Gas barrier laminate

By optimizing the composition and structure of the gas barrier laminate and controlling the proportions of Zn, N, PO₂⁻, and PO₃⁻, the problem of decreased barrier performance of existing materials after cooking has been solved, achieving a balance between high gas barrier efficiency and productivity, making it suitable for packaging cooked foods.

CN119255911BActive Publication Date: 2026-11-20RM TOHCELLO CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202280094677.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-12
Publication Date
2026-11-20
Estimated Expiration
2042-04-12

Smart Images

  • Figure CN119255911B_ABST
    Figure CN119255911B_ABST
Patent Text Reader

Abstract

A gas barrier laminate having a substrate layer, a gas barrier layer provided on at least one surface of the substrate layer, and an inorganic layer provided between the substrate layer and the gas barrier layer, wherein a composition ratio of Zn measured by X-ray photoelectron spectroscopy of the gas barrier layer is 1 to 10 atomic%, and when a mass peak intensity of C3H3O2 measured by time-of-flight secondary ion mass spectrometry of the gas barrier layer is set as I(C3H3O2), a value of I(ZnPO4H) / I(C3H3O2) is 6 x 10-2 or more. 64 ZnPO4H ‑ 64 ZnPO4H ‑ ) and a mass peak intensity of C3H3O2 ‑ ‑ 64 ZnPO4H ‑ ) and a mass peak intensity of C3H3O2 ‑ ‑4 ‑2 A value of I(CN) / I(C3H3O2) is greater than 0 and 2 or less when a mass peak intensity of CN measured by time-of-flight secondary ion mass spectrometry of the gas barrier layer is set as ‑ ‑ ‑ ‑ CN​​​​​​​​
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to gas barrier laminates and related technologies. Background Technology

[0002] Typically, as a gas barrier material against water vapor or oxygen, a laminate is used, which is a laminate obtained by setting an inorganic layer with gas barrier properties on a substrate layer.

[0003] However, the inorganic layer cannot withstand friction and other factors. Such gas barrier laminates have the following problems: during post-processing printing, lamination, or filling of contents, cracks may occur on the inorganic layer due to friction and stretching, resulting in a reduction in gas barrier properties.

[0004] Therefore, as a gas barrier layer, for example, Patent Document 1 (International Publication No. 2016 / 017544) discloses a coating material for gas barrier, which includes a polycarboxylic acid, a polyamine compound, a polyvalent metal compound and a base, wherein (the number of moles of -COO- groups contained in the polycarboxylic acid) / (the number of moles of amino groups contained in the polyamine compound) = 100 / 20 to 100 / 90.

[0005] Patent document 1 discloses that if such a gas barrier coating material is used, a gas barrier film and its laminate with good gas barrier properties, especially oxygen barrier properties, can be provided under both low humidity and high humidity conditions.

[0006] Furthermore, Patent Document 2 (International Publication No. 03 / 091317) discloses a membrane made from a polycarboxylic acid (A) and a polyvalent metal compound (B), wherein the peak ratio of the infrared absorption spectrum of this membrane (A) is... 1560 / A 1700 The value is above 0.25.

[0007] Patent document 2 discloses the following: If such a membrane is obtained, it can have excellent gas barrier properties such as oxygen even in a high humidity atmosphere, water resistance (the appearance, shape and gas barrier properties will not be damaged by the influence of neutral water, high temperature water vapor and hot water), and be easily soluble in acids and / or alkalis.

[0008] Furthermore, Patent Document 3 (International Publication No. 2016 / 088534) discloses a gas-barrier polymer, which is formed by heating a mixture containing polycarboxylic acids and polyamine compounds. In the infrared absorption spectrum of this gas-barrier polymer, at a wavelength of 1493 cm⁻¹... -1 The above 1780cm -1 Let the total peak area within the following absorption band range be A, and let 1598 cm⁻¹ be used. -1 The above 1690cm-1 When the total peak area within the following absorption band range is set as B, the area ratio of the amide bond represented by B / A is 0.370 or higher.

[0009] Patent document 3 discloses a gas barrier polymer that can achieve excellent gas barrier performance under both high humidity and boiling / cooking conditions, as well as excellent balance in appearance, dimensional stability, and productivity in gas barrier films and gas barrier laminates.

[0010] In addition, as prior art concerning gas barrier materials, the following patent documents 4 to 6 can be cited.

[0011] Existing technical documents

[0012] Patent documents

[0013] Patent Document 1: International Publication No. 2016 / 017544

[0014] Patent Document 2: International Publication No. 03 / 091317

[0015] Patent Document 3: International Publication No. 2016 / 088534

[0016] Patent Document 4: Japanese Patent Application Publication No. 2005-225940

[0017] Patent Document 5: Japanese Patent Application Publication No. 2013-10857

[0018] Patent Document 6: International Publication No. 2011 / 122036 Summary of the Invention

[0019] The problem that the invention aims to solve

[0020] The technical requirements for various properties of gas barrier materials are gradually increasing.

[0021] Based on the inventors' insights and preliminary research, for example, regarding existing gas barrier materials as described in Patent Documents 1 to 3, there are the following issues.

[0022] Gas barrier materials, as described in Patent Document 1 or 2, which are formed from a system containing polycarboxylic acids and polyvalent metal compounds, suffer from deterioration in barrier performance after cooking due to their double-layer laminated structure.

[0023] Furthermore, the gas barrier material described in Patent Document 3, which is formed from a system containing polycarboxylic acids and polyamine compounds, suffers from deterioration in barrier performance after cooking due to its three-layer laminated structure.

[0024] As stated above, the inventors of this application have discovered that existing gas barrier materials as described in Patent Documents 1 to 3 suffer from deterioration in barrier performance after cooking due to their laminated structure.

[0025] That is, the inventors of this application have found that, based on the viewpoint of barrier properties after cooking, there is room for improvement in existing gas barrier materials.

[0026] The present invention was made in view of the above circumstances. One object of the present invention is to provide a barrier laminate that can be used as a barrier membrane with good barrier properties after cooking, such as water vapor permeability in a double-layer laminated structure.

[0027] (The purpose of this invention is particularly relevant to the first invention described later.)

[0028] In gas barrier materials, there is a need to further improve the barrier properties against gases such as water vapor. For example, in the manufacture of cooked foods, which involves heating the food after packaging it with a gas barrier material, it is required that good barrier properties be maintained even after the cooking process.

[0029] One of the objectives of this invention is to provide a gas barrier material with improved barrier properties for gases such as water vapor.

[0030] (The purpose of this invention is particularly relevant to the second invention described later.)

[0031] According to the inventors of this application, existing gas barrier materials as described in Patent Documents 1 to 3 suffer from deterioration of barrier performance after cooking due to their laminated structure.

[0032] One of the objectives of this invention is to provide a barrier laminate that, regardless of its lamination structure, can be used as a barrier film with good barrier properties after cooking.

[0033] (The purpose of this invention is particularly relevant to the third invention described later.)

[0034] According to the inventors of this application, there is still room for improvement in gas barrier materials, based on the viewpoint of achieving a good balance between productivity and barrier properties. Although many technologies have been developed to improve barrier performance, no technology has been reported to achieve a good balance between barrier properties and productivity.

[0035] One of the objectives of this invention is to provide a gas barrier material that offers an excellent balance between productivity and barrier properties and can provide ideal barrier properties in various layered structures.

[0036] (The purpose of this invention is particularly relevant to the fourth invention described later.)

[0037] The technical requirements for various properties of gas barrier materials are gradually increasing. According to the inventors of this application, for gas barrier materials as described in Patent Documents 4 and 5, long-term heating at high temperatures is required to crosslink polycarboxylic acids and polyamines, which sometimes reduces productivity.

[0038] Furthermore, if the heat treatment time for crosslinking polycarboxylic acids and polyamines is shortened in order to improve the productivity of such gas barrier materials, the proportion of amide bonds formed by crosslinking polycarboxylic acids and polyamines becomes lower, and sometimes the barrier properties decrease.

[0039] Therefore, the inventors of this application have discovered that existing gas barrier materials have room for improvement based on the viewpoint of achieving a good balance between productivity and barrier properties. Although many technologies have been developed to improve barrier performance, no technology has been reported to achieve a good balance between barrier properties and productivity.

[0040] One of the objectives of this invention is to provide a gas barrier material that offers an excellent balance between productivity and barrier properties.

[0041] (The purpose of this invention is particularly relevant to the fifth invention described later.)

[0042] Methods for solving problems

[0043] The inventors of this application have conducted repeated and in-depth research to achieve at least one of the aforementioned issues. As a result, it was discovered that the following laminate exhibits good barrier properties after cooking treatment. This laminate is a gas-barrier laminate having a gas-barrier layer in which the intensity ratio of a specific peak from Zn is within a certain range, as observed by, for example, X-ray photoelectron spectroscopy (XPS) analysis, is within a specific compositional ratio range, and by time-of-flight secondary ion mass spectrometry (TOF-SIMS) analysis, is within a specific range. Furthermore, the laminate also has a gas-barrier layer in which the intensity ratio of a specific peak from N is within a specific range, as observed by XPS analysis, is within a specific compositional ratio, and by TOF-SIMS analysis, is within a specific range. Moreover, the following first invention was completed.

[0044] In addition, the inventors of this application have completed the following second, third, fourth and fifth inventions.

[0045] [First Invention] 1.

[0047] A gas barrier laminate comprising a substrate layer, a gas barrier layer disposed on at least one side of the substrate layer, and an inorganic layer disposed between the substrate layer and the gas barrier layer.

[0048] The Zn composition, determined by X-ray photoelectron spectroscopy analysis of the aforementioned gas barrier layer, is 1–10 atomic%.

[0049] The data were determined by time-of-flight secondary ion mass spectrometry analysis of the aforementioned gas barrier layer. 64 ZnPO4H - Let the mass peak intensity be I( 64 ZnPO4H - ) and C3H3O2 - The mass peak intensity is set as I(C3H3O2) - )hour,

[0050] I( 64 ZnPO4H - ) / I(C3H3O2 - The value of ) is 6 × 10 -4 Above 5×10 -2 the following,

[0051] The composition ratio of N, as determined by X-ray photoelectron spectroscopy analysis of the aforementioned gas barrier layer, is greater than 0 atomic% and less than 12 atomic%.

[0052] The CN was determined by time-of-flight secondary ion mass spectrometry analysis of the aforementioned gas barrier layer. - The mass peak intensity is set as I(CN) - )hour,

[0053] I(CN - ) / I(C3H3O2 - The value of ) is greater than 0 and less than 2. 2.

[0055] As described in 1, in the gas barrier laminate, wherein the PO2 content, as determined by the aforementioned time-of-flight secondary ion mass spectrometry analysis of the aforementioned gas barrier layer, is... - Let the mass peak intensity be I(PO2) - ) and PO3 - The mass peak intensity is set as I(PO3) - )hour,

[0056] (I(PO2 - )+I(PO3 - )) / I(C3H3O2 - The value is above 0.02 and below 5. 3.

[0058] As described in 1 or 2, the gas barrier laminate, wherein the aforementioned I(PO2) - ) and the aforementioned I(PO3) -The strength ratio of I(PO2) - ) / I(PO3 - The value is above 0.05 and below 1. 4.

[0060] The gas barrier laminate as described in any one of 1 to 3, wherein the aforementioned gas barrier layer is composed of a cured material comprising at least a polycarboxylic acid, Zn, and a phosphorus compound or its salt containing one or more -P-OH groups. 5.

[0062] As described in 4, in the gas barrier laminate, the concentration of P atoms of the aforementioned phosphorus compound or its salt in the aforementioned mixture is 5 × 10⁻⁶ per mol of the aforementioned polycarboxylic acid. -4 Above 0.3 mol and below 0.3 mol. 6.

[0064] Gas barrier laminates as described in 4 or 5, wherein the aforementioned mixture further comprises polyamines. 7.

[0066] As described in 6, the gas barrier laminate is a polyamine, which is polyethyleneimine. 8.

[0068] The gas barrier laminate as described in any one of 4 to 7, wherein the aforementioned polycarboxylic acid comprises one or more polymers selected from the group consisting of polyacrylic acid, polymethacrylic acid, and copolymers of acrylic acid and methacrylic acid. 9.

[0070] The gas barrier laminate as described in any one of 1 to 8, wherein the thickness of the aforementioned gas barrier layer is 0.05 μm or more and 10 μm or less.

[0071] [Second Invention] 1.

[0073] A gas barrier laminate comprising a substrate layer, a gas barrier layer disposed on at least one side of the substrate layer, and an inorganic layer disposed between the substrate layer and the gas barrier layer.

[0074] When time-of-flight secondary ion mass spectrometry analysis was performed on the aforementioned gas barrier layer, PO2 - Let the mass peak intensity be I(PO2) - ), PO3 - The mass peak intensity is set as I(PO3) - ) and C3H3O2 - The mass peak intensity is set as I(C3H3O2) -When ), {I(PO2) - )+I(PO3 - )} / I(C3H3O2 - The value of ) is 0.02 to 5.

[0075] The aforementioned gas barrier layer contains one or more metallic elements selected from the group consisting of Zn, Ca, Mg, Ba and Al, and the composition ratio of the aforementioned metallic elements in the aforementioned gas barrier layer, as determined by X-ray photoelectron spectroscopy analysis, is 1 to 15 atoms. 2.

[0077] As described in 1, in the gas barrier laminate, wherein, when the aforementioned gas barrier layer is subjected to time-of-flight secondary ion mass spectrometry analysis, CN - The mass peak intensity is set as I(CN) - ) and C3H3O2 - The mass peak intensity is set as I(C3H3O2) - When I(CN) - ) / I(C3H3O2 - The value of ) is less than 2. 3.

[0079] As described in 1 or 2, in the gas barrier laminate, wherein the absorption spectrum obtained by infrared spectroscopy measurement of the aforementioned gas barrier layer using total reflectance measurement method,

[0080] 1493cm -1 The above 1780cm -1 Let the total peak area within the following absorption band range be A, and let 1493 cm⁻¹ be the maximum peak area. -1 The above is 1598cm -1 When the total peak area within the following absorption band range is set as D, the area ratio D / A is 0.5 or higher. 4.

[0082] The gas barrier laminate as described in any one of 1 to 3, wherein the aforementioned inorganic layer is in contact with the aforementioned substrate layer, or an undercoat layer is provided between the aforementioned inorganic layer and the aforementioned substrate layer. 5.

[0084] The gas barrier laminate as described in any one of 1 to 4, wherein the aforementioned inorganic layer comprises one or more inorganic substances selected from the group consisting of silicon oxide, aluminum oxide and aluminum. 6.

[0086] The gas barrier laminate as described in any one of 1 to 5, wherein the thickness of the aforementioned gas barrier layer is 0.01 to 15 μm. 7.

[0088] The gas barrier laminate as described in any one of 1 to 6, wherein a sealant layer is further provided on the side of the gas barrier layer opposite to the inorganic layer. 8.

[0090] As described in 7, the gas barrier laminate is wherein the aforementioned sealant layer is in contact with the aforementioned gas barrier layer, or the aforementioned gas barrier layer and the aforementioned sealant layer are bonded together by an adhesive layer. 9.

[0092] As described in 7, a polyamide-containing layer is disposed between the aforementioned gas barrier layer and the aforementioned sealant layer. 10.

[0094] The gas barrier laminate as described in any one of 1 to 9 is used in food packaging. 11.

[0096] The gas barrier laminate as described in any one of 1. to 10 is used in the manufacture of steamed or boiled foods. 12.

[0098] Packaging bags, which are made of any one of the gas barrier laminates described in 1 to 11. 13.

[0100] Food products obtained by packaging using any one of the gas barrier laminates described in 1. to 12.

[0101] [Third Invention] 1.

[0103] A gas barrier laminate comprising a substrate layer, a gas barrier layer disposed on at least one side of the substrate layer, and an inorganic layer disposed between the substrate layer and the gas barrier layer.

[0104] The Zn composition, determined by X-ray photoelectron spectroscopy analysis of the aforementioned gas barrier layer, is 1–10 atomic%.

[0105] The data were determined by time-of-flight secondary ion mass spectrometry analysis of the aforementioned gas barrier layer. 64 ZnPO4H - Let the mass peak intensity be I( 64 ZnPO4H - ) and C3H3O2 - The mass peak intensity is set as I(C3H3O2) - )hour,

[0106] I( 64 ZnPO4H - ) / I(C3H3O2 - The value of ) is 7 × 10 -4 Above 5×10 -2 the following. 2.

[0108] As described in 1, in the gas barrier laminate, wherein the PO2 content, as determined by the aforementioned time-of-flight secondary ion mass spectrometry analysis of the aforementioned gas barrier layer, is... - Let the mass peak intensity be I(PO2) - ) and PO3 - The mass peak intensity is set as I(PO3) - )hour,

[0109] (I(PO2 - )+I(PO3 - )) / I(C3H3O2 - The value is above 0.02 and below 5. 3.

[0111] As described in 1 or 2, the gas barrier laminate, wherein the aforementioned I(PO2) - ) and the aforementioned I(PO3) - The strength ratio of I(PO2) - ) / I(PO3 - The value is above 0.05 and below 1. 4.

[0113] The gas barrier laminate as described in any one of 1 to 3, wherein the aforementioned gas barrier layer is composed of a cured material comprising at least a polycarboxylic acid, Zn, and a phosphorus compound or its salt containing one or more -P-OH groups. 5.

[0115] As described in 4., in the gas barrier laminate, the concentration of the aforementioned phosphorus compound or its salt containing one or more -P-OH groups in the aforementioned mixture is 5 × 10⁻¹⁰ relative to 1 mol of carboxyl groups in the aforementioned polycarboxylic acid. -4 Above 0.3 mol and below 0.3 mol. 6.

[0117] The gas barrier laminate as described in 4 or 5, wherein the aforementioned polycarboxylic acid comprises one or more polymers selected from the group consisting of polyacrylic acid, polymethacrylic acid, and copolymers of acrylic acid and methacrylic acid. 7.

[0119] The gas barrier laminate as described in any one of 1 to 6, wherein the thickness of the aforementioned gas barrier layer is 0.05 μm or more and 10 μm or less.

[0120] [4th Invention] [1]

[0122] Gas barrier laminate, comprising:

[0123] Substrate layer,

[0124] A gas barrier layer disposed on at least one side of the aforementioned substrate layer, and

[0125] An inorganic layer disposed between the aforementioned substrate layer and the aforementioned gas barrier layer;

[0126] The aforementioned gas barrier layer is composed of a solidified material comprising a mixture of polycarboxylic acids, polyamine compounds, polyvalent metal compounds, and phosphorus compounds or their salts containing one or more -P-OH groups. [2]

[0128] The gas barrier laminate as described in [1] further includes an undercoating layer disposed between the aforementioned substrate layer and the aforementioned inorganic layer. [3]

[0130] As described in [1] or [2], the aforementioned inorganic layer is a vapor-deposited film disposed on the aforementioned substrate layer, or a vapor-deposited film disposed on the aforementioned interlayer when there is an interlayer between the aforementioned substrate layer and the aforementioned inorganic layer, and the aforementioned inorganic layer is composed of one or more inorganic substances selected from the group consisting of silicon oxide, aluminum oxide and aluminum. [4]

[0132] As described in any one of [1] to [3], in the infrared absorption spectrum of the aforementioned gas barrier layer,

[0133] 1300cm -1 The above 1490cm -1 The maximum peak height of absorbance within the following range is defined as α.

[0134] 1690cm -1 The above 1780cm -1 When the maximum peak height of absorbance is set as γ within the following range,

[0135] The ratio of free carboxyl groups, represented by γ / α, to the NH3 complex is 0.00 to 1.00. [5]

[0137] As described in any one of [1] to [4], in the infrared absorption spectrum of the aforementioned gas barrier layer,

[0138] 1493cm -1 The above 1780cm -1 Let the total peak area within the following absorption band range be A.

[0139] 1598cm -1 The above 1690cm -1 Let the total peak area within the following absorption band range be B.

[0140] 1690cm -1 The above 1780cm -1 Let the total peak area within the following absorption band range be C.

[0141] 1493cm -1 The above is 1598cm -1 When the total peak area within the following absorption band range is set as D,

[0142] The area ratio of the amide bond represented by B / A is between 0.200 and 0.370.

[0143] The area ratio of carboxylic acids, expressed as C / A, is less than 0.150.

[0144] The area ratio of carboxylate, expressed as D / A, is 0.580 or higher and 0.800 or lower. [6]

[0146] The gas barrier laminate as described in any one of [1] to [5], wherein the thickness of the aforementioned gas barrier layer is more than 0.01 μm and less than 15 μm. [7]

[0148] Gas barrier laminate as described in any one of [1] to [6], wherein the aforementioned multivalent metal compound is a compound of one or more metals with a valence of more than two selected from the group consisting of Zn, Ca, Mg, Ba and Al. [8]

[0150] The gas barrier laminate as described in any one of [1] to [7], wherein (the number of moles of P atoms from the aforementioned phosphorus compound or its salt in the aforementioned mixture) / (the number of moles of -COO- groups from the aforementioned polycarboxylic acid in the aforementioned mixture) is 0.001 or more and 0.3 or less. [9]

[0152] Gas barrier laminate as described in any one of [1] to [8], wherein the aforementioned phosphorus compound is one or more selected from the group consisting of phosphoric acid, phosphorous acid, hypophosphoric acid, polyphosphoric acid, phosphonic acid and their salts.

[10]

[0154] The gas barrier laminate as described in any one of [1] to [9], wherein (the number of moles of the polyvalent metal from the aforementioned polyvalent metal compound in the aforementioned mixture) / (the number of moles of the -COO- group from the aforementioned polycarboxylic acid in the aforementioned mixture) is 0.10 or more and 0.80 or less.

[11]

[0156] The gas barrier laminate as described in any one of [1] to

[10] , wherein (the number of moles of the polyvalent metal from the aforementioned polyvalent metal compound in the aforementioned mixture) / (the number of moles of the amino group from the aforementioned polyamine compound in the aforementioned mixture) is 0.25 or more and 0.65 or less.

[12]

[0158] The gas barrier laminate as described in any one of [1] to

[11] , wherein the aforementioned polycarboxylic acid comprises one or more polymers selected from the group consisting of polyacrylic acid, polymethacrylic acid, and copolymers of acrylic acid and methacrylic acid.

[13]

[0160] The gas barrier laminate as described in any one of [1] to

[12] , wherein the aforementioned polyamine compound comprises polyethyleneimine.

[14]

[0162] The gas barrier laminate as described in any one of [1] to

[13] , wherein the aforementioned substrate layer comprises one or more resins selected from the group consisting of polyamide, polyethylene terephthalate and polybutylene terephthalate.

[0163] [Fifth Invention] [1]

[0165] Gas barrier laminate, comprising:

[0166] Substrate layer,

[0167] A gas barrier layer disposed on at least one side of the aforementioned substrate layer, and

[0168] An inorganic layer disposed between the aforementioned substrate layer and the aforementioned gas barrier layer;

[0169] The aforementioned gas barrier layer is composed of a cured material containing a mixture of polycarboxylic acids, polyamine compounds, and polyvalent metal compounds. [2]

[0171] The gas barrier laminate as described in [1] further includes an undercoating layer disposed between the aforementioned substrate layer and the aforementioned inorganic layer. [3]

[0173] As described in [1] or [2], the aforementioned inorganic layer is a vapor-deposited film disposed on the aforementioned substrate layer, or a vapor-deposited film disposed on the aforementioned interlayer when there is an interlayer between the aforementioned substrate layer and the aforementioned inorganic layer, and the aforementioned inorganic layer is composed of one or more inorganic substances selected from the group consisting of silicon oxide, aluminum oxide and aluminum. [4]

[0175] Gas barrier laminate as described in any one of [1] to [3], wherein the aforementioned inorganic layer comprises an aluminum oxide layer composed of aluminum oxide. [5]

[0177] As described in any one of [1] to [4], in the infrared absorption spectrum of the aforementioned gas barrier layer,

[0178] 1300cm -1 The above 1490cm -1 The maximum peak height of absorbance within the following range is defined as α.

[0179] 1690cm -1 The above 1780cm -1 When the maximum peak height of absorbance is set as γ within the following range,

[0180] The ratio of free carboxyl groups, represented by γ / α, to the NH3 complex is 0.00 to 1.00. [6]

[0182] As described in any one of [1] to [5], in the infrared absorption spectrum of the aforementioned gas barrier layer,

[0183] 1493cm -1 The above 1780cm -1 Let the total peak area within the following absorption band range be A.

[0184] 1598cm -1 The above 1690cm -1 Let the total peak area within the following absorption band range be B.

[0185] 1690cm -1 The above 1780cm -1 Let the total peak area within the following absorption band range be C.

[0186] 1493cm -1 The above is 1598cm -1 When the total peak area within the following absorption band range is set as D,

[0187] The area ratio of the amide bond represented by B / A is between 0.200 and 0.370.

[0188] The area ratio of carboxylic acids, expressed as C / A, is less than 0.150.

[0189] The area ratio of carboxylate, expressed as D / A, is 0.580 or higher and 0.800 or lower. [7]

[0191] The gas barrier laminate as described in any one of [1] to [6], wherein the thickness of the aforementioned gas barrier layer is more than 0.01 μm and less than 15 μm. [8]

[0193] Gas barrier laminate as described in any one of [1] to [7], wherein the aforementioned multivalent metal compound is a compound of one or more metals with a valence of more than two selected from the group consisting of Zn, Ca, Mg, Ba and Al. [9]

[0195] The gas barrier laminate as described in any one of [1] to [8], wherein (the number of moles of the polyvalent metal from the aforementioned polyvalent metal compound in the aforementioned mixture) / (the number of moles of the -COO- group from the aforementioned polycarboxylic acid in the aforementioned mixture) is 0.10 or more and 0.80 or less.

[10]

[0197] The gas barrier laminate as described in any one of [1] to [9], wherein (the number of moles of the polyvalent metal from the aforementioned polyvalent metal compound in the aforementioned mixture) / (the number of moles of the amino group from the aforementioned polyamine compound in the aforementioned mixture) is 0.25 or more and 0.75 or less.

