High-performance hafnium oxide-boron nitride composite ceramic and preparation method and application thereof

By generating HfO₂-x vol%BN-y vol%Co-z vol%W composite ceramics at low temperature through pressureless sintering, the problem of densification of hafnium oxide and boron nitride ceramics was solved, and high-performance hafnium oxide-boron nitride composite ceramics suitable for high-temperature environments were prepared.

CN119219413BActive Publication Date: 2026-11-20SHAOXING UNIVERSITY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411264360.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2026-11-20
Estimated Expiration
2044-09-10

Smart Images

  • Figure CN119219413B_ABST
    Figure CN119219413B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of composite ceramic materials, and discloses a high-performance hafnium oxide-boron nitride composite ceramic, a preparation method and an application thereof. The composition of the composite ceramic is HfO2-xvol%BN-yvol%Co-zvol%W, where 0<x≤15, 0<y≤15, 0<z≤15; the composite ceramic is prepared by first subjecting a mixed powder of HfO2, Co, W and amorphous boron powder to compression molding, then performing cold isostatic pressing to form a green body, placing the green body in a tube furnace filled with N2, heating to 600 to 800°C for heat preservation, and then heating to 1400 to 1600°C for heat preservation. The composite ceramic has a relative density of >99%, a hardness of 30 to 45 GPa, and a fracture toughness of 8 to 15 MPa·m 1 / 2 , the ceramic grain size is 1 to 2 μm, and the weight change rate after heat treatment at 1500 to 1800°C is 0.2 to 0.8%, which can be applied in the preparation of high-temperature components.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of ceramic materials technology, and more specifically, it relates to a high-performance hafnium oxide-boron nitride composite ceramic, its preparation method, and its application. Background Technology

[0002] Hafnium oxide (HfO2) is a ceramic material widely used in materials science, possessing excellent properties such as high strength, high hardness, wear resistance, and high-temperature stability. However, due to its unique structure, hafnium oxide is difficult to obtain as a dense material using common processing methods. In the preparation of hafnium oxide ceramics, sintering temperature is one of the important factors affecting its properties.

[0003] The sintering temperature of hafnium oxide ceramics is typically between 1800 and 2000℃, with higher sintering temperatures yielding denser materials. Higher sintering temperatures promote grain growth. Under high-temperature conditions, grains in the material grow larger, resulting in relatively larger grains in the sintered material. Larger grains lead to lower strength and poorer toughness. Therefore, a suitable sintering temperature can produce dense, high-strength, and high-toughness hafnium oxide ceramic materials. Besides sintering temperature, factors such as sintering time, pressure, and additives also affect the sintering effect of hafnium oxide ceramics. Among these, the addition of additives can effectively improve the sintering effect of hafnium oxide ceramics, resulting in a denser and more uniform material.

[0004] Hexagonal boron nitride (h-BN) ceramics possess a crystal structure similar to graphite, making them an excellent high-temperature material. They also exhibit low thermal expansion coefficients, high thermal conductivity, thermal shock resistance, and corrosion resistance. Therefore, h-BN ceramics have been applied in components used in high-temperature environments, such as crucibles and thermocouple jackets. Literature reports that adding h-BN to oxide and boride ceramics improves their fracture toughness; however, the strong covalent bonds in h-BN ceramics make them difficult to sinter using traditional sintering techniques. Self-propagating high-temperature synthesis (SHS), also known as combustion synthesis, provides an effective method for preparing refractory compounds without the use of sintering aids. However, the production cost of ceramics prepared using this method is relatively high. In-situ reaction synthesis (reactive hot pressing) methods for preparing ceramic composites exhibit good mechanical properties. However, how to achieve low-temperature in-situ synthesis of ceramic composites requires further research. Summary of the Invention

[0005] To address the shortcomings and drawbacks of the existing technology, a high-performance hafnium oxide-boron nitride composite ceramic is provided, which exhibits high toughness and high hardness.

