Preparation method of carbon fiber anti-bending anti-electromagnetic interference copper clad plate
By introducing carbon fiber pre-oxidized fibers and powder into carbon fiber copper clad laminates and combining them with a hot-pressing process, copper clad laminates with excellent bending resistance and electromagnetic interference resistance are prepared, solving the problem of insufficient electromagnetic interference resistance in existing technologies and achieving a highly efficient electromagnetic shielding effect.
Patent Information
- Application Number
- CN202411612583.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-13
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-11-13
AI Technical Summary
While existing carbon fiber copper-clad laminates improve bending and impact resistance, they fail to fully realize their potential in electromagnetic interference resistance.
Carbon fiber pre-oxidized filaments were used as the fiber skeleton, and carbon fiber powder was filled into the gaps between them. The composite film and copper foil were then hot-pressed together to prepare carbon fiber copper-clad laminate that is resistant to bending and electromagnetic interference.
It improves the bending resistance of copper-clad laminates and has excellent electromagnetic shielding capabilities. The process is simple and easy to implement, making it suitable for large-scale production.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of copper clad laminate technology, and in particular to a method for preparing a carbon fiber clad laminate that is resistant to bending and electromagnetic interference. Background Technology
[0002] Copper-clad laminates (CCLs) are a fundamental material in the electronics industry, primarily used in the manufacturing of printed circuit boards (PCBs), widely employed in electronic products such as televisions, radios, computers, and mobile communications. With technological advancements, PCBs must possess various high-quality, high-tech characteristics, directly incorporating numerous contemporary high-tech advancements in PCB manufacturing. Consequently, the comprehensive performance requirements for CCLs are becoming increasingly stringent. In the trend towards lightweight and miniaturized equipment, the compactness of internal electronic components is increasing, leading to more pronounced interference between different devices. As a core component, electromagnetic interference resistance is a crucial characteristic of CCLs.
[0003] Carbon fiber, as a special fiber, occupies a significant proportion in the preparation of high-performance composite materials. With a carbon content exceeding 90%, carbon fiber possesses excellent electromagnetic shielding capabilities and extremely high bending strength. Given the thinness of copper-clad laminates (CCLs) and their placement within electronic devices, superior bending resistance and electromagnetic shielding are crucial for their high-end applications. Chinese patent CN 114714711 A discloses a high-wear-resistant and corrosion-resistant epoxy resin CCL and its preparation method. Modified carbon fiber is added to the transition layer between the insulating layer and the copper foil. The modified carbon fiber has increased surface roughness, which improves the bonding force between the carbon fiber and other components and imparts impact resistance to the CCL. In this patent, the carbon fiber distribution is uniformly disordered, contributing little to the increased impact resistance but little to the bending resistance. Chinese patent CN 10314437 A discloses a composite material using unidirectional carbon fiber prepreg fabric and a copper-clad laminate using this composite material. The prepreg fabric is prepared using unidirectionally woven carbon fiber, and then this fabric is used as a functional layer to prepare the copper-clad laminate. The unidirectionally woven carbon fiber prepreg fabric has high bending resistance, thereby increasing the bending resistance of the copper-clad laminate. However, both of these patents only utilize the high strength and high modulus of carbon fiber to increase the bending and impact resistance of the copper-clad laminate, and neither addresses the electromagnetic interference resistance of the copper-clad laminate. Summary of the Invention
[0004] Existing carbon fiber copper-clad laminates only utilize the high strength and high modulus of carbon fiber to increase the bending resistance and impact resistance of the laminate, failing to fully leverage the role of carbon fiber in the laminate. To address this issue, this invention provides a method for preparing a carbon fiber bending-resistant and electromagnetic interference-resistant copper-clad laminate, comprising the following steps: 1) Preparation of carbon fiber-epoxy resin emulsion The carbon fiber short fibers are acid-washed to remove surface grease, washed with water and dried, then ball-milled into powder. After sieving, the carbon fiber powder is placed in an epoxy resin emulsion and stirred evenly for later use. 2) Preparation of carbon fiber-pre-oxidized carbon fiber composite films A polyimide film of a certain size is laid flat on a polytetrafluoroethylene plate. The two ends of the carbon fiber pre-oxidized filament bundle are fixed so that the filament bundle is evenly laid on the polyimide film. A curing agent is added to the epoxy resin emulsion obtained in step 1), and after stirring evenly, it is loaded into a spraying machine and sprayed onto the carbon fiber pre-oxidized filament bundle at a uniform speed. Then, a hot roller is used to roll back and forth. After curing and molding, the polyimide film is removed from the polytetrafluoroethylene plate and the edges are trimmed to obtain a carbon fiber-pre-oxidized carbon fiber composite film. 3) Preparation of copper-clad laminate One side of the composite film polyimide obtained in step 2) is hot-pressed with copper foil to obtain a carbon fiber anti-bending and anti-electromagnetic interference copper-clad laminate.
