Flexible non-flammable fabric, its preparation method and application
By independently developing non-flammable fibers and specific spinning processes, we have solved the problems of complexity and poor spinnability in blending flame-retardant fabric fibers, and produced high-performance flexible non-flammable fabrics suitable for fireproof products and special industry clothing.
Patent Information
- Application Number
- CN202411567900.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-05
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-11-05
AI Technical Summary
Existing flame-retardant fabrics suffer from complex fiber blending processes and poor spinnability of carbon fibers, resulting in unstable flame-retardant effects and insufficient mechanical properties.
Using independently developed non-flammable fibers, flexible non-flammable fabrics are prepared through specific spinning processes and pretreatment solutions. Non-flammable fibers with high breaking elongation and high tensile strength are mixed with blended fibers to enhance the cohesion between fibers and antistatic properties.
The prepared flexible non-flammable fabric has a high limiting oxygen index, high temperature resistance, non-combustibility, non-melting and shrinkage, is lightweight and easy to clean, and is suitable for fireproof products and special industry clothing. Its performance is superior to similar products on the market.
Smart Images

Figure CN119243395B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of new materials technology, specifically relating to a flexible non-flammable fabric, its preparation method, and its application. Background Technology
[0002] Textiles are necessities in people's daily lives. As people's living standards improve, their demands for textile fabrics are also increasing. Textiles with special functions are becoming increasingly popular, such as those with magnetic shielding. Among these, flame retardancy is currently the most in-demand functional product on the market, along with flame retardancy, heat insulation, and antistatic properties. Therefore, flame-retardant fabrics have become a textile product with urgent demand in today's market. Currently, most common flame-retardant fabrics on the market are made of fibers such as polyester or aramid, which have a certain degree of flame retardancy, but they generally suffer from defects such as a rough and stiff feel, low strength, shrinkage upon exposure to fire, and carbonization starting at 370℃. Therefore, they still cannot meet the current market demand for flame-retardant fabrics.
[0003] Non-flammable fabrics are known as industrial wool. They are characterized by high temperature resistance, non-flammability, non-melting and shrinkage, non-dripping, corrosion resistance, and cut resistance. They can be widely used in industries such as fire protection, metallurgy, petroleum, electrical welding, and steel mills. They can be used in the development of products such as fire suits, fire blankets, special industry work clothes, curtains, bedding, military supplies, and seat covers. Currently, most non-flammable fabrics in the publicly available technologies are flame-retardant fabrics obtained by blending composite fibers. For example, patent publication number CN105105380B discloses an elastic flame-retardant composite fabric and its preparation method and application. It uses a flame-retardant adhesive to bond flame-retardant polyester fabric, flame-retardant heat-insulating elastic polyester roll, and flame-retardant non-woven fabric. However, the elasticity of the flame-retardant adhesive is poor. Once the fabric is stretched, the flame-retardant adhesive will crack or break, which can easily reduce the fire-retardant effect. Although blended flame-retardant fabrics can improve the flame retardancy of the fabric, since it is a blend of multiple fibers, it needs to go through spinning, weaving, and dyeing and finishing processes. These processes also greatly affect or even determine the flame retardancy, mechanical and wearability properties of the final fabric. For example, carbon fiber, which has flame retardancy, has high modulus, high strength, and high rigidity. However, the cohesion between fibers is poor, and the spinnability is poor, so spinning is very difficult. Summary of the Invention
[0004] In view of the problems existing in the prior art, the present invention aims to provide a flexible non-flammable fabric and its preparation method, which solves the defects of complex composite fiber blending process and poor spinnability of carbon fiber. The present invention uses independently developed non-flammable fibers and adopts a specific spinning process to prepare a non-flammable fabric with functions such as non-combustibility, non-melting and shrinkage, corrosion resistance, cut resistance and wear resistance, easy cleaning and non-deterioration.
[0005] To achieve the above objectives, the present invention provides the following technical solution: A flexible non-flammable fabric, wherein the fabric is made of non-flammable fibers and mixed fibers through ring spinning to form yarn, and the yarn is knitted by warp and weft knitting; the non-flammable fibers have a weight part of 70-100 parts, and the mixed fibers have a weight part of 0-30 parts.
[0006] This invention uses independently developed non-flammable fibers with a breaking elongation of over 24%, high tensile strength, and excellent fiber properties. The limiting oxygen index is over 45%, which can be used to process non-flammable fabrics. Furthermore, the pre-oxidized fiber prepared by this invention can be used to spin high-count yarns of 32-40 count, while traditional pre-oxidized fiber can only be spun into 21-count yarns.
[0007] Preferably, the non-flammable fiber is prepared by the following method: (1) Acrylonitrile, N-vinylamide monomers, isobutyl itaconic acid and initiator are mixed and polymerized, and then the mixture is filtered, demonomeric and defoamed to obtain polyacrylonitrile spinning solution. (2) After the polyacrylonitrile spinning solution is spun into polyacrylonitrile precursor fiber, the polyacrylonitrile precursor fiber is soaked in a 5% cobalt sulfate solution for 5-10 min, and then soaked in a pretreatment solution composed of a mixed aqueous solution of succinic acid and sodium lauroyl methyl taurate for 10-15 min. The soaked precursor fiber is pre-oxidized by gradient heating to obtain non-flammable fiber.
[0008] Preferably, the mixed fiber includes one or more of the following: methylene blue, aramid, metal fibers, and synthetic fibers. In addition to the above-mentioned fibers, the non-flammable fiber of the present invention can also be combined with other fiber materials (such as ceramic fibers). Depending on different needs, other fibers can be mixed into the non-flammable fiber to impart various functions to the fabric, such as improving the fabric's conductivity, shielding performance, elastic modulus, insulation, chemical corrosion resistance, and thermal insulation performance.