[0006] Another objective of the present invention is to provide a preparation method for the above high-performance hafnia-boron nitride composite ceramic. This method in-situ generates HfO₂-x vol% BN-y vol% Co-z vol% W composite ceramic at low temperature through pressureless sintering.

[0007] A further objective of the present invention is to provide an application of the above high-performance hafnia-boron nitride composite ceramic.

[0008] The objectives of the present invention are achieved through the following technical solutions:

[0009] A high-performance hafnia-boron nitride composite ceramic is HfO₂-x vol% BN-y vol% Co-z vol%, where 0<x≤15, 0<y≤15, 0<z≤15; the composite ceramic is prepared by first subjecting a mixed powder of HfO₂, Co, W and amorphous boron powder to die pressing, then performing cold isostatic pressing at 100 to 200 MPa to form a green body, filling N₂ into a tube furnace, heating to 600 to 800°C for heat preservation, and then heating to 1400 to 1600°C for heat preservation to obtain the product.

[0010] Preferably, the relative density of the composite ceramic is >99%, the hardness is 30 to 45 GPa, and the fracture toughness is 8 to 15 MPa·m 1 / 2 , the ceramic grain size is 1 to 2 μm, and the weight change rate of the composite ceramic after heat treatment at 1500 to 1800°C for 1 to 4 h is 0.2 to 0.8%.

[0011] Preferably, the purity of the HfO₂, Co, W and amorphous boron powder is 99 wt% or more, and the particle size of the HfO₂, Co, W and amorphous boron powder is 0.1 to 2 μm.

[0012] Preferably, the molar ratio of the HfO₂ to the amorphous boron powder is (1 to 10):(1 to 10).

[0013] Preferably, the protective atmosphere is N₂.

[0014] The preparation method of the hafnia-boron nitride composite ceramic comprises the following specific steps:

[0015] S1. Using HfO₂, Co, W and amorphous boron powder as raw materials, adding a solvent and a milling medium, mixing on a ball mill, and drying to obtain a mixed powder;

[0016] S2. Subjecting the mixed powder to die pressing and then applying pressure via cold isostatic pressing at 100 to 200 MPa to obtain a green body;

[0017] S3. Placing the green body in a tube furnace and filling 1 to 10 m 3 / minN2, heat to 600-800℃ and hold, then heat to 1400-1600℃ and hold to obtain HfO2-x vol%BN-y vol%Co-z vol%W composite ceramic.

[0018] Preferably, the solvent in step S1 is ethanol, propanol, methanol or acetone.

[0019] Preferably, the mixing time in step S1 is 10-24 hours, and the cold isostatic pressing time in step S2 is 5-15 minutes.

[0020] Preferably, in step S3, the heating rate to 600-800℃ is 5-10℃ / min, the heating rate to 1400-1600℃ is 2-5℃ / min, and the holding time is 0.5-2h.

[0021] The high-performance hafnium oxide-boron nitride composite ceramic is used in crucibles and thermocouple jackets in high-temperature environments.

[0022] This invention utilizes HfO2, Co, W, and amorphous boron powder as raw materials to generate HfO2-xvol%BN-yvol%Co-zvol%W composite ceramics through low-temperature in-situ pressureless sintering. Since pure HfO2 or BN requires high sintering temperatures, the addition of Co and W as additives significantly reduces the sintering temperature and, through in-situ BN generation, further improves the performance of the hafnium oxide-boron nitride composite ceramics. A suitable sintering temperature yields dense, high-strength, and high-toughness hafnium oxide-boron nitride composite ceramics suitable for high-temperature applications.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. This invention uses HfO2, Co, W, and amorphous boron powder as raw materials. A protective atmosphere is introduced, and the amorphous boron powder is used as a reactant. Part of it reacts with nitrogen in situ to form uniformly distributed BN, and part of it reacts with HfO2 to form HfB2. The grain size of the composite ceramic is finer (1~1.5) μm. W can compensate for the reduction in mechanical properties and high-temperature properties of hafnium oxide-boron nitride composite ceramic materials caused by low-melting-point Co. At the same time, some HfB2 is generated, which has high melting point, high hardness, good corrosion resistance and oxidation resistance, etc., significantly improving the mechanical properties of hafnium oxide-boron nitride composite ceramics.