[0005] Further, in step 1), the sieve fineness is 300~500 mesh; the epoxy resin emulsion is 60~100 parts by weight, the carbon fiber powder is 5~20 parts by weight, and it also contains the following substances in parts by weight: coupling agent 2~5 parts, dispersant 1~2 parts, and defoamer 0.5~1 parts.
[0006] Furthermore, in step 2), the carbon fiber pre-oxidized filament has a specification of 10~25D and a laying thickness of 5~15 fiber diameters; the curing agent is ethylenediamine or polyamide curing agent.
[0007] Furthermore, in step 3), the hot pressing temperature is 280~320℃ and the hot pressing pressure is 5~15MPa.
[0008] This invention relates to a carbon fiber-reinforced copper-clad laminate (CCL) with bending resistance and electromagnetic interference suppression. The pre-oxidized carbon fiber filaments serve as the fiber skeleton, as they are non-conductive. This enhances the bending resistance of the CCL without compromising its functionality by making it conductive. The carbon fiber powder filling the gaps in the pre-oxidized filaments provides electromagnetic shielding. Furthermore, a polyimide film separates the copper foil from the carbon fiber powder, resulting in excellent bending resistance and electromagnetic interference suppression. Moreover, the fabrication process of this invention involves only the hot pressing of the composite film and copper foil, making the process simple, easy to implement, and suitable for large-scale production. Detailed Implementation
[0009] The present invention will be described below with reference to examples. These examples are only used to explain the present invention and are not intended to limit the scope of the present invention.
[0010] Example 1 A method for preparing a carbon fiber resistant, bend-resistant, and electromagnetic interference-resistant copper-clad laminate includes the following steps: 1) Preparation of carbon fiber-epoxy resin emulsion Stir the short carbon fiber in dilute hydrochloric acid at 40℃ for 30 minutes to remove the grease on the surface of the carbon fiber. After washing and drying, the carbon fiber is ball-milled into powder. The powder is sieved to obtain 500 mesh powder. Weigh out 20 parts of carbon fiber powder, 100 parts of epoxy resin emulsion, 3 parts of KH550 coupling agent, 1.5 parts of RD-9001 dispersant and 1 part of Dow 103 polyether defoamer by weight, mix them and stir evenly for later use. 2) Preparation of carbon fiber-pre-oxidized carbon fiber composite films A polyimide film of a certain size is laid flat on a polytetrafluoroethylene plate by electrostatic adsorption. The two ends of the carbon fiber pre-oxidized filament bundle are fixed so that the filament bundle is evenly laid on the polyimide film. The carbon fiber pre-oxidized filament is 10D and the laying thickness is 15 fiber diameters. Ethylenediamine curing agent is added to the epoxy resin emulsion obtained in step 1), and after stirring evenly, it is loaded into a spraying machine and sprayed evenly on the carbon fiber pre-oxidized filament bundle. Then, it is rolled back and forth 3 times with a hot roller at 50°C. After curing and molding, the polyimide film is removed from the polytetrafluoroethylene plate and the edges are trimmed to obtain a carbon fiber-pre-oxidized carbon fiber composite film. 3) Preparation of copper-clad laminate One side of the composite film polyimide obtained in step 2) is hot-pressed with copper foil at a temperature of 310°C and a pressure of 10 MPa to obtain a carbon fiber anti-bending and anti-electromagnetic interference copper-clad laminate.
[0011] Example 2 A method for preparing a carbon fiber resistant, bend-resistant, and electromagnetic interference-resistant copper-clad laminate includes the following steps: 1) Preparation of carbon fiber-epoxy resin emulsion Stir the carbon fiber short fibers in dilute hydrochloric acid at 50℃ for 20 minutes to remove the grease on the surface of the carbon fiber. After washing and drying, the fibers are ball-milled into powder and sieved to obtain 400-mesh powder. Weigh out 15 parts of carbon fiber powder, 80 parts of epoxy resin emulsion, 2 parts of KH560 coupling agent, 1 part of magnesium stearate dispersant and 1 part of white oil by weight, mix them and stir evenly for later use. 2) Preparation of carbon fiber-pre-oxidized carbon fiber composite films A polyimide film of a certain size is laid flat on a polytetrafluoroethylene plate by water film adsorption. The two ends of the carbon fiber pre-oxidized filament bundle are fixed so that the filament bundle is evenly laid on the polyimide film. The carbon fiber pre-oxidized filament is 25D and the laying thickness is 5 fiber diameters. Polyamide curing agent 651 is added to the epoxy resin emulsion obtained in step 1), and after stirring evenly, it is loaded into a spraying machine and sprayed evenly on the carbon fiber pre-oxidized filament bundle. Then, it is rolled back and forth 5 times with a hot roller at 40°C. After curing and molding, the polyimide film is removed from the polytetrafluoroethylene plate and the edges are trimmed to obtain a carbon fiber-pre-oxidized carbon fiber composite film. 3) Preparation of copper-clad laminate One side of the composite film polyimide obtained in step 2) is hot-pressed with copper foil at a temperature of 280°C and a pressure of 15MPa to obtain a carbon fiber copper-clad laminate that is resistant to bending and electromagnetic interference.