[0009] This invention also provides a method for preparing a flexible non-flammable fabric, comprising the following steps: (1) Pretreatment: Add non-combustible fiber and mixed fiber raw materials to the pretreatment solution according to the weight, purge with nitrogen, and cure in hydrothermal at 70-90℃ for 30-40 min; wherein the pretreatment solution includes polyether phosphate, modified multi-walled carbon nanotubes, surfactant, and ethanol aqueous solution; (2) Spinning: The fiber raw material pretreated in step (1) is processed into yarn through opening, carding, drawing, roving, spinning, coiling and twisting processes; (3) Weaving: The yarn produced in step (2) is woven to obtain the basic fabric; (4) Setting: The base fabric woven in step (3) is desized in water containing detergent at a temperature of 95°C for 40-70 minutes to remove the sizing on the fabric surface, and then dried on a setting machine at 90-115°C to obtain the flexible non-flammable fabric.
[0010] Preferably, the pretreatment liquid in step (1) is composed of the following raw materials in parts by weight: 10-20 parts of polyether phosphate, 2-10 parts of modified multi-walled carbon nanotubes, 1-5 parts of surfactant, and 65-87 parts of ethanol aqueous solution.
[0011] Preferably, the modified multi-walled carbon nanotubes are obtained by oxidizing multi-walled carbon nanotubes and then subjecting them to an acylation reaction; the acylation reaction involves reacting the oxidized multi-walled carbon nanotubes with thionyl chloride. The modified multi-walled carbon nanotubes have a larger specific surface area, and the acylation treatment can enhance the bonding ability of carbon nanotubes with other materials.
[0012] Preferably, the surfactant is a cationic surfactant or a nonionic surfactant. The cationic surfactant includes one or more of dodecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, and octadecyldimethylbenzylammonium chloride; the nonionic surfactant includes one or more of polyoxyethylene alkylamine and tetrabromobisphenol.
[0013] Preferably, the ethanol aqueous solution contains 50% ethanol by mass.
[0014] Preferably, the pretreatment solution is prepared by the following method: 10-20 parts by weight of polyether phosphate, 2-10 parts by weight of modified multi-walled carbon nanotubes, and 1-5 parts by weight of surfactant are mixed and heated to 50-80°C. Then, 65-87 parts by weight of ethanol aqueous solution are added, and the mixture is stirred and emulsified for 0.5-1 hour. The mixture is then cooled to room temperature and removed to obtain the pretreatment solution.
[0015] Preferably, the cleaning agent in step (4) is a soap.
[0016] The present invention also provides applications of the non-combustible fabric prepared by the above method, for use in fire suits, fire blankets, special protective clothing, seat covers for transportation vehicles, curtains and tablecloths in public places.
[0017] Compared with the prior art, the beneficial effects of the present invention are: This invention utilizes independently developed non-flammable fibers, which possess high tensile strength, elongation exceeding 24%, and limiting oxygen index exceeding 45%, exhibiting excellent non-flammability and spinnability. By pretreating the non-flammable fibers with an independently developed pretreatment liquid, static electricity between fibers is reduced, resulting in stronger cohesion. Improved spinning and weaving processes then produce fabrics with high strength, flexibility, and high breaking strength. The non-flammable fibers prepared by this invention can be used to spin 30-40 count high-count fabrics, while most similar fibers on the market can only be spun into 21 count yarns.
[0018] This invention relates to a self-developed pretreatment solution for non-flammable fibers, which is composed of polyether phosphate, modified multi-walled carbon nanotubes, surfactants, and an aqueous ethanol solution. By compounding and mixing polyether phosphate with antistatic properties and modified multi-walled carbon nanotubes, the strength of the fibers can be improved while enhancing antistatic performance. The addition of surfactants improves the compatibility of the compound system, allowing the antistatic polyether phosphate and multi-walled carbon nanotubes to interact, thereby enhancing the antistatic and mechanical properties of the non-flammable fibers in the pretreatment solution.
[0019] (3) The flexible non-combustible fabric prepared by the method of the present invention has the significant characteristics of non-combustibility, non-melting shrinkage and non-dripping. The carbonization temperature is as high as 640℃ and the maximum temperature resistance is as high as 1100℃. It can be used for a long time in an air environment of 500℃ and can be sustained for about 3 minutes at a high temperature of 800℃. Its performance is significantly higher than that of similar flame-retardant fabrics on the market. The limiting oxygen index is between 42-50%, which is 14-22% higher than that of similar flame-retardant products. It can be widely used in various fire protection products and places.
[0020] (4) The flexible non-flammable fabric prepared by the method of the present invention also has the advantages of light weight and high breaking strength. When blended with other fibers, its warp strength can reach 1100N, weft strength 1000N, tear strength greater than 100N, and good air permeability. It is easy to clean, does not deform, and can be used to make special industry clothing. Attached Figure Description
[0021] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0022] Figure 1 This is a photograph of the non-flammable fabric prepared in Example 3 of the present invention; Figure 2 This is a burn-through test result of the non-flammable fabric prepared in Example 3 of the present invention; Figure 3 These are images showing the burn-through resistance test results of commercially available non-flammable fabrics; Figure 4 This is an experimental diagram of the combustion process of the flame-retardant bag prepared using the non-flammable fabric of Example 3 of the present invention. Detailed Implementation
[0023] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. In the absence of conflict, the embodiments and features in the embodiments of the present invention can be combined with each other.