[11]

[0199] The gas barrier laminate as described in any one of [1] to

[10] , wherein the aforementioned polycarboxylic acid comprises one or more polymers selected from the group consisting of polyacrylic acid, polymethacrylic acid, and copolymers of acrylic acid and methacrylic acid.

[12]

[0201] The gas barrier laminate as described in any one of [1] to

[11] , wherein the aforementioned polyamine compound comprises polyethyleneimine.

[13]

[0203] Gas barrier laminate as described in any one of [1] to

[12] , wherein the aforementioned substrate layer is a layer comprising one or more resins selected from the group consisting of polyamide, polyethylene terephthalate and polybutylene terephthalate.

[0204] Invention Effects

[0205] According to the present invention, for example, a gas barrier laminate with good barrier properties after cooking can be provided.

[0206] According to the present invention, for example, a gas barrier material with improved gas barrier properties can be provided.

[0207] According to the present invention, for example, a gas barrier laminate with good barrier properties after cooking can be provided regardless of the laminate structure.

[0208] According to the present invention, for example, a gas barrier material can be provided that offers an excellent balance between productivity and barrier properties and can provide ideal barrier properties in various layered structures.

[0209] According to the present invention, for example, a gas barrier material with an excellent balance between productivity and barrier properties can be provided. Attached Figure Description

[0210] [ Figure 1 [A cross-sectional view illustrating an example of the structure of the gas barrier laminate of the double-layered structure in the first embodiment.]

[0211] [ Figure 2 [A cross-sectional view illustrating an example of the structure of the three-layer gas barrier laminate in the first embodiment.]

[0212] [ Figure 3 [Y] is the trigonometric function Y used for data analysis of mass spectrometry analysis in the first embodiment. j (m) A graph (line graph) for illustration.

[0213] [ Figure 4 [A graph (line plot) showing an example of curve fitting for mass spectrometry analysis data in the first embodiment.]

[0214] [ Figure 5 [A cross-sectional view illustrating an example of the structure of the gas barrier laminate in the second embodiment.]

[0215] [ Figure 6 [A cross-sectional view illustrating an example of the structure of the gas barrier laminate in the second embodiment.]

[0216] [ Figure 7[Y] is the trigonometric function Y used for data analysis in the second embodiment of mass spectrometry analysis. j (m) A graph (line graph) for illustration.

[0217] [ Figure 8 [A graph (line plot) showing an example of curve fitting for mass spectrometry analysis data in the second embodiment.]

[0218] [ Figure 9 [A cross-sectional view illustrating an example of the structure of the gas barrier laminate of the double-layered structure in the third embodiment.]

[0219] [ Figure 10 [A cross-sectional view illustrating an example of the structure of the three-layer gas barrier laminate in the third embodiment.]

[0220] [ Figure 11 [Y] is the trigonometric function Y used for data analysis in the third embodiment of mass spectrometry analysis. j (m) A graph (line graph) for illustration.

[0221] [ Figure 12 [A graph (curve diagram) showing an example of curve fitting for mass spectrometry analysis data in the third embodiment.]

[0222] [ Figure 13 [A cross-sectional view illustrating an example of the structure of the gas barrier laminate in the fourth embodiment.]

[0223] [ Figure 14 [A cross-sectional view illustrating an example of the structure of the gas barrier laminate in the fourth embodiment.]

[0224] [ Figure 15 [A cross-sectional view illustrating an example of the structure of the gas barrier laminate in the fifth embodiment.]

[0225] [ Figure 16 [A cross-sectional view illustrating an example of the structure of the gas barrier laminate in the fifth embodiment.] Detailed Implementation

[0226] Hereinafter, embodiments of the first to fifth inventions will be described using the accompanying drawings.

[0227] Specifically, the embodiment of the first invention is described as the first embodiment, the embodiment of the second invention is described as the second embodiment, the embodiment of the third invention is described as the third embodiment, the embodiment of the fourth invention is described as the fourth embodiment, and the embodiment of the fifth invention is described as the fifth embodiment.

[0228] All figures are schematic diagrams for illustrative purposes and may not be consistent with the actual dimensions.

[0229] Regarding the reference numerals in the figures, the same reference numerals sometimes denote different elements in different embodiments. For example, in the figures used to illustrate the first embodiment... Figure 2 In the accompanying drawing, reference numeral 10 denotes a "three-layer laminated barrier membrane," but on the other hand, in the figure used to illustrate the fourth embodiment... Figure 13 In the figure, reference numeral 10 indicates "gas barrier membrane".

[0230] Unless otherwise specified, the "~" between numerical values ​​in the text indicates above to below.

[0231] In the description of groups (atomic groups) in this specification, the lack of a description of substitution or unsubstitutability includes both cases with and without substituents. For example, the term "alkyl" includes not only unsubstituent alkyl groups (unsubstituted alkyl groups) but also substituted alkyl groups (substituted alkyl groups).

[0232] The term "(meth)propylene-" in this specification indicates that it includes both the concepts of "propylene-" and "methpropylene-". The same applies to similar terms such as "(meth)acrylate".

[0233] <First Implementation>

[0234] The gas barrier laminate involved in the first embodiment is the following gas barrier laminate:

[0235] It comprises a substrate layer, a gas barrier layer disposed on at least one side of the substrate layer, and an inorganic layer disposed between the substrate layer and the gas barrier layer.

[0236] The Zn composition of the gas barrier layer, as determined by X-ray photoelectron spectroscopy analysis, is 1–10 atomic%.

[0237] The data were determined by time-of-flight secondary ion mass spectrometry analysis of the aforementioned gas barrier layer. 64 ZnPO4H - The peak intensity is set to I( 64 ZnPO4H - ) and C3H3O2 - The peak intensity is set to I(C3H3O2) - )hour,

[0238] I( 64 ZnPO4H - ) / I(C3H3O2- The value of ) is 6 × 10 -4 Above 5×10 -2 the following,

[0239] The composition ratio of N, determined by X-ray photoelectron spectroscopy analysis of the aforementioned gas barrier layer, is greater than 0 atomic% and less than 12 atomic%.

[0240] The CN content was determined by time-of-flight secondary ion mass spectrometry analysis of the aforementioned gas barrier layer. - The peak intensity is set to I(CN) - )hour,

[0241] I(CN - ) / I(C3H3O2 - The value of ) is greater than 0 and less than 2.

[0242] The Zn composition ratio of 1 to 10 atomic percent, as determined by X-ray photoelectron spectroscopy, refers to the presence of Zn at a certain concentration in the gas barrier layer.

[0243] In addition, C3H3O2 was detected from the gas barrier layer by mass spectrometry analysis. - This refers to the fact that the gas barrier layer contains polyacrylic acid or its derivatives / similar compounds (polyacrylic acid, etc.). Furthermore, it is believed that I(C3H3O2) - The value is related to the amount (concentration) of carboxyl groups in the gas barrier layer.

[0244] Since the gas barrier layer contains Zn at a certain concentration, and there are also polycarboxylic acids with carboxyl groups in the gas barrier laminate, it is believed that the polycarboxylic acids in the gas barrier layer form a cross-link with Zn. The gas barrier layer that forms the Zn cross-link together with the inorganic layer disposed between the substrate layer and the gas barrier layer shall bear the gas barrier property of the gas barrier laminate.

[0245] Furthermore, it was detected from the gas barrier layer by mass spectrometry analysis. 64 ZnPO4H - This refers to the presence of bonds between phosphorus compounds, represented by phosphate, and Zn in the gas barrier layer, which is considered to be I( 64 ZnPO4H - The value of is related to the amount (concentration) of bonds between phosphorus compounds and Zn. Moreover, it can be inferred that Zn is not only bonded to the carboxyl groups of polycarboxylic acids, but also that some Zn is chemically bonded to each other through polyphosphoric acid compounds.

[0246] In addition, I ( 64 ZnPO4H - ) / I(C3H3O2 -The value is related to the amount (concentration) of phosphorus compounds bonded to Zn relative to the carboxyl group of the polycarboxylic acid.

[0247] However, zinc phosphate is known to be a water-insoluble compound, and the bond between the phosphorus compound and Zn is a bond that is not easily broken relative to hydration caused by processes such as boiling. Therefore, it is believed that the presence of the phosphorus compound-Zn bond in the gas barrier layer inhibits the excessive expansion and contraction of the gas barrier layer due to processes such as boiling, which could damage the adjacent inorganic layer and thus greatly reduce the gas barrier properties.

[0248] On the other hand, CN was detected from the gas barrier layer by mass spectrometry analysis. - This refers to the fact that the gas barrier layer contains polyamines. It is assumed that, as determined by X-ray photoelectron spectroscopy analysis, the N composition is greater than 0 atomic% and less than 12 atomic% and I(CN) - ) / I(C3H3O2 - A value greater than 0 and less than 2 indicates that polyamines are also present in the gas barrier layer containing polycarboxylic acids, and is a value related to the amount (concentration) of amino groups from the polyamines.

[0249] Because polyamines and polycarboxylic acids are present at a certain concentration in the gas barrier layer, the carboxyl groups from the polycarboxylic acids can bond not only to Zn but also to amino groups. Furthermore, amide crosslinks can be formed through the dehydration condensation reaction of the carboxyl and amino groups. It is believed that polycarboxylic acids utilize Zn and polyamines to form a well-balanced crosslinked body based on ionic and amide crosslinks, forming a metal crosslinked gas barrier layer. Together with the inorganic layer disposed between the substrate layer and the gas barrier layer, this forms the gas barrier property of the gas barrier laminate.

[0250] That is, since the composition ratio of Zn is 1 to 10 atomic%, I( 64 ZnPO4H - ) / I(C3H3O2 - The value of ) is 6 × 10 -4 Above 5×10 -2 Furthermore, if the N composition percentage is greater than 0 atomic% and less than 12 atomic% (I(CN)...), - ) / I(C3H3O2 - The value of ) is greater than 0 and less than 2, therefore, the barrier properties are well maintained after cooking.

[0251] Figure 1The diagram shows a schematic cross-sectional view of an example of a double-laminated barrier film including the gas barrier laminate according to the first embodiment. The double-laminated barrier film 1 includes a gas barrier laminate 8. This gas barrier laminate 8 includes a substrate layer 2, a gas barrier layer 5 located on at least one side of the substrate layer 2, and an inorganic layer 4 located between the substrate layer 2 and the gas barrier layer 5. Additionally, an undercoat layer (UC layer) 3 may be provided below the inorganic layer 4, i.e., above the substrate layer 2. For example, in the case of the double-laminated barrier film 1, the gas barrier laminate 8 may be bonded to unstretched polypropylene (CPP) 7 via an adhesive layer 6.

[0252] in addition, Figure 2 The diagram shows a schematic cross-sectional view of an example of a three-layer laminated barrier film comprising the gas barrier laminate according to the first embodiment. In the three-layer laminated barrier film 10, for example, a nylon film 9 may be bonded to the first adhesive layer 61 of the barrier laminate 8, on which the first adhesive layer 61 is provided, and the nylon film 9 is bonded to the unstretched polypropylene 7 through a second adhesive layer 62.

[0253] The gas barrier layer 5 of the gas barrier laminate 8 according to the first embodiment was found to contain at least zinc (Zn) and nitrogen (N) layers by X-ray photoelectron spectroscopy (XPS) analysis. Furthermore, analysis by time-of-flight secondary ion mass spectrometry (TOF-SIMS) analysis revealed the presence of... 64 ZnPO4H - The peak, C3H3O2 - The peak, CN - The peak.

[0254] In the gas barrier layer of the gas barrier laminate according to the first embodiment, high water resistance was detected. 64 ZnPO4H - The peak, thus, becomes a gas barrier laminate with good barrier properties after cooking.

[0255] [XPS Analysis]

[0256] The Zn composition contained in the gas barrier layer is 1 atomic% or more, preferably 1.5 atomic% or more, and more preferably 2 atomic% or more, as shown in XPS analysis. Furthermore, the Zn composition contained in the gas barrier layer is 10 atomic% or less, preferably 8 atomic% or less, and more preferably 7 atomic% or less. This corresponds to a Zn peak intensity relative to the carbon peak intensity, i.e., a Zn / C ratio of 0.01 or more to 0.2 or less (atoms / atoms).

[0257] As mentioned above, Zn exists in a certain amount in the gas barrier layer, thereby improving the barrier properties after cooking.

[0258] Furthermore, the composition of N in the gas barrier layer is greater than 0% in XPS analysis, preferably 2 atomic% or more, and more preferably 3 atomic%. Additionally, the composition of N is 12 atomic% or less, preferably 10 atomic% or less, and more preferably 9 atomic% or less. This corresponds to a peak intensity of N relative to the peak intensity of carbon, i.e., an N / C ratio of 0 or more to 0.2 or less (atoms / atoms).

[0259] As mentioned above, when the N composition of the gas barrier layer is greater than 0 atomic% and less than 12 atomic%, the barrier performance after cooking becomes good.

[0260] The following shows an example of specific conditions applicable to XPS analysis in the first embodiment.

[0261] Analytical apparatus: KRATOS AXIS-NOVA

[0262] X-ray source: Monochromatic Al-Kα

[0263] X-ray source output: 15kV, 10mA

[0264] Analysis area: 300×700μm

[0265] During analysis: a neutralization gun for charge correction was used.

[0266] In XPS analysis, a 1×1 cm sample cut from the gas barrier layer can be used. Furthermore, to analyze the interior of the gas barrier layer, it is preferable to sputter-etch its surface before analysis. To minimize damage to the gas barrier layer, it is desirable to use an Ar-gas cluster ion beam (Ar-GCIB) source for sputter etching. Ar-gas cluster ion beams are known as a method for etching without damaging the chemical structure of the sample.

[0267] In XPS analysis, a broad-spectral scan is used to identify the detectable elements, and a narrow-scan method is used to obtain the spectra for each element. Then, based on the obtained spectra, the Shirley method is used to calculate the background, which is then removed from the spectrum. For each element measured, the background-removed spectrum is obtained, and the atomic percentage (atomic %) of the detected element is calculated using the relative sensitivity coefficient method based on the obtained peak areas.

[0268] It should be noted that the detection sensitivity of atomic composition ratios in typical XPS analysis is considered to be around 0.1 atomic percent. For example, in cases where trace amounts of phosphorus compounds are added to the gas barrier layer, the presence of P may sometimes be undetectable by XPS analysis.

[0269] [TOF-SIMS Analysis]

[0270] In the fragments detected during TOF-SIMS analysis of the gas barrier layer 64 ZnPO4H - The peak intensity is set to I( 64 ZnPO4H - ) and C3H3O2 - The peak intensity of the fragment is set to I(C3H3O2). - )hour,

[0271] I( 64 ZnPO4H - ) / I(C3H3O2 - The value of ) is 6 × 10 -4 The preferred value is 7×10. -4 The above is preferred to be 1×10 -3 That's all. Additionally, it's 5×10 -2 The following is preferred: 3×10 -2 The following is more preferably 2×10 -2 the following.

[0272] As mentioned above, upon detecting bonds with high water resistance 64 ZnPO4H - The mass peak, and I ( 64 ZnPO4H - ) / I(C3H3O2 - When the value of ) is within the above range, it becomes a gas barrier laminate with good barrier properties after cooking. Additionally, if ( 64 ZnPO4H - ) / I(C3H3O2 - If the value is too large, the particles of zinc phosphate compound will grow in the gas barrier layer, causing unevenness in the gas barrier layer and showing a tendency to deteriorate the barrier performance after cooking.

[0273] In addition, CN was detected in the fragments during TOF-SIMS analysis of the gas barrier layer. - The mass peak intensity is set as I(CN) - )hour,

[0274] I(CN - ) / I(C3H3O2 - The value of I(CN) is greater than 0, preferably 0.2 or more, and more preferably 0.4 or more. Additionally, I(CN) - ) / I(C3H3O2 - The value of ) is 2 or less, preferably 1.8 or less, and more preferably 1.5 or less.

[0275] If it is such a gas barrier layer, it becomes a gas barrier laminate with good barrier performance after cooking.

[0276] The following shows an example of specific conditions applicable to the TOF-SIMS analysis of the first embodiment.

[0277] To analyze the interior of the gas barrier layer, it is preferable to sputter-etch the surface of the gas barrier layer using the Ar-gas cluster ion beam (Ar-GCIB) included with the TOF-SIMS analysis apparatus before TOF-SIMS analysis. The use of Ar-GCIB can reduce damage to the gas barrier layer.

[0278] An example of specific conditions applicable to the Ar-GCIB of the first embodiment is shown.

[0279] GCIB: 5kV, 5μA

[0280] GCIB processing time: The point at which the spectral pattern of TOF-SIMS no longer changes.

[0281] TOF-SIMS analysis can be performed, for example, as described below.

[0282] Analytical apparatus: PHI nano-TOFII manufactured by ULVAC-PHI

[0283] Primary ion: Bi3 2+

[0284] Primary ion source output: 30kV, 0.5μA

[0285] Analysis area: 300×300μm (scanning area of ​​the primary ion beam)

[0286] During analysis, charge neutralization can be achieved through irradiation with low-energy electron beams and low-energy Ar ions attached to the device. Furthermore, similar to XPS analysis, TOF-SIMS analysis can use a 1×1 cm sample cut from a gas barrier layer.

[0287] At this point, PO2, as observed by TOF-SIMS analysis targeting the gas barrier layer, - Let the mass peak intensity be I(PO2) - ) and PO3 - The mass peak intensity is set as I(PO3) - )hour,

[0288] (I(PO2 - )+I(PO3 - )) / I(C3H3O2 - The value of I(PO2) is preferably 0.02 or higher, more preferably 0.05 or higher, and even more preferably 0.07 or higher. Additionally, I(PO2)- )+I(PO3 - ) / I(C3H3O2 - The value of ) is preferably 5 or less, more preferably 3 or less, and even more preferably 2.5 or less.

[0289] PO2 detected - PO3 - The mass peak refers to the fact that the gas barrier layer contains phosphorus compounds, such as phosphate, containing more than one P-OH group. Furthermore, it is believed that (I(PO2) - )+I(PO3 - )) / I(C3H3O2 - The value is related to the amount (concentration) of phosphorus compounds in the gas barrier layer relative to the carboxyl groups of polycarboxylic acids.

[0290] At this time, the above I(PO2) - ) and I(PO3) - The strength ratio of I(PO2) - ) / I(PO3 - The value of I(PO2) is preferably 0.05 or higher, more preferably 0.08 or higher, and even more preferably 0.1. Additionally, I(PO2) - ) / I(PO3 - The value of ) is 1 or less, preferably 0.9 or less, and more preferably 0.8 or less.

[0291] PO2 was detected in TOF-SIMS analysis. - and PO3 - The mass peak refers to the proportion of phosphorus compounds containing more than one p-OH group, such as phosphoric acid (H3PO4), whose ratio is I(PO2). - ) / I(PO3 - This becomes a value reflecting the types of phosphorus compounds.

[0292] I( ) reflects the amount (concentration) of zinc phosphate bonds in the gas barrier layer. 64 ZnPO4H - ) / I(C3H3O2 - This influences the types of phosphorus compounds. Specifically, it also relates to I(PO2) - ) / I(PO3 - The value of I(PO2) above. - ) / I(PO3 - The value of I( ) is above 0.05 and below 1, which enables I( 64 ZnPO4H - ) / I(C3H3O2 -The value of ) is within a suitable range, which can well maintain the barrier performance of the gas barrier laminate of the first embodiment after cooking.

[0293] The analysis of data obtained from TOF-SIMS can be performed as follows.

[0294] In order to perform detailed spectral analysis, in the first embodiment, for each positive and negative secondary ion, the mass number m is obtained using an analytical device. i and the corresponding count c i As a pair of raw data columns and total ion counts (C T Here, i = 0, 1, 2, ..., N, and the original data column is for m. i And they are arranged in ascending order. It should be noted that C... T It is the total count of secondary ions detected by the detector.

[0295] Let the range of mass numbers around the mass spectral peak of interest be defined as i = n1, n1+1, ..., n2. Using the following formula... i The data c of the counts obtained through analysis within this range i To approximate the result. Specifically, this is achieved by using the background level b. 0 and K trigonometric functions Y j (m i Curve fitting to c i To approximate. Here, b 0 It is a constant.

[0296] [Mathematical Expression 1]

[0297]

[0298] Y j (m i )yes Figure 3 As shown, in mass number x 0 j It has a peak value Y 0 j The function is represented by the following formula.

[0299] [Mathematical Expression 2]

[0300]

[0301] Here, b 0 x 0 j Y 0 j B - j B +j These become the fitting parameters. Furthermore, with respect to j, j = 1, ..., K. For example, the background of the spectrum is not a constant value but rather relative to m. i In the case of linear change, b 0 With trigonometric function Y j (m i The background is approximated by combining different mass functions. When the mass spectral peak of interest is a single peak, the background is removed and approximation is performed using one trigonometric function. When the mass spectral peak of interest is close to other mass peaks, these other mass peaks are also included in the approximation using multiple trigonometric functions. When the approximated mass spectral peak of interest is set as the j=kth peak among K trigonometric functions, the peak intensity I is determined by Y up to i=n1, ..., n2. k (m i The sum of ) is expressed by the total ion count (C T The numerical representation obtained by standardization is calculated by the following formula.

[0302] [Mathematical Expression 3]

[0303]

[0304] If a mass spectrum peak has a tail, it becomes difficult to define the range of mass numbers corresponding to the count. In the first embodiment, to avoid this, a trigonometric function is used to approximate the mass spectrum peak. Thus, the count at the tail of the mass spectrum peak is ignored. Curve fitting is performed so that the central portion of the mass spectrum peak matches the trigonometric function.

[0305] In addition, sometimes other components (e.g., other types of mass peaks with the same mass number) are observed to overlap with the target peak component. In such cases, trigonometric functions are used to approximate the other components that overlap with the target peak component, thereby determining the target peak component.

[0306] The mass numbers of the fragments of interest in the first embodiment were calculated in advance and are shown below. The atomic mass numbers of the isotopes are referenced at http: / / physics.nist.gov / .

[0307] [Table 1]

[0308]

[0309] [ 64 ZnPO4H - [Calculation of peak mass intensity]

[0310] Zn is known to have five isotopes. In TOF-SIMS analysis, the main isotopes detected are those of Zn and Zn. 64 Zn, 66 Zn,68 Zn-related fragments. In the first embodiment, the focus is on the fragments with the highest presence rate. 64 Zn. In representing 64 Zn was detected in fragments of bonds between Zn and phosphorus compounds containing P-OH. 64 ZnPO4H - , 64 ZnP2O6H - , 64 ZnP2O7H - , 64 ZnP3O9 - etc., but focusing on those with larger peak mass. 64 ZnPO4H - .

[0311] Focusing on the mass number range of negative secondary ion spectra (159.5–160.3), based on the equivalent... 64 Zn 31 P 16 O4 1 H - The trigonometric function and m obtained by approximating the mass peak near 159.890 i The data is used to calculate the sum of the counts, using C. T Standardize and use the resulting value as 64 ZnPO4H - The mass peak intensity.

[0312] An example of curve fitting is shown below. Figure 4 The calculation results of the parameters used at this time and the sum of the counts are shown in Table 2. Figure 4 In the example shown, based on the target 64 ZnP O4H - The trigonometric function and m obtained by approximating the mass peak i The sum of the counts obtained from the data is 1514. The total ion count of the negative secondary ions at this point (C...) T ) = 8571746, therefore, 64 ZnPO4H - Mass peak intensity I ( 64 ZnPO4H - )for:

[0313] I( 64 ZnPO4H - ) = 1514 / 8571746 = 1.77 × 10 -4 .

[0314] [Table 2]

[0315]

[0316] Examples of curve fitting are shown. Figure 4 To supplement.

[0317] (i) In order to obtain measurement data near the target peak position c i The approximation curve y i It requires "background b" 0 The curves of "triangular function approximation of other components" and "triangular function Y as the target" j (m i The curve is )”.

[0318] (ii) in Figure 4 In the example, in order to obtain the measurement data c reproducible in the range of mass number (m / z) from 159.7 to 160.2. i The "approximation curve y" i “background b” was used 0 "The triangular function Y as the target" j (m i The curve for “triangular function approximation of other components” (in Table 2, j=2) and two curves for “triangular function approximation of other components” (in Table 2, j=0, 1).

[0319] [C3H3O2 - [Calculation of peak mass intensity]

[0320] Focusing on the mass number range of negative secondary ion spectra (70.7–71.4), based on the data obtained from curve fitting, the corresponding... 12 C3 1 H3 16 O2 - The trigonometric function Y is obtained by approximating the mass peak near 71.013. k (m i ) and m i The data is used to calculate the sum of the counts, using C. T Standardize and use the resulting value as C3H3O2 - Mass peak intensity I(C3H3O2) - ).

[0321] [PO2 - [Calculation of peak mass intensity]

[0322] Focusing on the mass number range of negative secondary ion spectra (62.5–63.3), based on the equivalent... 31 P 16 O2 - The trigonometric function and m obtained by approximating the mass peak near 62.964 iThe data is used to calculate the sum of the counts, using C. T Standardize and use the resulting value as PO2 - Mass peak intensity I(PO2) - ).

[0323] [PO3 - [Calculation of peak mass intensity]

[0324] Focusing on the mass number range of negative secondary ion spectra (78.5–79.3), based on the equivalent... 31 P 16 O3 - The trigonometric function and m obtained by approximating the mass peak near 78.959 i The data is used to calculate the sum of the counts, using C. T Standardize and use the resulting value as PO3 - Mass peak intensity I(PO3) - ).

[0325] [CN - [Calculation of peak mass intensity]

[0326] Focusing on the mass number range of negative secondary ion spectra (25.5–26.3), based on the equivalent... 12 C 14 N - The trigonometric function and m obtained by approximating the mass peak near 26.003 i The data is used to calculate the sum of the counts, using C. T Standardize and use the resulting value as CN - Mass peak intensity I (CN) - ).

[0327] The gas barrier layer is preferably formed from a solidified material comprising a mixture of polycarboxylic acids, Zn, and phosphorus compounds containing one or more -P-OH groups, such as phosphoric acid (H3PO4) or their salts.

