Light-transmitting photosensitive layered body, cured film, circuit board, and electronic device
By introducing a light-converting agent into the photosensitive laminate, the anti-Stokes phenomenon is used to absorb and convert long-wavelength light, solving the problem of low wavelength matching of photoinitiators, improving the speed and effect of photocuring, simplifying the preparation process, and making it suitable for photosensitive laminates, cured films, circuit boards and electronic devices.
Patent Information
- Application Number
- CN202411353734.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-09-26
AI Technical Summary
In existing technologies, the wavelength matching problem of photoinitiators leads to low utilization of longer wavelength light, affecting the speed and effect of photocuring. Furthermore, the combination of initiators with two or more layers has problems such as low utilization and complicated preparation process.
A photosensitive laminate containing a light-converting agent is used. The light-converting agent absorbs long-wavelength light and converts it into short-wavelength light. By utilizing the anti-Stokes phenomenon, the utilization rate of the light source is improved, and the photocuring speed and effect of the photosensitive layer are enhanced.
The use of light-converting agents expands the selectivity of photoinitiators, improves the speed and effect of photocuring, simplifies the preparation process, and is suitable for photosensitive laminates, cured films, circuit boards and electronic devices.
Smart Images

Figure BDA0005062991810000041 
Figure BDA0005062991810000051 
Figure BDA0005062991810000161
Abstract
Description
Technical Field
[0001] This invention relates to the field of photosensitive laminate technology, and more specifically, to a photosensitive laminate, a curing film, a circuit board, and electronic devices. Background Technology
[0002] Photoinitiators are key components of photocurable products, often playing a decisive role in the curing speed and effect. In photoresists, the curing speed and effect are reflected in the exposure time (affecting production efficiency) and the quality of properties such as resolution, steepness, deep curing ability, and resistance to metal oxides. When selecting a photoinitiator, the matching between its absorption spectrum and the emission spectrum of the light source must be considered. Currently, commonly used exposure machine light sources are high-pressure mercury lamps and LED lamps, with wavelengths generally ranging from 300-405 nm and peak values from 365-405 nm. However, the maximum absorption wavelength of commonly used photoinitiators is generally less than 390 nm, and some are less than 370 nm (maximum absorption wavelength refers to the maximum absorption value of a substance in a spectrum, usually used to measure the substance's ability to absorb light of a certain wavelength). Therefore, the utilization rate of light in the 370-405 nm band is relatively low.
[0003] To improve light utilization, a common practice is to use a mixture of photoinitiators with characteristic peaks at short and long wavelengths respectively (single-layer film CN112625149A). Further, bilayer or multilayer structures are prepared, with each layer using a different photoinitiator (CN116300315A). However, while mixing different initiators improves the utilization of longer wavelengths to some extent, most conventional photoinitiators only "absorb at longer wavelengths" rather than having "characteristic peaks at longer wavelengths," resulting in limited improvement in utilization. Using bilayer or multilayer structures with different initiators for each layer not only leads to lower initiator utilization but also complicates the preparation process, hindering industrial applications. Some researchers have tried to improve light utilization by adding light-converting agents to the photosensitive layer. However, these agents are mostly inorganic particles, which have poor dispersibility, potentially affecting resolution and flexibility. Furthermore, they may cause light to scatter throughout the film, leading to photocuring reactions in non-patterned areas, affecting pattern accuracy and hindering deep curing.
[0004] In view of this, the present invention is hereby proposed. Summary of the Invention
[0005] The main objective of this invention is to provide a photosensitive laminate, a cured film, a circuit board, and an electronic device to solve the problem that the utilization rate of longer wavelength light is still low when using photoinitiators of different wavelengths or using different initiators in different layers of a double or multi-layer structure.
[0006] To achieve the above objectives, according to one aspect of the present invention, a photosensitive laminate is provided, the photosensitive laminate comprising a support layer, a photosensitive layer and an optional protective layer stacked sequentially, and the photosensitive laminate containing a photoconverting agent having an absorption wavelength >390nm and an emission wavelength ≤390nm.
[0007] Furthermore, the support layer contains a light-converting agent. By mass, the material of the support layer includes 65-99 parts of a first resin, 0.1-15 parts of a light-converting agent, 0.9-30 parts of a first filler, 0.1-5 parts of a light-converting agent, 0.9-30 parts of a first filler, and 0.1-5 parts of a first additive.
[0008] Furthermore, the first resin is selected from at least one of polyethylene terephthalate, polyethylene naphthalate, polyethylene, and polypropylene.
[0009] Furthermore, the first filler is selected from at least one of calcium titanate, calcium carbonate, titanium dioxide, zinc oxide, antimony trioxide, silicon oxide, hollow glass microspheres, and barium sulfate.
[0010] Furthermore, the first auxiliary agent is selected from at least one of ultraviolet absorbers, hindered amine light stabilizers, antioxidants, heat stabilizers, catalysts, hydrolysis stabilizers, nucleating and penetrating agents, and toughening agents.
[0011] Furthermore, the photosensitive layer stack also includes a photosensitive layer, which is disposed between the support layer and the photosensitive layer or on the side of the support layer away from the photosensitive layer, and contains a photosensitive agent.
[0012] Further, by mass parts, the light conversion layer comprises 60-90 parts of a second resin, 0.1-50 parts of a light conversion agent, 0-30 parts of a second filler, 0.001-20 parts of a curing agent, and 0.001-1 parts of a second auxiliary agent.
[0013] Furthermore, the second resin is selected from at least one of acrylic resin, fluorocarbon resin, polyester resin, epoxy resin, polyurethane resin, and terpene resin.
[0014] Furthermore, the second filler is selected from at least one of calcium titanate, calcium carbonate, titanium dioxide, zinc oxide, antimony trioxide, silicon oxide, hollow glass spheres, and barium sulfate.
[0015] Furthermore, the curing agent is selected from at least one of hexamethylene diisocyanate trimer, hexamethylene diisocyanate prepolymer, isophorone diisocyanate trimer, isophorone diisocyanate prepolymer, hydrogenated styrene diisocyanate trimer, hydrogenated styrene diisocyanate prepolymer, methyl etherified polyhydroxymethyl melamine resin, butyl etherified polyhydroxymethyl melamine resin, mixed etherified polyhydroxymethyl melamine resin, polyamide, polymethylene diamine, diethylenetriamine, pentamethyldiethylenetriamine, triethylenetetramine, diethylenetriamine, triethylenetetramine, and (2,3-dimethyl)dibutyltriamine.
[0016] Furthermore, the second auxiliary agent is selected from at least one of ultraviolet absorbers, hindered amine light stabilizers, antioxidants, heat stabilizers, catalysts, hydrolysis stabilizers, nucleating and penetrating agents, and toughening agents.
[0017] Furthermore, the photosensitive layer includes a first photosensitive layer and a second photosensitive layer stacked sequentially, the first photosensitive layer being disposed between the support layer and the second photosensitive layer, and the first photosensitive layer containing a light-converting agent.
[0018] Further, by mass parts, the material of the first photosensitive layer includes 100 parts of alkali-soluble resin, 5 to 50 parts of photopolymerizable monomer, 0.1 to 10 parts of photoinitiator and 0.01 to 30 parts of light-converting agent; and / or, the material of the second photosensitive layer includes 100 parts of second alkali-soluble resin, 5 to 50 parts of second photopolymerizable monomer and 0.1 to 10 parts of second photoinitiator.