[0012] Example 3 A method for preparing a carbon fiber resistant, bend-resistant, and electromagnetic interference-resistant copper-clad laminate includes the following steps: 1) Preparation of carbon fiber-epoxy resin emulsion Stir the short carbon fiber in dilute hydrochloric acid at 40℃ for 60 minutes to remove the grease on the surface of the carbon fiber. After washing and drying, the carbon fiber is ball-milled into powder. The powder is sieved to obtain 300 mesh powder. Weigh out 5 parts by weight of carbon fiber powder, 60 parts by weight of epoxy resin emulsion, 5 parts by weight of KH560 coupling agent, 2 parts by weight of RD-9001 dispersant and 0.5 parts by weight of Dow 103 polyether defoamer. Mix them and stir evenly for later use. 2) Preparation of carbon fiber-pre-oxidized carbon fiber composite films A polyimide film of a certain size is laid flat on a polytetrafluoroethylene plate by water film adsorption. The two ends of the carbon fiber pre-oxidized filament bundle are fixed so that the filament bundle is evenly laid on the polyimide film. The carbon fiber pre-oxidized filament is 20D and the laying thickness is 10 fiber diameters. Ethylenediamine curing agent is added to the epoxy resin emulsion obtained in step 1), and after stirring evenly, it is loaded into a spraying machine and sprayed evenly on the carbon fiber pre-oxidized filament bundle. Then, it is rolled back and forth 4 times with a hot roller at 50°C. After curing and molding, the polyimide film is removed from the polytetrafluoroethylene plate and the edges are trimmed to obtain a carbon fiber-pre-oxidized carbon fiber composite film. 3) Preparation of copper-clad laminate One side of the composite film polyimide obtained in step 2) is hot-pressed with copper foil at a temperature of 320°C and a pressure of 5 MPa to obtain a carbon fiber anti-bending and anti-electromagnetic interference copper-clad laminate.
[0013] Comparative Example 1 A method for preparing a pre-oxidized carbon fiber resistant copper-clad laminate includes the following steps: 1) Preparation of epoxy resin emulsion Weigh out 100 parts of epoxy resin emulsion, 3 parts of KH550 coupling agent, 1.5 parts of RD-9001 dispersant and 1 part of Dow 103 polyether defoamer by weight, mix them and stir evenly for later use. 2) Preparation of pre-oxidized carbon fiber composite films A polyimide film of a certain size is laid flat on a polytetrafluoroethylene plate by electrostatic adsorption. The two ends of the carbon fiber pre-oxidized filament bundle are fixed so that the filament bundle is evenly laid on the polyimide film. The carbon fiber pre-oxidized filament is 10D and the laying thickness is 15 fiber diameters. Ethylenediamine curing agent is added to the epoxy resin emulsion obtained in step 1), and after stirring evenly, it is loaded into a spraying machine and sprayed evenly on the carbon fiber pre-oxidized filament bundle. Then, it is rolled back and forth 3 times with a hot roller at 50°C. After curing and molding, the polyimide film is removed from the polytetrafluoroethylene plate and the edges are trimmed to obtain a pre-oxidized carbon fiber composite film. 3) Preparation of copper-clad laminate One side of the composite film polyimide obtained in step 2) is hot-pressed with copper foil at a temperature of 310°C and a pressure of 10 MPa to obtain a carbon fiber anti-bending and anti-electromagnetic interference copper-clad laminate.
