarns with different properties. Some preferred options are as follows:

[0027] The skin material is any one of PA6, PA66, LMPET, CDP, and ECDP, and the temperature of the screw extruder corresponding to the skin material is set to 240-300℃.

[0028] The core material is conventional polyester, and the temperature of the screw extruder corresponding to the core material is set to 275~305℃.

[0029] The mass ratio of the outer layer material to the core layer material is 1-3:9-7.

[0030] By varying and coordinating the specific composition and ratio of the aforementioned skin and core materials, the finished composite industrial yarn is endowed with different functional characteristics.

[0031] More preferably, in the above scheme, when polyester is the core material, the pre-crystallization temperature, drying temperature, and melt extrusion conditions are different depending on the skin material:

[0032] When PA66 is used as the skin material, the corresponding pre-crystallization temperature is 70-90℃, the drying temperature is 90-110℃, the screw extruder five-zone temperature is set to 270-280℃, 285-290℃, 288-295℃, 288-295℃, 295-300℃, and the die pressure is 70-76 bar.

[0033] When PA6 is used as the skin material, the corresponding pre-crystallization temperature is 60-80℃, the drying temperature is 80-100℃, the screw extruder five-zone temperature is set to 240-252℃, 255-265℃, 258-264℃, 260-268℃, and 269-273℃, and the die pressure is 75-81 bar.

[0034] When LMPET is used as the skin material, the corresponding pre-crystallization temperature is 70-90℃, the drying temperature is 90-110℃, the screw extruder five-zone temperature is set to 248-252℃, 259-264℃, 265-270℃, 296-270℃, and 268-272℃, and the die pressure is 75-78 bar.

[0035] In the above scheme, after drying, the moisture content of the sheath and core materials is controlled below 100 ppm to minimize hydrolysis reactions that may occur during spinning, ensuring the spinnability of the composite fiber and the quality of the finished yarn. The sheath and core materials are separately fed into a screw extruder for melt extrusion. The melting temperature and die pressure of each component are controlled to ensure that the two components have similar melt viscosity and flow properties during subsequent spinning, resulting in good bonding and optimized finished yarn quality. The temperature of the spinning assembly is well matched to the thermal properties, melt viscosity, and shear viscosity of the sheath and core materials, ensuring minimal difference in melt viscosity and uniform flowability between the two components. The composite fiber flowing from the spinning assembly is rapidly cooled and solidified by a side-blowing device to maintain the stability of its sheath-core structure. The cooled composite fiber is further stretched and heat-set to improve its strength and orientation. Finally, the stretched and set sheath-core composite fiber is wound and packaged.

[0036] The implementation of this invention will bring significant economic and social benefits. On the one hand, the widespread application of high-performance core-sheath composite industrial filament fibers will promote the development and upgrading of related industries, and improve the added value and market competitiveness of products. On the other hand, efficient production processes and reasonable raw material combinations will further enrich the differentiated varieties of industrial filament fibers, broaden their application scenarios, and increase their market share.

[0037] With its superior performance and environmentally friendly characteristics, the high-performance core-sheath composite industrial filament fiber of this invention shows broad application prospects in multiple fields such as textiles, automobiles, medical, and aerospace. In the textile industry, it can be used to produce high-performance clothing fabrics and industrial textiles; in the automotive industry, it can be used for airbags and tire cords; in the medical field, it can be used to manufacture surgical sutures, etc. Furthermore, its excellent comprehensive performance also gives the core-sheath composite industrial filament fiber potential application value in the electronics, electrical, and construction fields.

[0038] In summary, the high-performance core-sheath composite industrial filament fiber of this invention has achieved significant breakthroughs and innovations in structural design, interface strengthening, performance improvement, and environmental protection requirements, injecting new vitality into the development of the textile and composite materials industry. Attached Figure Description

[0039] To more clearly illustrate the technical solutions in the embodiments of this application, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0040] Figure 1 This is a schematic diagram of the spinning apparatus in this application;

[0041] Figure 2 This is a schematic diagram of the first cross-sectional structure of the spinneret corresponding to the core layer in this application;

[0042] Figure 3 This is a schematic diagram of a second cross-sectional structure of the spinneret corresponding to the core layer in this application.