[0019] Furthermore, the photosensitive layer contains a light-converting agent, which is distributed in a gradient within the photosensitive layer, and the content of the light-converting agent gradually decreases along the thickness direction away from the support layer.
[0020] Furthermore, by mass fraction, the photosensitive layer comprises 100 parts of a third alkali-soluble resin, 5 to 50 parts of a third photopolymerizable monomer, 0.1 to 10 parts of a third photoinitiator, and 0.01 to 30 parts of a light-converting agent; the content of the light-converting agent decreases in a gradient along the thickness direction away from the support layer.
[0021] To achieve the above objectives, according to a second aspect of the present invention, a curing film is provided, which is formed by photocuring or photothermal dual curing of the photosensitive layer provided in the first aspect.
[0022] According to a third aspect of the present invention, a circuit board is provided, the circuit board comprising the cured film provided in the second aspect above.
[0023] According to a fourth aspect of the present invention, an electronic device is provided, the electronic device comprising the cured film provided in the second aspect or the circuit board provided in the third aspect.
[0024] By applying the technical solution of this application, the photosensitive laminate provided by this application contains a light-converting agent. This light-converting agent has an "upconversion function" and can induce an "anti-Stokes" phenomenon, absorbing long wavelengths and low energy, and releasing short wavelengths and high energy. Thus, when the photosensitive laminate is irradiated by the exposure machine, the longer wavelength light emitted by the exposure machine is absorbed by the light-converting agent and converted into shorter wavelength light that can be absorbed by the photoinitiator. This achieves high utilization of the light source while still using conventional photoinitiators, thereby expanding the selectivity of the photoinitiator and improving the photocuring speed and photocuring effect of the photosensitive layer. Detailed Implementation
[0025] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. The present invention will now be described in detail with reference to the embodiments.
[0026] As analyzed in the background section of this application, photoinitiators are key components of photocurable products. However, the maximum absorption wavelength of commonly used photoinitiators is generally less than 390 nm, and some are less than 370 nm (the molar extinction coefficient of a certain wavelength reflects the absorption intensity of the photoinitiator at that wavelength). Therefore, the utilization rate of light in the 370-405 nm wavelength range is relatively low. Existing technologies employ a mixture of photoinitiators of different wavelengths or use different initiators in different layers of a double-layer or multi-layer structure to improve the utilization rate of high-wavelength light, but the problem of low utilization rate of longer wavelength light still exists. To solve this problem, this application provides a photosensitive laminate, a curable film, a circuit board, and an electronic device.
[0027] In a first typical embodiment of this application, a photosensitive laminate is provided, which includes a support layer, a photosensitive layer and an optional protective layer stacked sequentially, and the photosensitive laminate contains a photoconverting agent with an absorption wavelength >390nm and an emission wavelength ≤390nm.
[0028] By applying the technical solution of this application, a light-converting agent is added to the photosensitive laminate provided by this application. The light-converting agent has an "upconversion function" and can induce an "anti-Stokes" phenomenon, absorbing long wavelengths and low energy, and releasing short wavelengths and high energy. Thus, when the exposure machine irradiates the light-converting photosensitive laminate, the longer wavelength light emitted by the exposure machine is absorbed by the light-converting agent and converted into shorter wavelength light that can be absorbed by the photoinitiator. This achieves high utilization of the light source while still using conventional photoinitiators, thereby expanding the selectivity of photoinitiators and improving the photocuring speed and photocuring effect of the photosensitive layer.
[0029] In this application, any light-converting substance that meets the requirements of absorption wavelength ≥390nm and emission wavelength ≤390nm can be used as the light-converting agent of this application.
[0030] [Light conversion agent]
[0031] Specifically, in this application, the aforementioned light-converting agent includes at least four categories. The first category of light-converting agent can be selected from at least one of NaLuF4, NaGdF4, NaYbF4, NaYF4, NaYGd, NaYLu, NaYNd, NaGd(WO4)2, LiErF4, BaYF5, BaLuF5, BaGdF5, BaYb2F8, CaS, LiLa(MoO4)2, Gd2O3, GdF3, ZrYO, YAIO, CaWO4, and light-converting materials composed of rare earth doped materials or derivatives of the aforementioned materials. The rare earth elements include at least one of Yb, Er, Tm, Eu, Sm, Bi, and Ho. Preferably, the light-converting agent is selected from at least one of NaGdF4, NaYF4, NaYGd, GdF3, and light-converting materials composed of rare earth doped materials or derivatives of the aforementioned materials.
[0032] The second type of light-converting agent may also be selected from at least one of 2,4,5,6-tetra(9-carbazolyl)-isophthalonitrile, triphenylamine derivatives, and light-converting materials composed of rare earth-doped materials or derivatives of the above materials, wherein the rare earth elements include at least one of Yb, Er, Tm, Eu, Sm, Bi, and Ho.
[0033] The third type of light-converting agent may also be selected from donor-acceptor complex light-converting agents, including a donor and an acceptor, wherein the donor is selected from at least one of the compounds shown in formulas (I) to (III), and the acceptor is selected from at least one of the compounds shown in formulas (IV) to (VI); when the donor is selected from the compound shown in formula (I), the acceptor is selected from at least one of the compounds shown in formulas (IV) to (VI); when the donor is selected from at least one of the compounds shown in formulas (II) to (III), the acceptor is selected from the compound shown in formula (VI).
[0034]
[0035]
[0036] The fourth type of light-converting agent can also be selected from metal halide perovskite light-converting agents. The metal halide perovskite light-converting agent is composed of alkaline earth metal cations, transition metal cations, and halogens, and the metal halide perovskite light-converting agent has a perovskite structure. Among them, the alkaline earth metal includes at least one of beryllium, magnesium, calcium, strontium, barium, and francium, and the transition metal includes at least one of scandium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper, and zinc. Preferably, the metal halide perovskite light-converting agent is CsPbX3; X is Cl, Br, or I. More preferably, the metal halide perovskite light-converting agent is formed by dispersing CsPbBr3 in Cs4PbBr6 crystals, and has a CsPbBr3 / Cs4PbBr6 doped structure.
[0037] The photosensitive laminate provided in this application contains a photosensitive agent. Specifically, the photosensitive laminate has at least the following four embodiments.
[0038] [First Implementation Method]
[0039] In this embodiment, the support layer of the photosensitive laminate contains a light-converting agent. When the exposure machine irradiates the support layer, the light-converting agent in the support layer absorbs the longer wavelength light emitted by the exposure machine and converts it into shorter wavelength light, which then irradiates the photosensitive layer, thereby improving the photocuring speed and photocuring effect of the photosensitive layer.
[0040] In some specific embodiments, the material of the support layer, by weight, includes 65-99 parts of a first resin, 0.1-15 parts of a light-converting agent, 0.9-30 parts of a first filler, and 0.1-5 parts of a first additive.
[0041] Typical, but not limiting, by weight, the amount of the first resin in the support layer material is 65 parts, 68 parts, 70 parts, 72 parts, 75 parts, 78 parts, 80 parts, 82 parts, 85 parts, 88 parts, 90 parts, 92 parts, 95 parts, 97 parts, 99 parts, or any range of two such values; the amount of the light-converting agent is 0.1 parts, 0.2 parts, 0.5 parts, 0.8 parts, 1 part, 2 parts, 5 parts, etc. The dosage of the first filler is 0.9 parts, 1 part, 2 parts, 5 parts, 8 parts, 10 parts, 15 parts, 20 parts, 25 parts, 30 parts, or any two of these values; the dosage of the first auxiliary agent is 0.1 parts, 0.2 parts, 0.5 parts, 0.8 parts, 1 part, 2 parts, 3 parts, 4 parts, 5 parts, or any two of these values.