[0024] A flexible non-flammable fabric comprising at least the following raw materials in parts by weight: 70-100 parts of non-flammable fiber and 0-30 parts of mixed fiber.
[0025] As a preferred embodiment, the flexible non-flammable fabric of the present invention comprises the following raw materials in parts by weight: 70-90 parts of non-flammable fiber and 10-30 parts of mixed fiber.
[0026] As another preferred embodiment, the flexible non-flammable fabric of the present invention comprises the following raw materials in parts by weight: 70-90 parts of non-flammable fiber and 10-30 parts of aramid fiber.
[0027] As another preferred embodiment, the flexible non-flammable fabric of the present invention comprises the following raw materials in parts by weight: 70-90 parts of non-flammable fiber and 10-30 parts of methylene fiber.
[0028] As another preferred embodiment, the flexible non-flammable fabric of the present invention comprises the following raw materials in parts by weight: 70-90 parts of non-flammable fiber and 10-30 parts of metal fiber.
[0029] As another preferred embodiment, the flexible non-flammable fabric of the present invention comprises the following raw materials in parts by weight: 70-90 parts of non-flammable fiber and 10-30 parts of synthetic fiber.
[0030] As another preferred embodiment, the flexible non-flammable fabric of the present invention comprises the following raw materials in parts by weight: 70-90 parts of non-flammable fiber, 5-15 parts of methylene fiber, and 5-15 parts of aramid fiber.
[0031] As another preferred embodiment, the flexible non-flammable fabric of the present invention comprises the following raw materials in parts by weight: 70-90 parts of non-flammable fiber, 5-15 parts of aramid fiber, and 5-15 parts of metal fiber.
[0032] As another preferred embodiment, the flexible non-flammable fabric of the present invention comprises the following raw materials in parts by weight: 70-90 parts of non-flammable fiber, 5-15 parts of aramid fiber, and 5-15 parts of synthetic fiber.
[0033] As another preferred embodiment, the flexible non-flammable fabric of the present invention comprises the following raw materials in parts by weight: 70-90 parts of non-flammable fiber, 5-15 parts of metal fiber, and 5-15 parts of synthetic fiber.
[0034] As another preferred embodiment, the flexible non-flammable fabric of the present invention comprises the following raw materials in parts by weight: 70-90 parts of non-flammable fiber, 3-10 parts of methylene fiber, 4-10 parts of aramid fiber, and 3-10 parts of synthetic fiber.
[0035] As another preferred embodiment, the flexible non-flammable fabric of the present invention comprises the following raw materials in parts by weight: 70-90 parts of non-flammable fiber, 4-10 parts of aramid fiber, 3-10 parts of metal fiber, and 3-10 parts of synthetic fiber.
[0036] As another preferred embodiment, the flexible non-flammable fabric of the present invention comprises the following raw materials in parts by weight: 70-90 parts of non-flammable fiber, 3-10 parts of methylene fiber, 4-10 parts of aramid fiber, and 3-10 parts of metal fiber.
[0037] As another preferred embodiment, the flexible non-flammable fabric of the present invention comprises the following raw materials in parts by weight: 70-90 parts of non-flammable fiber, 4-10 parts of methylene fiber, 3-10 parts of metal fiber, and 3-10 parts of synthetic fiber.
[0038] It should be noted that the aramid fibers include, but are not limited to, aramid 1414 and aramid 1313. In this embodiment of the invention, aramid 1313 is selected.
[0039] It should be noted that the metal fibers include, but are not limited to, stainless steel fibers, copper fibers, and alloy fibers. In this embodiment of the invention, the metal fiber used is 316L stainless steel fiber.
[0040] It should be noted that the synthetic fibers include, but are not limited to, at least one of polyester fibers, polyolefin fibers, polyurethane elastic fibers, polyoxymethylene fibers, and phenolic fibers. The synthetic fiber selected in this embodiment of the invention is polyurethane elastic fiber.
[0041] The method for preparing the non-combustible fiber includes the following steps: (1) Acrylonitrile, N-vinylamide monomers, isobutyl itaconic acid and initiator are mixed and polymerized, and then the mixture is filtered, demonomeric and defoamed to obtain polyacrylonitrile spinning solution. (2) After the polyacrylonitrile spinning solution is spun into polyacrylonitrile precursor fiber, the polyacrylonitrile precursor fiber is soaked in a 5% cobalt sulfate solution for 5-10 min, and then soaked in a pretreatment solution composed of a mixed aqueous solution of succinic acid and sodium lauroyl methyl taurate for 10-15 min. The soaked precursor fiber is pre-oxidized by gradient heating to obtain non-flammable fiber.
[0042] In step (1) of the method for preparing non-flammable fiber, the N-vinylamide monomer is N-vinylacetamide, N,N'-vinylbisacrylamide, or N-ethylacrylamide.