[0025] 2. This invention employs a low-temperature in-situ method. The low melting point of Co significantly reduces the sintering temperature of hafnium oxide-boron nitride composite ceramic materials, improving sintering performance. This enables the low-temperature (1400-1600℃) in-situ preparation of high-performance hafnium oxide-boron nitride composite ceramics, and also improves the density uniformity and mechanical properties of the composite ceramics, such as wear resistance, strength, and hardness.

[0026] 3. The hexagonal boron nitride (BN) generated in situ by this invention is an excellent high-temperature material with low coefficient of thermal expansion, high thermal conductivity, resistance to thermal shock and corrosion, which broadens its application range.

[0027] Explanation of the attached diagram

[0028] Figure 1 The XRD patterns are of the hafnium oxide-boron nitride composite ceramics prepared in Examples 1-3 and Comparative Example 1. Detailed Implementation

[0029] The present invention will be further described below with reference to specific embodiments, but these should not be construed as limiting the invention. Unless otherwise specified, the technical means used in the embodiments are conventional means well known to those skilled in the art. Unless otherwise specified, the reagents, methods, and equipment used in the present invention are conventional reagents, methods, and equipment in this technical field.

[0030] Example 1

[0031] 1. 8.42 g of HfO2 powder (purity 99.3%, particle size 1 μm), 0.47 g of Co powder (purity 99.3%, particle size 1 μm), 0.47 g of W powder (purity 99.3%, particle size 2 μm) and 0.76 g of amorphous boron powder (purity 99.3%, particle size 2 μm) were added to Si3N4 ball milling media and propanol solvent and mixed for 23 h to obtain a mixed powder. The molar ratio of amorphous boron powder to HfO2 was 7:4.

[0032] 2. The mixed powder is subjected to cold isostatic pressing at 150 MPa for 5 minutes to obtain a green body;

[0033] 3. Place the billet in a tube furnace and fill it with 5m of water. 3 The HfO2-5 vol%BN-5 vol%Co-5 vol%W composite ceramic was prepared by heating at 7℃ / min to 650℃ and holding for 1.5h, and then heating at 3℃ / min to 1600℃ and holding for 1.5h.

[0034] The HfO2-5 vol%BN-5 vol%Co-5 vol%W composite ceramic has a relative density of 99.2%, a hardness of 35 GPa, and a fracture toughness of 10 MPa·m. 1 / 2 The grain size was 1.5 μm, and the weight of the ceramic increased by 0.6 wt% after heat treatment at 1600℃ for 2 h. Compared with the HfO2-5 vol%BN-5 vol%Co composite ceramic of Comparative Example 1, the addition of W improved the performance of the hafnium oxide-boron nitride composite ceramic.

[0035] Example 2

[0036] 1. 14.73 g of HfO2 powder (purity 99.6%, particle size 2 μm), 0.87 g of Co powder (purity 99.6%, particle size 2 μm), 1.73 g of W powder (purity 99.6%, particle size 1 μm) and 0.43 g of amorphous boron powder (purity 99.6%, particle size 1 μm) were added to Si3N4 ball milling media and methanol solvent and mixed for 21 h to obtain a mixed powder. The molar ratio of amorphous boron powder to HfO2 was 4:7.

[0037] 2. The mixed powder is subjected to cold isostatic pressing at 100 MPa for 10 minutes to obtain a green body;

[0038] 3. Place the billet in a tube furnace and fill it with 5m of water. 3 The HfO2-5 vol%BN-5 vol%Co-10 vol%W composite ceramic was prepared by heating at 8℃ / min to 700℃ and holding for 1.5h, and then heating at 4℃ / min to 1500℃ and holding for 1.5h.