[0328] If the gas barrier layer is formed from a cured product containing a mixture of these components, the carboxyl groups from the polycarboxylic acid form metal ion crosslinks through Zn. Additionally, Zn reacts with phosphorus compounds containing P-OH groups to form water-resistant bonds. While the detailed mechanism is unclear, it is believed that because these metal ion crosslinks formed through Zn and the bonds between Zn and phosphorus compounds are uniformly and appropriately present in the gas barrier layer, a dense gas barrier layer is formed, and excessive expansion and contraction of the gas barrier layer due to processes such as boiling are suppressed.

[0329] The composition ratio of Zn in the gas barrier layer involved in the first embodiment and the I(64 ZnPO4H - ) / I(C3H3O2 - The value of ) and I(PO2) - )+I(PO3 - ) / I(C3H3O2 - The value of ) and I(PO2) - ) / I(PO3 - The value of ) can be controlled by appropriately adjusting the manufacturing conditions of the gas barrier layer.

[0330] In the first embodiment, for example, the concentration of phosphoric acid relative to the polycarboxylic acid can be used as a criterion for controlling the Zn composition ratio and I( 64 ZnPO4H - ) / I(C3H3O2 - One factor in the value of ).

[0331] The following details the polycarboxylic acids, zinc or compounds thereof, phosphorus compounds, and other additives that may be used in the first embodiment.

[0332] (Polycarboxylic acids)

[0333] Polycarboxylic acids are compounds having two or more carboxyl groups within their molecules. Specifically, examples include homopolymers or copolymers of α,β-unsaturated carboxylic acids such as acrylic acid, methacrylic acid, itaconic acid, fumaric acid, crotonic acid, cinnamic acid, 3-hexenoic acid, and 3-hexenediaic acid. Alternatively, they can be copolymers of the aforementioned α,β-unsaturated carboxylic acids with esters such as ethyl esters, olefins such as ethylene, etc.

[0334] Among them, the preferred polymers are homopolymers of acrylic acid and methacrylic acid or copolymers thereof, more preferably one or more polymers selected from polyacrylic acid, polymethacrylic acid, and copolymers of acrylic acid and methacrylic acid, further preferably at least one polymer selected from polyacrylic acid and polymethacrylic acid, and particularly preferably at least one polymer selected from homopolymers of acrylic acid and homopolymers of methacrylic acid.

[0335] In this first embodiment, the term "polyacrylic acid" includes both homopolymers of acrylic acid and copolymers of acrylic acid with other monomers. In the case of copolymers of acrylic acid with other monomers, for polyacrylic acid, 100% by mass of the polymer contains structural units derived from acrylic acid, typically 90% by mass or more, preferably 95% by mass or more, and more preferably 99% by mass or more.

[0336] Furthermore, in the first embodiment, the term "polymethacrylic acid" includes both homopolymers of methacrylic acid and copolymers of methacrylic acid with other monomers. In the case of copolymers of methacrylic acid with other monomers, for polymethacrylic acid, 100% by mass of the polymer contains structural units derived from methacrylic acid, typically 90% by mass or more, preferably 95% by mass or more, and more preferably 99% by mass or more.

[0337] Polycarboxylic acids are polymers formed by the polymerization of carboxylic acid monomers. From the viewpoint of excellent balance between gas barrier properties and operability, the molecular weight of polycarboxylic acids is preferably 500 to 2,500,000, more preferably 5,000 to 2,000,000, even more preferably 10,000 to 1,500,000, and even more preferably 100,000 to 1,200,000.

[0338] Here, the molecular weight of polycarboxylic acids is the weight-average molecular weight converted from polyethylene oxide, which can be determined using gel permeation chromatography (GPC).

[0339] By neutralizing polycarboxylic acids with a volatile base, gelation can be suppressed when zinc and polyamines (described later) are mixed with the polycarboxylic acids. Therefore, from the viewpoint of preventing gelation, it is preferable to prepare partially or completely neutralized or neutralized carboxyl groups using a volatile base. The neutralized product can be obtained by partially or completely neutralizing the carboxyl groups of the polycarboxylic acid with a volatile base (i.e., partially or completely preparing a carboxylate from the carboxyl groups of the polycarboxylic acid). This prevents gelation when polyamines or zinc are added.

[0340] Partial neutralization is prepared by adding a volatile base to an aqueous solution of a polycarboxylic acid polymer. The desired degree of neutralization can be achieved by adjusting the molar ratio of the polycarboxylic acid to the volatile base. In the first embodiment, from the viewpoint of sufficiently suppressing gelation caused by the neutralization reaction with the amino group of the polyamine, the degree of neutralization of the polycarboxylic acid obtained using the volatile base is preferably 30 to 100 equivalents, more preferably 50 to 100 equivalents.

[0341] As a volatile base, any water-soluble base can be used.

[0342] Examples of volatile bases include, for example, tertiary amines such as ammonia, morpholine, alkylamines, 2-dimethylaminoethanol, N-methylmorpholine, ethylenediamine, triethylamine, or aqueous solutions of these, or mixtures thereof. From the viewpoint of obtaining good gas barrier properties, aqueous ammonia solutions are preferred.

[0343] The mixture constituting the gas barrier laminate according to the first embodiment preferably further comprises a carbonate ammonium salt. The carbonate ammonium salt is a substance added to improve the solubility of zinc and prepare a homogeneous solution containing zinc by making the zinc described later into a zinc ammonium carbonate complex.

[0344] Examples of carbonate-based ammonium salts include ammonium carbonate and ammonium bicarbonate. Ammonium carbonate is preferred from the viewpoint that it is easily volatile and does not easily remain in the resulting gas barrier layer.

[0345] (Zinc)

[0346] Zinc (Zn) can form water-resistant Zn phosphate bonds with phosphorus compounds, which can be detected by TOF-SIMS analysis. 64 ZnPO4H - The indicated mass peak. Additionally, if the gas barrier layer contains a polycarboxylic acid, it forms a salt with the polycarboxylic acid. Zn can be any zinc or zinc compound that can be added to the mixture forming the gas barrier layer; for example, metallic zinc, zinc oxide (ZnO), zinc compounds, etc., can be used. The amount of zinc added can be set to 0.1 mol to 0.5 mol relative to 1 mol of the carboxyl group of the aforementioned polycarboxylic acid.

[0347] (Phosphorus compounds)

[0348] As described above, when performing mass spectrometry analysis on the barrier layer, it is preferable to detect PO2. - and / or PO3 - To create such a barrier layer, the mixture before curing preferably contains a phosphorus compound or a salt thereof.

[0349] Phosphorus compounds or their salts contain one or more -P-OH groups in their molecular structure. Phosphorus compounds can be complexed in mixtures in the form of salts.

[0350] From the viewpoint of further improving the steam barrier properties after cooking, the phosphorus compound preferably contains two or more -P-OH groups, more preferably three or more -P-OH groups. Furthermore, from a productivity viewpoint, the number of -P-OH groups in the phosphorus compound can, for example, be ten or less.

[0351] Specific examples of phosphorus compounds include phosphoric acid, phosphorous acid, phosphonic acid, hypophosphoric acid, polyphosphoric acid, and their derivatives.

[0352] Specifically, polyphosphoric acid has a condensation structure of two or more phosphoric acids in its molecular structure. Examples include diphosphoric acid (pyrophosphoric acid), triphosphoric acid, and polyphosphoric acid formed by the condensation of four or more phosphoric acids.

[0353] Specific examples of derivatives include esters of the aforementioned phosphorus compounds such as phosphoric acid starch and cross-linked phosphoric acid starch; halides such as chlorides; acid anhydrides such as phosphorus tetraoxide; and compounds with structures such as triazine (methylenephosphonic acid) and N,N,N',N'-ethylenediaminetetra(methylenephosphonic acid) having hydrogen atoms bonded to phosphorus atoms replaced by alkyl groups.

[0354] From the viewpoint of further improving the balance between barrier properties and productivity, the phosphorus compound is one or more selected from the group consisting of phosphoric acid, phosphorous acid, hypophosphoric acid, polyphosphoric acid, phosphonic acid and their salts, more preferably at least one selected from the group consisting of phosphoric acid and phosphorous acid, phosphonic acid and their salts.

[0355] Furthermore, specific examples of salts in phosphorus compounds include salts of monovalent metals such as sodium and potassium, and ammonium salts. From a barrier perspective, ammonium salts are preferred for phosphorus compounds.

[0356] The concentration of phosphorus atoms in the phosphorus compound is typically 5 × 10⁻¹⁰ relative to 1 mol of carboxyl groups in the aforementioned polycarboxylic acid mixture. -4 mol or more, preferably 1×10 -3 mol or more, more preferably 3 × 10 -3 The concentration is 1 mol or more, typically 0.3 mol or less, preferably 0.1 mol or less, and more preferably 0.05 mol or less. In phosphorus compounds containing one P atom in their chemical formula, such as phosphoric acid, the number of moles of P atoms has the same meaning as the number of moles of phosphorus compound.

[0357] It is believed that phosphorus compounds of this concentration, or phosphorus compounds derived from their salts, can reliably form Zn bonds with water-resistant phosphorus compounds. This suppresses excessive expansion and contraction of the gas barrier layer due to cooking processes, thereby further improving the gas barrier properties of the gas barrier laminate after cooking. The presence of the bond between the phosphorus compound and Zn was determined by the aforementioned TOF-SIMS analysis. 64 ZnPO4H - The quality peak reflects this.

[0358] (Polyamines)

[0359] The mixture constituting the gas barrier laminate according to the first embodiment preferably further comprises a polyamine. By including a polyamine, the barrier properties of the obtained gas barrier laminate can be improved, as can the interlayer adhesion of the obtained gas barrier laminate, and good delamination resistance can be achieved.

[0360] Polyamines are polymers having two or more amino groups on their main chain, side chain, or terminal. Specifically, examples include aliphatic polyamines such as polyallylamine, polyvinylamine, polyethyleneimine, and poly(propyleneimine); polyamides such as polylysine and polyarginine, which have amino groups on their side chains; and so on. Alternatively, polyamines can be formed by modifying a portion of the amino groups. From the viewpoint of obtaining good gas barrier properties, polyethyleneimine is more preferred. The amount of polyamine added can be set to 0 mol or more and 0.9 mol or less, relative to 1 mol of carboxyl groups contained in the aforementioned polycarboxylic acids.

[0361] From the viewpoint of excellent balance between gas barrier properties and operability, the weight-average molecular weight of the polyamine is preferably 50 to 2,000,000, more preferably 100 to 1,000,000, even more preferably 1,500 to 500,000, even more preferably 1,500 to 100,000, even more preferably 1,500 to 50,000, even more preferably 3,500 to 20,000, even more preferably 5,000 to 15,000, and particularly preferably 7,000 to 12,000.

[0362] In this first embodiment, the molecular weight of the polyamine can be determined using the boiling point elevation method or the viscosity method.

[0363] (Manufacturing method of gas barrier layer)

[0364] The gas barrier layer according to the first embodiment can be manufactured, for example, as described below.

[0365] First, prepare a completely or partially neutralized solution of the carboxyl groups that constitute the polycarboxylic acid.

[0366] A volatile base is added to a polycarboxylic acid, which completely or partially neutralizes the carboxyl groups of the polycarboxylic acid. By neutralizing the carboxyl groups of the polycarboxylic acid, gelation that would occur during the addition of zinc or polyamines due to the reaction of the carboxyl groups constituting the polycarboxylic acid with zinc or the amino groups constituting the polyamines is effectively prevented in subsequent processes, resulting in a uniform intermediate for gas barrier coating materials.

[0367] Next, a zinc salt compound and a carbonate ammonium salt are added to the above intermediate and dissolved. The generated zinc ions react with the -COO- group constituting the polycarboxylic acid to form a zinc salt. Here, the -COO- group forming the salt with the zinc ions refers to both the unneutralized carboxyl group and the neutralized -COO- group. In the case of the neutralized -COO- group, zinc ions from the zinc ions replace and coordinate to form a -COO- group zinc salt. Then, phosphoric acid is added after the formation of the zinc salt, thereby obtaining a coating material (mixture) for gas barrier applications. At this point, a polyamine can be further added.

[0368] The gas barrier coating material (mixture) thus manufactured is applied onto the inorganic layer described later, and then dried and cured to form a gas barrier layer. There are no particular limitations on the method of applying the gas barrier coating material to the substrate layer; conventional methods can be used. Examples include various known coating machines such as Mayer bar coaters, air knife coaters, direct gravure coaters, gravure offset coaters, curved gravure coaters, reverse gravure coaters, and jet nozzle type gravure coaters; top-feed reverse coaters, bottom-feed reverse coaters, and nozzle-feed reverse coaters; five-roll coaters; lip coaters; bar coaters; bar reverse coaters; and die coaters.

[0369] The coating amount (wet thickness) of the gas barrier coating material (mixture) is preferably 0.05 μm or more, more preferably 1 μm or more. Furthermore, the coating amount is preferably 300 μm or less, more preferably 200 μm or less, and even more preferably 100 μm or less.

[0370] Furthermore, the average thickness of the gas barrier layer after drying and curing is preferably 0.05 μm to 10 μm, more preferably 0.08 μm to 5 μm, and even more preferably 0.1 μm to 1 μm. If the thickness is below the upper limit mentioned above, warping of the obtained gas barrier laminate or gas barrier film can be suppressed. Conversely, if the thickness is above the lower limit mentioned above, the barrier performance of the obtained gas barrier laminate or gas barrier film can be improved.

[0371] For drying and heat treatment, heat treatment can be performed after drying, or drying and heat treatment can be performed simultaneously.

[0372] The methods for drying and heating are not particularly limited as long as they achieve the objectives of this invention; any method that can cure the gas barrier coating material or heat the cured gas barrier coating material is acceptable. Examples include ovens and dryers based on convective heat transfer; heating rollers based on conductive heat transfer; infrared, far-infrared, and near-infrared heaters based on radiative heat transfer using electromagnetic waves; and microwaves based on internal heating. From a manufacturing efficiency perspective, an apparatus capable of performing both drying and heating is preferred for the drying and heating process. Specifically, from the viewpoint of being usable for various purposes such as drying, heating, and annealing, a hot air oven is preferred; and from the viewpoint of excellent heat transfer efficiency to the film, a heating roller is preferred. Furthermore, methods for drying and heating can be appropriately combined. A hot air oven and a heating roller can be used together; for example, when the gas barrier coating material is dried using a hot air oven and then heated using a heating roller, the heating process time is shortened, which is preferable from a manufacturing efficiency perspective. In addition, it is preferable to use only a hot air oven for drying and heating.

[0373] For example, ideally, the heat treatment should be performed under the following conditions: a heat treatment temperature of 80–250°C and a heat treatment time of 1 second–10 minutes; preferably, a heat treatment temperature of 120–240°C and a heat treatment time of 1 second–1 minute; more preferably, a heat treatment temperature of 170°C–230°C and a heat treatment time of 1 second–30 seconds. Furthermore, by using a heating roller as described above, heat treatment can be performed in a short time. Importantly, the heat treatment temperature and heat treatment time should be adjusted according to the wet thickness of the gas barrier coating material.

[0374] For gas barrier coating materials (mixtures), the zinc salts constituting the -COO- groups of the polycarboxylic acid form metal crosslinks and water-resistant Zn phosphate bonds (reflected by the aforementioned TOF-SIMS analysis). 64 ZnPO4H - The mass peak of the gas can be dried and heat-treated to obtain a gas barrier layer with excellent gas barrier properties.

[0375] (Inorganic layer)

[0376] Inorganic materials constituting inorganic layer 4 include, for example, metals, metal oxides, metal nitrides, metal fluorides, and metal nitrides, which are capable of forming barrier films.

[0377] As inorganic substances constituting inorganic layer 4, examples include one or more of the following: elements selected from Group 2A of the periodic table such as beryllium, magnesium, calcium, strontium, and barium; transition elements of the periodic table such as titanium, zirconium, ruthenium, hafnium, and tantalum; elements from Group 2B of the periodic table such as zinc; elements from Group 3A of the periodic table such as aluminum, gallium, indium, and thallium; elements from Group 4A of the periodic table such as silicon, germanium, and tin; and elements from Group 6A of the periodic table such as selenium and tellurium, as well as their elements, oxides, nitrides, fluorides, or nitrogen oxides.

[0378] It should be noted that in the first embodiment, the group names of the periodic table are represented in the old CAS form.

[0379] Furthermore, among the aforementioned inorganic materials, considering the excellent balance between barrier properties and cost, it is preferable to select one or more inorganic materials from the group consisting of silicon oxide, aluminum oxide, and aluminum, and more preferably aluminum oxide.

[0380] It should be noted that, in addition to silicon dioxide, silicon oxide may also contain silicon monoxide and silicon suboxide.

[0381] The inorganic layer is formed from the aforementioned inorganic material. The inorganic layer 4 can be composed of a single inorganic layer or multiple inorganic layers. Furthermore, if the inorganic layer 4 is composed of multiple inorganic layers, they can be composed of inorganic layers of the same type or inorganic layers of different types.

[0382] From the perspective of balancing barrier properties, sealing properties, and operability, the thickness of the inorganic layer 4 is usually between 1 nm and 1000 nm, preferably between 1 nm and 500 nm.

[0383] In the first embodiment, the thickness of the inorganic layer can be determined using observation images obtained from a transmission electron microscope or a scanning electron microscope.

[0384] There are no particular limitations on the method for forming the inorganic layer. For example, vacuum evaporation, ion plating, sputtering, chemical vapor deposition, physical vapor deposition (CVD), plasma CVD, sol-gel methods, etc., can be used to form the inorganic layer 4 on one or both sides of the substrate layer 2. Among these, sputtering, ion plating, CVD, PVD, and plasma CVD are ideal for film formation under reduced pressure. Therefore, it is predicted that silicon-containing chemically active molecules such as silicon nitride and silicon oxynitride will react rapidly, thereby improving the surface smoothness of the inorganic layer 4 and reducing pores.

[0385] For these bonding reactions to proceed rapidly, it is ideal for the inorganic atom or compound to be a chemically active molecular or atomic species.

[0386] (Substrate layer)

[0387] Substrate layer 2 can be used without particular limitation as long as it is a substrate layer to which a solution of a gas barrier coating material can be applied. Examples include organic materials such as thermosetting resins, thermoplastic resins, or paper; inorganic materials such as glass, ceramics, silicon dioxide, silicon oxynitride, silicon nitride, concrete, aluminum, alumina, iron, copper, stainless steel, etc.; and multilayer substrate layers formed by combinations of organic materials or combinations of organic and inorganic materials. Among these, for example, in the case of various film applications such as packaging materials and panels, plastic films using thermosetting resins or thermoplastic resins, or organic materials such as paper, are preferred.

[0388] Known thermosetting resins can be used as thermosetting resins. Examples include epoxy resins, unsaturated polyester resins, phenolic resins, urea-melamine resins, polyurethane resins, silicone resins, and polyimides.

[0389] Known thermoplastic resins can be used as thermoplastic resins. Examples include polyolefins (polyethylene, polypropylene, poly(4-methyl-1-pentene), poly(1-butene), etc.), polyesters (polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, etc.), polyamides (nylon-6, nylon-66, poly(m-phenylene adipamide), etc.), polyvinyl chloride, polyimide, ethylene-vinyl acetate copolymer or its saponification, polyvinyl alcohol, polyacrylonitrile, polycarbonate, polystyrene, ion-crosslinked polymers, fluoropolymers, or mixtures thereof.

[0390] Among them, from the viewpoint of good transparency, one or more resins selected from the group consisting of polypropylene, polyethylene terephthalate, polyethylene naphthalate, polyamide, polyimide and polybutylene terephthalate are preferred; from the viewpoint of excellent resistance to pinholes, damage and heat resistance, one or more resins selected from the group consisting of polyamide, polyethylene terephthalate and polybutylene terephthalate are preferred.

[0391] Furthermore, depending on the application of the gas barrier laminate 8, the substrate layer 2 formed from thermoplastic resin can be a single layer or two or more layers.

[0392] Alternatively, a substrate layer can be formed by stretching a film formed from the above-mentioned thermosetting resin or thermoplastic resin along at least one direction, preferably a biaxial direction.

[0393] As the substrate layer 2 according to the first embodiment, from the viewpoint of excellent transparency, rigidity and heat resistance, it is preferably a biaxial stretch film formed of one or more thermoplastic resins selected from polypropylene, polyethylene terephthalate, polyethylene naphthalate, polyamide, polyimide and polybutylene terephthalate, and more preferably a biaxial stretch film formed of one or more thermoplastic resins selected from polyamide, polyethylene terephthalate and polybutylene terephthalate.

[0394] Alternatively, polyvinylidene chloride, polyvinyl alcohol, ethylene-vinyl alcohol copolymer, acrylic resin, urethane resin, etc., can be coated on the surface of the substrate layer 2.

[0395] Furthermore, for substrate layer 2, surface treatment can be performed to improve adhesion. Specifically, surface activation treatments such as corona treatment, flame treatment, plasma treatment, and primer coating treatment can be performed.

[0396] From the viewpoint of obtaining good film properties, the thickness of the substrate layer 2 is preferably 1 to 1000 μm, more preferably 1 to 500 μm, and even more preferably 1 to 300 μm.

[0397] The shape of the substrate layer 2 is not particularly limited. For example, it can be a sheet or film shape, a tray, a cup, a hollow body, etc.

[0398] (Base coating)

[0399] In the gas barrier laminate 8, from the viewpoint of improving the adhesion between the substrate layer 2 and the inorganic layer 4, a primer layer 3 can be formed on the surface of the substrate layer 2. The primer layer is preferably a layer formed using an epoxy (meth)acrylate compound or a urethane (meth)acrylate compound.

[0400] The aforementioned base coating 3 is preferably a layer formed by curing at least one selected from epoxy (meth)acrylate compounds and urethane (meth)acrylate compounds.

[0401] Examples of epoxy (meth)acrylate compounds include compounds obtained by reacting bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, bisphenol S type epoxy compounds, phenol Novola C type epoxy compounds, cresol Novolac type epoxy compounds, aliphatic epoxy compounds, etc., with acrylic acid or methacrylic acid, and acid-modified epoxy (meth)acrylates obtained by reacting the above epoxy compounds with carboxylic acids or their anhydrides. These epoxy (meth)acrylate compounds are coated onto the surface of a substrate layer together with a diluent containing a photopolymerization initiator and, if necessary, other photopolymerization initiators or thermally reactive monomers. Subsequently, they are irradiated with ultraviolet light or the like, and a crosslinking reaction occurs to form a base layer.

[0402] Examples of urethane (meth)acrylate compounds include, for instance, compounds obtained by acrylate esterification of oligomers (hereinafter also referred to as polyurethane oligomers) formed from polyol compounds and polyisocyanate compounds.

[0403] Polyurethane oligomers can be obtained from the condensation products of polyisocyanate compounds and polyol compounds. Specific examples of polyisocyanate compounds include adducts of methylene bis(terephthalic acid diisocyanate), hexamethylene diisocyanate-hexanetriol, hexamethylene diisocyanate, toluene diisocyanate, toluene diisocyanate-trimethylolpropane adduct, 1,5-naphthalene diisocyanate, thiopropyl diisocyanate, ethylbenzene-2,4-diisocyanate, 2,4-toluene diisocyanate dimers, hydrogenated dimethyl phthalate diisocyanate, and tris(4-phenylisocyanate)thiophosphate. Specific examples of polyol compounds include polyether polyols such as polyoxytetramethylene glycol, polyester polyols such as polyadipate polyols and polycarbonate polyols, and copolymers of acrylates and hydroxyethyl methacrylate. Examples of monomers constituting acrylates include methyl methacrylate, ethyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, methoxyethyl methacrylate, butoxyethyl methacrylate, and phenyl methacrylate.

[0404] These epoxy (meth)acrylate compounds and urethane (meth)acrylate compounds can be used together as needed. Furthermore, various known methods can be cited as methods for polymerizing them, specifically methods such as irradiation with energy rays containing ionizing radiation or heating.

[0405] When using ultraviolet light to cure and form a primer, it is preferable to use acetophenone, benzophenone, Michler's benzoyl benzoate, α-pentyl oxime ester, or thioxanone as photopolymerization initiators, and n-butylamine, triethylamine, or tri-n-butylphosphine as photosensitizers, in combination. Alternatively, in the first embodiment, epoxy (meth)acrylate compounds and urethane (meth)acrylate compounds may be used in combination.

[0406] Furthermore, these epoxy (meth)acrylate compounds and urethane (meth)acrylate compounds can be diluted using (meth)acrylate monomers. Examples of such (meth)acrylate monomers include methyl methacrylate, ethyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, methoxyethyl methacrylate, butoxyethyl methacrylate, phenyl methacrylate, trimethylolpropane tri(meth)acrylate, hexanediol (meth)acrylate, tripropylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, etc.

[0407] In the case of using urethane (meth)acrylate compounds as the base coating, the oxygen barrier properties of the obtained gas barrier laminate 8 can be further improved.

[0408] The thickness of the base coating in the first embodiment, measured by coating amount, is typically 0.01 to 100 g / m. 2 Within the range of 0.05–50 g / m³, it is preferred. 2 Within the range.

[0409] (Adhesive layer)

[0410] Additionally, an adhesive layer 6 can be provided on the gas barrier layer 5. The adhesive layer 6 may contain any known adhesive. Examples of adhesives include laminated adhesives composed of organotitanium resins, polyethyleneimine resins, urethane resins, epoxy resins, acrylic resins, polyester resins, resins containing oxazoline groups, modified silicone resins and alkyl titanates, polyester polybutadiene, etc.; or one-component and two-component polyols and polyisocyanates, aqueous urethanes, ion-crosslinked polymers, etc. Alternatively, water-based adhesives using acrylic resins, vinyl acetate resins, urethane resins, polyester resins, etc., as main raw materials may also be used.

[0411] Furthermore, depending on the intended use of the gas barrier laminate 8, other additives such as curing agents and silane coupling agents can be added to the adhesive. When the gas barrier laminate is intended for use in hot water treatment such as boiling, from the viewpoint of heat resistance and water resistance, a dry lamination adhesive, represented by a polyurethane adhesive, is preferred, and a solvent-based two-component curing polyurethane adhesive is more preferred.