[0043] A method for preparing a non-combustible fiber includes the following steps: (1) Preparation of polyacrylonitrile spinning solution: 98 parts of acrylonitrile, 0.6 parts of N-vinylacetamide, and 0.2 parts of isobutyl itaconic acid were dissolved in 380 parts of N,N-dimethylformamide. Then, 20 parts of benzoyl peroxide-N,N-diethylaniline were added and the temperature was raised. The remaining 1.0 parts of N-vinylacetamide and 0.2 parts of isobutyl itaconic acid were continuously added dropwise at 60°C. The addition was completed within 3 hours. The reaction was carried out at 65°C for 2 hours. Then, the temperature was raised to the second stage at 75°C at a heating rate of 0.1°C / min and the reaction was carried out for 12 hours to obtain polyacrylonitrile polymer. After filtration and demonolysis, polyacrylonitrile spinning solution was obtained. (2) Preparation of polyacrylonitrile precursor fibers: a. The polyacrylonitrile spinning solution is degassed under negative pressure and extruded from the spinneret. Polyacrylonitrile primary fibers are obtained by wet spinning. The spinneret orifice diameter is 0.07-0.08 mm. The coagulation bath is a 60% DMSO aqueous solution at a temperature of 55℃. b. Remove the solvent from the desalinated water obtained in step (1); after desalination, perform two-stage hot water stretching. The first stage hot water temperature is 60℃ and the stretching ratio is 1.4 times; the second stage hot water temperature is 90℃ and the stretching ratio is 1.6 times. c. After hot water drawing, the washed yarn is air-dried and then oiled in a silicone oil aqueous solution with a mass fraction of 0.65%. d. The oiled fibers are dried and densified at 152°C, and then subjected to high-pressure steam drawing at a steam pressure of 0.45 MPa and a drawing ratio of 4 times to obtain the polyacrylonitrile precursor fiber; (3) The polyacrylonitrile precursor fiber was immersed in a 5% cobalt sulfate solution for 8 minutes, and then immersed in a pretreatment solution for 12 minutes, wherein the mass concentration of succinic acid in the pretreatment solution was 0.3% and the mass concentration of sodium lauroyl methyl taurate was 1.3%; (4) Preparation of non-combustible fiber: The above polyacrylonitrile precursor fiber is placed in an oxidation furnace. The furnace temperature is raised from 25℃ to 200℃ in an air atmosphere at a rate of 3℃ / min and held for 10 min. Then the temperature is raised to 220℃ at a rate of 2℃ / min and held for 10 min. After that, the temperature is raised to 240℃ at a rate of 1℃ / min and held for 30 min. The fiber is then naturally cooled to room temperature to obtain non-combustible fiber 1#.
[0044] A method for preparing a non-combustible fiber includes the following steps: (1) Preparation of polyacrylonitrile spinning solution: 98 parts of acrylonitrile, 0.6 parts of N,N'-vinylbisacrylamide, and 0.2 parts of isobutyl itaconic acid were dissolved in 380 parts of N,N-dimethylformamide. Then, 20 parts of benzoyl peroxide-N,N-diethylaniline were added and the temperature was raised. The remaining 1.0 parts of N-vinylacetamide and 0.2 parts of isobutyl itaconic acid were continuously added dropwise at 60°C. The addition was completed within 3 hours. The reaction was carried out at 65°C for 2 hours. Then, the temperature was raised to the second stage at 75°C at a rate of 0.1°C / min and the reaction was carried out for 12 hours to obtain polyacrylonitrile polymer. After filtration and demonolysis, polyacrylonitrile spinning solution was obtained. (2) Preparation of polyacrylonitrile precursor fibers: a. The polyacrylonitrile spinning solution is degassed under negative pressure and extruded from the spinneret. Polyacrylonitrile primary fibers are obtained by wet spinning. The spinneret orifice diameter is 0.07-0.08 mm. The coagulation bath is a 60% DMSO aqueous solution at a temperature of 55℃. b. Remove the solvent from the desalinated water obtained in step (1); after desalination, perform two-stage hot water stretching. The first stage hot water temperature is 60℃ and the stretching ratio is 1.4 times; the second stage hot water temperature is 90℃ and the stretching ratio is 1.6 times. c. After hot water drawing, the washed yarn is air-dried and then oiled in a silicone oil aqueous solution with a mass fraction of 0.65%. d. The oiled fibers are dried and densified at 152°C, and then subjected to high-pressure steam drawing at a steam pressure of 0.45 MPa and a drawing ratio of 4 times to obtain the polyacrylonitrile precursor fiber; (3) The polyacrylonitrile precursor fiber was immersed in a 5% cobalt sulfate solution for 8 minutes, and then immersed in a pretreatment solution for 12 minutes, wherein the mass concentration of succinic acid in the pretreatment solution was 0.3% and the mass concentration of sodium lauroyl methyl taurate was 1.3%; (4) Preparation of non-combustible fiber: The above polyacrylonitrile precursor fiber is placed in an oxidation furnace. The furnace temperature is raised from 25℃ to 200℃ in an air atmosphere at a rate of 3℃ / min and held for 10 min. Then the temperature is raised to 220℃ at a rate of 2℃ / min and held for 10 min. After that, the temperature is raised to 240℃ at a rate of 1℃ / min and held for 30 min. The fiber is then naturally cooled to room temperature to obtain non-combustible fiber #2.