[0042] The specific type of the first resin is not limited, including but not limited to any one or more of polyethylene terephthalate, polyethylene naphthalate, polyethylene, and polypropylene.
[0043] The first filler mentioned above is a commonly used filler in this field, including but not limited to any one or more of calcium titanate, calcium carbonate, titanium dioxide, zinc oxide, antimony trioxide, silicon oxide, hollow glass microspheres, and barium sulfate.
[0044] The specific type of the aforementioned first auxiliary agent is not limited, and includes, but is not limited to, any one or more of the following: ultraviolet absorbers, hindered amine light stabilizers, antioxidants, heat stabilizers, catalysts, hydrolysis stabilizers, nucleating and brightening agents, and toughening agents. In this embodiment, the specific composition of the photosensitive layer is not particularly limited; the photosensitive layer may or may not contain a light-converting agent. In some specific embodiments, by weight, the material of the photosensitive layer includes 100 parts of alkali-soluble resin, 5-50 parts of photopolymerizable monomer, and 0.01-10 parts of photoinitiator.
[0045] [Alkali-soluble resin]
[0046] The above-mentioned alkali-soluble resin is a commonly used alkali-soluble resin in the art, preferably with an acid value of 10-200 KOH / g and a weight-average molecular weight of 2000-150000.
[0047] Typical, but not limiting, acid values of alkali-soluble resins include 10 KOH / g, 20 KOH / g, 50 KOH / g, 80 KOH / g, 100 KOH / g, 150 KOH / g, 200 KOH / g, or any range of two such values; weight-average molecular weights include 2000, 5000, 8000, 10000, 20000, 50000, 80000, 100000, 120000, 150000, or any range of two such values.
[0048] In some embodiments, the alkali-soluble resin includes at least one of acrylate resins and / or alkali-soluble polyimide resins; wherein the monomers of the acrylate resins include, but are not limited to, itaconic acid, crotonic acid, acrylic acid, methacrylic acid, maleic acid half ester, maleic acid, fumaric acid, vinylacetic acid and its anhydrides, methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, isooctyl methacrylate, lauryl methacrylate, octadecyl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, and 4-hydroxyethyl methacrylate. At least one of the following: hydroxybutyl acrylate, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, (meth)acrylonitrile, (meth)acrylate glycidyl acrylate, N,N-dimethyl(meth)acrylate ethyl acrylate, N,N-diethyl(meth)acrylate ethyl acrylate, N,N-dimethyl(meth)acrylate propyl acrylate, N,N-diethyl(meth)acrylate propyl acrylate, N,N-dimethyl(meth)acrylate butyl acrylate, N,N-diethyl(meth)acrylate butyl acrylate, (meth)acrylamide, N-hydroxymethylacrylamide, N-butoxymethylacrylamide, styrene, (meth)acrylate benzyl acrylate, phenoxyethyl(meth)acrylate, and (alkoxylated)nonylphenol(meth)acrylate. Methyl methacrylate refers to methyl acrylate with or without methyl substitution, i.e., methyl acrylate or methyl methacrylate. Other similar expressions in this application, such as ethyl methacrylate and monofunctional (meth)acrylates, have the same meaning.
[0049] [Photopolymerizable monomers]
[0050] In this application, the photopolymerizable monomer can be a monomer containing an olefinic unsaturated group, or it can be selected from conventional photopolymerizable monomers, including but not limited to monofunctional (meth)acrylates, difunctional (meth)acrylates, trifunctional (meth)acrylates, or polyfunctional (meth)acrylates, specifically such as (ethoxy)phenol (meth)acrylate, stearate acrylate, ethoxy(propoxy)nonylphenol (meth)acrylate, ethoxy(propoxy)tetrahydrofurfuryl (meth)acrylate, etc. 1,6-Hexanediol diacrylate, tricyclodecanediethanol diacrylate, dioxanediol diacrylate, ethoxylated (propoxylated)bisphenol A di(meth)acrylate, polyethylene glycol (400) diacrylate, polypropylene glycol (600) diacrylate, ethoxylated (propoxylated)trimethylolpropane tri(meth)acrylate, pentaerythritol triacrylate, tri(2-hydroxyethyl)isocyanurate triacrylate, dipentaerythritol hexaacrylate, ethoxylated pentaerythritol tetraacrylate, and dipentaerythritol hexaacrylate.
[0051] [Photoinitiator]
[0052] In this application, the photoinitiator is selected from conventional photoinitiators, such as diacene compounds, acetophenone compounds, oxime ester compounds, phosphine oxide compounds, anthrone compounds, benzoyl ether compounds, benzophenone compounds, anthraquinone compounds, thioxanthone compounds, hexaaryl diimidazole compounds, acridine compounds, etc., including but not limited to 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone, 2-(acetoxyiminomethyl)thioxan-9-one, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]acetone 1-(O-acetyloxime), 1-hydroxycyclohexylphenyl ketone, 2-hydroxy-2-methyl- One or more of the following: 1-phenyl-1-propanone, 1-[4-(2-hydroxy)-phenyl]-3-hydroxy-2-methyl-1-propanone-1-one, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 2-methyl-1-(4-methylthiophenyl)-2-morpholino-1-propanone, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone, diethyl 2,4-oxalate, 2,4-diethylthiazolinone, 2-isopropylthioxanthanone, 2-ethylanthanone, 2,4-diethylthioxanthanone, and benzophenone.
[0053] [Thermosetting agent]
[0054] In some embodiments of this application, the material of the photosensitive layer further includes a thermosetting agent. In this case, the laminate formed by the photosensitive material has a solder resist function and can be used as a solder resist film or an interlayer insulating film. Preferably, the thermosetting agent comprises 5-20 parts by mass of 100 parts by mass of alkali-soluble resin.
[0055] Specifically, the thermosetting agent is selected from one or more of epoxy resin, isocyanate or isocyanurate compounds or triazine compounds; wherein the epoxy resin includes, but is not limited to, bisphenol type epoxy resin, biphenyl type epoxy resin, phenolic epoxy resin, epoxy resin containing naphthalene ring, and alicyclic epoxy resin; bisphenol type epoxy resin includes, for example, bisphenol A type epoxy resin, bisphenol F type epoxy resin, and bisphenol S type epoxy resin; phenolic epoxy resin includes, for example, phenolic phenolic type epoxy resin and phenolic type epoxy resin. The epoxy resin preferably has an epoxy equivalent of 50–350 g / eq. (e.g., 50 g / eq., 80 g / eq., 100 g / eq., 150 g / eq., 200 g / eq., 250 g / eq., 300 g / eq., 350 g / eq.) and a softening point of 40–150℃ (e.g., 40℃, 50℃, 80℃, 100℃, 120℃, 150℃).
[0056] [Other components]
[0057] In some embodiments of this application, the material of the photosensitive layer further includes 20 to 150 parts of colorant or filler, 2 to 10 parts of additives, and 30 parts of solvent.