[0039] The properties of hafnium oxide-boron nitride composite ceramics are further improved by adding 10 vol% W. The relative density of the HfO2-5 vol%BN-5 vol%Co-10 vol%W composite ceramic is 99.5%, the hardness is 40 GPa, and the fracture toughness is 13 MPa·m. 1 / 2 The grain size is 1.2 μm, and the weight of the ceramic increases by 0.4 wt% after heat treatment at 1700℃ for 3 hours.

[0040] Example 3

[0041] 1. 21.05 g of HfO2 powder (purity 99.9%, particle size 1 μm), 1.31 g of Co powder (purity 99.9%, particle size 2 μm), 3.95 g of W powder (purity 99.9%, particle size 2 μm) and 0.11 g of amorphous boron powder (purity 99.9%, particle size 1 μm) were added to a ball milling medium Si3N4 balls and ethanol solvent and mixed for 24 h to obtain a mixed powder. The molar ratio of amorphous boron powder to HfO2 was 1:10.

[0042] 2. The mixed powder is subjected to cold isostatic pressing at 200 MPa for 15 minutes to obtain a green body;

[0043] 3. Place the billet in a tube furnace and fill it with 5m of water. 3 The HfO2-5 vol%BN-5 vol%Co-15 vol%W composite ceramic was prepared by heating at 10℃ / min to 800℃ and holding for 2h, and then heating at 5℃ / min to 1400℃ and holding for 2h.

[0044] Figure 1The images show the XRD patterns of hafnium oxide-boron nitride composites prepared in Comparative Example 1 and Examples 1-3. (a) is the HfO₂-5 vol%BN-5 vol%Co composite ceramic of Comparative Example 1, (b) is the HfO₂-5 vol%BN-5 vol%Co-5 vol%W composite ceramic of Example 1, (c) is the HfO₂-5 vol%BN-5 vol%Co-10 vol%W composite ceramic of Example 2, and (d) is the HfO₂-5 vol%BN-5 vol%Co-15 vol%W composite ceramic of Example 3. Figure 1 As can be seen from the data, the main phase of the composite ceramics in Comparative Example 1 and Examples 1-3 is HfO2, with additional peaks for BN, Co, and HfB2. This indicates that when N2 is introduced, some boron powder reacts with N2 to form the BN phase in situ, and some boron powder reacts with HfO2 to form the HfB2 phase in situ, further reducing the sintering temperature. As the W content increases, the peak value of its diffraction peaks increases, thereby improving the performance of the hafnium oxide-boron nitride composite ceramics.

[0045] The properties of hafnium oxide-boron nitride composite ceramics are further improved by adding 15 vol% W. The relative density of the HfO2-5 vol%BN-5 vol%Co-15 vol%W composite ceramic is 99.9%, the hardness is 45 GPa, and the fracture toughness is 15 MPa·m. 1 / 2 The grain size is 1 μm, and the ceramic weight increased by 0.2 wt% after heat treatment at 1800℃ for 4 hours. The performance is further improved after adding a higher content of W.

[0046] Comparative Example 1

[0047] 1. 2.1 g of HfO2 powder (purity 99.9%, particle size 2 μm), 0.11 g of Co powder (purity 99.9%, particle size 1 μm) and 1.08 g of amorphous boron powder (purity 99.9%, particle size 2 μm) were added to a ball milling medium Si3N4 balls and ethanol solvent and mixed for 22 h to obtain a mixed powder. The molar ratio of amorphous boron powder to HfO2 was 10:1.

[0048] 2. The mixed powder is subjected to cold isostatic pressing at 200 MPa for 5 minutes to obtain a green body;

[0049] 3. Place the billet in a tube furnace and fill it with 5m of water. 3 The HfO2-5 vol%BN-5 vol%Co composite ceramic was prepared by heating at a rate of 5℃ / min to 600℃ and holding for 1 hour, followed by heating at a rate of 2℃ / min to 1600℃ and holding for 1 hour.