[0412] The gas barrier laminate 8 according to the first embodiment has excellent gas barrier performance after cooking, and can also be used appropriately as a packaging material for various purposes such as medical use, industrial use, and daily necessities, including packaging materials, especially food packaging materials for contents requiring high gas barrier properties.

[0413] In addition, the gas barrier laminate 8 of the first embodiment can be suitably used, for example, as a vacuum insulation film requiring high barrier performance; a sealing film for sealing electroluminescent elements, solar cells, etc.; and so on.

[0414] <Second Implementation Method>

[0415] Figure 5 A cross-sectional view illustrating an example of the structure of the gas barrier laminate of the second embodiment.

[0416] The gas barrier laminate 100 includes a substrate layer 101, a gas barrier layer 103 disposed on at least one side of the substrate layer 101, and an inorganic layer 102 disposed between the substrate layer 101 and the gas barrier layer 103.

[0417] When time-of-flight secondary ion mass spectrometry (TOF-SIMS) was performed on the gas barrier layer 103, PO2 - Let the mass peak intensity be I(PO2) - ), PO3 - The mass peak intensity is set as I(PO3) - ) and C3H3O2 - The mass peak intensity is set as I(C3H3O2) - When ), {I(PO2) - )+I(PO3 - )} / I(C3H3O2 - The value of ) is 0.02 to 5, preferably 0.05 to 3.

[0418] In addition, the gas barrier layer 103 contains one or more metal elements selected from the group consisting of Zn, Ca, Mg, Ba and Al. The composition ratio of the aforementioned metal elements in the gas barrier layer 103, as determined by X-ray photoelectron spectroscopy analysis of the gas barrier layer 103, is 1 to 15 atomic percent, preferably 1.5 to 12 atomic percent.

[0419] {I(PO2 - )+I(PO3 - )} / I(C3H3O2 - The value of ) is 0.02 to 5, and the composition ratio of the above-mentioned metal elements in the gas barrier layer 103 is 1 to 15 atomic percent, which can be given meaning as follows.

[0420] PO2 was detected from the gas barrier layer 103 by mass spectrometry analysis. - PO3 - This refers to the fact that the gas barrier layer 103 contains phosphorus compounds, such as phosphoric acid. Furthermore, it is believed that I(PO2) - )+I(PO3 - The value is related to the amount (concentration) of phosphorus compounds in the gas barrier layer 103.

[0421] In addition, C3H3O2 was detected in the gas barrier layer 103 by mass spectrometry analysis. - This refers to the fact that the gas barrier layer 103 contains polyacrylic acid or its derivatives / similar compounds (such as polyacrylic acid) as a polycarboxylic acid. Furthermore, it is believed that I(C3H3O2) - The value is related to the amount (concentration) of carboxyl groups of polycarboxylic acids contained in the gas barrier layer 103.

[0422] According to the inventors' insights and research, phosphorus compounds, such as phosphoric acid, interact with multivalent metals such as Zn, Ca, Mg, Ba, and Al, thereby forming phosphate-multivalent metal bonds in the gas barrier layer 103. Although the details are unclear, it is believed that these phosphate-multivalent metal bonds are not easily broken by hydration, and therefore exhibit resistance to cooking treatments. The presence of these phosphate-multivalent metal bonds ensures good gas barrier properties even after cooking treatments.

[0423] {I(PO2 - )+I(PO3 - )} / I(C3H3O2 - The value of 0.02 to 5 indicates that the gas barrier layer 103 contains a relatively sufficient amount of phosphorus compounds, based on polycarboxylic acids, etc.

[0424] Furthermore, the composition ratio of the aforementioned metal elements in the gas barrier layer 103 is 1 to 15 atomic percent, which means that the gas barrier layer 103 contains an appropriate amount of polyvalent metals that are cross-linked with phosphoric acid, etc.

[0425] That is, the gas barrier layer 103 {I(PO2) - )+I(PO3 - )} / I(C3H3O2 - The value of ) is 0.02 to 5 and the composition ratio of the above-mentioned metal elements in the gas barrier layer 103 is 1 to 15 atomic percent. This corresponds to the presence of a sufficient amount of phosphate-polyvalent metal bonds in the gas barrier layer 103 (which is resistant to boiling treatment, etc.).

[0426] Furthermore, according to the inventors of this application, by including one or more metal elements selected from Zn, Ca, Mg, Ba, and Al in the gas barrier layer 103, a cross-linking structure such as -COO...M...OOC-, which can be formed between the carboxyl groups of polyacrylic acid and the metal element, can be introduced into the gas barrier layer 103. It is believed that by including such a cross-linking structure in the barrier layer 103, the barrier properties are further improved.

[0427] To be on the safe side, it should be stated beforehand that the so-called "composition ratio of Zn, Ca, Mg, Ba and Al in the gas barrier layer 103" means the total ratio of the elements in the case where the gas barrier layer 103 contains multiple metal elements.

[0428] The analysis of the gas barrier layer 103 based on TOF-SIMS is supplemented in advance.

[0429] To analyze the interior of the gas barrier layer 103, it is preferable to sputter-etch the surface of the gas barrier layer 103 using an Ar-gas cluster ion beam (Ar-GCIB) attached to a TOF-SIMS analyzer before analysis, thereby exposing the interior of the gas barrier layer 103. The use of Ar-GCIB reduces damage to the gas barrier layer 103 caused by etching.

[0430] An example of specific conditions for Ar-GCIB etching is shown.

[0431] GCIB output: 5kV, 5μA

[0432] GCIB processing time: The point at which the spectral pattern of TOF-SIMS no longer changes.

[0433] Additionally, an example of specific conditions for TOF-SIMS analysis is shown.

[0434] Analytical apparatus: PHI NaNo TOF II manufactured by ULVAC-PHI

[0435] Primary ion: Bi3 ++

[0436] Primary ion source output: 30kV, 0.5μA

[0437] Analysis area: 300×300μm (as the scanning area for the primary ion beam)

[0438] During analysis, charge neutralization is achieved through low-energy electron beams and low-energy Ar ion irradiation attached to the device.

[0439] The analysis method for the data obtained from TOF-SIMS is recorded in advance.

[0440] For detailed mass spectrometry analysis, it is preferable to obtain the mass number m for each positive and negative secondary ion using the analytical apparatus. i and the corresponding count c i As a pair of raw data columns and total ion count (C T Here, i = 0, 1, ..., N. The original data column is for m. i And sorted in ascending order. C T It is the total count of secondary ions detected by the detector.

[0441] Let the range of mass numbers around the mass spectral peak of interest be defined as i = N1, N1+1, ..., N2. Using the following formula... i The data c of the counts obtained through analysis within this range i To approximate the result. Specifically, this is achieved by using the background level b. 0 and K trigonometric functions Y j (m i Curve fitting to c i To approach.

[0442] [Mathematical Expression 4]

[0443]

[0444] In the above mathematical formula, b 0 Y is a constant. j (m i )yes Figure 7 As shown, in mass number x 0 j It has a peak value Y 0 j The function (trigonometric function) is represented by the following formula.

[0445] [Mathematical Expression 5]

[0446]

[0447] Trigonometric function Y j (m i The full width at half maximum (FWHM) is (B - j +B + j ) / 2.

[0448] b 0 x 0 j Y 0 j B - j B + j These become the fitting parameters. With respect to j, j = 1, ..., K.

[0449] For example, the background of the spectrum is not a constant value but is relative to m. i In the case of linear change, b 0 With trigonometric function Y j (m i The combination of these factors approximates the baseline.

[0450] When the mass spectrum peak of interest is a single peak, the background is removed and one trigonometric function is used for approximation. When the mass spectrum peak of interest is close to other mass peaks, the other mass peaks are also included and multiple trigonometric functions are used for approximation.

[0451] When the target mass spectrum peak, after approximation, is set to the j=kth peak among K trigonometric functions, the peak intensity I is determined by Y up to i=N1, ..., N2. k (m i The sum of ) is expressed by the total ion count (C T The numerical representation obtained by standardization is calculated by the following formula.

[0452] [Mathematical Expression 6]

[0453]

[0454] If a mass spectrum peak has a tail, it becomes difficult to define the range of mass numbers corresponding to the count. Therefore, in the above text, to avoid this, a trigonometric function was used to approximate the mass spectrum peak. This ignores the count at the tail of the mass spectrum peak. Curve fitting is performed so that the central portion of the mass spectrum peak matches the trigonometric function.

[0455] The mass numbers of the fragments of interest in Embodiment 2 are calculated in advance and are shown below. Atomic masses of isotopes are referenced at https: / / physics.nist.gov / .

[0456] [Table 3]

[0457]

[0458] The calculation of the mass peak intensity of the fragments of interest in the second embodiment is supplemented in advance.

[0459] (PO2 - (Calculation of peak mass intensity)

[0460] Focusing on the mass number range of negative secondary ion spectra (62.5–63.3), based on the equivalent... 31 P 16 O2 - The trigonometric function and m obtained by approximating the mass peak near 62.964 i The data is used to calculate the sum of the counts, using C. T Standardize and use the resulting value as PO2 - Mass peak intensity I(PO2) - ).

[0461] An example of curve fitting is shown below. Figure 8 The calculation results of the parameters used and the sum of the counts are shown in the table below. Based on the target PO2... - The triangular function and m obtained by approximating the shape of the mass peak i The total count obtained from the data is 436. The total ion count of the negative secondary ions at this time (C...) T ) = 6838528, therefore, PO2 - Mass peak intensity I(PO2) - As described below.

[0462] I(PO2 - ) = 436 / 6838528 = 5.48 × 10 -5

[0463] [Table 4]

[0464]

[0465] Examples of curve fitting were shown in advance. Figure 8 To supplement.

[0466] (i) In order to obtain measurement data near the target peak position c i The approximation curve y i It requires "background b"0 The curves of "triangular function approximation of other components" and "triangular function Y as the target" j (m i The curve is )”.

[0467] (ii) in Figure 8 In the example, in order to obtain reproducible measurement data c in the range of mass number (m / z) around 62.94 to 62.98. i The "approximation curve y" i “background b” was used 0 "The trigonometric function Y as the target" j (m i The curves for “trigonometric function approximation of other components” (in Table 2, j=1) and “trigonometric function approximation of other components” (in Table 2, j=0).

[0468] (iii) Trigonometric functions were not used to approximate the large peaks around m / z of 63 to 63.05 because they did not significantly overlap with the target peak components.

[0469] (PO3 - (Calculation of peak mass intensity)

[0470] Focusing on the mass number range of negative secondary ion spectra (78.5–79.3), based on the equivalent... 31 P 16 O3 - The trigonometric function and m obtained by approximating the mass peak near 78.959 i The data is used to calculate the sum of the counts, using C. T Standardize and use the resulting value as PO3 - Mass peak intensity I(PO3) - ).

[0471] (C3H3O2 - (Calculation of peak mass intensity)

[0472] Focusing on the mass number range of negative secondary ion spectra (70.7–71.4), based on the data obtained from curve fitting, the corresponding... 12 C3 1 H3 16 O2 - The trigonometric function Y is obtained by approximating the mass peak near 71.013. k (m i ) and m i The data is used to calculate the sum of the counts, using C. T Standardize and use the resulting value as C3H3O2 - Mass peak intensity I(C3H3O2)- ).

[0473] (CN - (Calculation of peak mass intensity)

[0474] Focusing on the mass number range of negative secondary ion spectra (70.7–71.4), based on the data obtained from curve fitting, the corresponding... 12 C 14 N - The trigonometric function Y is obtained by approximating the mass peak near 26.003. k (m i ) and m i The data is used to calculate the sum of the counts, using C. T Standardize and use the resulting value as CN - Mass peak intensity I (CN) - ).

[0475] The preliminary analysis of the gas barrier layer 103 based on X-ray photoelectron spectroscopy is supplemented.

[0476] This illustrates an example of the specific conditions under which the analysis is performed.

[0477] Analytical apparatus: KRATOS AXIS-NOVA

[0478] X-ray source: Monochromatic Al-Kα

[0479] X-ray source output: 15kV, 10mA

[0480] Analysis area: 300×700μm

[0481] The analysis used a neutralizing electron gun for charge correction.

[0482] To analyze the interior of the gas barrier layer 103, it is desirable to sputter-etch the surface of the gas barrier layer prior to analysis. However, to mitigate the damage to the gas barrier layer caused by etching, it is desirable to use etching based on an Ar-gas cluster ion beam source.

[0483] The elements to be detected are determined by a broad-spectral scan, and the spectra of each element are obtained by a narrow-scan method. Then, the background determined by the Shirley method is removed from the obtained spectra, and the atomic composition ratio (atomic %) of the detected element is calculated using the relative sensitivity coefficient method based on the obtained peak area.

[0484] Furthermore, the detection sensitivity of atomic composition ratios in typical XPS analysis is considered to be around 0.1 atomic percent. For example, in cases where trace amounts of phosphorus compounds are added to the gas barrier layer, the presence of P may sometimes be undetectable by XPS analysis.

[0485] As another perspective, the gas barrier layer 103 preferably contains a relatively large amount of carboxylate structures (and, as a result, a small amount of free carboxyl groups). This means that the gas barrier layer 103 contains, to some extent, a cross-linked structure of, for example, metal-carboxyl groups. By including a relatively large amount of carboxylate structures in the gas barrier layer 103, the gas barrier properties can be further improved.

[0486] Specifically, in the absorption spectrum obtained by infrared spectroscopy measurement of the gas barrier layer 103 using total internal reflection measurement, the 1493 cm⁻¹... -1 The above 1780cm -1 Let the total peak area within the following absorption band range be A, and let 1493 cm⁻¹ be the maximum peak area. -1 The above is 1598cm -1 When the total peak area within the following absorption band range is set as D, the area ratio D / A is preferably 0.5 or more, more preferably 0.58 or more, and even more preferably 0.6 or more. The upper limit of D / A is, for example, 0.8 or less.

[0487] Based on past insights into infrared spectroscopy and the insights of the inventors of this application, since the absorption of νC=O based on free carboxylic acids is 1700 cm⁻¹ -1 Near the same location, the absorption of ν(C=O) based on carboxylates is 1540–1560 cm⁻¹. -1 Therefore, the D / A ratio can be used as an indicator of the amount of carboxylate structures contained in the gas barrier layer 103. Furthermore, as will be described later, in the case where the gas barrier layer 103 contains polyamines, the ratio is sometimes between 1630 and 1685 cm⁻¹. -1 Absorption based on amide bonds (ν(C=O)) was observed nearby.

[0488] Specifically, infrared spectroscopy measurements can be performed using total reflectance measurement, as described below.

[0489] First, a 1cm × 3cm sample for measurement is cut out from the gas barrier layer 103.

[0490] Next, the infrared absorption spectrum of the surface of the gas barrier layer 103 was obtained by infrared total reflectance measurement (ATR method).

[0491] In the obtained infrared absorption spectrum, 1493 cm⁻¹ -1 The measuring point at 1780cm -1 The measurement points at point N are connected by a straight line (baseline: N), and the difference spectrum between the obtained infrared absorption spectrum and N is set as the spectrum (S). BNHowever, when the thickness of the gas barrier layer 103 is less than about 0.5 μm, the measured infrared absorption spectrum contains the influence of layers lower than the gas barrier layer.

[0492] In this case, a substrate consisting only of the lower layer without a gas barrier layer is also prepared as the test sample. Similarly, the ATR-IR spectrum of the substrate surface is obtained, and the difference spectrum with the baseline N is calculated and set as the spectrum (S). SN ). At 1493cm -1 Up to 1780cm -1 When a distinct absorption peak is observed within the wavenumber range, differential spectral analysis is performed according to the following formula to obtain a spectrum that excludes the influence of the substrate (S). BN ').

[0493] <spectrum (S) BN ')>=< Spectrum (S) BN )>-α*<spectrum(S SN )>

[0494] Here, α is a coefficient used to exclude the influence of the substrate, and 0 ≤ α < 1.

[0495] In the obtained difference spectrum (S BN In '), 1493cm -1 Up to 1780cm -1 The area of ​​the spectrum in the wavenumber range is taken as the total peak area A, and 1493 cm⁻¹ is used as the peak area. -1 Up to 1598cm -1 The area of ​​the spectrum within the wavenumber range is taken as the total peak area D.

[0496] Here, as a specific example, for the case where the substrate layer is a polyethylene terephthalate (PET) film, the method for determining the coefficient α used to exclude the influence of the substrate composed of the substrate layer, inorganic layer, etc. is supplemented.

[0497] PET at 1700cm -1 There is a large absorption peak nearby, therefore for 1493 cm⁻¹ -1 Up to 1780cm -1 The calculation of the peak area within the wavenumber range has an impact. To eliminate this effect, the usual difference spectral analysis method is used. For example, as with 1493 cm⁻¹ -1 Up to 1780cm -1 The sharp absorption peak of PET, which is adjacent to the wavenumber range and does not overlap with the absorption peak of the gas barrier layer, was selected at 1340 cm⁻¹. -1 The nearby absorption peak is used as a reference peak. The spectrum obtained through the above differential spectral analysis (S...) BN In '), with 1340cm -1The coefficient α is adjusted to determine how the nearby reference peak disappears, thereby obtaining a 1700 cm⁻¹ peak. -1 The influence of the absorption peak of nearby PET was eliminated in the spectrum (S BN ').

[0498] Alternatively, the coefficient α can also be obtained as the area ratio of the infrared absorption spectrum, as described below.

[0499] For the infrared absorption spectrum obtained from the surface of the gas barrier layer and the infrared absorption spectrum of the substrate consisting only of the lower layer without a gas barrier layer, 1325 cm⁻¹... -1 The measuring point at 1355cm -1 The measurement points at 1325cm are connected by a straight line (baseline: M). -1 ~1355cm -1 Within the wavenumber range, the difference spectrum between the obtained infrared absorption spectrum and the baseline M is obtained, and denoted as the spectrum (S). BM ), spectrum (S) SM For the spectrum (S) BM ) and spectrum (S SM If 1325cm -1 Above 1355cm -1 The peak areas below are respectively set as areas (A) BM ), area (A) SM If ), then the coefficient α can be obtained by the following formula.

[0500] α=A BM / A SM

[0501] For the determination of infrared absorption spectra (infrared total internal reflection measurement: ATR method), for example, an IRT-5200 instrument manufactured by Nippon Spectrophotometer Co., Ltd. can be used, equipped with a PKM-GE-S (germanium) crystal, at an incident angle of 45 degrees, room temperature, and a resolution of 4 cm⁻¹. -1 The test was conducted under the condition of a cumulative total of 100 tests.

[0502] Figure 6 A cross-sectional view is shown schematically to illustrate other configurations of the gas barrier laminate.

[0503] Figure 6 The basic structure of the gas barrier laminate 110 and Figure 5 The gas barrier laminate 100 is similar, but differs in that the substrate layer 101 and the inorganic layer 102 are not directly in contact, and that it also includes an undercoat layer 104 disposed between the substrate layer 101 and the inorganic layer 102.

[0504] The same effect as that of the gas barrier laminate 100 can be obtained in the gas barrier laminate 110. Furthermore, in the gas barrier laminate 110, by providing an undercoat layer 104 between the substrate layer 101 and the inorganic layer 102, the adhesion between the substrate layer 101 and the inorganic layer 102 can be further improved.

[0505] The gas barrier laminate of the second embodiment can be manufactured by using appropriate raw materials in appropriate amounts and selecting appropriate manufacturing methods and conditions. Details will be described thereafter, but from the perspective of forming a cross-linked structure, it is preferable to appropriately set, in addition to the type and amount of raw materials, the manufacturing conditions for forming, for example, the heat treatment temperature and time described later, during the formation of the gas barrier layer 103.

[0506] The following section provides a detailed description of the layers that a gas barrier laminate may contain.

[0507] (Gas barrier layer)

[0508] The gas barrier layer 103 is composed of a cured material, for example, a mixture containing polycarboxylic acids such as polyacrylic acid, polyamine compounds, and polyvalent metal compounds. More specifically, the gas barrier layer 103 is a film (gas barrier film 10) composed of the aforementioned cured material.

[0509] More specifically, the gas barrier layer 103 can be obtained, for example, by coating a mixture (gas barrier coating material) before curing onto a layer such as the inorganic layer 102 disposed immediately below the gas barrier layer 103, followed by drying and heat treatment to cure the gas barrier coating material.

[0510] The following describes the components that may be included in the mixture (gas barrier coating material) before curing. By appropriately selecting the types and amounts of these components and providing the gas barrier layer 103, the gas barrier laminate of the second embodiment can be manufactured.

[0511] • Polycarboxylic acids

[0512] Polycarboxylic acids are compounds having two or more carboxyl groups within their molecules. Specifically, examples include homopolymers or copolymers of α,β-unsaturated carboxylic acids such as (meth)acrylic acid, itaconic acid, fumaric acid, crotonic acid, cinnamic acid, 3-hexenoic acid, and 3-hexenediaic acid. Alternatively, they can be copolymers of the aforementioned α,β-unsaturated carboxylic acids with esters such as ethyl esters, olefins such as ethylene, etc.

[0513] Among them, the preferred polymers are homopolymers or copolymers of acrylic acid, methacrylic acid, itaconic acid, fumaric acid, crotonic acid, and cinnamic acid; more preferably, one or more polymers selected from the group consisting of polyacrylic acid, polymethacrylic acid, and copolymers of acrylic acid and methacrylic acid; further preferably, at least one polymer selected from polyacrylic acid and polymethacrylic acid; and even more preferably, at least one polymer selected from homopolymers of acrylic acid and homopolymers of methacrylic acid.

[0514] In this second embodiment, the term "polyacrylic acid" includes both homopolymers of acrylic acid and copolymers of acrylic acid with other monomers. In the case of copolymers of acrylic acid with other monomers, for polyacrylic acid, 100% by mass of the polymer contains structural units derived from acrylic acid, typically 90% by mass or more, preferably 95% by mass or more, and more preferably 99% by mass or more.

[0515] Furthermore, in the second embodiment, the term "polymethacrylic acid" includes both homopolymers of methacrylic acid and copolymers of methacrylic acid with other monomers. In the case of copolymers of methacrylic acid with other monomers, for polymethacrylic acid, 100% by mass of the polymer contains structural units derived from methacrylic acid, typically 90% by mass or more, preferably 95% by mass or more, and more preferably 99% by mass or more.

[0516] Polycarboxylic acids are polymers formed by the polymerization of carboxylic acid monomers. From the viewpoint of excellent balance between gas barrier properties and operability, the molecular weight of polycarboxylic acids is preferably 500 to 2,500,000, more preferably 5,000 to 2,000,000, even more preferably 10,000 to 1,500,000, and even more preferably 100,000 to 1,200,000.

[0517] In this second embodiment, the molecular weight of the polycarboxylic acid is the weight-average molecular weight converted from polyethylene oxide, which can be determined using gel permeation chromatography (GPC).

[0518] At least a portion of a polycarboxylic acid can be neutralized using a volatile base. By neutralizing the polycarboxylic acid with a volatile base, gelation can be suppressed when polyvalent metal compounds or polyamine compounds are mixed with the polycarboxylic acid. Therefore, from the viewpoint of preventing gelation, it is preferable to prepare a partially or completely neutralized carboxyl group using a volatile base. The neutralized product can be obtained by partially or completely neutralizing the carboxyl group of the polycarboxylic acid with a volatile base, that is, by partially or completely preparing a carboxylate of the polycarboxylic acid. This prevents gelation when polyamine compounds or polyvalent metal compounds are added.

[0519] Partial neutralization is prepared by adding a volatile base to an aqueous solution of a polycarboxylic acid polymer. The desired degree of neutralization can be achieved by adjusting the molar ratio of the polycarboxylic acid to the volatile base. In the second embodiment, from the viewpoint of sufficiently suppressing gelation caused by the neutralization reaction with the amino group of the polyamine compound, the degree of neutralization of the polycarboxylic acid obtained using the volatile base is preferably 70 to 300 equivalents, more preferably 90 to 250 equivalents, and even more preferably 100 to 200 equivalents.

[0520] As a volatile base, any water-soluble base can be used.

[0521] Examples of volatile bases include, for example, tertiary amines such as ammonia, morpholine, alkylamines, 2-dimethylaminoethanol, N-methylmorpholine, ethylenediamine, triethylamine, or aqueous solutions of these, or mixtures thereof. From the viewpoint of obtaining good gas barrier properties, aqueous ammonia solutions are preferred.

[0522] Polyamine compounds

[0523] The mixture before curing preferably contains a polyamine compound. Polyamine compounds can react with polycarboxylic acids to form a cross-linked structure (amide bond). This further improves gas barrier properties.

[0524] Polyamine compounds are compounds having two or more amino groups on their main chain, side chain, or terminal, and are preferably polymers. Specifically, examples include aliphatic polyamines such as polyallylamine, polyvinylamine, polyethyleneimine, and poly(propyleneimine); polyamides such as polylysine and polyarginine, which have amino groups on their side chains; and so on. Alternatively, polyamines can be formed by modifying a portion of the amino groups.

[0525] From the viewpoint of obtaining good gas barrier properties, the polyamine compound preferably contains polyethyleneimine, and more preferably polyethyleneimine.

[0526] From the viewpoint of achieving a good balance between gas barrier properties and operability, the number average molecular weight of the polyamine compound is preferably 50 to 2,000,000, more preferably 100 to 1,000,000, even more preferably 1,500 to 500,000, even more preferably 1,500 to 100,000, even more preferably 1,500 to 50,000, even more preferably 3,500 to 20,000, even more preferably 5,000 to 15,000, and even more preferably 7,000 to 12,000.

[0527] The molecular weight of polyamine compounds can be determined using the boiling point elevation method and the viscosity method.

[0528] From the viewpoint of further improving the gas barrier performance after cooking, the ratio of (moles of amino groups in the polyamine compound in the mixture) to (moles of -COO- groups in the polycarboxylic acid in the mixture) is preferably 0.20 or more, more preferably 0.25 or more, even more preferably 0.30 or more, even more preferably 0.35 or more, and even more preferably 0.40 or more.