[0045] A method for preparing a non-combustible fiber includes the following steps: (1) Preparation of polyacrylonitrile spinning solution: 98 parts acrylonitrile, 0.6 parts N-ethylacrylamide, and 0.2 parts isobutyl itaconic acid were dissolved in 380 parts N,N-dimethylformamide, and then 20 parts benzoyl peroxide-N,N-diethylaniline were added and the temperature was raised. The remaining 1.0 parts N-vinylacetamide and 0.2 parts isobutyl itaconic acid were continuously added dropwise at 60°C. The addition was completed within 3 hours. The reaction was carried out at 65°C for 2 hours. Then the temperature was raised to the second stage at 75°C at a heating rate of 0.1°C / min and the reaction was carried out for 12 hours to obtain polyacrylonitrile polymer. After filtration and demonolysis, polyacrylonitrile spinning solution was obtained. (2) Preparation of polyacrylonitrile precursor fibers: a. The polyacrylonitrile spinning solution is degassed under negative pressure and extruded from the spinneret. Polyacrylonitrile primary fibers are obtained by wet spinning. The spinneret orifice diameter is 0.07-0.08 mm. The coagulation bath is a 60% DMSO aqueous solution at a temperature of 55℃. b. Remove the solvent from the desalinated water obtained in step (1); after desalination, perform two-stage hot water stretching. The first stage hot water temperature is 60℃ and the stretching ratio is 1.4 times; the second stage hot water temperature is 90℃ and the stretching ratio is 1.6 times. c. After hot water drawing, the washed yarn is air-dried and then oiled in a silicone oil aqueous solution with a mass fraction of 0.65%. d. The oiled fibers are dried and densified at 152°C, and then subjected to high-pressure steam drawing at a steam pressure of 0.45 MPa and a drawing ratio of 4 times to obtain the polyacrylonitrile precursor fiber; (3) The polyacrylonitrile precursor fiber was immersed in a 5% cobalt sulfate solution for 8 minutes, and then immersed in a pretreatment solution for 12 minutes, wherein the mass concentration of succinic acid in the pretreatment solution was 0.3% and the mass concentration of sodium lauroyl methyl taurate was 1.3%; (4) Preparation of non-combustible fiber: The above polyacrylonitrile precursor fiber is placed in an oxidation furnace. The furnace temperature is raised from 25°C to 200°C in an air atmosphere at a rate of 3°C / min and held for 10 min. Then the temperature is raised to 220°C at a rate of 2°C / min and held for 10 min. After that, the temperature is raised to 240°C at a rate of 1°C / min and held for 30 min. The fiber is then naturally cooled to room temperature to obtain non-combustible fiber #3.
[0046] The preparation method of the flexible non-flammable fabric of the present invention includes the following steps: (1) Pretreatment: Add non-combustible fiber and mixed fiber raw materials to the pretreatment solution according to the weight, purge with nitrogen, and cure in hydrothermal at 70-90℃ for 30-40 min; wherein the pretreatment solution includes polyether phosphate, modified multi-walled carbon nanotubes, surfactant, and ethanol aqueous solution; (2) Spinning: The fiber raw material pretreated in step (1) is processed into yarn through opening, carding, drawing, roving, spinning, coiling and twisting processes; (3) Weaving: The yarn produced in step (2) is woven to obtain the basic fabric; (4) Setting: The base fabric woven in step (3) is desized in water containing detergent at a temperature of 95°C for 40-70 minutes to remove the sizing on the fabric surface, and then dried on a setting machine at 90-115°C to obtain the flexible non-flammable fabric.
[0047] It should be noted that modified multi-walled carbon nanotubes are obtained by oxidizing multi-walled carbon nanotubes and then subjecting them to an acyl chloride reaction with thionyl chloride.
[0048] It should be noted that the surfactant is a cationic surfactant or a nonionic surfactant. The cationic surfactant includes one or more of dodecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, and octadecyldimethylbenzylammonium chloride; the nonionic surfactant includes one or more of polyoxyethylene alkylamine and tetrabromobisphenol.
[0049] It should be noted that the specific process of spinning in step (2) is as follows: Cleaning: After the pre-treated fiber raw materials are manually sorted, they are put into a bale grabber with a bale grabber speed of 960 r / min, a beater speed of 800 r / min, a fan speed of 950 r / min, a cotton lap dry weight of 320 g / m, and a cotton lap length of 27 m. Carding: Carding is produced on a carding machine with a carding roller speed of 300 r / min and a carding sliver output speed of 100-140 m / min. The fiber sliver obtained after carding has strong parallelism and mixing uniformity. Drawing: Two or more carded fiber slivers are drawn together in two stages, with a trumpet opening of 3.3mm. The fiber slivers are placed on a first drawing frame, passing through guide hooks, guide frames, and concave and convex rollers, and drawn together to obtain a first-stage fiber drawing sliver. The output speed of the first drawing frame is 250-450m / min, the roller spacing is 9*17mm, and the back zone draft is 1.7 times. Two or more first-stage fiber slivers are placed on a second drawing frame, passing through guide hooks, guide frames, and concave and convex rollers, and drawn together to obtain a second-stage fiber drawing sliver. The output speed of the second drawing frame is 250-450m / min, the roller spacing is 15*20mm, and the back zone draft is 1.6 times. Roving: The fiber sliver prepared above is placed on a roving frame, and after passing through the guide frame and the drafting zone rollers, it is drafted and twisted to obtain roving; the spindle speed is 750-900 r / min, the twist is 350 twists / m, the roller spacing is 25*33 mm, the back zone draft is 1.26 times, and the nip spacing is 6.5 mm; Fine yarn: The roving is then placed on the fine spinning machine and drafted and twisted into bobbin yarn through the yarn drying rod, trumpet mouth, drafting roller and guide hook; in the fine spinning machine, the spindle speed is 1200-1600m / min, the twist is 950 twists / m, the total draft ratio is 30.2 times, and the back zone draft is 1.3 times; Bundling: The obtained fine tube yarn is increased in package weight by a winding machine, and the yarn quality is detected by an electronic yarn clearer, removing unqualified yarns to finally obtain packaged single yarns; two single yarns are wound side by side to form a bundled yarn bobbin, ensuring that the tension on both sides is consistent; while ensuring good bobbin formation, the yarn tension should be as low as possible to protect the elasticity and strength of the original yarn, producing 30-40 count bundled yarns; the winding speed is 900-1300m / min, the tension value is 5-8, and the yarn drawing speed is 750-1250m / min; Twisted yarn: Two strands are twisted together to form a ply with a twist of 1050 twists / m and a double twist linear density of 18 tex. The resulting ply is the non-flammable fiber ring-spun yarn.