[0050] The HfO2-5 vol%BN-5 vol%Co composite ceramic has a relative density of 99%, a hardness of 30 GPa, and a fracture toughness of 8 MPa·m. 1 / 2 The grain size is 2μm, and the weight of the ceramic increases by 0.8wt% after heat treatment at 1500℃ for 1h.

[0051] The composite ceramic of this invention has a relative density >99%, a hardness of 30–45 GPa, and a fracture toughness of 8–15 MPa·m. 1 / 2 The ceramic grain size is 1-2 μm. The weight change rate of this composite ceramic after heat treatment at 1500-1800℃ for 1-4 hours is 0.2-0.8%. It has high toughness and high hardness and can be used in the preparation of high-temperature parts.

[0052] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.

Claims

1. A high-performance hafnium oxide-boron nitride composite ceramic, characterized in that, The hafnium oxide-boron nitride composite ceramic has a composition of HfO2-x vol% BN-y vol% Co-z vol% W, where 0<x≤15, 0<y≤15, 0<z≤15; the composite ceramic is prepared by first compression-molding a mixed powder of HfO2, Co, W and amorphous boron powder, then subjecting it to cold isostatic pressing at 100~200 MPa to form a green body, placing the green body in a tubular furnace filled with N2, heating up to 600~800°C for heat preservation, then heating up to 1400~1600°C for heat preservation; the composite ceramic has a relative density of >99%, a hardness of 30~45 GPa, and a fracture toughness of 8~15 MPa·m 1 / 2 , the ceramic grain size is 1~2 μm, and the weight change rate of the composite ceramic after heat treatment at 1500~1800°C for 1~4h is 0.2~0.8%; the purities of said HfO2, Co, W and amorphous boron powder are all above 99wt%, and the particle sizes of said HfO2, Co, W and amorphous boron powder are all 0.1~2µm; the molar ratio of said HfO2 to amorphous boron powder is (1~10):(1~10).

2. The method for preparing high-performance hafnium oxide-boron nitride composite ceramics according to claim 1, characterized in that, The specific steps include the following: S1. HfO2, Co, W and amorphous boron powder are added to solvent and ball milling media, mixed by ball milling and then dried to obtain a mixed powder; S2. After molding the mixed powder, cold isostatic pressing is performed at 100~200 MPa to obtain a green body; S3. Place the billet in a tube furnace and fill it with 1~10 m... 3 The temperature is increased to 600~800℃ and held for a period of time, then increased to 1400~1600℃ and held for a period of time to obtain HfO2-x vol% BN-y vol% Co-z vol% W composite ceramic.

3. The method for preparing high-performance hafnium oxide-boron nitride composite ceramics according to claim 2, characterized in that, The solvent mentioned in step S1 is one or more of ethanol, propanol, methanol or acetone.

4. The method for preparing high-performance hafnium oxide-boron nitride composite ceramics according to claim 2, characterized in that, The mixing time in step S1 is 10~24h, and the cold isostatic pressing time in step S2 is 5~15min.

5. The method for preparing high-performance hafnium oxide-boron nitride composite ceramics according to claim 2, characterized in that, In step S3, the heating rate to 600~800℃ is 5~10℃ / min, the heating rate to 1400~1600℃ is 2~5℃ / min, and the holding time is 0.5~2h.

6. The application of the high-performance hafnium oxide-boron nitride composite ceramic of claim 1 in the preparation of high-temperature components.

Citation Information

Patent Citations

  • Aluminium oxide, titanium carbide and silicon nitride composite reinforced zirconium boride-based multi-element nano-composite ceramic die

    CN104163630A

  • Aluminium nitride-based multi-element nano-composite ceramic die material and preparation method thereof

    CN104163632A

  • Superfine high-entropy solid solution powder as well as preparation method and application thereof

    CN109516812A