[0529] From the same point of view, the ratio of (moles of amino groups contained in the polyamine compound in the mixture) to (moles of -COO- groups contained in the polycarboxylic acid in the mixture) is preferably 0.90 or less, more preferably 0.85 or less, even more preferably 0.80 or less, even more preferably 0.75 or less, and even more preferably 0.70 or less.

[0530] Although the detailed reasons are unclear, it is believed that by achieving a good balance between amide crosslinking (which is formed by amino groups constituting polyamine compounds) and metal crosslinking (which is formed by polyvalent metals constituting polycarboxylic acids and polyvalent metal salts) to form a dense structure, a gas barrier layer 103 with excellent gas barrier performance after cooking and a gas barrier laminate having the same can be obtained.

[0531] Regarding polyamine compounds, when performing time-of-flight secondary ion mass spectrometry analysis on the gas barrier layer 103, CN... - The peak intensity is set to I(CN) - ) and C3H3O2 - The peak intensity is set to I(C3H3O2) - When I(CN) - ) / I(C3H3O2 - The value of ) is 2 or less, preferably 1.8 or less, and more preferably 1.5 or less. I(CN) - ) / I(C3H3O2 - The lower limit for the value of ) is, for example, 0, preferably 0.2, and more preferably 0.4. Details regarding time-of-flight secondary ion mass spectrometry analysis are as described above.

[0532] CN detected by mass spectrometry analysis - It originates from polyamines. Therefore, it is believed that I(CN) - ) / I(C3H3O2 - The value of ) is appropriate, which corresponds to the above-mentioned "the good balance between amide crosslinking (which is formed by amino groups constituting polyamine compounds) and metal crosslinking (which is formed by polyvalent metals constituting salts of polycarboxylic acids and polyvalent metals) forms a dense structure".

[0533] ·Metal

[0534] As described above, the gas barrier layer 103 preferably contains one or more metallic elements selected from the group consisting of Zn, Ca, Mg, Ba, and Al. Therefore, the mixture before curing preferably contains compounds of these metals. Among them, for suitability for packaging cooked foods, compounds containing Mg and compounds containing Zn are preferred, and compounds containing Zn are more preferred.

[0535] Examples of metal compounds include oxides, hydroxides, halides, carbonates, phosphates, phosphites, hypophosphites, sulfates, and sulfites of the aforementioned metals. From the viewpoint of water resistance and impurities, metal oxides or metal hydroxides are preferred.

[0536] The preferred metal compound is one or more compounds selected from the group consisting of oxides such as magnesium oxide, calcium oxide, barium oxide, zinc oxide, and magnesium hydroxide, and hydroxides such as calcium hydroxide, barium hydroxide, and zinc hydroxide. More preferably, it is at least one of zinc oxide and zinc hydroxide, and even more preferably, it is zinc oxide.

[0537] In the second embodiment, from the viewpoint of further improving the gas barrier performance after cooking, the ratio of (moles of metal compounds in the mixture) to (moles of -COO- groups contained in the polycarboxylic acid in the mixture) is preferably 0.1 or more, more preferably 0.13 or more, even more preferably 0.15 or more, and even more preferably 0.18 or more.

[0538] From the same point of view, the ratio of (moles of polyvalent metal compounds in the mixture) to (moles of -COO- groups contained in the polycarboxylic acid in the mixture) is preferably 0.80 or less, more preferably 0.70 or less, even more preferably 0.60 or less, even more preferably 0.55 or less, and even more preferably 0.50 or less.

[0539] In the second embodiment, from the viewpoint of further improving the gas barrier performance after cooking, the ratio of (moles of metal compounds in the mixture) to (moles of amino groups from polyamine compounds in the mixture) is preferably 0.25 or more, more preferably 0.35 or more, and even more preferably 0.40 or more.

[0540] From the same point of view, the ratio of (moles of metal compounds in the mixture) to (moles of amino groups from polyamine compounds in the mixture) is preferably 0.75 or less, more preferably 0.60 or less, and even more preferably 0.55 or less.

[0541] Phosphorus compounds or their salts

[0542] As described above, PO2 was detected during mass spectrometry analysis of the barrier layer 103.- and / or PO3 - To establish such a barrier layer 103, the mixture prior to curing preferably contains a phosphorus compound or a salt thereof.

[0543] Phosphorus compounds or their salts contain one or more -P-OH groups in their molecular structure. Phosphorus compounds can be complexed in mixtures in the form of salts.

[0544] From the viewpoint of further improving the steam barrier properties after cooking, the phosphorus compound preferably contains two or more -P-OH groups, more preferably three or more -P-OH groups. Furthermore, from a productivity viewpoint, the number of -P-OH groups in the phosphorus compound can, for example, be ten or less.

[0545] Specific examples of phosphorus compounds include phosphoric acid, phosphorous acid, phosphonic acid, hypophosphoric acid, polyphosphoric acid, and their derivatives.

[0546] Specifically, polyphosphoric acid has a condensation structure of two or more phosphoric acids in its molecular structure. Examples include diphosphoric acid (pyrophosphoric acid), triphosphoric acid, and polyphosphoric acid formed by the condensation of four or more phosphoric acids.

[0547] Specific examples of derivatives include esters of the aforementioned phosphorus compounds such as phosphoric acid starch and cross-linked phosphoric acid starch; halides such as chlorides; acid anhydrides such as phosphorus tetraoxide; and compounds with structures such as triazine (methylenephosphonic acid) and N,N,N',N'-ethylenediaminetetra(methylenephosphonic acid) having hydrogen atoms bonded to phosphorus atoms replaced by alkyl groups.

[0548] From the viewpoint of further improving the balance between barrier properties and productivity, the phosphorus compound is one or more selected from the group consisting of phosphoric acid, phosphorous acid, hypophosphoric acid, polyphosphoric acid, phosphonic acid and their salts, more preferably at least one selected from the group consisting of phosphoric acid and phosphorous acid, phosphonic acid and their salts.

[0549] Furthermore, specific examples of salts in phosphorus compounds include salts of monovalent metals such as sodium and potassium, and ammonium salts. From a barrier perspective, ammonium salts are preferred for phosphorus compounds.

[0550] In the second embodiment, from the viewpoint of improving barrier properties, the ratio of (the number of moles of P atoms in the phosphorus compound or phosphorus compound derived from its salt) to (the number of moles of -COO- groups derived from the polycarboxylic acid in the mixture) is preferably 0.0005 or more, more preferably 0.001 or more, even more preferably 0.003 or more, and even more preferably 0.005 or more. In phosphorus compounds containing one P atom in their chemical formula, such as phosphoric acid, the number of moles of P atoms and the number of moles of the phosphorus compound have the same meaning.

[0551] Furthermore, from the viewpoint of barrier properties and productivity (stability of the coating solution, uniformity / appearance of the coating film), the ratio of (moles of phosphorus compounds in the mixture or phosphorus compounds from its salts) to (moles of -COO- groups from polycarboxylic acids in the mixture) is preferably 0.3 or less, more preferably 0.1 or less, even more preferably 0.08 or less, and even more preferably 0.05 or less.

[0552] Other ingredients

[0553] The mixture before curing may contain components other than those mentioned above.

[0554] For example, the mixture preferably also contains ammonium carbonate salts. Ammonium carbonate salts are substances added to improve the solubility of polyvalent metal compounds by converting them into ammonium carbonate complexes, thereby preparing a homogeneous solution containing the polyvalent metal compounds. By including ammonium carbonate salts in the mixture before curing, the solubility of the polyvalent metal compounds can be increased, resulting in a more homogeneous mixture containing the polyvalent metal compounds.

[0555] As a carbonate-based ammonium salt, examples include ammonium carbonate and ammonium bicarbonate. From the perspective of easy volatilization and not easy to remain in the obtained gas barrier layer, ammonium carbonate is preferred.

[0556] From the viewpoint of further improving the solubility of polyvalent metal compounds, the ratio of (moles of ammonium carbonate salt in the mixture) to (moles of metal compound in the mixture) is preferably 0.05 or more, more preferably 0.10 or more, even more preferably 0.25 or more, even more preferably 0.50 or more, and particularly preferably 0.75 or more.

[0557] Furthermore, from the viewpoint of further improving the coatability of the coating material for gas barrier applications, the ratio of (moles of ammonium carbonate salt in the coating material for gas barrier applications) to (moles of metal compound in the coating material for gas barrier applications) is preferably 10.0 or less, more preferably 5.0 or less, even more preferably 2.0 or less, and even more preferably 1.5 or less.

[0558] Furthermore, from the viewpoint of suppressing depressions when coating as a gas barrier coating material, the mixture before curing preferably also contains a surfactant.

[0559] When the total solid component of the mixture is set to 100% by mass, the amount of surfactant added is preferably 0.01 to 3% by mass, more preferably 0.01 to 1% by mass.

[0560] Examples of surfactants include anionic surfactants, nonionic surfactants, cationic surfactants, and amphoteric surfactants. From the viewpoint of obtaining good coatability, nonionic surfactants are preferred, and polyoxyethylene alkyl ethers are more preferred.

[0561] Examples of nonionic surfactants include polyoxyalkylene alkyl ethers, polyoxyalkylene alkyl ethers, polyoxyalkylene fatty acid esters, sorbitan fatty acid esters, organosilicon surfactants, alkynyl alcohol surfactants, and fluorinated surfactants.

[0562] Examples of polyoxyethylene alkyl aryl ethers include, for example, polyoxyethylene nonylphenyl ether, polyoxyethylene octylphenyl ether, and polyoxyethylene dodecylphenyl ether.

[0563] Examples of polyoxyethylene alkyl ethers include, for example, polyoxyethylene oil-based ethers and polyoxyethylene lauryl ethers.

[0564] Examples of polyoxyethylene fatty acid esters include, for example, polyoxyethylene oleate, polyoxyethylene laurate, and polyoxyethylene distearate.

[0565] Examples of sorbitan fatty acid esters include, for example, sorbitan laurate, sorbitan monostearate, sorbitan monooleate, sorbitan sesquioleate, polyoxyethylene monooleate, and polyoxyethylene stearate.

[0566] Examples of organosilicon surfactants include, for example, dimethylpolysiloxane.

[0567] Examples of alkynyl alcohol surfactants include 2,4,7,9-tetramethyl-5-decyn-4,7-diol, 3,6-dimethyl-4-octyyn-3,6-diol, and 3,5-dimethyl-1-hexyn-3-ol.

[0568] Examples of fluorinated surfactants include, for example, fluoroalkyl esters.

[0569] The mixture before curing may contain additives other than those mentioned above. For example, it may contain various additives such as lubricants, slip agents, anti-caking agents, antistatic agents, anti-fogging agents, pigments, dyes, and inorganic or organic fillers.

[0570] Furthermore, from the viewpoint of improving the coatability when applied as a gas barrier coating material, the concentration of the solid component of the mixture before curing is preferably set to 0.5 to 15% by mass, and more preferably 1 to 10% by mass.

[0571] Method for manufacturing gas barrier layer

[0572] Specifically, the gas barrier layer 103 can be manufactured by applying a mixture (gas barrier coating material) before curing and then curing it.

[0573] The mixture can be obtained as described below.

[0574] First, a volatile base is appropriately added to the polycarboxylic acid, thereby completely or partially neutralizing the carboxyl groups of the polycarboxylic acid. A polyvalent metal salt compound and a suitable ammonium carbonate salt are then mixed to form a metal salt in all or part of the carboxyl groups of the polycarboxylic acid that has been neutralized by the volatile base, and in the carboxyl groups of the polycarboxylic acid that has not been neutralized by the volatile base.

[0575] Then, a polyamine compound is added, followed by a phosphorus compound or its salt, to obtain a mixture before curing. This forms a salt between the phosphorus compound and the amino group of the polyvalent metal compound or polyamine.

[0576] By mixing polycarboxylic acids, polyvalent metal salts, phosphorus compounds or their salts, appropriate ammonium carbonates, and polyamine compounds through this step, the formation of aggregates can be suppressed, resulting in a more homogeneous mixture. This allows for a more efficient dehydration condensation reaction between the -COO- groups in the polycarboxylic acids and the amino groups in the polyamine compounds.

[0577] More specifically, as described below. The following explanation will take the case of a mixture containing a volatile base and a carbonate-based ammonium salt as an example.

[0578] First, prepare a completely or partially neutralized solution of the carboxyl groups that constitute the polycarboxylic acid.

[0579] Adding a volatile base to a polycarboxylic acid completely or partially neutralizes its carboxyl groups. By neutralizing the carboxyl groups of the polycarboxylic acid, gelation that occurs when polyvalent metal compounds or polyamine compounds are added can be effectively prevented due to the reaction between the carboxyl groups constituting the polycarboxylic acid and the amino groups constituting the polyvalent metal compounds or polyamine compounds, thus obtaining a more homogeneous mixture.

[0580] Next, a polyvalent metal salt compound and a carbonate ammonium salt are added and dissolved. The resulting polyvalent metal ions react with the -COO- group constituting the polycarboxylic acid to form a polyvalent metal salt. Here, the -COO- group that forms the salt with the polyvalent metal ions refers to both the unneutralized carboxyl group and the neutralized -COO- group. In the case of the neutralized -COO- group, the polyvalent metal ions from the aforementioned polyvalent metal compound replace and coordinate to form a -COO- group polyvalent metal salt.

[0581] Then, after forming the polyvalent metal salt, a polyamine compound and a phosphorus compound or their salts are further added, thereby obtaining a mixture. At this point, the polyvalent metal salt located at the -COO- group also coordinates with the -PO- group in the phosphorus compound, forming a -COO-polyvalent metal -OP- structure. Furthermore, an ionic bond is formed between the -NH2 group in the polyamine and the -PO- group in the phosphorus compound.

[0582] The mixture thus manufactured is applied as a gas barrier coating material to the inorganic layer 102 or to an interlayer formed on the inorganic layer 102 between the gas barrier layer 103 and the inorganic layer 102, and then dried and cured to form the gas barrier layer 103. At this time, the polyvalent metal salt constituting the -COO- group of the polycarboxylic acid forms a metal crosslink, the amino group constituting the polyamine forms an amide crosslink, and the -PO- group in the phosphorus compound forms an ionic crosslink with the polyvalent metal or the amino group in the polyamine, thus obtaining a gas barrier layer 103 with excellent gas barrier properties. A more detailed manufacturing method for the gas barrier layer 103 is described later.

[0583] From the viewpoint of improving barrier properties, the thickness of the gas barrier layer 103 after drying and curing is preferably 0.01 μm or more, more preferably 0.05 μm or more, and even more preferably 0.1 μm or more.

[0584] Furthermore, from the viewpoint of reducing the overall thickness of the gas barrier laminate, the thickness of the dried and cured gas barrier layer 103 is preferably 15 μm or less, more preferably 5 μm or less, and even more preferably 1 μm or less.

[0585] (Substrate layer)

[0586] The substrate layer 101 can be a single layer or two or more layers. The shape of the substrate layer 101 is not limited; for example, it can be a sheet or film shape, a shallow dish, a cup, a hollow body, etc.

[0587] As the material for the substrate layer 101, any material capable of stably forming an inorganic layer 102 on the substrate layer 101 and capable of being coated with a solution of a gas barrier coating material on the top of the inorganic layer 102 can be used without limitation. Examples of materials for the substrate layer 101 include, for instance, resins such as thermosetting resins and thermoplastic resins, organic materials such as paper; inorganic materials such as glass, ceramics, silicon dioxide, silicon oxynitride, silicon nitride, concrete, aluminum, alumina, iron, copper, stainless steel, and other metals; and multilayer substrate layers formed by combinations of organic materials or combinations of organic and inorganic materials. Among these, for example, in applications such as packaging materials and panels, plastic films selected from the group consisting of thermosetting resins and thermoplastic resins, or organic materials such as paper, are preferred.

[0588] Known thermosetting resins can be used as thermosetting resins. Examples include epoxy resins, unsaturated polyester resins, phenolic resins, urea-melamine resins, polyurethane resins, silicone resins, and polyimides.

[0589] Known thermoplastic resins can be used as thermoplastic resins. Examples include polyolefins (polyethylene, polypropylene, poly(4-methyl-1-pentene), poly(1-butene), etc.), polyesters (polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, etc.), polyamides (nylon-6, nylon-66, poly(m-phenylene adipamide), etc.), polyvinyl chloride, polyimide, ethylene-vinyl acetate copolymer or its saponification, polyvinyl alcohol, polyacrylonitrile, polycarbonate, polystyrene, ion-crosslinked polymers, fluoropolymers, or mixtures thereof.

[0590] Among them, from the viewpoint of achieving good transparency, one or more resins selected from the group consisting of polypropylene, polyethylene terephthalate (PET), polyethylene naphthalate, polyamide, polyimide and polybutylene terephthalate are preferred.

[0591] Furthermore, from the viewpoint of excellent resistance to pinholes, damage, and heat resistance, it is preferable to use one or more resins selected from the group consisting of polyamide, polyethylene terephthalate, and polybutylene terephthalate. Similarly, from the same viewpoint, the substrate layer 101 is preferably a layer comprising one or more resins selected from the group consisting of polyamide, polyethylene terephthalate, and polybutylene terephthalate, and more preferably a layer comprising one or more of these resins.

[0592] Furthermore, when a hygroscopic material such as polyamide is used in the substrate layer 101, the substrate layer 101 absorbs moisture and swells in the gas barrier laminate, which can easily reduce the gas barrier performance under high humidity, the gas barrier performance after cooking, and the gas barrier performance when filled with acidic contents. However, in the second embodiment, even when a hygroscopic material is used as the substrate layer 101, the reduction in the gas barrier performance of the gas barrier laminate under high humidity and the gas barrier performance after cooking can be appropriately suppressed.

[0593] Alternatively, a film formed of thermosetting resin or thermoplastic resin can be stretched along at least one direction, preferably a biaxial direction, to form a substrate layer 101.

[0594] From the viewpoint of excellent transparency, rigidity and heat resistance, the substrate layer 101 is preferably a biaxially stretched film formed of one or more thermoplastic resins selected from the group consisting of polypropylene, polyethylene terephthalate, polyethylene naphthalate, polyamide, polyimide and polybutylene terephthalate, more preferably a biaxially stretched film formed of one or more thermoplastic resins selected from the group consisting of polyamide, polyethylene terephthalate and polybutylene terephthalate.

[0595] Alternatively, polyvinylidene chloride, polyvinyl alcohol, ethylene-vinyl alcohol copolymer, acrylic resin, urethane resin, etc., can be coated on the surface of the substrate layer 101.

[0596] Furthermore, for the substrate layer 101, in order to improve adhesion to the gas barrier layer 103, a surface-treated substrate layer can be applied. Specifically, the surface of the substrate layer 101 opposite to the gas barrier layer 103 can be subjected to surface activation treatments such as corona treatment, flame treatment, plasma treatment, or primer coating treatment.

[0597] From the viewpoint of obtaining good film properties, the thickness of the substrate layer 101 is preferably 1 μm or more, more preferably 5 μm or more, even more preferably 10 μm or more, and preferably 1000 μm or less, more preferably 500 μm or less, and even more preferably 300 μm or less.

[0598] (Base coat)

[0599] like Figure 6 As explained, a primer layer 104 can be provided between the substrate layer 101 and the inorganic layer 102. By providing the primer layer 104, their adhesion can be further improved, and the barrier properties after cooking can be further improved.

[0600] From the viewpoint of improving the adhesion between the substrate layer 101 and the inorganic layer 102, the material for the base coating layer 104 may be, for example, one or more selected from the group consisting of polyurethane resin, polyester resin, oxazoline resin, and (meth)acrylic resin.

[0601] Examples of polyurethane resins include various polyurethane resins, polyurethane polyurea resins, and their prepolymers. Specific examples of such urethane resins include reactions of diisocyanate components such as toluene diisocyanate, xylene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, cyclohexane diisocyanate, isophorone diisocyanate, and dicyclohexyl diisocyanate with diol components such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, neopentyl glycol, cyclohexanediol, bisphenol, polyester glycol, polyether glycol, polycarbonate glycol, and polyethylene glycol; reactions of urethane prepolymers with isocyanate groups at the ends with amino compounds, aminosulfonates, polyhydroxycarboxylic acids, and acidic sulfurous acid; and so on.

[0602] Furthermore, from the viewpoint of improving barrier properties after cooking and the adhesion between the substrate layer 101 and the inorganic layer 102, it is preferable that the polyurethane resin in the base layer 104 is composed of a polyurethane resin having an aromatic ring structure in its main chain. For example, a polyurethane resin having an aromatic ring structure in its main chain can be obtained as a water-dispersible polyurethane resin through the reaction of a polyol, an organic polyisocyanate, and a chain extender. This allows the introduction of an aromatic ring structure into the main chain of the polyurethane resin.

[0603] As a polyurethane resin having an aromatic ring structure in the main chain, more specifically, the polyurethane resin described in Japanese Patent Application Publication No. 2018-171827 can be used.

[0604] For polyurethane resins such as water-dispersible polyurethane resins, crosslinking agents can be used to improve heat resistance, water resistance, and hydrolysis resistance. The crosslinking agent can be an external crosslinking agent that is a different component from the polyurethane resin, or an internal crosslinking agent that pre-introduces reaction sites capable of forming a crosslinked structure into the molecular structure of the polyurethane resin.

[0605] As a crosslinking agent, compounds having isocyanate groups, oxazoline groups, carbodiimide groups, epoxy groups, melamine resin groups, and silanol groups can be suitably used, with compounds having carbodiimide groups being more suitable. Furthermore, when using a compound having carbodiimide groups as a crosslinking agent, the amount of the compound added is preferably 0.1 to 3.0 mol, more preferably 0.2 to 2.0 mol, and particularly preferably 0.3 to 1.0 mol, relative to 1.0 mol of carboxyl groups in the polyurethane resin.

[0606] Various polyester resins and their modifiers can be cited as examples of the polyester resin used in the primer layer 104. Specific examples of such polyester resins include reaction products of polycarboxylic acid components such as terephthalic acid, phthalic acid, isophthalic acid, trimellitic acid, pyromellitic acid, 2-sulfonic isophthalic acid, 5-sulfonic isophthalic acid, adipic acid, sebacic acid, succinic acid, and dodecanoic acid with diol components such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, neopentyl glycol, cyclohexanediol, and bisphenol, as well as modifiers based on acrylic resins, epoxy resins, etc.

[0607] When an oxazoline resin is used in the base coating 104, the base coating 104 is preferably composed of an oxazoline-based resin composition comprising an aqueous polymer containing an oxazoline group, an aqueous (meth)acrylic resin, and an aqueous polyester resin.

[0608] The oxazoline-based resin composition is, for example, composed of an aqueous polymer containing oxazoline groups with an oxazoline group content of 6.0 to 9.0 mmol / g, an aqueous (meth)acrylic resin with a carboxyl group content of 0.5 to 3.5 mmol / g, and an aqueous polyester resin with a carboxyl group content of 0.5 to 2.0 mmol / g.

[0609] In addition, the total amount of the aqueous polymer containing oxazoline, the aqueous (meth)acrylic resin and the aqueous polyester resin is set to 100% by mass. For example, the oxazoline resin composition contains 10 to 55% by mass of the aqueous polymer containing oxazoline, 10 to 80% by mass of the aqueous (meth)acrylic resin and 10 to 80% by mass of the aqueous polyester resin.

[0610] Furthermore, in the oxazoline resin composition, for example, the ratio of the molar number of oxazoline groups to the molar number of carboxyl groups [expressed as the ratio of the molar number of oxazoline groups (x mmol) to the molar number of carboxyl groups (y mmol) (x / y) × 100 [mol%]] is 150–420 mol%.

[0611] As the oxazoline resin used in the base coating 104, more specifically, the oxazoline resin described in International Publication No. 2016 / 186074 may be used.

[0612] From the viewpoint of obtaining good adhesion, the thickness of the base coating 104 is preferably 0.001 μm or more, more preferably 0.005 μm or more, even more preferably 0.01 μm or more, even more preferably 0.05 μm or more, even more preferably 0.1 μm or more, and even more preferably 0.2 μm or more.

[0613] Furthermore, from an economic point of view, the thickness of the base coating 104 is preferably 1.0 μm or less, more preferably 0.6 μm or less, even more preferably 0.5 μm or less, even more preferably 0.1 μm, and even more preferably 0.05 μm or less.

[0614] (Inorganic layer)

[0615] Inorganic materials constituting the inorganic layer 102 may include, for example, metals, metal oxides, metal nitrides, metal fluorides, and metal nitrides, which are capable of forming barrier films.

[0616] As inorganic substances constituting inorganic layer 102, examples include one or more of the following: elements selected from Group 2A of the periodic table such as beryllium, magnesium, calcium, strontium, and barium; transition elements of the periodic table such as titanium, zirconium, ruthenium, hafnium, and tantalum; elements from Group 2B of the periodic table such as zinc; elements from Group 3A of the periodic table such as aluminum, gallium, indium, and thallium; elements from Group 4A of the periodic table such as silicon, germanium, and tin; and elements from Group 6A of the periodic table such as selenium and tellurium, as well as their elements, oxides, nitrides, fluorides, or nitrogen oxides (the group names of the periodic table are represented in the old CAS form).

[0617] Furthermore, among the aforementioned inorganic materials, from the perspective of excellent balance in terms of barrier properties, cost, etc., it is preferable to select one or more inorganic materials selected from the group consisting of silicon oxide, aluminum oxide, and aluminum, and more preferably aluminum oxide.

[0618] It should be noted that, in addition to silicon dioxide, silicon oxide may also contain silicon monoxide and silicon suboxide.

[0619] The inorganic layer 102 is formed from the aforementioned inorganic material. From the perspective of excellent balance between barrier properties and cost, the inorganic layer 102 preferably includes an alumina layer composed of alumina.

[0620] The inorganic layer 102 can be composed of a single inorganic layer or multiple inorganic layers. Furthermore, if the inorganic layer 102 is composed of multiple inorganic layers, they can be composed of inorganic layers of the same type or inorganic layers of different types.