[0043] Numbering in the diagram: 1. Main screw extruder (core layer); 2. Auxiliary screw extruder (skin layer); 3. Core layer material melt pipe; 4. Skin layer material melt pipe; 5. Main insulation box; 6. Auxiliary insulation box; 7. Insulation board; 8. Spinning assembly; 9. Nascent fiber; 10. Side blowing device; 11. First roll GR1; 12. Second roll GR2; 13. Third roll GR3; 14. Fourth roll GR4; 15. Fifth roll GR5; 16. Sixth roll GR6; 17. Seventh roll GR7; 18. Eighth roll GR8; 19. Ninth roll GR9; 20. Tenth roll GR10; 21. Winding device; 22. Skin layer material area; 23. Core layer material area. Detailed Implementation

[0044] To make the technical problems, technical solutions, and beneficial effects to be solved by this application clearer, the technical solutions in the embodiments of this application will be further described in detail below with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are only used to explain this application and are not intended to limit the technical solutions of this application. All other embodiments obtained by those skilled in the art based on the embodiments in this application without creative effort are within the scope of protection of this application.

[0045] It should be noted that when a component is referred to as "fixed to" or "set on" another component, it can be located directly or indirectly on that other component. When a component is referred to as "connected to" another component, it can be directly or indirectly connected to that other component. The terms "upper," "lower," "left," "right," "front," "rear," "vertical," "horizontal," "top," "bottom," "inner," and "outer," etc., indicate the orientation or position based on the orientation or position shown in the accompanying drawings, and are only for ease of description and should not be construed as limiting the present technical solution.

[0046] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or specifying the number of technical features. "A plurality of" means two or more, unless otherwise explicitly defined.

[0047] Example 1

[0048] The preparation method of high-performance core-sheath composite industrial yarn in this embodiment uses PA66 as the sheath material and conventional polyester PET as the core material. The raw material mass ratio of PA66 to PET is set to 3:7. The raw materials are pre-crystallized and dried, melt extruded, blended and spun, cooled and oiled, drawn and shaped, and wound to obtain the finished yarn.

[0049] The specific process is as follows:

[0050] Step 1: Pre-crystallize and dry the PA66 and PET chips;

[0051] The pre-crystallization temperature for PA66 chips was set at 80℃, and the drying temperature at 100℃; the pre-crystallization temperature for PET chips was set at 115℃, and the drying temperature at 130℃, with the vacuum level maintained below 100Pa. The pre-crystallization time was set at 2.5 hours, and the drying time at 20 hours. The moisture content of the dried PA66 chips and PET chips was 70 ppm and 50 ppm, respectively.

[0052] The physical properties of PA66 chips and PET chips are shown in Table 1.

[0053] Table 1: Physical properties of PA66 and PET

[0054] project PA66 project PET relative viscosity 3.12 Intrinsic viscosity (dl / g) 1.013 Terminal carboxyl group (mol / t) 11.4 Melting point (°C) 260.2 Diethylene glycol (%) 1.04 L value 88.7 b value 4.6 .

[0055] Step Two: As Figure 1 As shown in Table 2, the dried PET chips and PA66 chips are fed into the main screw extruder 1 and the auxiliary screw extruder 2 for melt extrusion, respectively. The screw parameters for each zone of the PET chips and PA66 chips are set as shown in Table 2.

[0056] Table 2: Parameters of each zone of the screw extruder

[0057] Screw Zones PET (core layer) PA66 (cortical) Zone 1 (°C) 280 275 Zone 2 (°C) 292 287 Three zones (°C) 295 293 Four zones (°C) 295 293 Die head (°C) 300 298 Head pressure (bar) 84 76 .

[0058] Step 3: As Figure 1 As shown, the core material PET and the outer layer material PA66 are extruded by a screw and flow into the spinning assembly 8 through melt pipes 3 and 4, respectively. The spinning assembly includes a filter element and a spinneret. During its flow, the melt passes through the main insulation box 5 and the secondary insulation box 6. An insulation plate 7 is installed between the main insulation box and the secondary insulation box to reduce heat transfer between the two boxes.

[0059] The spinneret corresponding to the core layer structure can be adopted Figure 2 The serrated structure shown in the diagram forms a core-sheath composite fiber in which the cross-section of the inner core layer is set to an irregular shape. This allows the inner core layer structure to better support the first fiber, i.e., the sheath structure, and increases the interfacial cohesion between the sheath structure and the core layer structure, thereby enhancing the overall performance of the composite fiber.