[0014] Comparative Example 2 A method for preparing a carbon fiber anti-electromagnetic interference copper-clad laminate includes the following steps: 1) Preparation of carbon fiber-epoxy resin emulsion Stir the carbon fiber short fibers in dilute hydrochloric acid at 50℃ for 20 minutes to remove the grease on the surface of the carbon fiber. After washing and drying, the fibers are ball-milled into powder and sieved to obtain 400-mesh powder. Weigh out 15 parts of carbon fiber powder, 80 parts of epoxy resin emulsion, 2 parts of KH560 coupling agent, 1 part of magnesium stearate dispersant and 1 part of white oil by weight, mix them and stir evenly for later use. 2) Preparation of carbon fiber epoxy resin-polyimide thin composite film A polyimide film of a certain size is laid flat on a polytetrafluoroethylene plate by water film adsorption. Polyamide curing agent 651 is added to the epoxy resin emulsion obtained in step 1), and after stirring evenly, it is loaded into a spraying machine and sprayed onto the polyimide film at a uniform speed. Then, it is rolled back and forth 5 times with a hot roller at 40°C. After curing and forming, the polyimide film is removed from the polytetrafluoroethylene plate and the edges are trimmed to obtain a carbon fiber epoxy resin-polyimide thin composite film. 3) Preparation of copper-clad laminate One side of the composite film polyimide obtained in step 2) is hot-pressed with copper foil at a temperature of 280°C and a pressure of 15MPa to obtain a carbon fiber copper-clad laminate that is resistant to bending and electromagnetic interference.
[0015] Table 1 shows the performance test results of the copper-clad laminates obtained in Examples 1-3 and Comparative Examples 1-2. The data in the table show that the copper-clad laminates obtained in Examples 1-3 have excellent resistance to bending and electromagnetic interference. The copper-clad laminate in Comparative Example 1 did not contain carbon fiber powder, so its electromagnetic interference resistance was poor, but its mechanical properties were the best. The copper-clad laminate in Comparative Example 2 did not contain carbon fiber pre-oxidized fibers, so its physical properties of resistance to bending and impact were poor, but its electromagnetic interference resistance was good.
[0016] Table 1. Performance testing of copper-clad laminates obtained in Examples 1-3 and Comparative Examples 1-2 Note: The standard for testing bending strength is GB / T 9341-2000; the standard for testing dielectric constant Dk is GB / T 43801-2024; and the standard for testing impact strength is ASTM / D256-99.
[0017] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing a carbon fiber resistant, bend-resistant, and electromagnetic interference-resistant copper-clad laminate, characterized in that, Includes the following steps: 1) Preparation of carbon fiber-epoxy resin emulsion The carbon fiber short fibers are acid-washed to remove surface grease, washed with water and dried, then ball-milled into powder. After sieving, the carbon fiber powder is placed in an epoxy resin emulsion and stirred evenly for later use. 2) Preparation of carbon fiber-pre-oxidized carbon fiber composite films A polyimide film of a certain size is laid flat on a polytetrafluoroethylene plate. The two ends of the carbon fiber pre-oxidized filament bundle are fixed so that the filament bundle is evenly laid on the polyimide film. A curing agent is added to the epoxy resin emulsion obtained in step 1), and after stirring evenly, it is loaded into a spraying machine and sprayed onto the carbon fiber pre-oxidized filament bundle at a uniform speed. Then, a hot roller is used to roll back and forth. After curing and molding, the polyimide film is removed from the polytetrafluoroethylene plate and the edges are trimmed to obtain a carbon fiber-pre-oxidized carbon fiber composite film. 3) Preparation of copper-clad laminate One side of the composite film polyimide obtained in step 2) is hot-pressed with copper foil to obtain a carbon fiber anti-bending and anti-electromagnetic interference copper-clad laminate.
2. The preparation method according to claim 1, characterized in that, In step 1), the sieving fineness is 300~500 mesh.
3. The preparation method according to claim 1, characterized in that, In step 1), the epoxy resin emulsion is 60-100 parts by weight, the carbon fiber powder is 5-20 parts by weight, and it also contains the following substances in parts by weight: coupling agent 2-5 parts, dispersant 1-2 parts, and defoamer 0.5-1 parts.
4. The preparation method according to claim 1, characterized in that, In step 2), the carbon fiber pre-oxidized filament has a specification of 10~25D and a laying thickness of 5~15 fiber diameters.
5. The preparation method according to claim 1, characterized in that, In step 2), the curing agent is ethylenediamine or polyamide curing agent.
6. The preparation method according to claim 1, characterized in that, In step 3), the hot pressing temperature is 280~320℃ and the hot pressing pressure is 5~15MPa.
Citation Information
Patent Citations
Epoxy resin copper-clad plate with high wear resistance and corrosion resistance and preparation method thereof
CN114714711A
Preparation method and application of double-sided flexible copper-clad plate
CN116512699A