[0621] From the viewpoint of balancing improved barrier properties and improved operability, the thickness of the inorganic layer 102 is usually 1 nm or more, preferably 4 nm or more, and usually 1000 nm or less, preferably 500 nm or less.

[0622] Here, the thickness of the inorganic layer 102 can be determined, for example, using observation images obtained by transmission electron microscopy or scanning electron microscopy.

[0623] The method for forming the inorganic layer 102 is not limited. For example, it can be formed on one or both sides of the substrate layer 101 using vacuum evaporation, ion plating, sputtering, chemical vapor deposition, physical vapor deposition (CVD), plasma CVD, sol-gel methods, etc. Among these, sputtering, ion plating, chemical vapor deposition (CVD), physical vapor deposition (PVD), and plasma CVD are ideal for film formation under reduced pressure. Therefore, it is predicted that silicon-containing chemically active molecules such as silicon nitride and silicon oxynitride will react rapidly, thereby improving the surface smoothness of the inorganic layer 102 and reducing pores. For these bonding reactions to occur rapidly, it is ideal for the inorganic atoms or compounds to be chemically active molecules or atoms.

[0624] Furthermore, from the viewpoint of improving the balance between the barrier properties and productivity of the gas barrier laminate, the inorganic layer 102 is preferably a vapor-deposited film.

[0625] From the viewpoint of improving the balance between the barrier properties and productivity of the gas barrier laminate, the inorganic layer 102 is a vapor-deposited film disposed on the substrate layer 101, or a vapor-deposited film disposed on the interlayer when there is an interlayer between the substrate layer 101 and the inorganic layer 102, and is composed of one or more inorganic substances selected from the group consisting of silicon oxide, aluminum oxide and aluminum.

[0626] (Sealant layer)

[0627] From a practical point of view, such as the manufacture of steamed or boiled foods, it is preferable to provide a sealant layer on the side of the gas barrier layer 103 opposite to the inorganic layer 102.

[0628] The sealant layer is in contact with the gas barrier layer 103, or the gas barrier layer 103 and the sealant layer are bonded together by an adhesive layer. The adhesive layer will be explained later.

[0629] Examples of sealant layers include: layers formed from resin compositions comprising one or more polyolefins selected from α-olefins such as ethylene, propylene, 1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene; polyethylene such as high-density polyethylene, medium-density polyethylene, linear low-density polyethylene, and low-density polyethylene; homopolymer polypropylene; random copolymers of propylene and α-olefins having 2 or more but less than 10 carbon atoms; and low-crystallinity or amorphous ethylene-propylene random copolymers; layers formed from resin compositions comprising ethylene-vinyl acetate copolymer (EVA); layers formed from resin compositions comprising EVA and polyolefins; and so on.

[0630] From the viewpoint of heat-sealing properties, it is preferable that they contain one or more thermoplastic resins selected from low-density polyethylene, linear low-density polyethylene, homopolymer polypropylene, and random copolymers of propylene and α-olefins having 2 or 4 to 10 carbon atoms.

[0631] In addition, the preferred forms of thermoplastic resins are unstretched or stretched low-density polyethylene, linear low-density polyethylene (stretched LLDPE), and random copolymers of propylene and α-olefins with 2 or more but less than 10 carbon atoms.

[0632] From the viewpoint of applicability in the manufacture of steamed or boiled foods, the sealant layer preferably comprises an unstretched polypropylene polymer. Examples of polypropylene polymers include homopolymers of propylene and random copolymers of propylene with α-olefins having 2 or more but less than 10 carbon atoms.

[0633] The sealant layer may contain components other than thermoplastic resins. For example, it may contain additives such as antifogging agents and anti-caking agents, as well as adhesive resins such as urethane resins, urea resins, melamine resins, epoxy resins, and alkyd resins.

[0634] Alternatively, the sealant layer can be provided as an adhesive, which can be provided by drying and curing an adhesive containing adhesive resins such as acrylic resins, urethane resins, urea resins, melamine resins, epoxy resins, and alkyd resins.

[0635] The thickness of the sealant layer is preferably 10–100 μm, more preferably 15–80 μm, and even more preferably 20–60 μm. By setting this thickness, sufficient heat sealing can be obtained, and the membrane can be handled well.

[0636] (Adhesive layer)

[0637] An adhesive layer may also be provided in the gas barrier laminate. Specifically, the gas barrier layer 103 and the aforementioned sealant layer can be bonded together using the adhesive layer.

[0638] The adhesive layer may contain a known adhesive. Examples of adhesives include laminated adhesives composed of organotitanium resins, polyethyleneimine resins, urethane resins, epoxy resins, acrylic resins, polyester resins, resins containing oxazoline groups, modified silicone resins and alkyl titanates, polyester polybutadiene, etc.; or one-component and two-component polyols and polyisocyanates, aqueous urethanes, ion-crosslinked polymers, etc. Alternatively, water-based adhesives with acrylic resins, vinyl acetate resins, urethane resins, polyester resins, etc., as the main raw materials may be used.

[0639] Furthermore, depending on the application of the gas barrier laminate, other additives such as curing agents and silane coupling agents can be added to the adhesive. When the gas barrier laminate is used for hot water treatment such as boiling, from the viewpoint of heat resistance and water resistance, dry lamination adhesives, represented by polyurethane adhesives, are preferred, and solvent-based two-component curing polyurethane adhesives are more preferred.

[0640] (Layer containing polyamide)

[0641] Between the gas barrier layer 103 and the sealant layer, a layer containing polyamide (e.g., a nylon layer) may or may not be provided. By providing a polyamide layer, the strength of the film itself can be improved. For example, the bag is less likely to break when it is dropped.

[0642] The polyamide layer may contain one or more of the following: nylon-6, nylon-66, poly(m-phenylene adipamide).

[0643] When a polyamide layer is provided, its thickness is preferably 8 to 100 μm, more preferably 10 to 50 μm, and particularly preferably 13 to 30 μm.

[0644] (Method for manufacturing gas barrier laminates)

[0645] In the second embodiment, the method for manufacturing the gas barrier laminate 100 may include the following steps: a step of preparing a substrate layer 101; a step of forming an inorganic layer 102 on the substrate layer 101; and a step of forming a gas barrier layer 103 on the upper part of the substrate layer 101 on which the inorganic layer 102 is formed.

[0646] After the step of forming the inorganic layer 102 and before the step of forming the gas barrier layer 103, the step of forming an undercoat layer 104 on the inorganic layer 102 may also be included.

[0647] The process of forming an inorganic layer 102 on the substrate layer 101 is as described above as a method for forming the inorganic layer 102.

[0648] The process of forming the gas barrier layer 103 includes, for example, the following steps: applying the mixture before curing as a gas barrier coating material to the inorganic layer 102, followed by drying, thereby obtaining the coating layer; and heating the coating layer to cause the carboxyl groups contained in the polycarboxylic acid to undergo a dehydration condensation reaction with the amino groups contained in the polyamine compound, thereby forming the gas barrier layer 103 having amide bonds.

[0649] There is no limitation on the method of coating the gas barrier coating material onto the inorganic layer 102, and known methods can be used. For example, methods can be described using known coating machines such as Mayer bar coaters, air knife coaters, direct gravure coaters, gravure offset coaters, curved gravure coaters, reverse gravure coaters, and jet nozzle type gravure coaters; reverse roller coaters such as top-feed reverse coaters, bottom-feed reverse coaters, and nozzle-feed reverse coaters; five-roll coaters; lip coaters; bar coaters; bar reverse coaters; and die coaters.

[0650] From the viewpoint of improving the barrier properties of the resulting gas barrier laminate, the coating amount (wet thickness) is preferably 0.05 μm, more preferably 1 μm or more.

[0651] Furthermore, from the viewpoint of suppressing warping of the obtained gas barrier laminate and from the viewpoint of more effectively carrying out the dehydration condensation reaction between the -COO- group contained in the polycarboxylic acid and the amino group contained in the polyamine compound, the wet thickness is preferably 300 μm or less, more preferably 200 μm or less, and even more preferably 100 μm or less.

[0652] For drying and heat treatment, heat treatment can be performed after drying, or drying and heat treatment can be performed simultaneously.

[0653] The method for drying and heating is not limited as long as the effects of the present invention can be obtained; it can be a method that can cure the gas barrier coating material or a method that can heat the cured gas barrier coating material. For example, methods based on convection heat transfer, such as ovens and dryers; methods based on conduction heat transfer, such as heating rollers; methods based on radiation heat transfer using electromagnetic waves, such as infrared, far-infrared, and near-infrared heaters; and methods based on internal heating, such as microwaves. From the viewpoint of manufacturing efficiency, an apparatus capable of performing both drying and heating is preferred as an apparatus for drying and heating. Specifically, from the viewpoint of being able to be used for various purposes such as drying, heating, and annealing, a hot air oven is preferred, and from the viewpoint of excellent heat transfer efficiency to the film, a heating roller is preferred. In addition, the methods for drying and heating can be appropriately combined. Specifically, a hot air oven and a heating roller can be used together. For example, when the gas barrier coating material is dried using a hot air oven and then heated using a heating roller, the heating process time is shortened, which is preferred from the viewpoint of manufacturing efficiency. In addition, it is preferable to use only a hot air oven for drying and heating.

[0654] Regarding the heat treatment conditions, for example, the heat treatment temperature is 80–250°C, and the heat treatment time is 1 second–10 minutes; preferably, the heat treatment temperature is 120–240°C, and the heat treatment time is 1 second–1 minute; more preferably, the heat treatment temperature is 170°C–230°C, and the heat treatment time is 1 second–30 seconds; even more preferably, the heat treatment temperature is 200°C–220°C, and the heat treatment time is 1 second–10 seconds. Furthermore, by using a heating roller as described above, heat treatment can be performed in a short time.

[0655] It should be noted that, from the viewpoint of effectively forming cross-linked structures (e.g., the formation of amide bonds between -COO- groups contained in polycarboxylic acids and amino groups contained in polyamine compounds), it is important to adjust the heat treatment temperature and time according to the wet thickness of the coating material used for gas barrier. By selecting appropriate heat treatment temperature and time, suitable cross-linked structures can be formed.

[0656] By drying and heat-treating the coating material for gas barrier, the carboxyl groups of polycarboxylic acids react with polyamines and polyvalent metal compounds to form covalent bonds and / or ionic crosslinks, thereby forming a gas barrier layer 103 that also has good gas barrier properties after cooking.

[0657] (Specific examples of layered structure)

[0658] In the second embodiment, a specific example of a laminated structure comprising a gas barrier laminate is shown below.

[0659] (Example of laminated structure 1) Substrate layer 101 (PET substrate) / Inorganic layer 102 (alumina vapor deposition layer) / Gas barrier layer 103 / Adhesive layer / Polyolefin layer

[0660] (Example of laminated structure 2) Substrate layer 101 (PET substrate) / base coating 104 / inorganic layer 102 (alumina vapor deposition layer) / gas barrier layer 103 / adhesive layer / polyolefin layer

[0661] (Example of laminated structure 3) Substrate layer 101 (PET substrate) / Inorganic layer 102 (alumina vapor deposition layer) / Gas barrier layer 103 / Adhesive layer / Polyamide layer / Adhesive layer / Polyolefin layer

[0662] (Example of laminated structure 4) Substrate layer 101 (PET substrate) / Base coating 104 / Inorganic layer 102 (alumina vapor deposition layer) / Gas barrier layer 103 / Adhesive layer / Polyamide layer / Adhesive layer / Polyolefin layer

[0663] Here, by including a polyolefin layer composed of polyolefins such as polyethylene, polypropylene, poly(4-methyl-1-pentene), and poly(1-butene) in the laminated structure, the gas barrier laminate can achieve good resistance to pinholes, damage, and heat, and further suppress the reduction of gas barrier performance under high humidity and after cooking treatment.

[0664] (use)

[0665] The gas barrier laminate of the second embodiment has excellent gas barrier properties and can be appropriately used as a packaging material for various applications, such as packaging materials, especially food packaging materials for contents requiring high gas barrier properties, medical applications, industrial applications, and everyday grocery applications. The gas barrier laminate of the second embodiment is particularly preferred for food packaging applications, and more preferably for the manufacture of retortable foods.

[0666] In addition, the gas barrier laminate in the second embodiment can also be suitably used as a vacuum insulation film requiring high barrier performance; a sealing film for sealing electroluminescent elements, solar cells, etc.; and so on.

[0667] (Packaging bags made of gas barrier laminates, and food products packaged using gas barrier laminates)

[0668] Packaging bags can be constructed using the gas barrier laminate described above. These packaging bags are preferably used, for example, in the manufacture of retortable foods. That is, it is possible to manufacture foods (retortable foods) packaged using a gas barrier laminate.

[0669] In a gas barrier laminate constituting a packaging bag, typically, the side containing the substrate layer is called the outer surface side, and the side containing the gas barrier layer is called the inner surface side. In the case of a sealant layer, the side containing the sealant layer is called the inner surface side.

[0670] The methods for manufacturing steamed or boiled foods can employ conventional methods in this field. For foods that have been heat-sealed in packaging bags, moist heat sterilization can be performed using pressurized hot water or steam at 100°C or higher (e.g., at 130°C for about 30 minutes), thereby producing foods that can be stored at room temperature for extended periods.

[0671] <Third Implementation Method>

[0672] The gas barrier laminate involved in the third embodiment is the following gas barrier laminate:

[0673] It comprises a substrate layer, a gas barrier layer disposed on at least one side of the substrate layer, and an inorganic layer disposed between the substrate layer and the gas barrier layer.

[0674] The Zn composition of the gas barrier layer, as determined by X-ray photoelectron spectroscopy analysis, is 1–10 atomic%.

[0675] The data were determined by time-of-flight secondary ion mass spectrometry analysis of the aforementioned gas barrier layer. 64 ZnPO4H - Let the mass peak intensity be I( 64 ZnPO4H - ) and C3H3O2 - The mass peak intensity is set as I(C3H3O2) - )hour,

[0676] I( 64 ZnPO4H - ) / I(C3H3O2 - The value of ) is 7 × 10 -4 Above 5×10 -2 the following.

[0677] The Zn composition ratio of 1 to 10 atomic percent, as determined by X-ray photoelectron spectroscopy analysis, refers to the presence of Zn at a certain concentration in the gas barrier layer.

[0678] In addition, C3H3O2 was detected from the gas barrier layer by mass spectrometry analysis. - This refers to the fact that the gas barrier layer contains polyacrylic acid or its derivatives / similar compounds (polyacrylic acid, etc.). Furthermore, it is believed that I(C3H3O2) - The value is related to the amount (concentration) of carboxyl groups in the polycarboxylic acids contained in the gas barrier layer.

[0679] Since the gas barrier layer contains Zn at a certain concentration, and there are also polycarboxylic acids with carboxyl groups in the gas barrier layer, it is believed that the polycarboxylic acids in the gas barrier layer form a cross-link with Zn. The gas barrier layer that forms the Zn cross-link together with the inorganic layer disposed between the substrate layer and the gas barrier layer shall bear the gas barrier property of the gas barrier laminate.

[0680] Furthermore, it was detected from the gas barrier layer by mass spectrometry analysis. 64 ZnPO4H - This refers to the presence of bonds between phosphorus compounds, represented by phosphate, and Zn in the gas barrier layer, which is considered to be I( 64 ZnPO4H - The value of is related to the amount (concentration) of bonds between phosphorus compounds and Zn. Moreover, it can be inferred that Zn is not only bonded to the carboxyl groups of polycarboxylic acids, but also that some Zn is chemically bonded to each other through polycarboxylic acid compounds.

[0681] In addition, I ( 64 ZnPO4H - ) / I(C3H3O2 - The value is related to the amount (concentration) of the bond between phosphoric acid and Zn relative to the carboxyl group of the polycarboxylic acid.

[0682] However, zinc phosphate is known to be an insoluble compound in water, and the bond between the phosphorus compound and Zn is not easily broken by water (which is one of the reasons for the decrease in barrier properties after cooking). Therefore, it is believed that the presence of the phosphorus compound-Zn bond in the gas barrier layer inhibits the following situation: excessive swelling and contraction of the gas barrier layer due to cooking or other processes can damage the adjacent inorganic layer, thereby greatly reducing the gas barrier properties.

[0683] That is, since the composition ratio of Zn is 1 to 10 atomic%, I( 64 ZnPO4H-) / I(C3H3O2 - The value of ) is 7 × 10 -4 Above 5×10 -2 Therefore, it is able to maintain its barrier properties well after cooking.

[0684] Figure 9 The diagram shows a schematic cross-sectional view of an example of a double-laminated barrier film including the gas barrier laminate according to the third embodiment. The double-laminated barrier film 1 includes a gas barrier laminate 8. This gas barrier laminate 8 includes a substrate layer 2, a gas barrier layer 5 located on at least one side of the substrate layer 2, and an inorganic layer 4 located between the substrate layer 2 and the gas barrier layer 5. Additionally, an undercoat layer (UC layer) 3 may be provided below the inorganic layer 4, i.e., above the substrate layer 2. For example, in the case of the double-laminated barrier film 1, the gas barrier laminate 8 may be bonded to unstretched polypropylene (CPP) 7 via an adhesive layer 6.

[0685] in addition, Figure 10 The diagram shows a schematic cross-sectional view of an example of a three-layer laminated barrier film comprising the gas barrier laminate according to the third embodiment. In the three-layer laminated barrier film 10, for example, a nylon film 9 may be bonded to the first adhesive layer 61 of the barrier laminate 8, on which the first adhesive layer 61 is provided, and the nylon film 9 is bonded to the unstretched polypropylene 7 through a second adhesive layer 62.

[0686] In the third embodiment, the gas barrier layer 5 of the gas barrier laminate 8 was at least detected as a zinc (Zn) layer by X-ray photoelectron spectroscopy (XPS) analysis. Furthermore, analysis by time-of-flight secondary ion mass spectrometry (TOF-SIMS) analysis revealed the presence of... 64 The peaks of ZnPO4H- and C3H3O2- The peak.

[0687] In the gas barrier layer of the gas barrier laminate according to the third embodiment, high water resistance was detected. 64 The peak of ZnPO4H- makes it a gas barrier laminate with good barrier performance after cooking, regardless of the laminate structure.

[0688] [XPS Analysis]

[0689] The Zn composition contained in the gas barrier layer is 1 atomic% or more, preferably 2 atomic% or more, and more preferably 3 atomic% or more, as shown in XPS analysis. Furthermore, the Zn composition contained in the gas barrier layer is 10 atomic% or less, preferably 9.5 atomic% or less, and more preferably 9 atomic% or less. This corresponds to a Zn peak intensity relative to the carbon peak intensity, i.e., a Zn / C ratio of 0.01 or more to 0.2 or less (atoms / atoms).

[0690] As mentioned above, Zn exists in a certain amount in the gas barrier layer, thereby improving the barrier properties after cooking.

[0691] The following shows an example of specific conditions applicable to XPS analysis in the third embodiment.

[0692] Analytical apparatus: KRATOS AXIS-NOVA

[0693] X-ray source: Monochromatic Al-Kα

[0694] X-ray source output: 15kV, 10mA

[0695] Analysis area: 300×700μm

[0696] During analysis: a neutralization gun for charge correction was used.

[0697] In XPS analysis, a 1×1 cm sample cut from the gas barrier layer can be used. Furthermore, to analyze the interior of the gas barrier layer, it is preferable to sputter-etch its surface before analysis. To minimize damage to the gas barrier layer, it is desirable to use an Ar-gas cluster ion beam (Ar-GCIB) source for sputter etching. Ar-gas cluster ion beam etching is known as a method that can etch without damaging the chemical structure of the sample.

[0698] In XPS analysis, a broad-spectral scan is used to identify the detectable elements, and a narrow-scan method is used to obtain the spectra for each element. Then, based on the obtained spectra, the Shirley method is used to calculate the background, which is then removed from the spectrum. For each element measured, the background-removed spectrum is obtained, and the atomic percentage (atomic %) of the detected element is calculated using the relative sensitivity coefficient method based on the obtained peak areas.

[0699] It should be noted that the detection sensitivity of atomic composition ratios in typical XPS analysis is considered to be around 0.1 atomic percent. For example, in cases where trace amounts of phosphorus compounds are added to the gas barrier layer, the presence of P may sometimes be undetectable by XPS analysis.

[0700] [TOF-SIMS Analysis]

[0701] In the fragments detected during TOF-SIMS analysis of the gas barrier layer 64 The peak intensity of ZnPO4H- is set to I( 64 ZnPO4H-) and C3H3O2 - The peak intensity of the fragment is set to I(C3H3O2). - )hour,

[0702] I( 64 ZnPO4H - ) / I(C3H3O2 - The value of ) is 7 × 10 -4 The preferred value is 1×10. -3 The above is preferred, specifically 2×10 -3 That's all. Additionally, it's 5×10 -2 The following is preferred: 3×10 -2 The following is more preferably 2×10 -2 the following.

[0703] As mentioned above, fragments were detected as originating from bonds with high water resistance. 64 ZnPO4H - The mass peak, and I ( 64 ZnPO4H - ) / I(C3H3O2 - When the value of I( is within the above range, it becomes a gas barrier laminate with good barrier performance after cooking, regardless of the laminate structure. Furthermore, if I( 64 ZnPO4H-) / I(C3H3O2 - If the value of ) is too large, the particles of zinc phosphate bonds will grow in the gas barrier layer, causing inhomogeneity in the gas barrier layer and tending to deteriorate the gas barrier performance.

[0704] The following shows an example of specific conditions applicable to the TOF-SIMS analysis of the third embodiment.

[0705] To analyze the interior of the gas barrier layer, it is preferable to sputter-etch the surface of the gas barrier layer using the Ar-gas cluster ion beam (Ar-GCIB) included with the TOF-SIMS analysis apparatus before TOF-SIMS analysis. The use of Ar-GCIB can reduce damage to the gas barrier layer.

[0706] An example of specific conditions applicable to the third embodiment of Ar-GCIB is shown.

[0707] GCIB: 5kV, 5μA

[0708] GCIB processing time: The point at which the spectral pattern of TOF-SIMS no longer changes.

[0709] TOF-SIMS analysis can be performed, for example, as described below.

[0710] Analytical apparatus: PHI nano-TOFII manufactured by ULVAC-PHI

[0711] Primary ion: Bi3 2+

[0712] Primary ion source output: 30kV, 0.5μA

[0713] Analysis area: 300×300μm (scanning area of ​​the primary ion beam)

[0714] During analysis, charge neutralization can be achieved through irradiation with low-energy electron beams and low-energy Ar ions attached to the device. Furthermore, similar to XPS analysis, TOF-SIMS analysis can use a 1×1 cm sample cut from a gas barrier layer.

[0715] At this point, PO2, as observed by TOF-SIMS analysis targeting the gas barrier layer, - Let the mass peak intensity be I(PO2) - ) and PO3 - The mass peak intensity is set as I(PO3) - )hour,

[0716] I(PO2 - )+I(PO3 - ) / I(C3H3O2 - The value of I(PO2) is preferably 0.02 or higher, more preferably 0.07 or higher, and even more preferably 0.1 or higher. Additionally, I(PO2) - )+I(PO3 -) / I(C3H3O2 - The value of ) is preferably 5 or less, more preferably 4 or less, and even more preferably 3 or less.

[0717] PO2 detected - PO3 - The mass peak refers to the fact that the gas barrier layer contains phosphorus compounds, such as phosphate, containing more than one P-OH group. Furthermore, it is believed that I(PO2) - )+I(PO3 - ) / I(C3H3O2 - The value is related to the amount (concentration) of phosphorus compounds in the gas barrier layer relative to the carboxyl groups of polycarboxylic acids.

[0718] At this time, the above I(PO2) - ) and I(PO3) - The strength ratio of I(PO2) - ) / I(PO3 - The value of I(PO2) is preferably 0.05 or higher, more preferably 0.08 or higher, and even more preferably 0.1. Additionally, I(PO2) - ) / I(PO3 - The value of ) is 1 or less, preferably 0.9 or less, and more preferably 0.8 or less.

[0719] PO2 was detected in TOF-SIMS analysis. - and PO3 - The mass peak refers to the presence of phosphorus compounds such as phosphoric acid (H3PO4), and its ratio is I(PO2). - ) / I(PO3 - This value reflects the types of phosphorus compounds containing P-OH groups.

[0720] I (reflects the amount (concentration) of zinc phosphate bonds) 64 ZnPO4H - ) / I(C3H3O2 - This influences the types of phosphorus compounds. Specifically, it also relates to I(PO2) - ) / I(PO3 - The value of I(PO2) above. - ) / I(PO3 - The value of I( ) is above 0.05 and below 1, which enables I( 64 ZnPO4H - ) / I(C3H3O2 - The value of ) is within a suitable range, which can well maintain the barrier performance of the gas barrier laminate of the third embodiment after cooking.

[0721] The analysis method for data obtained from TOF-SIMS analysis can be carried out as follows.

[0722] In order to perform detailed spectral analysis, in the third embodiment, for each positive and negative secondary ion, the mass number m is obtained using an analytical device. i and the corresponding count c i As a pair of raw data columns and total ion count (C T Here, i = 0, 1, 2, ..., N, and the original data column is for m. i And they are arranged in ascending order. It should be noted that C... T It is the total count of secondary ions detected by the detector.

[0723] Let the range of mass numbers around the mass spectral peak of interest be defined as i = n1, n1+1, ..., n2. Using the following formula... i The data c of the counts obtained through analysis within this range i To approximate the result. Specifically, this is achieved by using the background level b. 0 and K trigonometric functions Y j (m i Curve fitting to c i To approximate. Here, b 0 It is a constant.

[0724] [Mathematical Expression 7]

[0725]

[0726] Y j (m i )yes Figure 11 As shown, in mass number x 0 j It has a peak value Y 0 j The function is represented by the following formula.