[0060] Step 4: After the nascent fibers are ejected from the spinneret of the spinning assembly 8, they are solidified and shaped using side-blowing cooling. The side-blowing wind speed is set to 1.5m / s and the temperature is set to 30℃.

[0061] Step 5: After cooling, the filament bundle undergoes oiling, stretching, setting, and winding. Since the outer layer is PA66 fiber, a nylon-specific oiling agent is selected, and an oiling nozzle is used for oiling.

[0062] The parameter settings for each drafting roller in the spinning process are shown in Table 3.

[0063] Table 3: Process parameters of spinning drawing rollers

[0064] Roller Name Rotational speed (m / min) Temperature (°C) GR1+2 480 / GR3+4 500 90 GR5+6 1900 100 GR7+8 2800 240 GR9+10 2750 150 .

[0065] The PA66 / PET core-sheath composite industrial yarn obtained in this embodiment not only has advantages such as high modulus and high strength, but also has the high wear resistance and heat resistance of PA66 material, and can be applied to high-end clothing, carpets, airbags, tire cords and other fields.

[0066] Example 1-1

[0067] This embodiment has the same setup as Embodiment 1, except that the raw material mass ratio of the sheath material PA66 and the core material PET is replaced with 2:8, 1:9, 4:6, and 5:5, respectively. Different ratios can achieve relatively good cohesive properties, but the composite industrial yarns with different ratios show slight differences in mechanical strength and other aspects. Therefore, the solution in this application can achieve composite industrial yarns with different properties by changing the ratio of the sheath and core materials.

[0068] Examples 1-2

[0069] This embodiment has the same setup as Embodiment 1, except that the spinneret uses a conventional circular cross-section. Compared to the product of Embodiment 1, the cohesive properties of the product obtained in this embodiment are relatively poor. It is evident that the serrated spinneret used in Embodiment 1 can significantly increase the contact area at the core-skin interface, and compared to a spinneret with a conventional circular cross-section, Embodiment 1 more easily achieves higher strength.

[0070] Example 2

[0071] This embodiment provides a method for preparing high-performance core-sheath composite industrial filament fibers. Unlike Embodiment 1, this embodiment uses PA6 as the sheath material and conventional polyester PET as the core material. The raw material mass ratio of PA6 to PET is 3:7. The raw materials undergo pre-crystallization drying, melt extrusion, blending spinning, cooling and oiling, drawing and setting, and winding to obtain the finished filament. The specific process is as follows:

[0072] Step 1: Pre-crystallize and dry the PA6 and PET slices;

[0073] The pre-crystallization temperature for PA6 chips was set at 65℃, and the drying temperature at 90℃; the pre-crystallization temperature for PET chips was set at 115℃, and the drying temperature at 130℃, with the vacuum level maintained below 100Pa. The pre-crystallization time was set at 2.5 hours, and the drying time at 24 hours. The moisture content of the dried PA6 chips and PET chips was 50 ppm and 50 ppm, respectively.

[0074] The physical properties of the PA6 and PET slices used are shown in Table 4.

[0075] Table 4: Physical Properties of PA6 and PET

[0076] project PA6 project PET relative viscosity 3.45 Intrinsic viscosity (dl / g) 1.013 Terminal carboxyl group (mol / t) 11.4 Melting point (°C) 260.2 Diethylene glycol (%) 1.04 L value 88.7 b value 4.6 .

[0077] Step Two: As Figure 1 As shown in Table 5, the dried PET chips and PA6 chips are fed into the main screw extruder 1 and the auxiliary screw extruder 2 for melt extrusion, respectively. The screw parameters for each zone of the PET chips and PA6 chips are set as shown in Table 5.

[0078] Table 5: Parameters of each zone of the screw extruder

[0079]

[0080]

[0081] Step 3: As Figure 1 As shown, the core material PET and the outer layer material PA6 are extruded by a screw and flow into the spinning assembly 8 through melt pipes 3 and 4, respectively. The spinning assembly includes a filter element and a spinneret. During its flow, the melt passes through the main insulation box 5 and the secondary insulation box 6. An insulation plate 7 is installed between the main insulation box and the secondary insulation box to reduce heat transfer between the two boxes.