[0058] Colorants or fillers include pigments and dyes that enable the photosensitive layer to exhibit specific color and optical effects, as well as extender fillers that give the photosensitive layer certain mechanical or thermal properties. Specifically, colorants or fillers are selected from at least one of silicon dioxide, titanium dioxide, barium sulfate, calcium carbonate, aluminum hydroxide, kaolin, talc, titanium dioxide, aluminum oxide, silicon nitride, aluminum nitride, carbon black, indigo blue, indigo green, toluidine red, and chrome yellow. Other commonly available colorants or fillers can also be selected according to actual needs.
[0059] The additives include color developers, plasticizers, defoamers, polymerization inhibitors, antioxidants, and leveling agents; the color developer is selected from at least one of pentyl bromide, ethylene dibromide, benzyl bromide, dibromomethane, tribromomethylphenyl sulfone, trichloroacetamide, pentyl iodide, and chloroethane; the plasticizer is selected from phthalic acid compounds or sulfonamide compounds; preferably, the plasticizer is selected from at least one of diethyl phthalate, diphenyl phthalate, and p-toluenesulfonamide; the defoamer is selected from non-silicone defoamers. The agent is selected from at least one of the following: foaming agent, polyether defoamer, silicone defoamer, and polyether-modified silicone defoamer; the polymerization inhibitor is selected from at least one of the following: p-methoxyphenol, hydroquinone, pyrogallol, tert-butylcatechol, and aluminum salt of N-nitrosophenylhydroxylamine; the antioxidant is selected from at least one of the following: amine antioxidant, phenolic antioxidant, thioester-assisted antioxidant, phosphite-assisted antioxidant, and thioether-assisted antioxidant; and the leveling agent is selected from at least one of the following: modified polysiloxane and long-chain resin.
[0060] The addition of a solvent helps to promote thorough mixing among the components of the photosensitive resin composition. The solvent can be a conventional organic solvent that can effectively dissolve each component, and γ-butyrolactone is preferred.
[0061] [Second Embodiment]
[0062] In this embodiment, the photosensitive laminate further includes a light-converting layer, which is disposed between the support layer and the photosensitive layer or on the side of the support layer away from the photosensitive layer. A light-converting agent is contained within the light-converting layer. When the exposure machine irradiates the photosensitive laminate, the light emitted by the exposure machine passes through the support layer and enters the light-converting layer. The light-converting agent contained in the light-converting layer absorbs the longer wavelength light emitted by the exposure machine and converts it into shorter wavelength light. This shorter wavelength light then irradiates the photosensitive layer, thereby improving the photocuring speed and effect of the photosensitive layer.
[0063] In some specific embodiments, the material of the light-converting layer, by weight, includes 60-90 parts of a second resin, 0.1-50 parts of a light-converting agent, 0-30 parts of a second filler, and 0.001-20 parts of a curing agent.
[0064] Typically, but not limitingly, in the material of the light-converting layer, the amount of the second resin, by weight, is 60 parts, 65 parts, 70 parts, 75 parts, 80 parts, 85 parts, 90 parts, or any combination of two values; the amount of the light-converting agent, by weight, is 0.1 parts, 0.2 parts, 0.5 parts, 1 part, 2 parts, 5 parts, 10 parts, 20 parts, 30 parts, 40 parts, 50 parts, or any combination of two values; the amount of the second filler, by weight, is 0 parts, 1 part, 2 parts, 5 parts, 10 parts, 15 parts, 20 parts, 25 parts, 30 parts, or any combination of two values; and the amount of the second auxiliary agent, by weight, is 0.001 parts, 0.002 parts, 0.005 parts, 0.008 parts, 0.01 parts, 0.05 parts, 0.1 parts, 0.2 parts, 0.5 parts, 1 part, or any combination of two values.
[0065] The specific type of the second resin is not limited, including but not limited to any one or more of acrylic resin, fluorocarbon resin, polyester resin, epoxy resin, polyurethane resin, and terpene resin.
[0066] The specific type of curing agent is not limited, including but not limited to any one or more of the following: hexamethylene diisocyanate trimer, hexamethylene diisocyanate prepolymer, isophorone diisocyanate trimer, isophorone diisocyanate prepolymer, hydrogenated styrene diisocyanate trimer, hydrogenated styrene diisocyanate prepolymer, methyl etherified polyhydroxymethyl melamine resin, butyl etherified polyhydroxymethyl melamine resin, mixed etherified polyhydroxymethyl melamine resin, polyamide, polymethylene diamine, diethylenetriamine, pentamethyldiethylenetriamine, triethylenetetramine, diethylenetriamine, triethylenetetramine, and (2,3-dimethyl)dibutyltriamine.
[0067] The specific types of the second filler and the second additive are the same as those of the first filler and the first additive, and will not be repeated here.
[0068] In some embodiments, the light-converting layer is prepared by: depositing the light-converting layer material on at least one side of the support layer at 60-200°C using one of the following processes: texture coating, mask coating, spraying, inkjet printing, screen printing, or transfer printing; and drying the material to obtain the light-converting layer.
[0069] In this embodiment, the specific composition of the photosensitive layer is the same as that of the photosensitive layer in the first embodiment, and will not be repeated here.
[0070] In this embodiment, the specific composition of the support layer is not limited. The support layer may or may not contain a light-converting agent. In some specific embodiments, the material of the support layer, by weight, includes 65-99 parts of a first resin, 0.1-15 parts of a light-converting agent, 0.9-30 parts of a first filler, and 0.1-5 parts of a first additive.
[0071] In this embodiment, the thickness of the light-converting layer is 1-30 μm.
[0072] [Third Implementation Method]
[0073] In this embodiment, the photosensitive layer contains a light-converting agent, and the photosensitive layer comprises a first photosensitive layer and a second photosensitive layer stacked sequentially. The first photosensitive layer is disposed between a support layer and the second photosensitive layer, and the light-converting agent is contained within the first photosensitive layer. When an exposure machine irradiates the photosensitive laminate, the light emitted by the exposure machine passes through the support layer and enters the first photosensitive layer. The light-converting agent contained in the first photosensitive layer absorbs the longer wavelength light emitted by the exposure machine and converts it into shorter wavelength light, which then irradiates the first and second photosensitive layers, thereby improving the photocuring speed and photocuring effect of the first and second photosensitive layers. Since the second photosensitive layer does not contain a light-converting agent, it does not affect deep curing properties and has minimal impact on resolution.
[0074] In some specific embodiments, the material of the first photosensitive layer, by weight, comprises 100 parts of a first alkali-soluble resin, 5 to 50 parts of a first photopolymerizable monomer, 0.1 to 10 parts of a first photoinitiator, and 0.01 to 30 parts of a light-converting agent. Typically, but not limitingly, by weight, the amount of the first photosensitive layer material, with the first alkali-soluble resin being 100 parts, may be 5 parts, 10 parts, 15 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, or any combination of two such values. The range of values for the concentration of the light-converting agent is 0.1 parts, 0.2 parts, 0.5 parts, 0.8 parts, 1.0 parts, 2.0 parts, 5.0 parts, 8.0 parts, 10 parts, 15 parts, 20 parts, 25 parts, 30 parts, or any two of these values; the range of values for the concentration of the first initiator is 0.01 parts, 0.02 parts, 0.05 parts, 0.08 parts, 0.1 parts, 0.2 parts, 0.5 parts, 0.8 parts, 1.0 parts, 2.0 parts, 5.0 parts, 8.0 parts, 10 parts, or any two of these values.