[0727] [Mathematical Expression 8]

[0728]

[0729] Here, b 0 x 0 j Y 0 j B - j B + j These become the fitting parameters. Furthermore, with respect to j, j = 1, ..., K. For example, the background of the spectrum is not a constant value but rather relative to m. iIn the case of linear change, b 0 With trigonometric function Y j (m i The background is approximated by combining different mass functions. When the mass spectral peak of interest is a single peak, the background is removed and approximation is performed using one trigonometric function. When the mass spectral peak of interest is close to other mass peaks, these other mass peaks are also included in the approximation using multiple trigonometric functions. When the approximated mass spectral peak of interest is set as the j=kth peak among K trigonometric functions, the peak intensity I is determined by Y up to i=n1, ..., n2. k (m i The sum of ) is expressed by the total ion count (C T The numerical representation obtained by standardization is calculated by the following formula.

[0730] [Mathematical Expression 9]

[0731]

[0732] If a mass spectral peak has a tail, it becomes difficult to define the range of mass numbers corresponding to the count. In the third embodiment, to avoid this, a trigonometric function is used to approximate the mass spectral peak. Thus, the count at the tail of the mass spectral peak is ignored. Curve fitting is performed so that the central portion of the mass spectral peak matches the trigonometric function.

[0733] In addition, sometimes other components (e.g., other types of mass peaks with the same mass number) are observed to overlap with the target peak component. In such cases, trigonometric functions are used to approximate the other components that overlap with the target peak component, thereby determining the target peak component.

[0734] The mass numbers of the fragments of interest in the third embodiment were calculated in advance and are shown below. The atomic mass numbers of the isotopes are referenced at http: / / physics.nist.gov / .

[0735] [Table 5]

[0736]

[0737] [ 64 ZnPO4H - [Calculation of peak mass intensity]

[0738] Zn is known to have five isotopes. In TOF-SIMS analysis, the main isotopes detected are those of Zn and Zn. 64 Zn, 66 Zn, 68 Zn-related fragments. In the third embodiment, the focus is on the fragments with the highest presence rate. 64 Zn. In representing 64Zn was detected in fragments of bonds between Zn and phosphorus compounds containing P-OH. 64 ZnPO4H - , 64 ZnP2O6H - , 64 ZnP2O7H - , 64 ZnP3O9H - etc., but focusing on those with larger peak mass. 64 ZnPO4H - .

[0739] Focusing on the mass number range of negative secondary ion spectra (159.5–160.3), based on the equivalent... 64 Zn 31 P 16 O4 1 H - The trigonometric function and m obtained by approximating the mass peak near 158.890 i The data is used to calculate the sum of the counts, using C. T Standardize and use the resulting value as 64 ZnPO4H - Mass peak intensity I ( 64 ZnPO4H - ).

[0740] An example of curve fitting is shown below. Figure 12 The calculation results of the parameters used at this time and the sum of the counts are shown in Table 6. Figure 12 In the example shown, based on the target 64 ZnPO4H - The trigonometric function and m obtained by approximating the mass peak i The sum of the counts obtained from the data is 1514. The total ion count of the negative secondary ions at this point (C...) T ) = 8571746, therefore, 64 ZnPO4H - Peak intensity I ( 64 ZnPO4H - )for:

[0741] I( 64 ZnPO4H - ) = 1514 / 8571746 = 1.77 × 10 -4 .

[0742] [Table 6]

[0743]

[0744] Examples of curve fitting are shown. Figure 12 To supplement.

[0745] (i) In order to obtain measurement data near the target peak position c i The approximation curve y i It requires "background b" 0 The curves of "triangular function approximation of other components" and "triangular function Y as the target" j (m i The curve is )”.

[0746] (ii) in Figure 12 In the example, in order to obtain the measurement data c reproducible in the range of mass number (m / z) from 159.7 to 160.2. i The "approximation curve y" i “background b” was used 0 "The trigonometric function Y as the target" j (m i The curve for “triangular function approximation of other components” (in Table 2, j=2) and two curves for “triangular function approximation of other components” (in Table 6, j=0, 1).

[0747] [C3H3O2 - [Calculation of peak mass intensity]

[0748] Focusing on the mass number range of negative secondary ion spectra (70.7–71.4), based on the data obtained from curve fitting, the corresponding... 12 C3 1 H3 16 O2 - The trigonometric function Y is obtained by approximating the mass peak near 71.013. k (m i ) and m i The data is used to calculate the sum of the counts, using C. T Standardize and use the resulting value as C3H3O2 - Mass peak intensity I(C3H3O2) - ).

[0749] [PO2 - [Calculation of peak mass intensity]

[0750] Focusing on the mass number range of negative secondary ion spectra (62.5–63.3), based on the equivalent... 31 P 16 O2 - The trigonometric function and m obtained by approximating the mass peak near 62.964 i The data is used to calculate the sum of the counts, using C. T Standardize and use the resulting value as PO2- Mass peak intensity I(PO2) - ).

[0751] [PO3 - [Calculation of peak mass intensity]

[0752] Focusing on the mass number range of negative secondary ion spectra (78.5–79.3), based on the equivalent... 31 P 16 O3 - The trigonometric function and m obtained by approximating the mass peak near 78.959 i The data is used to calculate the sum of the counts, using C. T Standardize and use the resulting value as PO3 - Mass peak intensity I(PO3) - ).

[0753] The gas barrier layer is preferably formed from a solidified material comprising a mixture of polycarboxylic acids, Zn, and phosphorus compounds containing one or more P-OH groups, such as phosphoric acid (H3PO4) or their salts.

[0754] If the gas barrier layer is formed from a cured product containing a mixture of these components, the carboxyl groups from the polycarboxylic acid form metal ion crosslinks through Zn. Additionally, Zn reacts with phosphorus compounds containing P-OH groups to form water-resistant bonds. While the detailed mechanism is unclear, it is believed that because these metal ion crosslinks formed through Zn and the bonds between Zn and phosphorus compounds are uniformly and appropriately present in the gas barrier layer, a dense gas barrier layer is formed, and excessive swelling and shrinkage of the gas barrier layer due to processes such as boiling are suppressed.

[0755] The composition ratio of Zn in the gas barrier layer involved in the third embodiment and I(in TOF-SIMS) 64 ZnPO4H - ) / I(C3H3O2 - The value of ) and I(PO2) - )+I(PO3 - ) / I(C3H3O2 - The value of ) and I(PO2) - ) / I(PO3 - The value of ) can be controlled by appropriately adjusting the manufacturing conditions of the gas barrier layer.

[0756] In the third embodiment, for example, the concentration of phosphoric acid relative to the polycarboxylic acid can be used as a criterion for controlling the Zn composition ratio and I( 64 ZnPO4H - ) / I(C3H3O2 -One factor in the value of ).

[0757] The following details the polycarboxylic acids, zinc or compounds thereof, phosphorus compounds, and other additives that may be used in the third embodiment.

[0758] (Polycarboxylic acids)

[0759] Polycarboxylic acids are compounds having two or more carboxyl groups within their molecules. Specifically, examples include homopolymers or copolymers of α,β-unsaturated carboxylic acids such as acrylic acid, methacrylic acid, itaconic acid, fumaric acid, crotonic acid, cinnamic acid, 3-hexenoic acid, and 3-hexenediaic acid. Alternatively, they can be copolymers of the aforementioned α,β-unsaturated carboxylic acids with esters such as ethyl esters, olefins such as ethylene, etc.

[0760] Among them, the preferred polymers are homopolymers of acrylic acid and methacrylic acid or copolymers thereof, more preferably one or more polymers selected from polyacrylic acid, polymethacrylic acid, and copolymers of acrylic acid and methacrylic acid, further preferably at least one polymer selected from polyacrylic acid and polymethacrylic acid, and particularly preferably at least one polymer selected from homopolymers of acrylic acid and homopolymers of methacrylic acid.

[0761] In this third embodiment, the term "polyacrylic acid" includes both homopolymers of acrylic acid and copolymers of acrylic acid with other monomers. In the case of copolymers of acrylic acid with other monomers, for polyacrylic acid, 100% by mass of the polymer contains structural units derived from acrylic acid, typically 90% by mass or more, preferably 95% by mass or more, and more preferably 99% by mass or more.

[0762] Furthermore, in the third embodiment, the term "polymethacrylic acid" includes both homopolymers of methacrylic acid and copolymers of methacrylic acid with other monomers. In the case of copolymers of methacrylic acid with other monomers, for polymethacrylic acid, 100% by mass of the polymer contains structural units derived from methacrylic acid, typically 90% by mass or more, preferably 95% by mass or more, and more preferably 99% by mass or more.

[0763] Polycarboxylic acids are polymers formed by the polymerization of carboxylic acid monomers. From the viewpoint of excellent balance between gas barrier properties and operability, the molecular weight of polycarboxylic acids is preferably 500 to 2,500,000, more preferably 5,000 to 2,000,000, even more preferably 10,000 to 1,500,000, and even more preferably 100,000 to 1,200,000.

[0764] Here, the molecular weight of polycarboxylic acids is the weight-average molecular weight converted from polyethylene oxide, which can be determined using gel permeation chromatography (GPC).

[0765] By neutralizing the polycarboxylic acid with a volatile base, gelation can be suppressed when zinc (described later) is mixed with the polycarboxylic acid. Therefore, from the viewpoint of preventing gelation, it is preferable to prepare a partially or completely neutralized carboxyl group using a volatile base. The neutralized product can be obtained by partially or completely neutralizing the carboxyl group of the polycarboxylic acid with a volatile base (i.e., partially or completely preparing a carboxylate from the carboxyl group of the polycarboxylic acid). This prevents gelation when zinc is added.

[0766] Partial neutralization is prepared by adding a volatile base to an aqueous solution of a polycarboxylic acid polymer. The desired degree of neutralization can be achieved by adjusting the ratio of the polycarboxylic acid to the volatile base. In the third embodiment, the degree of neutralization of the polycarboxylic acid obtained using the volatile base is preferably 30 to 100 equivalents, more preferably 50 to 100 equivalents.

[0767] As a volatile base, any water-soluble base can be used.

[0768] Examples of volatile bases include, for example, tertiary amines such as ammonia, morpholine, alkylamines, 2-dimethylaminoethanol, N-methylmorpholine, ethylenediamine, triethylamine, or aqueous solutions of these, or mixtures thereof. From the viewpoint of obtaining good gas barrier properties, aqueous ammonia solutions are preferred.

[0769] The mixture constituting the gas barrier laminate according to the third embodiment preferably further comprises a carbonate ammonium salt. The carbonate ammonium salt is a substance added to improve the solubility of zinc and prepare a homogeneous solution containing zinc by making the zinc described later into a zinc ammonium carbonate complex.

[0770] Examples of carbonate-based ammonium salts include ammonium carbonate and ammonium bicarbonate. Ammonium carbonate is preferred from the viewpoint that it is easily volatile and does not easily remain in the resulting gas barrier layer.

[0771] (Zinc)

[0772] Zinc (Zn) can form water-resistant Zn phosphate bonds with phosphorus compounds, which can be detected by TOF-SIMS analysis. 64 ZnPO4H - The indicated mass peak. Additionally, if the gas barrier layer contains a polycarboxylic acid, it forms a salt with the polycarboxylic acid. Zn can be any zinc or zinc compound that can be added to the mixture forming the gas barrier layer; for example, metallic zinc, zinc oxide (ZnO), zinc compounds, etc., can be used. The amount of zinc added can be set to 0.1 mol to 0.5 mol relative to 1 mol of the carboxyl group of the aforementioned polycarboxylic acid.

[0773] (Phosphorus compounds)

[0774] As described above, when performing mass spectrometry analysis on a gas barrier layer, it is preferable to detect PO2. - and / or PO3 - To create such a gas barrier layer, the mixture before curing preferably contains a phosphorus compound or a salt thereof.

[0775] Phosphorus compounds or their salts contain one or more -P-OH groups in their molecular structure. Phosphorus compounds can be complexed in mixtures in the form of salts.

[0776] From the viewpoint of further improving the steam barrier properties after cooking, the phosphorus compound preferably contains two or more -P-OH groups, more preferably three or more -P-OH groups. Furthermore, from a productivity viewpoint, the number of -P-OH groups in the phosphorus compound can, for example, be ten or less.

[0777] Specific examples of phosphorus compounds include phosphoric acid, phosphorous acid, phosphonic acid, hypophosphoric acid, polyphosphoric acid, and their derivatives.

[0778] Specifically, polyphosphoric acid has a condensation structure of two or more phosphoric acids in its molecular structure. Examples include diphosphoric acid (pyrophosphoric acid), triphosphoric acid, and polyphosphoric acid formed by the condensation of four or more phosphoric acids.

[0779] Specific examples of derivatives include esters of the aforementioned phosphorus compounds such as phosphoric acid starch and cross-linked phosphoric acid starch; halides such as chlorides; acid anhydrides such as phosphorus tetraoxide; and compounds with structures such as triazine (methylenephosphonic acid) and N,N,N',N'-ethylenediaminetetra(methylenephosphonic acid) having hydrogen atoms bonded to phosphorus atoms replaced by alkyl groups.

[0780] From the viewpoint of further improving the balance between barrier properties and productivity, the phosphorus compound is one or more selected from the group consisting of phosphoric acid, phosphorous acid, hypophosphoric acid, polyphosphoric acid, phosphonic acid and their salts, more preferably at least one selected from the group consisting of phosphoric acid and phosphorous acid, phosphonic acid and their salts.

[0781] Furthermore, specific examples of salts in phosphorus compounds include salts of monovalent metals such as sodium and potassium, and ammonium salts. From a barrier perspective, ammonium salts are preferred for phosphorus compounds.

[0782] The concentration of phosphorus atoms in a phosphorus compound is typically 5 × 10⁻¹⁰, relative to 1 mol of carboxyl groups in the aforementioned polycarboxylic acids. -4 mol or more, preferably 1×10 -3 mol or more, more preferably 5 × 10 mol -3The concentration is 1 mol or more, typically 0.3 mol or less, preferably 0.15 mol or less, and more preferably 0.1 mol or less. In phosphorus compounds containing one P atom in their chemical formula, such as phosphoric acid, the number of moles of P atoms has the same meaning as the number of moles of phosphorus compound.

[0783] It is believed that phosphorus compounds of this concentration, or phosphorus compounds derived from their salts, can reliably form Zn bonds with water-resistant phosphorus compounds. This suppresses excessive swelling and shrinkage of the gas barrier layer due to cooking processes, thereby further improving the gas barrier properties of the gas barrier laminate after cooking. The presence of the phosphorus compound-Zn bond was determined by the aforementioned TOF-SIMS analysis. 64 ZnPO4H - The quality peak reflects this.

[0784] (Other ingredients)

[0785] In the mixture constituting the gas barrier layer according to the third embodiment, other components may include, for example, polyamines, or may not include polyamines. When polyamines are included, the barrier properties of the obtained gas barrier laminate can be improved, as can the interlayer adhesion of the obtained gas barrier laminate, resulting in good delamination resistance.

[0786] It should be noted that the fragments detected in TOF-SIMS analysis can be detected independently. Therefore, the I( ) obtained by analyzing the TOF-SIMS analysis results 64 ZnPO4H - ) / I(C3H3O2 - ), (I(PO2) - )+I(PO3 - )) / I(C3H3O2 - ), I(PO2) - ) / I(PO3 - The value of ) is not affected by the presence or absence of polyamines.

[0787] Polyamines are polymers having two or more amino groups on their main chain, side chain, or terminal. Specifically, examples include aliphatic polyamines such as polyallylamine, polyvinylamine, polyethyleneimine, and poly(propyleneimine); polyamides such as polylysine and polyarginine, which have amino groups on their side chains; and so on. Alternatively, polyamines can be formed by modifying a portion of the amino groups. The amount of polyamine added can be set to a level between 0 mol and 0.9 mol of active hydrogen, relative to 1 mol of carboxyl groups contained in the aforementioned polycarboxylic acids.

[0788] From the viewpoint of excellent balance between gas barrier properties and operability, the weight-average molecular weight of the polyamine is preferably 50 to 2,000,000, more preferably 100 to 1,000,000, even more preferably 1,500 to 500,000, even more preferably 1,500 to 100,000, even more preferably 1,500 to 50,000, even more preferably 3,500 to 20,000, even more preferably 5,000 to 15,000, and particularly preferably 7,000 to 12,000.

[0789] In this third embodiment, the molecular weight of the polyamine can be determined using the boiling point elevation method or the viscosity method.

[0790] (Manufacturing method of gas barrier layer)

[0791] The gas barrier layer involved in the third embodiment can be manufactured, for example, as described below.

[0792] First, prepare a completely or partially neutralized solution of the carboxyl groups that constitute the polycarboxylic acid.

[0793] A volatile base is added to a polycarboxylic acid, which completely or partially neutralizes the carboxyl groups. By neutralizing the carboxyl groups of the polycarboxylic acid, gelation that would occur during the addition of zinc due to reaction with the carboxyl groups constituting the polycarboxylic acid is effectively prevented in subsequent processes, resulting in a uniform intermediate for gas barrier coating materials.

[0794] Next, a zinc salt compound and a carbonate ammonium salt are added to the above intermediate and dissolved. The generated zinc ions react with the -COO- group constituting the polycarboxylic acid to form a zinc salt. Here, the -COO- group that forms the salt with the zinc ions refers to both the unneutralized carboxyl group and the neutralized -COO- group. In the case of the neutralized -COO- group, zinc ions from the zinc ions replace and coordinate to form a -COO- group zinc salt. Then, phosphoric acid is added after the formation of the zinc salt, thereby obtaining a coating material (mixture) for gas barrier applications.

[0795] The gas barrier coating material (mixture) thus manufactured is applied onto the inorganic layer described later, and then dried and cured to form a gas barrier layer. There are no particular limitations on the method of applying the gas barrier coating material to the substrate layer; conventional methods can be used. Examples include various known coating machines such as Mayer bar coaters, air knife coaters, direct gravure coaters, gravure offset coaters, curved gravure coaters, reverse gravure coaters, and jet nozzle type gravure coaters; top-feed reverse coaters, bottom-feed reverse coaters, and nozzle-feed reverse coaters; five-roll coaters; lip coaters; bar coaters; bar reverse coaters; and die coaters.

[0796] The coating amount (wet thickness) of the gas barrier coating material (mixture) is preferably 0.05 μm or more, more preferably 1 μm or more. Furthermore, the coating amount is preferably 300 μm or less, more preferably 200 μm or less, and even more preferably 100 μm or less.

[0797] Furthermore, the average thickness of the gas barrier layer after drying and curing is preferably 0.05 μm to 10 μm, more preferably 0.08 μm to 5 μm, and even more preferably 0.1 μm to 1 μm. If the thickness is below the upper limit mentioned above, warping of the obtained gas barrier laminate or gas barrier film can be suppressed. Conversely, if the thickness is above the lower limit mentioned above, the barrier performance of the obtained gas barrier laminate or gas barrier film can be improved.

[0798] For drying and heat treatment, heat treatment can be performed after drying, or drying and heat treatment can be performed simultaneously.

[0799] The methods for drying and heating are not particularly limited as long as they achieve the objectives of this invention; any method that can cure the gas barrier coating material or heat the cured gas barrier coating material is acceptable. Examples include ovens and dryers based on convective heat transfer; heating rollers based on conductive heat transfer; infrared, far-infrared, and near-infrared heaters based on radiative heat transfer using electromagnetic waves; and microwaves based on internal heating. From a manufacturing efficiency perspective, an apparatus capable of performing both drying and heating is preferred for the drying and heating process. Specifically, from the viewpoint of being usable for various purposes such as drying, heating, and annealing, a hot air oven is preferred; and from the viewpoint of excellent heat transfer efficiency to the film, a heating roller is preferred. Furthermore, methods for drying and heating can be appropriately combined. A hot air oven and a heating roller can be used together; for example, when the gas barrier coating material is dried using a hot air oven and then heated using a heating roller, the heating process time is shortened, which is preferable from a manufacturing efficiency perspective. In addition, it is preferable to use only a hot air oven for drying and heating.

[0800] For example, ideally, the heat treatment should be performed under the following conditions: a heat treatment temperature of 80–250°C and a heat treatment time of 1 second–10 minutes; preferably, a heat treatment temperature of 120–240°C and a heat treatment time of 1 second–1 minute; more preferably, a heat treatment temperature of 170°C–230°C and a heat treatment time of 1 second–30 seconds. Furthermore, by using a heating roller as described above, heat treatment can be performed in a short time. Importantly, the heat treatment temperature and heat treatment time should be adjusted according to the wet thickness of the gas barrier coating material.

[0801] For gas barrier coating materials (mixtures), the zinc salts constituting the -COO- groups of the polycarboxylic acid form metal crosslinks and water-resistant Zn phosphate bonds (reflected by the aforementioned TOF-SIMS analysis). 64 ZnPO4H - The mass peak of the gas can be dried and heat-treated to obtain a gas barrier layer with excellent gas barrier properties.

[0802] (Inorganic layer)

[0803] Inorganic materials constituting inorganic layer 4 include, for example, metals, metal oxides, metal nitrides, metal fluorides, and metal nitrides, which are capable of forming barrier films.

[0804] As inorganic substances constituting inorganic layer 4, examples include one or more of the following: elements selected from Group 2A of the periodic table such as beryllium, magnesium, calcium, strontium, and barium; transition elements of the periodic table such as titanium, zirconium, ruthenium, hafnium, and tantalum; elements from Group 2B of the periodic table such as zinc; elements from Group 3A of the periodic table such as aluminum, gallium, indium, and thallium; elements from Group 4A of the periodic table such as silicon, germanium, and tin; and elements from Group 6A of the periodic table such as selenium and tellurium, as well as their elements, oxides, nitrides, fluorides, or nitrogen oxides.

[0805] It should be noted that in the third embodiment, the group names of the periodic table are represented in the old CAS form.

[0806] Furthermore, among the aforementioned inorganic materials, considering the excellent balance between barrier properties and cost, it is preferable to select one or more inorganic materials from the group consisting of silicon oxide, aluminum oxide, and aluminum, and more preferably aluminum oxide.

[0807] It should be noted that, in addition to silicon dioxide, silicon oxide may also contain silicon monoxide and silicon suboxide.

[0808] The inorganic layer is formed from the aforementioned inorganic material. The inorganic layer 4 can be composed of a single inorganic layer or multiple inorganic layers. Furthermore, if the inorganic layer 4 is composed of multiple inorganic layers, they can be composed of inorganic layers of the same type or inorganic layers of different types.

[0809] From the perspective of balancing barrier properties, sealing properties, and operability, the thickness of the inorganic layer 4 is usually between 1 nm and 1000 nm, preferably between 1 nm and 500 nm.

[0810] In the third embodiment, the thickness of the inorganic layer can be determined using observation images obtained from a transmission electron microscope or a scanning electron microscope.

[0811] There are no particular limitations on the method for forming the inorganic layer. For example, vacuum evaporation, ion plating, sputtering, chemical vapor deposition, physical vapor deposition (CVD), plasma CVD, sol-gel methods, etc., can be used to form the inorganic layer 4 on one or both sides of the substrate layer 2. Among these, sputtering, ion plating, CVD, PVD, and plasma CVD are ideal for film formation under reduced pressure. Therefore, it is predicted that silicon-containing chemically active molecules such as silicon nitride and silicon oxynitride will react rapidly, thereby improving the surface smoothness of the inorganic layer 4 and reducing pores.

[0812] For these bonding reactions to proceed rapidly, it is ideal for the inorganic atom or compound to be a chemically active molecular or atomic species.

[0813] (Substrate layer)

[0814] Substrate layer 2 can be used without particular limitation as long as it is a substrate layer to which a solution of a gas barrier coating material can be applied. Examples include organic materials such as thermosetting resins, thermoplastic resins, or paper; inorganic materials such as glass, ceramics, silicon dioxide, silicon oxynitride, silicon nitride, concrete, aluminum, alumina, iron, copper, stainless steel, etc.; and multilayer substrate layers formed by combinations of organic materials or combinations of organic and inorganic materials. Among these, for example, in the case of various film applications such as packaging materials and panels, plastic films using thermosetting resins or thermoplastic resins, or organic materials such as paper, are preferred.

[0815] Known thermosetting resins can be used as thermosetting resins. Examples include epoxy resins, unsaturated polyester resins, phenolic resins, urea-melamine resins, polyurethane resins, silicone resins, and polyimides.

[0816] Known thermoplastic resins can be used as thermoplastic resins. Examples include polyolefins (polyethylene, polypropylene, poly(4-methyl-1-pentene), poly(1-butene), etc.), polyesters (polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, etc.), polyamides (nylon-6, nylon-66, poly(m-phenylene adipamide), etc.), polyvinyl chloride, polyimide, ethylene-vinyl acetate copolymer or its saponification, polyvinyl alcohol, polyacrylonitrile, polycarbonate, polystyrene, ion-crosslinked polymers, fluoropolymers, or mixtures thereof.

[0817] Among them, from the viewpoint of good transparency, one or more resins selected from the group consisting of polypropylene, polyethylene terephthalate, polyethylene naphthalate, polyamide, polyimide and polybutylene terephthalate are preferred; from the viewpoint of excellent resistance to pinholes, damage and heat resistance, one or more resins selected from the group consisting of polyamide, polyethylene terephthalate and polybutylene terephthalate are preferred.

[0818] Furthermore, depending on the application of the gas barrier laminate 8, the substrate layer 2 formed from thermoplastic resin can be a single layer or two or more layers.

[0819] Alternatively, a substrate layer can be formed by stretching a film formed from the above-mentioned thermosetting resin or thermoplastic resin along at least one direction, preferably a biaxial direction.

[0820] As the substrate layer 2 according to the third embodiment, from the viewpoint of excellent transparency, rigidity and heat resistance, it is preferably a biaxial stretch film formed of one or more thermoplastic resins selected from polypropylene, polyethylene terephthalate, polyethylene naphthalate, polyamide, polyimide and polybutylene terephthalate, and more preferably a biaxial stretch film formed of one or more thermoplastic resins selected from polyamide, polyethylene terephthalate and polybutylene terephthalate.

[0821] Alternatively, polyvinylidene chloride, polyvinyl alcohol, ethylene-vinyl alcohol copolymer, acrylic resin, urethane resin, etc., can be coated on the surface of the substrate layer 2.

[0822] Furthermore, for substrate layer 2, surface treatment can be performed to improve adhesion. Specifically, surface activation treatments such as corona treatment, flame treatment, plasma treatment, and primer coating treatment can be performed.