[0082] The spinneret corresponding to the core layer structure uses Figure 3 The cross-shaped structure is shown. The spinneret is selected with a special cross-section. In the resulting core-sheath composite fiber, the cross-section of the inner core structure is set to an irregular shape, so that the inner core structure can better support the first fiber, i.e., the sheath structure, and increase the interfacial cohesion between the sheath structure and the core structure, thereby enhancing the overall performance of the composite fiber.

[0083] Step 4: After the nascent fibers are ejected from the spinneret of the spinning assembly 8, they are cooled and solidified by side blowing air. The side blowing air speed is set to 2.0 m / s and the temperature is set to 20℃.

[0084] Step 5: After cooling, the filament bundle undergoes oiling, stretching, setting, and winding. Since the outer layer is PA6 fiber, a nylon-specific oiling agent is selected, and an oiling nozzle is used for oiling.

[0085] The parameter settings for each drafting roller in the spinning process are shown in Table 6.

[0086] Table 3: Process parameters of spinning drawing rollers

[0087] Roller Name Rotational speed (m / min) Temperature (°C) GR1+2 460 / GR3+4 480 85 GR5+6 1870 95 GR7+8 2750 230 GR9+10 2700 145 .

[0088] The PA6 / PET core-sheath composite industrial yarn obtained in this embodiment not only has advantages such as high modulus and high strength, but also has the high impact resistance, high wear resistance and good surface quality of PA6 material, and can be applied to various high-end fabrics, pipe skeletons, ropes and conveyor belts.

[0089] Example 3

[0090] This embodiment provides a method for preparing high-performance core-sheath composite industrial filament fibers. Unlike Embodiment 1, this embodiment uses low-melting-point polyester (LMPET) as the sheath material and conventional polyester PET as the core material. The raw material mass ratio of LMPET to PET is 3:7. The raw materials undergo pre-crystallization drying, melt extrusion, blending spinning, cooling and oiling, drawing and setting, and winding to obtain the finished filament. The specific process is as follows:

[0091] Step 1: Pre-crystallize and dry the LMPET chips and PET chips;

[0092] The pre-crystallization temperature for LMPET chips was set at 85℃, and the drying temperature at 105℃; the pre-crystallization temperature for PET chips was set at 110℃, and the drying temperature at 120℃, with the vacuum level maintained below 100Pa. The pre-crystallization time was set at 2 hours, and the drying time at 18 hours. The moisture content of the dried LMPET chips and PET chips was 50 ppm and 40 ppm, respectively.

[0093] The physical properties of the LMPET chips and PET chips used are shown in Table 7.

[0094] Table 7: Physical Properties of LMPET and PET

[0095] project PET LMPET Intrinsic viscosity (dL / g) 1.013 1.018 Terminal carboxyl group (mol / t) 11.4 14.4 Melting point (°C) 260.2 223.6 Diethylene glycol (%) 1.04 1.32 L value 88.7 74.6 b value 4.6 3.3 .

[0096] Step Two: As Figure 1 As shown in Table 8, the dried PET chips and PA6 chips are fed into the main screw extruder 1 and the auxiliary screw extruder 2 for melt extrusion, respectively. The screw parameters for each zone of the PET chips and LMPET chips are set as shown in Table 8.

[0097] Table 8: Parameters of each zone of the screw extruder

[0098] Screw Zones PET (core layer) LMPET (dermal layer) Zone 1 (°C) 280 250 Zone 2 (°C) 292 262 Three zones (°C) 295 265 Four zones (°C) 295 265 Die head (°C) 300 270 Head pressure (bar) 84 78

[0099] Step 3: As Figure 1 As shown, the core material PET and the sheath material LMPET are extruded by a screw and flow into the spinning assembly 8 through melt pipes 3 and 4, respectively. The spinning assembly includes a filter element and a spinneret. During its flow, the melt passes through the main insulation box 5 and the secondary insulation box 6. An insulation plate 7 is installed between the main insulation box and the secondary insulation box to reduce heat transfer between the two boxes.

[0100] The spinneret corresponding to the core layer structure can be adopted Figure 2 The serrated structure shown can also be adopted Figure 3 The cross-shaped structure shown is an integral part of the core-sheath composite fiber structure. The core layer structure has an irregular cross-section, allowing it to better support the first fiber (the sheath structure) and increase the interfacial cohesion between the sheath and core layers, thus enhancing the overall performance of the composite fiber.