[0050] It should be noted that the cleaning agent is a soap-based detergent.
[0051] Example 1 A method for preparing a flexible, non-combustible fabric includes the following steps: (1) Pretreatment: 100 parts by weight of non-combustible fiber 1# is added to the pretreatment solution, nitrogen is introduced, and it is cured in hydrothermal at 70°C for 40 min; wherein the pretreatment solution is prepared by the following method: 10 parts by weight of polyether phosphate, 2 parts by weight of modified multi-walled carbon nanotubes, and 1 part by weight of dodecyltrimethylammonium chloride are mixed and heated to 50°C, then 87 parts by weight of ethanol aqueous solution are added, stirred and emulsified for 1 hour, and then cooled to room temperature and taken out as the pretreatment solution; (2) Spinning: The fiber raw material pretreated in step (1) is processed into yarn through opening, carding, drawing, roving, spinning, coiling and twisting processes; (3) Weaving: The yarn produced in step (2) is woven to obtain the basic fabric; (4) Setting: The base fabric woven in step (3) is desized in soaping agent at 95°C for 40 minutes to remove the sizing on the fabric surface, and then dried on a setting machine at 90°C to obtain a flexible non-flammable fabric.
[0052] Example 2 A method for preparing a flexible, non-combustible fabric includes the following steps: (1) Pretreatment: 100 parts by weight of non-combustible fiber 1# is added to the pretreatment solution, nitrogen is introduced, and it is cured in hydrothermal at 90°C for 30 min; wherein the pretreatment solution is prepared by the following method: 20 parts by weight of polyether phosphate, 10 parts by weight of modified multi-walled carbon nanotubes, and 5 parts by weight of polyoxyethylene alkylamine are mixed and heated to 80°C, then 65 parts by weight of ethanol aqueous solution are added, stirred and emulsified for 0.5 hours, and then cooled to room temperature to take out the pretreatment solution; (2) Spinning: The fiber raw material pretreated in step (1) is processed into yarn through opening, carding, drawing, roving, spinning, coiling and twisting processes; (3) Weaving: The yarn produced in step (2) is woven to obtain the basic fabric; (4) Setting: The base fabric woven in step (3) is desized in a soaping agent at a temperature of 95°C for 70 minutes to remove the sizing on the fabric surface. Then it is dried on a setting machine at 115°C to obtain a flexible non-flammable fabric.
[0053] Example 3 A method for preparing a flexible, non-combustible fabric includes the following steps: (1) Pretreatment: 100 parts by weight of non-combustible fiber 1# is added to the pretreatment solution, nitrogen is introduced, and it is cured in hydrothermal at 80°C for 40 min; wherein the pretreatment solution is prepared by the following method: 17 parts by weight of polyether phosphate, 7 parts by weight of modified multi-walled carbon nanotubes, and 4 parts by weight of hexadecyltrimethylammonium bromide are mixed and heated to 72°C, then 72 parts by weight of ethanol aqueous solution is added, and the mixture is stirred and emulsified for 0.6 hours, and then cooled to room temperature to take out the pretreatment solution; (2) Spinning: The fiber raw material pretreated in step (1) is processed into yarn through opening, carding, drawing, roving, spinning, coiling and twisting processes; (3) Weaving: The yarn produced in step (2) is woven to obtain the basic fabric; (4) Setting: The base fabric woven in step (3) is desized in a soaping agent at a temperature of 95°C for 65 minutes to remove the sizing on the fabric surface. Then it is dried on a setting machine at 110°C to obtain a flexible non-flammable fabric.
[0054] Example 4 A method for preparing a flexible, non-combustible fabric includes the following steps: Compared with Example 3, the non-flammable fiber 1# in Example 3 was replaced with non-flammable fiber 2#, and the remaining method steps were the same as those in Example 3, to prepare a flexible non-flammable fabric.
[0055] Example 5 A method for preparing a flexible, non-combustible fabric includes the following steps: Compared with Example 3, the non-flammable fiber 1# in Example 3 was replaced with non-flammable fiber 3#, and the remaining method steps were the same as those in Example 3, to prepare a flexible non-flammable fabric.
[0056] Example 6 Compared with Example 3, 100 parts by weight of non-flammable fiber 1# in Example 3 were replaced with 80 parts by weight of non-flammable fiber 1# and 20 parts by weight of aramid 1313 fiber. The remaining method steps were the same as those in Example 3, and a flexible non-flammable fabric was prepared.
[0057] Example 7 Compared with Example 3, 100 parts by weight of non-flammable fiber 1# in Example 3 were replaced with 80 parts by weight of non-flammable fiber 1# and 20 parts by weight of nylon fiber. The remaining method steps were the same as those in Example 3, and a flexible non-flammable fabric was prepared.
[0058] Example 8 Compared with Example 3, 100 parts by weight of non-combustible fiber 1# in Example 3 were replaced with 92 parts by weight of non-combustible fiber 1# and 8 parts by weight of 316L stainless steel fiber. The remaining method steps were the same as those in Example 3, and a flexible non-combustible fabric was prepared.
[0059] Example 9 Compared with Example 3, 100 parts by weight of non-combustible fiber 1# in Example 3 were replaced with 80 parts by weight of non-combustible fiber 1# and 20 parts by weight of polyurethane elastic fiber. The remaining method steps were the same as those in Example 3, and a flexible non-combustible fabric was prepared.