[0075] The specific meanings of the first alkali-soluble resin, the first photopolymerizable monomer, and the first photoinitiator are as described in the first embodiment above, and will not be repeated here.
[0076] In this embodiment, the specific composition of the second photosensitive layer is not limited. Any composition commonly used in the art for photosensitive layers is acceptable. It can be the same as or different from the first photosensitive layer. In some specific embodiments, the only difference between the second photosensitive layer and the first photosensitive layer is that the second photosensitive layer does not contain a light-converting agent.
[0077] In this embodiment, the thickness of the first photosensitive layer is 5-20 μm, and the thickness of the second photosensitive layer is 5-55 μm.
[0078] In this embodiment, the specific composition of the support layer is not limited. The support layer may or may not contain a light-converting agent.
[0079] [Fourth Implementation Method]
[0080] In this embodiment, the photosensitive layer contains a light-converting agent, which is gradient-distributed within the photosensitive layer, and its content gradually decreases along the direction away from the support layer. When the exposure machine irradiates the photosensitive laminate, the light emitted by the exposure machine passes through the support layer and enters the photosensitive layer. The light-converting agent contained in the photosensitive layer absorbs the longer wavelength light emitted by the exposure machine and converts it into shorter wavelength light, which then irradiates the photosensitive layer. Furthermore, the content of the light-converting agent gradually decreases along the direction away from the exposure machine, thereby preventing excessively high levels of the light-converting agent from affecting the mechanical properties, deep curing properties, and resolution of the photosensitive layer, while simultaneously improving the photocuring speed and effect of the photosensitive layer.
[0081] In some embodiments, the photosensitive layer comprises at least two stacked photosensitive layers, and the content of the light-converting agent in each photosensitive layer gradually decreases in the direction away from the support layer. For example, the photosensitive layer comprises a first photosensitive layer, a second photosensitive layer, and a third photosensitive layer stacked sequentially, and the content of the light-converting agent in the first photosensitive layer is greater than the content of the light-converting agent in the second photosensitive layer, which is greater than the content of the light-converting agent in the third photosensitive layer, and the third photosensitive layer is located away from the support layer.
[0082] In some specific embodiments, the photosensitive layer material, by weight, comprises 100 parts of a second alkali-soluble resin, 5 to 50 parts of a second photopolymerizable monomer, 0.01 to 10 parts of a second photoinitiator, and 0.01 to 30 parts of a light-converting agent, with the content of the light-converting agent decreasing in a gradient away from the thickness direction of the support layer. Typically, but not limitingly, by weight, the amount of the second photopolymerizable monomer in the photosensitive layer material, with 100 parts of the second alkali-soluble resin, is such as 5 parts, 10 parts, 15 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, or any range of two such values; the amount of the light-converting agent is such as 0.01 parts, 0.02 parts, 0.05 parts, 0.08 parts, 0.1 parts, 0.2 parts, or 0.5 parts. The dosage of the second initiator may be 0.8 parts, 1.0 parts, 2.0 parts, 5.0 parts, 8.0 parts, 10 parts, 15 parts, 20 parts, 25 parts, 30 parts, or any range of two values; the dosage of the second initiator may be 0.01 parts, 0.02 parts, 0.05 parts, 0.08 parts, 0.1 parts, 0.2 parts, 0.5 parts, 0.8 parts, 1.0 parts, 2.0 parts, 5.0 parts, 8.0 parts, 10 parts, or any range of two values.
[0083] The specific meanings of the second alkali-soluble resin, the second photopolymerizable monomer, and the photoinitiator are as described in the first embodiment above, and will not be repeated here.
[0084] In this embodiment, the specific composition of the support layer is not limited. Its specific composition is the same as that of the support layer in the third embodiment, and will not be described again here.
[0085] In some embodiments, the protective layer is selected from at least one of PET film, PP film, PE film, PEN film, PI film, and release paper. The thickness of the support layer and the protective layer is 5-50 μm, and the total thickness of the photosensitive layer is 10-60 μm.
[0086] In a second typical embodiment of this application, a curing film is also provided, which is formed by photocuring or photothermal curing of the photosensitive layer provided in the second typical embodiment.
[0087] In a fourth typical embodiment of this application, a circuit board is also provided, which includes the cured film provided in the third typical embodiment described above.
[0088] In the fifth typical embodiment of this application, an electronic device is also provided, which includes the curing film provided in the three typical embodiments described above or the circuit board provided in the fourth typical embodiment described above.
[0089] The beneficial effects of this application will be further illustrated below with reference to embodiments and comparative examples.
[0090] Example 1-1
[0091] This embodiment provides a light-converting photosensitive laminate, which includes a support layer, a photosensitive layer and a protective layer stacked sequentially. The support layer contains a light-converting agent, and the protective layer is a PET film with a thickness of 15 μm.
[0092] The support layer comprises: 99 parts by weight of polyethylene terephthalate (PET) as the first resin, 5 parts by weight of NaYGd:Er as the light conversion agent, 0.9 parts by weight of silica, 0.05 parts by weight of hydrolysis stabilizer I powder (Rhein Chemicals), 0.04 parts by weight of antioxidant triethylene glycol ether-di(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate, and 0.01 parts by weight of heat stabilizer N-phenylmaleimide-styrene-methyl methacrylate. The support layer is prepared by melt extrusion and has a thickness of 25 μm.
[0093] The photosensitive layer material comprises: 100 parts of alkali-soluble acid-modified epoxy acrylate resin (Nippon Kayaku ZFR-1401H, bisphenol F type, acid value 98 mg KOH / g, molecular weight 25000), 10 parts of photopolymerizable monomer poly(propylene glycol) diacrylate, 3 parts of photoinitiator 2,4,6-trimethylbenzoyl diphenylphosphine oxide, and 15 parts of thermosetting agent cresol phenolic varnish-type epoxy resin (DICEPICLON N-660, epoxy equivalent 202-212 g / eq). The mixture of photosensitive layer materials is coated onto the surface of the support layer to a thickness of 30 μm and dried at 85°C for 10 min to obtain the photosensitive layer.
[0094] Examples 1-2
[0095] The difference from Example 1-1 is that the light conversion agent NaYGd:Er in the support layer of this example is 15 parts.
[0096] Examples 1-3
[0097] The difference from Example 1-1 is that the light conversion agent NaYGd:Er in the support layer of this example is 0.1 parts.
[0098] Examples 1-4
[0099] The difference from Example 1-1 is that the light-converting agent in the support layer of this example is 5 parts of 2,45,6-tetra(9-carbazolyl)-isophthalonitrile.
[0100] Examples 1-5
[0101] The difference from Example 1-1 is that the light-converting agent in the support layer of this example is 5 parts of donor formula (I) + acceptor formula (IV) (molar ratio 1:1).
[0102] Examples 1-6
[0103] The difference from Example 1-1 is that the light conversion agent in the support layer of this example is 5 parts of CsPbBr3 / Cs4PbBr6.
[0104] Examples 1-7
[0105] The difference from Example 1-1 is that the first resin in the support layer of this example is 99 parts by weight of polypropylene.
[0106] Examples 1-8
[0107] The difference from Example 1-1 is that the first resin in the support layer of this example is 65 parts by weight of polyethylene terephthalate.