[0101] Step 4: After the nascent fibers are ejected from the spinneret of the spinning assembly 8, they are solidified and shaped using side-blowing cooling. The side-blowing wind speed is set to 1.0 m / s and the temperature is set to 40℃.

[0102] Step 5: After cooling, the filament bundle undergoes oiling, stretching, shaping, and winding.

[0103] The parameter settings for each drafting roller in the spinning process are shown in Table 9.

[0104] Table 9: Process parameters of spinning drawing rollers

[0105]

[0106]

[0107] The LMPET / PET core-sheath composite industrial yarn obtained in this embodiment not only has advantages such as high modulus and high strength, but also has excellent melt flowability, crystallinity, dyeability and spinnability. It can be applied to high-end apparel textiles and industrial textiles, nonwovens, automotive industry, construction industry and coating industry.

[0108] The above-described embodiments are merely illustrative of several feasible implementations of the present invention, and their descriptions are relatively specific and detailed. However, they should not be construed as limiting the scope of the present invention, nor are the embodiments intended to limit the scope of protection in the claims of the present invention. For those skilled in the art, various modifications and improvements can be made without departing from the concept of the present invention. All equivalent implementations or changes that do not depart from the present invention should be included in the technology of the present invention.

Claims

1. A method for preparing a high-performance core-sheath composite industrial filament, characterized in that: Using any one of PA6, PA66, LMPET, CDP, or ECDP as the skin layer material and conventional high-viscosity polyester PET as the core layer material, the mass ratio of skin layer material to core layer material is 1-3:9-7. The skin layer material and core layer material are then treated as follows: Step 1: After the skin material and core material are pre-crystallized, they are dried until the moisture content is ≤100ppm; Step two: The skin layer material and the core layer material are fed into a screw extruder for melt extrusion. The temperature settings for the screw extruder corresponding to the skin material are: 240–300℃, and the die pressure is 70–81 bar. The core layer material is set to a screw extruder temperature of 275–305℃ and a die pressure of 80–84 bar. Step 3: The melt corresponding to the skin material and the melt corresponding to the core material are respectively introduced into the inner and outer layers of the spinning nozzle through the composite spinning assembly. The spinneret of the composite spinning assembly is a shaped spinneret. After spinning, drawing, cooling and solidification, stretching and heat setting, and winding, a skin-core composite industrial yarn is obtained. The cross-section of the irregular spinneret is serrated or cross-shaped; The parameters of each drafting roller in the spinning process are set as follows: The first pair of rollers, GR1+2, has a roller speed of 420~560m / min. The second pair of rollers, GR3+4, has a roller speed of 420–620 m / min and a roller temperature of 80–100 °C. The third pair of rollers, GR5+6, has a roller speed of 1800–2000 m / min and a roller temperature of 90–110℃. The fourth pair of rollers, GR7+8, has a roller speed of 2700–2900 m / min and a roller temperature of 230–240℃. The fifth pair of rollers, GR9+10, has a roller speed of 2650–2850 m / min and a roller temperature of 140–160 °C. The draw ratio is 5.5 to 6.5 times.

2. The method for preparing a high-performance core-sheath composite industrial filament according to claim 1, characterized in that: The pre-crystallization temperature of the core layer material is 90–120°C, and the drying temperature is 110–140°C.

3. The method for preparing a high-performance core-sheath composite industrial filament according to claim 1, characterized in that: The cooling process employs side-blowing cooling for curing and molding, with the side-blowing wind speed set to 0.5–2.0 m / s and the temperature set to 20–40°C.

4. The method for preparing a high-performance core-sheath composite industrial filament according to claim 1, characterized in that: The composite spinning assembly includes a main housing and a secondary housing. The heat transfer systems of the main housing and the secondary housing are independent of each other and are separated by an insulation board. The melt corresponding to the outer layer material and the melt corresponding to the core layer material are respectively introduced into the inner and outer layers of the spinning nozzle through the main housing and the secondary housing.

Citation Information

Patent Citations

  • Preparation method of skin-core composite stock solution colored chinlon 6

    CN117626473A

  • Spinneret plate for producing high-performance sheath-core type double-component fibers

    CN219260293U

  • Melt spinning of multi-component multifilaments, has separate heating systems to maintain the melting temperature of each individual polymer until they are mixed at the spinneret

    DE10143070A1