[0060] Example 10 Compared with Example 3, 100 parts by weight of non-flammable fiber 1# in Example 3 were replaced with 80 parts by weight of non-flammable fiber 1#, 10 parts by weight of aramid 1313 fiber and 10 parts by weight of nylon fiber. The remaining method steps were the same as those in Example 3, and a flexible non-flammable fabric was prepared.
[0061] Example 11 Compared with Example 3, 100 parts by weight of non-combustible fiber 1# in Example 3 were replaced with 80 parts by weight of non-combustible fiber 1#, 6 parts by weight of nylon fiber, 8 parts by weight of aramid 1313 fiber, and 6 parts by weight of 316L stainless steel fiber. The remaining method steps were the same as those in Example 3, and a flexible non-combustible fabric was prepared.
[0062] Comparative Example 1 Compared with Example 3, all 100 parts by weight of non-flammable fiber 1# in Example 3 were replaced with aramid 1313 fiber, and the remaining method steps were the same as those in Example 3, and a non-flammable fabric was prepared.
[0063] Comparative Example 2 Compared with Example 6, 80 parts by weight of non-flammable fiber 1# in Example 6 were replaced with aramid 1313 fiber, and 20 parts by weight of aramid 1313 fiber were replaced with non-flammable fiber 1#. The remaining method steps were the same as those in Example 6, and a non-flammable fabric was prepared.
[0064] Comparative Example 3 Compared with Example 7, 80 parts by weight of non-flammable fiber 1# in Example 7 were replaced with aramid 1313 fiber, and the remaining method steps were the same as those in Example 7, and a non-flammable fabric was prepared.
[0065] Comparative Example 4 Compared with Example 10, 80 parts by weight of non-flammable fiber 1# in Example 10 were replaced with aramid fiber, and 10 parts by weight of aramid 1313 fiber were replaced with non-flammable fiber 1#. The remaining method steps were the same as those in Example 10, and a non-flammable fabric was prepared.
[0066] Comparative Example 5 Compared with Example 11, 80 parts by weight of non-flammable fiber 1# in Example 11 were replaced with aramid fiber, and 8 parts by weight of aramid 1313 fiber were replaced with non-flammable fiber 1#. The remaining method steps were the same as those in Example 11, and a non-flammable fabric was prepared.
[0067] Comparative Example 6 Compared with Example 3, in Comparative Example 11, the pretreatment liquid was replaced with an aqueous ethanol solution in the pretreatment step, while the remaining method steps were the same as those in Example 3, and a non-flammable fabric was prepared.
[0068] Comparative Example 7 Compared with Example 3, in Comparative Example 11, 7 parts by weight of modified multi-walled carbon nanotubes in the pretreatment solution were completely replaced with polyether phosphate in the pretreatment step, and the remaining method steps were the same as those in Example 3, and a non-flammable fabric was prepared.
[0069] Comparative Example 8 Compared with Example 3, in Comparative Example 11, 4 parts by weight of hexadecyltrimethylammonium bromide in the pretreatment solution were replaced with modified multi-walled carbon nanotubes in the pretreatment step, and the remaining method steps were the same as those in Example 3, and a non-flammable fabric was prepared.
[0070] Comparative Example 9 Compared with Example 3, in Comparative Example 11, 17 parts by weight of polyether phosphate in the pretreatment solution were replaced with modified multi-walled carbon nanotubes in the pretreatment step, and the remaining method steps were the same as those in Example 3, and a non-flammable fabric was prepared.
[0071] Experimental Analysis Example 1 The non-flammable fabrics prepared in Examples 1-11 and Comparative Examples 1-9 were subjected to performance tests. Their flammability, antistatic properties, and strength were measured respectively. The test results are shown in Table 1.
[0072] Combustion performance testing is conducted according to GB 8624-2012 "Classification of Combustion Performance of Building Materials and Products", which includes testing the limiting oxygen index and vertical combustion performance (including afterflame time, smoldering time, damage length, and combustion drips). The strength was determined according to GB / T 3923.1-2013 "Textiles - Tensile Properties of Fabrics - Part 1: Determination of Breaking Strength and Elongation at Break" by conducting warp and weft breaking strength tests respectively. The antistatic performance is tested according to GB 12014-2019 "Appendix A of Protective Clothing - Static Electricity" to assess the antistatic performance of the fabric.
[0073] As shown in Table 1, the non-flammable fabric prepared by this invention exhibits excellent combustion performance, with a limiting oxygen index exceeding 45%, and strong tensile strength and antistatic properties. Comparative Examples 1-5 show that the non-flammable fabric prepared using the independently developed flame-retardant fiber of this invention outperforms the commonly used flame-retardant fiber, aramid 1313, in both combustion performance and tensile strength. Furthermore, Comparative Examples 2-5 demonstrate that the independently developed flame-retardant fiber can be blended with other commercially available fibers to prepare non-flammable fabrics. Depending on the specific needs of different scenarios, different fibers can be selected for blending to further improve certain properties of the fabric. Antistatic test data shows that the non-flammable fabric prepared by this invention has lower surface resistance and better antistatic performance. Comparative Examples 6-9 show that using the independently developed pretreatment method significantly enhances the antistatic performance of the prepared fabric. The synergistic effect of several components in the pretreatment process enhances the antistatic effect; the absence of any component significantly impacts the antistatic effect.