[0108] Example 2-1
[0109] This embodiment provides a light-converting photosensitive laminate, which includes a support layer, a light-converting layer, a photosensitive layer and a protective layer stacked sequentially. The light-converting layer contains a light-converting agent, and the protective layer is a PET film with a thickness of 15 μm.
[0110] The support layer is made of the following materials: 99 parts by weight of polyethylene terephthalate, 0.9 parts by weight of silicon dioxide, 0.05 parts by weight of hydrolysis stabilizer I powder (Rhein Chemical), 0.04 parts by weight of antioxidant triethylene glycol ether-di(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate, and 0.01 parts by weight of heat stabilizer N-phenylmaleimide-styrene-methyl methacrylate. The support layer is prepared by melt extrusion and has a thickness of 25 μm.
[0111] The materials of the light conversion layer include: 90 parts by weight of the second resin, acrylic resin AC-1 (Changxing Chemical); 5 parts by weight of the light conversion agent, NaYGd:Er; 4 parts by weight of the curing agent, isophorone diisocyanate prepolymer; 5 parts by weight of the curing agent, triethylenetetramine; and 1 part by weight of the catalyst, stannous octoate. The light conversion layer is prepared by coating the material composition of the light conversion layer onto one side of the support layer at 150°C using a textured coating process, with a coating thickness of 7 μm. After drying, the light conversion layer is obtained.
[0112] The photosensitive layer comprises: 100 parts of alkali-soluble acid-modified epoxy acrylate resin (Nippon Kayaku ZFR-1401H, bisphenol F type, acid value 98 mg KOH / g, molecular weight 25000), 10 parts of photopolymerizable monomer poly(propylene glycol) diacrylate, 3 parts of photoinitiator 2,4,6-trimethylbenzoyl diphenylphosphine oxide, and 15 parts of thermosetting agent cresol phenolic varnish-type epoxy resin (DICEPICLON N-660, epoxy equivalent 202-212 g / eq). The photosensitive layer is prepared by coating the material composition of the photosensitive layer onto the surface of the photoconversion layer to a thickness of 30 μm, and drying at 85°C for 10 min to obtain the photosensitive layer.
[0113] Example 2-2
[0114] The difference from Example 2-1 is that the photosensitive laminate provided in this example includes a photosensitive layer, a support layer, a photosensitive layer and a protective layer stacked in sequence.
[0115] During its preparation, the material composition of the photosensitive layer is coated on the surface of the support layer away from the light-converting layer.
[0116] Example 2-3
[0117] The difference from Example 2-1 is that the light-converting agent NaYGd:Er in the light-converting layer of this example is 50 parts.
[0118] Examples 2-4
[0119] The difference from Example 2-1 is that the light-converting agent NaYGd:Er in the light-converting layer of this example is 0.1 parts.
[0120] Examples 2-5
[0121] The difference from Example 2-1 is that the second resin in the light-converting layer of this example is 90 parts by weight of fluorocarbon resin GK570 (Daikin, Japan).
[0122] Examples 2-6
[0123] The difference from Example 2-1 is that the second resin in the light conversion layer of this example is 90 parts by weight of epoxy resin SM716 (Jiangsu Sanmu Chemical Co., Ltd.).
[0124] Examples 2-7
[0125] The difference from Example 2-1 is that the second resin in the light-converting layer of this example is 60 parts.
[0126] Example 3-1
[0127] This embodiment provides a light-converting sensitive laminate, which includes a support layer, a photosensitive layer, and a protective layer stacked sequentially. The photosensitive layer contains a light-converting agent, and the protective layer is a PET film with a thickness of 15 μm. The photosensitive layer includes a first photosensitive layer, a second photosensitive layer, and a third photosensitive layer stacked sequentially, and the mass content of the light-converting agent in the first photosensitive layer is greater than the mass content of the light-converting agent in the second photosensitive layer, which in turn is greater than the mass content of the light-converting agent in the third photosensitive layer.
[0128] The support layer comprises: 99 parts by weight of polyethylene terephthalate, 0.9 parts by weight of silica, 0.05 parts by weight of hydrolysis stabilizer I powder (Rhein Chemicals), 0.04 parts by weight of antioxidant triethylene glycol ether-di(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate, and 0.01 parts by weight of heat stabilizer N-phenylmaleimide-styrene-methyl methacrylate. This support layer is prepared by melt extrusion.
[0129] The materials of the first photosensitive layer include: 100 parts of alkali-soluble acid-modified epoxy acrylate resin (Nippon Kayaku ZFR-1401H, bisphenol F type, acid value 98mgKOH / g, molecular weight 25000), 10 parts of light conversion agent NaYGd:Er, 10 parts of photopolymerizable monomer poly(propylene glycol) diacrylate, 3 parts of photoinitiator 2,4,6-trimethylbenzoyl diphenylphosphine oxide, and 15 parts of thermosetting agent cresol phenolic varnish-type epoxy resin (DIC EPICLON N-660, epoxy equivalent 202-212g / eq). The preparation method of the first photosensitive layer is as follows: the material composition of the photosensitive layer is coated on the surface of the support layer with a coating thickness of 10μm, and dried at 65℃ for 6min to obtain the first photosensitive layer.
[0130] The materials for the second photosensitive layer include: 100 parts of alkali-soluble acid-modified epoxy acrylate resin (Nippon Kayaku ZFR-1401H, bisphenol F type, acid value 98mgKOH / g, molecular weight 25000), 6 parts of light conversion agent NaYGd:Er, 10 parts of photopolymerizable monomer poly(propylene glycol) diacrylate, 3 parts of photoinitiator 2,4,6-trimethylbenzoyl diphenylphosphine oxide, and 15 parts of thermosetting agent cresol phenolic varnish-type epoxy resin (DIC EPICLON N-660, epoxy equivalent 202-212g / eq). The preparation method for the second photosensitive layer is as follows: the material composition of the second photosensitive layer is coated onto the surface of the first photosensitive layer to a thickness of 10μm, and dried at 75℃ for 6min to obtain the second photosensitive layer.
[0131] The materials for the third photosensitive layer are: 100 parts of alkali-soluble acid-modified epoxy acrylate resin (Nippon Kayaku ZFR-1401H, bisphenol F type, acid value 98mgKOH / g, molecular weight 25000), 2 parts of light conversion agent NaYGd:Er, 10 parts of photopolymerizable monomer poly(propylene glycol) diacrylate, 3 parts of photoinitiator 2,4,6-trimethylbenzoyl diphenylphosphine oxide, and 15 parts of thermosetting agent cresol phenolic varnish-type epoxy resin (DIC EPICLON N-660, epoxy equivalent 202-212g / eq). The preparation method of the third photosensitive layer is as follows: the material composition of the third photosensitive layer is coated onto the surface of the second photosensitive layer with a coating thickness of 10μm, and dried at 85℃ for 6min to obtain the third photosensitive layer. This results in a photosensitive layer in which the first, second, and third photosensitive layers are sequentially stacked.
[0132] Example 3-2
[0133] The difference from Example 3-1 is that this example includes five photosensitive layers, each with a thickness of 6μm; according to the stacking order, the materials of the second, third, and fourth photosensitive layers are the same as those of the first, second, and third photosensitive layers in Example 3-1, respectively.