[0074]
[0075] Example 2 The inventors conducted burn-through tests on the non-combustible fabrics prepared above, using the non-combustible fabric prepared in Example 3 of this invention (experimental example) and a commercially available (alumina) non-combustible fabric (comparative example) for burn-through tests; (See attached) Figure 2-3 These are test experiments conducted by the inventor in the laboratory. The results show that the non-flammable fabric prepared using the method of this invention has strong burn-through resistance. The comparison chart shows that commercially available non-flammable fabrics exhibit large-area burn-through (see attached image). Figure 3Furthermore, the non-flammable fabric of this invention only develops small cracks even after prolonged burning (see appendix). Figure 2 This further proves that the non-combustible fabric prepared by this invention has high non-combustible properties. Simultaneously, the inventors processed the non-combustible fabric prepared in Example 3 into flame-retardant bags and tested the flame-retardant effect of the bags in the laboratory. The inventors filled the flame-retardant bags with wood, then poured in diesel fuel and ignited them, observing the combustion of the bags in the field combustion experiment. Figure 4 It can be seen that the non-flammable fabric prepared by the present invention has the significant characteristics of not burning, not melting and shrinking, and not dripping. According to the combustion data test, the carbonization temperature of the non-flammable fabric of the present invention is as high as 640℃, which has a significant non-flammable effect.
[0076] In summary, this invention utilizes independently developed flame-retardant fibers to spin and prepare non-flammable fabrics, exhibiting significant characteristics of non-combustibility, non-melting shrinkage, and non-dripping. It boasts a carbonization temperature as high as 640℃, a maximum temperature resistance of 1100℃, and a limiting oxygen index between 42-50%, allowing for long-term use in air environments at 500℃. Its performance is significantly superior to similar flame-retardant fabrics currently on the market. Furthermore, it possesses advantages such as light weight and high tensile strength, with a warp strength reaching 1100N, a weft strength of 1000N, and a tear strength greater than 100N. It also exhibits good breathability, is easy to clean, and does not deform, making it suitable for applications such as fire suits, fire blankets, special protective clothing, seat covers for transportation vehicles, curtains in public places, and tablecloths.
[0077] The above description is merely a preferred embodiment of the present invention and is not intended to limit the scope of protection of the present invention.
Claims
1. A flexible, non-flammable fabric, characterized in that, The fabric is made of non-flammable fiber and mixed fiber through ring spinning to form yarn, and the yarn is knitted by warp and weft; the weight of the non-flammable fiber is 70-100 parts, and the weight of the mixed fiber is 0-30 parts; wherein the non-flammable fiber is prepared by the following method: (1) acrylonitrile, N-vinylamide monomer, isobutyl itaconic acid and initiator are mixed and polymerized, and then filtered, de-monomeric and defoamed to obtain polyacrylonitrile spinning solution; (2) polyacrylonitrile spinning solution is spun to obtain polyacrylonitrile precursor fiber, the polyacrylonitrile precursor fiber is soaked in a 5% cobalt sulfate solution for 5-10 min, and then soaked in a first pretreatment solution composed of a mixed aqueous solution of succinic acid and sodium lauroyl methyl taurate for 10-15 min, and the soaked precursor fiber is pre-oxidized by gradient heating to obtain non-flammable fiber.
2. The flexible non-flammable fabric according to claim 1, characterized in that, The mixed fiber includes one or a mixture of two of metal fibers and synthetic fibers; the synthetic fiber includes any one of methylene fiber and aramid fiber.
3. A method for preparing the flexible non-flammable fabric according to any one of claims 1-2, characterized in that, Includes the following steps: (1) Pretreatment: Add non-combustible fiber and mixed fiber raw materials to the second pretreatment liquid according to the weight, purge with nitrogen, and cure in hot water at 70-90℃ for 30-40 min; wherein the second pretreatment liquid includes polyether phosphate, modified multi-walled carbon nanotubes, surfactant and ethanol aqueous solution; (2) Spinning: The fiber raw material pretreated in step (1) is processed into yarn through opening, carding, drawing, roving, spinning, winding and twisting processes; (3) Weaving: The yarn produced in step (2) is woven to obtain the basic fabric; (4) Setting: The base fabric woven in step (3) is desized in water containing detergent at a temperature of 95°C for 40-70 minutes to remove the sizing on the fabric surface, and then dried on a setting machine at 90-115°C to obtain the flexible non-flammable fabric.
4. The method for preparing the flexible non-flammable fabric according to claim 3, characterized in that, Step (1) The second pretreatment liquid is composed of the following raw materials in parts by weight: 10-20 parts of polyether phosphate, 2-10 parts of modified multi-walled carbon nanotubes, 1-5 parts of surfactant, and 65-87 parts of ethanol aqueous solution.
5. The method for preparing the flexible non-flammable fabric according to claim 4, characterized in that, The modified multi-walled carbon nanotubes are obtained by oxidizing multi-walled carbon nanotubes and then subjecting them to an acyl chloride reaction.
6. The method for preparing the flexible non-flammable fabric according to claim 4, characterized in that, The surfactant is a cationic surfactant or a nonionic surfactant. The cationic surfactant includes one or more of dodecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, and octadecyldimethylbenzylammonium chloride. The nonionic surfactant is a polyoxyethylene alkylamine.
7. The method for preparing the flexible non-flammable fabric according to claim 3, characterized in that, The ethanol aqueous solution contains 50% ethanol by mass.
8. The method for preparing the flexible non-flammable fabric according to claim 3, characterized in that, The cleaning agent mentioned in step (4) is a soap detergent.
9. The application of the non-flammable fabric prepared by the method for preparing the flexible non-flammable fabric according to claim 3, characterized in that, The fabric is used in fire blankets, special protective clothing, seat covers for transportation vehicles, curtains in public places, and tablecloths in public places.
Citation Information
Patent Citations
A kind of elastic flame-retardant composite fabric and its preparation method and application
CN105105380B
Noncombustible fabric and protective garment thereof
CN201817647U