[0134] The materials of the first photosensitive layer include: 100 parts of alkali-soluble acid-modified epoxy acrylate resin (Nippon Kayaku ZFR-1401H, bisphenol F type, acid value 98mgKOH / g, molecular weight 25000), 15 parts of light conversion agent NaYGd:Er, 10 parts of photopolymerizable monomer poly(propylene glycol) diacrylate, 3 parts of photoinitiator 2,4,6-trimethylbenzoyl diphenylphosphine oxide, and 15 parts of thermosetting agent cresol phenolic varnish-type epoxy resin (DIC EPICLON N-660, epoxy equivalent 202-212g / eq). The preparation method of the first photosensitive layer is as follows: the material composition of the photosensitive layer is coated on the surface of the support layer with a coating thickness of 6μm, and dried at 65℃ for 6min to obtain the first photosensitive layer.
[0135] The materials for the fifth photosensitive layer include: 100 parts of alkali-soluble acid-modified epoxy acrylate resin (Nippon Kayaku ZFR-1401H, bisphenol F type, acid value 98mgKOH / g, molecular weight 25000), 0.01 parts of light-converting agent NaYGd:Er, 10 parts of photopolymerizable monomer poly(propylene glycol) diacrylate, 3 parts of photoinitiator 2,4,6-trimethylbenzoyl diphenylphosphine oxide, and 15 parts of thermosetting agent cresol phenolic varnish-type epoxy resin (DIC EPICLON N-660, epoxy equivalent 202-212g / eq). The fifth photosensitive layer is prepared by coating the material composition of the photosensitive layer onto the surface of the fourth photosensitive layer to a thickness of 6μm, and drying at 65℃ for 6min to obtain the fifth photosensitive layer.
[0136] Example 4-1
[0137] This embodiment provides a photosensitive laminate comprising a support layer, a first photosensitive layer, a second photosensitive layer, and a protective layer stacked sequentially, wherein the first photosensitive layer contains a photosensitive agent, and the protective layer is a PET film with a thickness of 15 μm.
[0138] The support layer comprises: 99 parts by weight of polyethylene terephthalate, 0.9 parts by weight of silica, 0.05 parts by weight of hydrolysis stabilizer I powder (Rhein Chemicals), 0.04 parts by weight of antioxidant triethylene glycol ether-di(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate, and 0.01 parts by weight of heat stabilizer N-phenylmaleimide-styrene-methyl methacrylate. The support layer is prepared by melt extrusion.
[0139] The materials of the first photosensitive layer include: 100 parts of alkali-soluble acid-modified epoxy acrylate resin (Nippon Kayaku ZFR-1401H, bisphenol F type, acid value 98mgKOH / g, molecular weight 25000), 10 parts of light conversion agent NaYGd:Er, 10 parts of photopolymerizable monomer poly(propylene glycol) diacrylate, 3 parts of photoinitiator 2,4,6-trimethylbenzoyl diphenylphosphine oxide, and 15 parts of thermosetting agent cresol phenolic varnish-type epoxy resin (DIC EPICLON N-660, epoxy equivalent 202-212g / eq). The preparation method of the first photosensitive layer is as follows: the material composition of the first photosensitive layer is coated on the surface of the support layer with a coating thickness of 15μm, and dried at 70℃ for 8min to obtain the first photosensitive layer.
[0140] The materials for the second photosensitive layer include: 100 parts of alkali-soluble acid-modified epoxy acrylate resin (Nippon Kayaku ZFR-1401H, bisphenol F type, acid value 98 mg KOH / g, molecular weight 25000), 10 parts of photopolymerizable monomer poly(propylene glycol) diacrylate, 3 parts of photoinitiator 2,4,6-trimethylbenzoyl diphenylphosphine oxide, and 15 parts of thermosetting agent cresol phenolic varnish-type epoxy resin (DIC EPICLON N-660, epoxy equivalent 202-212 g / eq). The preparation method for the second photosensitive layer is as follows: the material composition of the second photosensitive layer is coated onto the surface of the first photosensitive layer to a thickness of 15 μm, and dried at 85°C for 10 min to obtain the second photosensitive layer.
[0141] Example 4-2
[0142] The difference from Example 4-1 is that the light conversion agent NaYGd:Er in the first photosensitive layer of this example is 30 parts.
[0143] Example 4-3
[0144] The difference from Example 4-1 is that the light conversion agent NaYGd:Er in the first photosensitive layer of this example is 0.01 parts.
[0145] Example 4-4
[0146] The difference from Example 4-1 is that the first photosensitive layer in this example contains 5 parts of poly(propylene glycol) diacrylate and 1 part of photoinitiator 2,4,6-trimethylbenzoyl diphenylphosphine oxide.
[0147] Examples 4-5
[0148] The difference from Example 4-1 is that the first photosensitive layer in this example contains 50 parts of poly(propylene glycol) diacrylate and 10 parts of photoinitiator 2,4,6-trimethylbenzoyl diphenylphosphine oxide.
[0149] Comparative Example 1
[0150] The difference from Example 1-1 is that the support layer does not contain a light-converting agent.
[0151] Comparative Example 2
[0152] This comparative example provides a photosensitive laminate comprising a support layer, a photosensitive layer, and a protective layer stacked sequentially, wherein the photosensitive layer is a single layer and contains a photosensitive agent, and the protective layer is a PET film with a thickness of 15 μm.
[0153] The support layer comprises: 99 parts by weight of polyethylene terephthalate, 0.9 parts by weight of silica, 0.05 parts by weight of hydrolysis stabilizer I powder (Rhein Chemicals), 0.04 parts by weight of antioxidant triethylene glycol ether-di(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate, and 0.01 parts by weight of heat stabilizer N-phenylmaleimide-styrene-methyl methacrylate. The support layer is prepared via melt extrusion.
[0154] The photosensitive layer comprises: 100 parts of alkali-soluble acid-modified epoxy acrylate resin (Nippon Kayaku ZFR-1401H, bisphenol F type, acid value 98 mg KOH / g, molecular weight 25000), 10 parts of light-converting agent NaYGd:Er, 10 parts of photopolymerizable monomer poly(propylene glycol) diacrylate, 3 parts of photoinitiator 2,4,6-trimethylbenzoyl diphenylphosphine oxide, and 15 parts of thermosetting agent cresol phenolic varnish-type epoxy resin (DIC EPICLON N-660, epoxy equivalent 202-212 g / eq). The photosensitive layer is prepared by coating the material composition of the photosensitive layer onto the surface of the support layer to a thickness of 30 μm, and drying at 85°C for 10 min to obtain the photosensitive layer.
[0155] [Testing Method]
[0156] Cross-cut test: Using a vacuum laminator, the laminated samples obtained in the examples and comparative examples were removed of their protective layers and then adhered to a commercial copper-clad laminate. The vacuum section had a pressure of 6 kgf, a vacuum time of 20 s, a pressing time of 30 s, and a temperature of 65°C. The leveling section had a pressure of 6 kgf, a leveling time of 50 s, and a temperature of 85°C. After adhesion, the laminate was exposed to a standard test mask at an energy of ST8 / 21 sensitivity, thermally cured, and all other layers were removed, leaving only the photosensitive layer. A cross-cut test was performed on the surface of the photosensitive layer using a cross-cut knife. Then, 3M 600 tape was pulled at a 90° angle, and any peeling was observed. This was repeated three times, with new tape used each time. The total number of peeling squares was recorded for each of the three tests. The test results are shown in Table 1.
[0157] Sensitivity: The laminated samples obtained in the examples and comparative examples were removed from their protective layers and then bonded to a commercial copper-clad laminate using a vacuum laminator. The vacuum section had a pressure of 6 kgf, a vacuum time of 20 s, a pressing time of 30 s, and a temperature of 65°C. The leveling section had a pressure of 6 kgf, a leveling time of 50 s, and a temperature of 85°C. After bonding, the samples were exposed and developed on an ST21 exposure scale. The lowest energy that was not developed and fully exposed on an ST8 scale was recorded as the sensitivity energy. The lower the sensitivity energy, the less energy is required to achieve a specific photoreaction level, and the stronger the sensitivity. The test results are shown in Table 1.
[0158] Edge steepness and resolution: The laminated samples obtained in the examples and comparative examples were removed from their protective layers and then bonded to commercial copper-clad laminates using a vacuum laminator. The vacuum section had a pressure of 6 kgf, a vacuum time of 20 s, a pressing time of 30 s, and a temperature of 65°C. The leveling section had a pressure of 6 kgf, a leveling time of 50 s, and a temperature of 85°C. After bonding, the samples were exposed to a standard test mask at an energy of ST8 / 21 sensitivity, developed, and thermally cured to remove other layers, leaving only the photosensitive layer. Edge steepness and resolution were observed and recorded under a metallographic microscope by sectioning. Edge steepness represents the width of the actual circuit sidewall that has been excessively etched, based on the ideal 90-degree angle between the circuit sidewall and the substrate. The smaller the side etch, the weaker the inverted trapezoidal shape of the edge, and the closer the sidewall is to a right angle, the better the steepness. In this invention, a smaller side etch number indicates better edge steepness. The test results are shown in Table 1.
[0159] Table 1
[0160]
[0161]
[0162] As can be seen from the above description, the embodiments of the present invention achieve the following technical effects:
[0163] The photosensitive laminate provided in this application contains a light-converting agent that has an "upconversion function" and can induce an "anti-Stokes" phenomenon. This agent absorbs long wavelengths and low energy, and releases short wavelengths and high energy. Thus, when the photosensitive laminate is irradiated by an exposure machine, the longer wavelength light emitted by the exposure machine is absorbed by the light-converting agent and converted into shorter wavelength light that can be absorbed by the photoinitiator. This achieves high utilization of the light source while still using a conventional photoinitiator, thereby expanding the selectivity of the photoinitiator and improving the photocuring speed and effect of the photosensitive layer.
[0164] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A photosensitive laminate, characterized in that, The photosensitive laminate includes a support layer, a photosensitive layer, and an optional protective layer stacked sequentially, and the photosensitive laminate contains a light-converting agent; the light-converting agent has an absorption wavelength > 390 nm and an emission wavelength ≤ 390 nm; The support layer contains the light-converting agent, while the photosensitive layer does not contain the light-converting agent. By mass, the material of the support layer includes 65-99 parts of the first resin, 0.1-15 parts of the light-converting agent, 0.9-30 parts of the first filler, and 0.1-5 parts of the first additive. Alternatively, the photosensitive laminate may further include a light-converting layer, which is disposed between the support layer and the photosensitive layer or on the side of the support layer away from the photosensitive layer, and the light-converting layer contains the light-converting agent; the photosensitive layer does not contain the light-converting agent, and the material of the light-converting layer, by weight, includes 60-90 parts of a second resin, 0.1-50 parts of the light-converting agent, 0-30 parts of a second filler, 0.001-20 parts of a curing agent, and 0.001-1 parts of a second auxiliary agent; Alternatively, the photosensitive layer comprises a first photosensitive layer and a second photosensitive layer stacked sequentially, the first photosensitive layer being disposed between the support layer and the second photosensitive layer, the first photosensitive layer containing the light-converting agent, and the second photosensitive layer not containing the light-converting agent; by mass parts, the material of the first photosensitive layer comprises 100 parts of a first alkali-soluble resin, 5-50 parts of a first photopolymerizable monomer, 0.1-10 parts of a first photoinitiator, and 0.01-30 parts of the light-converting agent; the material of the second photosensitive layer comprises 100 parts of a second alkali-soluble resin, 5-50 parts of a second photopolymerizable monomer, and 0.1-10 parts of a second photoinitiator; Alternatively, the photosensitive layer contains the light-converting agent, which is gradient-distributed within the photosensitive layer, and the content of the light-converting agent gradually decreases along the thickness direction away from the support layer; by mass parts, the material of the photosensitive layer comprises 100 parts of a third alkali-soluble resin, 5-50 parts of a third photopolymerizable monomer, 0.1-10 parts of a third photoinitiator, and 0.01-30 parts of the light-converting agent; and the content of the light-converting agent gradually decreases along the thickness direction away from the support layer.
2. The photosensitive laminate according to claim 1, characterized in that, When the support layer contains a light-converting agent, in the support layer, The first resin is selected from at least one of polyethylene terephthalate, polyethylene naphthalate, polyethylene, and polypropylene; And / or, the first filler is selected from at least one of calcium titanate, calcium carbonate, titanium dioxide, zinc oxide, antimony trioxide, silicon oxide, hollow glass microspheres, and barium sulfate; And / or, the first additive is selected from at least one of ultraviolet absorbers, hindered amine light stabilizers, antioxidants, heat stabilizers, catalysts, hydrolysis stabilizers, nucleating and penetrating agents, and toughening agents.
3. The photosensitive laminate according to claim 1, characterized in that, When the photosensitive laminate includes a photoconverting layer, the second resin in the photoconverting layer is selected from at least one of acrylic resin, fluorocarbon resin, polyester resin, epoxy resin, polyurethane resin, and terpene resin; And / or, the second filler is selected from at least one of calcium titanate, calcium carbonate, titanium dioxide, zinc oxide, antimony trioxide, silicon oxide, hollow glass microspheres, and barium sulfate; And / or, the curing agent is selected from at least one of hexamethylene diisocyanate trimer, hexamethylene diisocyanate prepolymer, isophorone diisocyanate trimer, isophorone diisocyanate prepolymer, hydrogenated styrene diisocyanate trimer, hydrogenated styrene diisocyanate prepolymer, methyl etherified polymethyl melamine resin, butyl etherified polymethyl melamine resin, mixed etherified polymethyl melamine resin, polyamide, polymethylene diamine, diethylenetriamine, pentamethyldiethylenetriamine, triethylenetetramine, diethylenetriamine, triethylenetetramine, and (2,3-dimethyl)dibutyltriamine; And / or, the second additive is selected from at least one of ultraviolet absorbers, hindered amine light stabilizers, antioxidants, heat stabilizers, catalysts, hydrolysis stabilizers, nucleating and penetrating agents, and toughening agents.
4. A cured film, characterized in that, The cured film is formed by photocuring or photothermal dual curing of the photosensitive layer in any one of claims 1 to 3.
5. A circuit board, characterized in that, The circuit board includes the cured film as described in claim 4.
6. An electronic device, characterized in that, The electronic device includes the cured film of claim 4 or the circuit board of claim 5.
Citation Information
Patent Citations
Photoinitiator composition, photosensitive solder resist composition containing same, and printed circuit board
CN112625149A
White photosensitive cover film and application in mini LED display module field
CN116300315A
Photosensitive film laminate, cured film, printed circuit board and electronic device
CN116859684A