[0823] From the viewpoint of obtaining good film properties, the thickness of the substrate layer 2 is preferably 1 to 1000 μm, more preferably 1 to 500 μm, and even more preferably 1 to 300 μm.

[0824] The shape of the substrate layer 2 is not particularly limited; for example, it can be a sheet or film shape, a shallow dish, a cup, a hollow body, etc.

[0825] (Base coating)

[0826] In the gas barrier laminate 8, from the viewpoint of improving the adhesion between the substrate layer 2 and the inorganic layer 4, a primer layer 3 can be formed on the surface of the substrate layer 2. The primer layer is preferably a layer formed using an epoxy (meth)acrylate compound or a urethane (meth)acrylate compound.

[0827] The aforementioned base coating 3 is preferably a layer formed by curing at least one selected from epoxy (meth)acrylate compounds and urethane (meth)acrylate compounds.

[0828] Examples of epoxy (meth)acrylate compounds include compounds obtained by reacting bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, bisphenol S type epoxy compounds, phenol Novola C type epoxy compounds, cresol Novolac type epoxy compounds, aliphatic epoxy compounds, etc., with acrylic acid or methacrylic acid, and acid-modified epoxy (meth)acrylates obtained by reacting the above epoxy compounds with carboxylic acids or their anhydrides. These epoxy (meth)acrylate compounds are coated onto the surface of a substrate layer together with a diluent containing a photopolymerization initiator and, if necessary, other photopolymerization initiators or thermally reactive monomers. Subsequently, they are irradiated with ultraviolet light or the like, and a crosslinking reaction occurs to form a base layer.

[0829] Examples of urethane (meth)acrylate compounds include, for instance, compounds obtained by acrylate esterification of oligomers (hereinafter also referred to as polyurethane oligomers) formed from polyol compounds and polyisocyanate compounds.

[0830] Polyurethane oligomers can be obtained from the condensation products of polyisocyanate compounds and polyol compounds. Specific examples of polyisocyanate compounds include adducts of methylene bis(terephthalic acid diisocyanate), hexamethylene diisocyanate-hexanetriol, hexamethylene diisocyanate, toluene diisocyanate, toluene diisocyanate-trimethylolpropane adduct, 1,5-naphthalene diisocyanate, thiopropyl diisocyanate, ethylbenzene-2,4-diisocyanate, 2,4-toluene diisocyanate dimers, hydrogenated dimethyl phthalate diisocyanate, and tris(4-phenylisocyanate)thiophosphate. Specific examples of polyol compounds include polyether polyols such as polyoxytetramethylene glycol, polyester polyols such as polyadipate polyols and polycarbonate polyols, and copolymers of acrylates and hydroxyethyl methacrylate. Examples of monomers constituting acrylates include methyl methacrylate, ethyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, methoxyethyl methacrylate, butoxyethyl methacrylate, and phenyl methacrylate.

[0831] These epoxy (meth)acrylate compounds and urethane (meth)acrylate compounds can be used together as needed. Furthermore, various known methods can be cited as methods for polymerizing them, specifically methods such as irradiation with energy rays containing ionizing radiation or heating.

[0832] When using ultraviolet light to cure and form a primer, it is preferable to use acetophenone, benzophenone, Michaelis-Menten benzoylbenzoate, α-pentyl oxime ester, or thioxanone as photopolymerization initiators, and n-butylamine, triethylamine, or tri-n-butylphosphine as photosensitizers, in combination. Alternatively, in the third embodiment, epoxy (meth)acrylate compounds and urethane (meth)acrylate compounds may be used in combination.

[0833] Furthermore, these epoxy (meth)acrylate compounds and urethane (meth)acrylate compounds can be diluted using (meth)acrylate monomers. Examples of such (meth)acrylate monomers include methyl methacrylate, ethyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, methoxyethyl methacrylate, butoxyethyl methacrylate, phenyl methacrylate, trimethylolpropane tri(meth)acrylate, hexanediol (meth)acrylate, tripropylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, etc.

[0834] In the case of using urethane (meth)acrylate compounds as the base coating, the oxygen barrier properties of the obtained gas barrier laminate 8 can be further improved.

[0835] The thickness of the base coating in the third embodiment, measured by coating amount, is typically between 0.01 and 100 g / m. 2 Within the range of 0.05–50 g / m³, it is preferred. 2 Within the range.

[0836] (Adhesive layer)

[0837] Additionally, an adhesive layer 6 can be provided on the gas barrier layer 5. The adhesive layer 6 may contain any known adhesive. Examples of adhesives include laminated adhesives composed of organotitanium resins, polyethyleneimine resins, urethane resins, epoxy resins, acrylic resins, polyester resins, resins containing oxazoline groups, modified silicone resins and alkyl titanates, polyester polybutadiene, etc.; or one-component and two-component polyols and polyisocyanates, aqueous urethanes, ion-crosslinked polymers, etc. Alternatively, water-based adhesives using acrylic resins, vinyl acetate resins, urethane resins, polyester resins, etc., as main raw materials may also be used.

[0838] Furthermore, depending on the intended use of the gas barrier laminate 8, other additives such as curing agents and silane coupling agents can be added to the adhesive. When the gas barrier laminate is intended for use in hot water treatment such as boiling, from the viewpoint of heat resistance and water resistance, a dry lamination adhesive, represented by a polyurethane adhesive, is preferred, and a solvent-based two-component curing polyurethane adhesive is more preferred.

[0839] Regarding the gas barrier laminate 8 according to the third embodiment, its gas barrier performance after cooking is excellent regardless of the lamination structure. Therefore, it is preferably used in packaging materials, especially food packaging materials for contents requiring high gas barrier properties. In addition, it can also be suitable for use as various packaging materials for medical, industrial, and everyday grocery applications.

[0840] Furthermore, the gas barrier laminate 8 of the third embodiment can be suitably used, for example, as a vacuum insulation film requiring high barrier performance; a sealing film for sealing electroluminescent elements, solar cells, etc.; and so on.

[0841] <Fourth Implementation Method>

[0842] Figure 13 A cross-sectional view illustrating an example of the configuration of the gas barrier laminate in the fourth embodiment. Figure 13 The gas barrier laminate 100 shown includes a substrate layer 101, a gas barrier layer 103 disposed on at least one side of the substrate layer 101, and an inorganic layer 102 disposed between the substrate layer 101 and the gas barrier layer 103. Furthermore, the gas barrier layer 103 is composed of a cured product comprising a mixture of polycarboxylic acids, polyamine compounds, polyvalent metal compounds, and phosphorus compounds containing one or more -P-OH groups or their salts.

[0843] The specific composition of each layer will be described later.

[0844] In the gas barrier laminate 100, a substrate layer 101, an inorganic layer 102, and a gas barrier layer 103 are stacked sequentially. Furthermore, the gas barrier layer 103 is composed of a cured product of the aforementioned mixture. Therefore, it exhibits excellent balance between barrier properties and productivity, and can provide ideal barrier properties in various layer structures.

[0845] More specifically, the gas barrier laminate 100 exhibits excellent barrier properties, such as oxygen barrier and water vapor barrier, after being subjected to a boiling treatment. Furthermore, since the gas barrier layer 103 in the gas barrier laminate 100 is composed of a cured product of the aforementioned mixture, even if, for example, the curing time (specifically, the heat treatment time) for obtaining the gas barrier layer 103 is short, a gas barrier laminate 100 with excellent barrier properties can still be obtained.

[0846] In addition, the gas barrier layer 103 is composed of a cured product containing a mixture of polycarboxylic acid, polyamine compound, polyvalent metal compound, and phosphorus compound or salt thereof containing one or more -P-OH groups. Therefore, for example, a gas barrier laminate 100 with excellent barrier properties and water resistance can also be obtained.

[0847] Figure 14 A cross-sectional view is shown schematically to illustrate other configurations of the gas barrier laminate. Figure 14 The basic structure and reference of the gas barrier laminate 110 shown Figure 13 The gas barrier laminate 100 described above is similar, but differs in that it also includes an undercoat layer 104 disposed between the substrate layer 101 and the inorganic layer 102.

[0848] The same effect as that of the gas barrier laminate 100 can be obtained in the gas barrier laminate 110. Furthermore, in the gas barrier laminate 110, by providing an undercoat layer 104 between the substrate layer 101 and the inorganic layer 102, the adhesion between the substrate layer 101 and the inorganic layer 102 can be further improved.

[0849] The composition of the layers contained in the gas barrier laminate will be explained in more detail below. First, the gas barrier layer 103 will be explained.

[0850] (Gas barrier layer)

[0851] The gas barrier layer 103 is composed of a cured material comprising a mixture of polycarboxylic acids, polyamine compounds, and polyvalent metal compounds. More specifically, the gas barrier layer 103 is a film (gas barrier film 10) composed of the aforementioned cured material.

[0852] More specifically, the gas barrier layer 103 can be obtained, for example, by coating a mixture before curing, i.e., a gas barrier coating material, onto a layer such as an inorganic layer 102 disposed immediately below the gas barrier layer 103, followed by drying and heat treatment to cure the gas barrier coating material.

[0853] In the infrared absorption spectrum of the gas barrier layer 103, at a depth of 1300 cm⁻¹ -1 The above 1490cm -1 The maximum peak height of absorbance within the following range is set as α, and 1690 cm⁻¹ is used. -1 The above 1780cm -1When the maximum peak height of absorbance within the following range is set as γ, from the viewpoint of the liquid stability of the gas barrier coating material before coating, the ratio of free carboxyl groups, expressed as γ / α, to the NH3 complex is preferably 0.00 or more, more preferably 0.01 or more, and even more preferably 0.02 or more.

[0854] Furthermore, from the viewpoint of improving the barrier properties of the gas barrier layer 103 obtained after coating, the above-mentioned γ / α is preferably 1.00 or less, more preferably 0.80 or less, even more preferably 0.60 or less, even more preferably 0.40 or less, even more preferably 0.20 or less, and even more preferably 0.10 or less.

[0855] Furthermore, in the infrared absorption spectrum of the gas barrier layer 103, 1493 cm⁻¹ -1 The above 1780cm -1 Let the total peak area within the following absorption band range be A, and let 1598 cm⁻¹ be the peak area. -1 The above 1690cm -1 Let the total peak area within the following absorption band range be B, and set 1690 cm⁻¹ as the maximum area. -1 The above 1780cm -1 Let the total peak area within the following absorption band range be C, and set 1493 cm⁻¹ as the maximum peak area. -1 The above is 1598cm -1 When the total peak area within the following absorption band range is set to D, the following shows a preferred example of the area ratio.

[0856] In the infrared absorption spectrum of the gas barrier layer 103, from the viewpoint of further improving the gas barrier performance after cooking, the area ratio of the amide bonds represented by B / A is preferably 0.200 or more, more preferably 0.220 or more, and even more preferably 0.250 or more.

[0857] Furthermore, from the viewpoint of further improving the balance between barrier properties and productivity, the area ratio of the amide bond represented by B / A is preferably 0.370 or less, more preferably 0.350 or less, and even more preferably 0.300 or less.

[0858] In the infrared absorption spectrum of the gas barrier layer 103, from the viewpoint of further improving the gas barrier performance after cooking, the area ratio of carboxylic acid expressed as C / A is preferably 0.150 or less, more preferably 0.100 or less, even more preferably 0.080 or less, and even more preferably 0.060 or less.

[0859] Furthermore, the lower limit of the area ratio of carboxylic acids represented by C / A is not limited, for example, it can be 0.000 or more, or it can be 0.0001 or more.

[0860] In the infrared absorption spectrum of the gas barrier layer 103, from the viewpoint of further improving the balance between barrier properties and productivity, the area ratio of the carboxylate, expressed as D / A, is preferably 0.580 or more, and more preferably 0.600 or more.

[0861] Furthermore, from the viewpoint of further improving the gas barrier performance after cooking, the D / A ratio is preferably 0.800 or less, more preferably 0.780 or less, even more preferably 0.760 or less, and even more preferably 0.740 or less.

[0862] Furthermore, from the viewpoint of achieving a more ideal balance between productivity and barrier properties in gas barrier laminates, it is also preferable that the area ratio of amide bonds represented by B / A is 0.200 or more and 0.370 or less, the area ratio of carboxylic acids represented by C / A is 0.150 or less, and the area ratio of carboxylate represented by D / A is 0.580 or more and 0.800 or less.

[0863] In the infrared absorption spectrum of the gas barrier layer 103, from the viewpoint of improving barrier properties, the area ratio of the carboxylate (represented by D / A) relative to the area ratio of the amide bond (represented by B / A) is preferably 1.2 or more, more preferably 1.5 or more, and more preferably 2.0 or more.

[0864] Furthermore, from the viewpoint of improving barrier properties after cooking, the area ratio of the carboxylate represented by D / A relative to the area ratio of the amide bond represented by B / A is preferably 4.0 or less, more preferably 3.5 or less, and even more preferably 3.0 or less.

[0865] Here, in the gas barrier layer 103, at 1700cm -1 The absorption of unreacted carboxylic acids based on the νC=O of the nearby visible infrared absorption spectrum, in the range of 1630–1685 cm⁻¹. -1 Absorption based on νC=O, which is a cross-linking structure, is visible in the vicinity at 1540–1560 cm⁻¹. -1 Nearby absorption based on carboxylates at νC=O is visible in the 1300–1490 cm⁻¹ region. -1 The absorption of δN-H based on ammonia that has formed a complex is visible nearby.

[0866] The 1300 cm⁻¹ in the infrared absorption spectrum is considered to be... -1 The above 1490cm -1 The maximum peak height α of absorbance in the following range indicates the amount of ammonia present in the complex, 1690 cm⁻¹. -1 The above 1780cm -1The maximum peak height γ in the following range is an indicator of the amount of free, i.e., unreacted carboxylic acid present.

[0867] In the fourth embodiment, specifically, the maximum peak heights α and γ can be measured by the following steps: A 1cm × 3cm sample is cut from the gas barrier layer 103. Then, the infrared absorption spectrum of the surface of the gas barrier layer 103 is obtained using total infrared reflectance (ATR) measurement. In the obtained infrared absorption spectrum, the peak heights α and γ are connected by a straight line at 900cm. -1 absorbance and 1900cm -1 Using the absorbance as a baseline, the maximum peak height within each absorbance range is calculated.

[0868] In addition, the 1493 cm⁻¹ in the infrared absorption spectrum is considered to be... -1 The above 1780cm -1 The total peak area A within the following absorption band range represents an indicator of the total stoichiometry of carboxylic acid, amide bond, and carboxylate, 1598 cm⁻¹. -1 The above 1690cm -1 The total peak area B within the following absorption band range represents an indicator of the amount of amide bonds present. Furthermore, it is believed that 1690 cm⁻¹... -1 The above 1780cm -1 The total peak area C within the following absorption band range represents an indicator of the amount of unreacted carboxylic acid present, 1493 cm⁻¹. -1 The above is 1598cm -1 The total peak area D within the absorption band below represents an indicator of the amount of carboxylate present.

[0869] In the fourth embodiment, specifically, the total peak areas A to D can be measured by the following steps.

[0870] First, a 1cm × 3cm sample for measurement is cut from the gas barrier layer 103. Next, the infrared absorption spectrum of the surface of the gas barrier layer 103 is obtained by infrared total reflectance measurement (ATR method). Based on the obtained infrared absorption spectrum, the total peak areas A to D are calculated by the following steps (1) to (4).

[0871] (1) 1780cm -1 With 1493cm -1 The absorbance values ​​are connected by a straight line (N), and the values ​​from 1493 cm⁻¹ will be represented by the absorbance values. -1 The above 1780cm -1 The absorption spectrum within the following absorption band range and the area enclosed by N are taken as the total peak area A.

[0872] (2) From 1690cm -1Draw a straight line (O) perpendicular to the absorbance (Q), and take the intersection of N and O as P, starting from 1598cm. -1 Draw a straight line (S) perpendicular to the absorbance (R), and take the intersection of N and S as T. The line drawn from 1598 cm⁻¹... -1 The above 1690cm -1 The area enclosed by the absorption spectrum within the following absorption band range and the lines S, T, N, P, O, absorbance Q, and R is taken as the total peak area B.

[0873] (3) The height of 1690cm -1 The above 1780cm -1 The area enclosed by the absorption spectrum and absorbance Q, line O, point P, and line N within the following absorption band range is taken as the total peak area C.

[0874] (4) The 1493cm -1 The above is 1598cm -1 The area enclosed by the absorption spectrum, absorbance R, line S, point T, and line N within the following absorption band range is taken as the total peak area D.

[0875] Next, the area ratios B / A, C / A, and D / A are calculated from the areas obtained using the above method.

[0876] It should be noted that, in the fourth embodiment, for the measurement of infrared absorption spectra (infrared total internal reflection measurement: ATR method), for example, an IRT-5200 device manufactured by Nippon Spectrophotometer Co., Ltd. can be used, equipped with a PKM-GE-S (germanium) crystal, at an incident angle of 45 degrees, room temperature, and a resolution of 4 cm⁻¹. -1 The test was conducted under the condition of a cumulative total of 100 tests.

[0877] The maximum peak heights α and γ of the gas barrier layer 103, as well as the area ratio of amide bonds (represented by B / A), the area ratio of carboxylic acids (represented by C / A), and the area ratio of carboxylate salts (represented by D / A), can be controlled by appropriately adjusting the manufacturing conditions of the gas barrier layer 103. Specifically, factors for controlling the maximum peak heights α and γ of the gas barrier layer 103, as well as the area ratios of amide bonds (represented by B / A), carboxylic acids (represented by C / A), and carboxylate salts (represented by D / A), include the proportions of polycarboxylic acids, polyamine compounds, polyvalent metal compounds, and phosphorus compounds, the preparation method of the mixture before curing, and the method, temperature, and time of heat treatment of the mixture.

[0878] Next, the components contained in the mixture (gas barrier coating material) before curing will be explained.

[0879] (Polycarboxylic acids)

[0880] Polycarboxylic acids are compounds having two or more carboxyl groups within their molecules. Specifically, examples include homopolymers or copolymers of α,β-unsaturated carboxylic acids such as (meth)acrylic acid, itaconic acid, fumaric acid, crotonic acid, cinnamic acid, 3-hexenoic acid, and 3-hexenediaic acid. Alternatively, they can be copolymers of the aforementioned α,β-unsaturated carboxylic acids with esters such as ethyl esters, olefins such as ethylene, etc.

[0881] Among them, the preferred polymers are homopolymers or copolymers of acrylic acid, methacrylic acid, itaconic acid, fumaric acid, crotonic acid, and cinnamic acid; more preferably, one or more polymers selected from the group consisting of polyacrylic acid, polymethacrylic acid, and copolymers of acrylic acid and methacrylic acid; further preferably, at least one polymer selected from polyacrylic acid and polymethacrylic acid; and even more preferably, at least one polymer selected from homopolymers of acrylic acid and homopolymers of methacrylic acid.

[0882] In this fourth embodiment, the term "polyacrylic acid" includes both homopolymers of acrylic acid and copolymers of acrylic acid with other monomers. In the case of copolymers of acrylic acid with other monomers, for polyacrylic acid, 100% by mass of the polymer contains structural units derived from acrylic acid, typically 90% by mass or more, preferably 95% by mass or more, and more preferably 99% by mass or more.

[0883] Furthermore, in the fourth embodiment, the term "polymethacrylic acid" includes both homopolymers of methacrylic acid and copolymers of methacrylic acid with other monomers. In the case of copolymers of methacrylic acid with other monomers, for polymethacrylic acid, 100% by mass of the polymer contains structural units derived from methacrylic acid, typically 90% by mass or more, preferably 95% by mass or more, and more preferably 99% by mass or more.

[0884] Polycarboxylic acids are polymers formed by the polymerization of carboxylic acid monomers. From the viewpoint of excellent balance between gas barrier properties and operability, the molecular weight of polycarboxylic acids is preferably 500 to 2,500,000, more preferably 5,000 to 2,000,000, even more preferably 10,000 to 1,500,000, and even more preferably 100,000 to 1,200,000.

[0885] In this fourth embodiment, the molecular weight of the polycarboxylic acid is the weight-average molecular weight converted from polyethylene oxide, which can be determined using gel permeation chromatography (GPC).

[0886] At least a portion of a polycarboxylic acid can be neutralized using a volatile base. By neutralizing the polycarboxylic acid with a volatile base, gelation can be suppressed when polyvalent metal compounds or polyamine compounds are mixed with the polycarboxylic acid. Therefore, from the viewpoint of preventing gelation, it is preferable to prepare a partially or completely neutralized carboxyl group using a volatile base. The neutralized product can be obtained by partially or completely neutralizing the carboxyl group of the polycarboxylic acid with a volatile base, that is, by partially or completely preparing a carboxylate of the polycarboxylic acid. This prevents gelation when polyamine compounds or polyvalent metal compounds are added.

[0887] Partial neutralization can be prepared by adding a volatile base to an aqueous solution of a polycarboxylic acid polymer. The desired degree of neutralization can be achieved by adjusting the molar ratio of the polycarboxylic acid to the volatile base. In the fourth embodiment, from the viewpoint of sufficiently suppressing gelation caused by the neutralization reaction with the amino group of the polyamine compound, the degree of neutralization of the polycarboxylic acid obtained using the volatile base is preferably 70 to 300 equivalents, more preferably 90 to 250 equivalents, and even more preferably 100 to 200 equivalents.

[0888] As a volatile base, any water-soluble base can be used.

[0889] Examples of volatile bases include, for example, tertiary amines such as ammonia, morpholine, alkylamines, 2-dimethylaminoethanol, N-methylmorpholine, ethylenediamine, triethylamine, or aqueous solutions of these, or mixtures thereof. From the viewpoint of obtaining good gas barrier properties, aqueous ammonia solutions are preferred.

[0890] (Polyamine compounds)

[0891] The mixture before curing contains polyamine compounds. By including polyamine compounds, the barrier properties of the resulting gas barrier material can be improved.

[0892] Polyamine compounds are compounds having two or more amino groups on their main chain, side chain, or terminal, and are preferably polymers. Specifically, examples include aliphatic polyamines such as polyallylamine, polyvinylamine, polyethyleneimine, and poly(propyleneimine); polyamides such as polylysine and polyarginine, which have amino groups on their side chains; and so on. Alternatively, polyamines can be formed by modifying a portion of the amino groups.

[0893] From the viewpoint of obtaining good gas barrier properties, the polyamine compound preferably contains polyethyleneimine, and more preferably polyethyleneimine.

[0894] From the viewpoint of achieving a good balance between gas barrier properties and operability, the number average molecular weight of the polyamine compound is preferably 50 to 2,000,000, more preferably 100 to 1,000,000, even more preferably 1,500 to 500,000, even more preferably 1,500 to 100,000, even more preferably 1,500 to 50,000, even more preferably 3,500 to 20,000, even more preferably 5,000 to 15,000, and even more preferably 7,000 to 12,000.

[0895] In this fourth embodiment, the molecular weight of the polyamine compound can be determined using the boiling point elevation method or the viscosity method.

[0896] From the viewpoint of further improving the gas barrier performance after cooking, the ratio of (moles of amino groups in the polyamine compound in the mixture) to (moles of -COO- groups in the polycarboxylic acid in the mixture) is preferably 0.20 or more, more preferably 0.25 or more, even more preferably 0.30 or more, even more preferably 0.35 or more, and even more preferably 0.40 or more.

[0897] From the same point of view, the ratio of (moles of amino groups contained in the polyamine compound in the mixture) to (moles of -COO- groups contained in the polycarboxylic acid in the mixture) is preferably 0.90 or less, more preferably 0.85 or less, even more preferably 0.80 or less, even more preferably 0.75 or less, and even more preferably 0.70 or less.

[0898] Although the detailed reasons are unclear, it is believed that by achieving a good balance between amide crosslinking (which is formed by amino groups constituting polyamine compounds) and metal crosslinking (which is formed by polyvalent metals constituting polycarboxylic acids and polyvalent metal salts) to form a dense structure, a gas barrier layer 103 with excellent gas barrier performance after cooking and a gas barrier laminate having the same can be obtained.

[0899] (Polyvalent metal compounds)

[0900] Polyvalent metal compounds specifically refer to metals and metal compounds belonging to groups 2 to 13 of the periodic table. More specifically, examples include metals with a valence of divalent or higher, such as magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), and aluminum (Al), as well as their oxides, hydroxides, halides, carbonates, phosphates, phosphites, hypophosphites, sulfates, or sulfites. From the viewpoint of water resistance and impurities, metal oxides or metal hydroxides are preferred.

[0901] From the viewpoint of further improving the gas barrier performance after cooking, the metal with a valence of 2 or higher in the polyvalent metal compound is preferably one or more metals selected from the group consisting of Zn, Ca, Mg, Ba and Al, and more preferably Zn.

[0902] From the same point of view, the polyvalent metal compound is preferably a compound of one or more metals with a divalent or higher valence selected from the group consisting of Zn, Ca, Mg, Ba and Al, and more preferably a compound of Zn.

[0903] From the same point of view, the polyvalent metal compound is preferably one or more compounds selected from the group consisting of oxides such as magnesium oxide, calcium oxide, barium oxide, zinc oxide, and magnesium hydroxide, and hydroxides such as calcium hydroxide, barium hydroxide, and zinc hydroxide, more preferably at least one of zinc oxide and zinc hydroxide, and even more preferably zinc oxide.

[0904] In the fourth embodiment, from the viewpoint of further improving the gas barrier performance after cooking, the ratio of (moles of polyvalent metal compounds in the mixture) to (moles of -COO- groups contained in the polycarboxylic acid in the mixture) is preferably 0.10 or more, more preferably 0.13 or more, even more preferably 0.15 or more, and even more preferably 0.18 or more.

[0905] From the same point of view, the ratio of (moles of polyvalent metal compounds in the mixture) to (moles of -COO- groups contained in the polycarboxylic acid in the mixture) is preferably 0.80 or less, more preferably 0.70 or less, even more preferably 0.60 or less, even more preferably 0.55 or less, and even more preferably 0.50 or less.

[0906] In the fourth embodiment, from the viewpoint of further improving the gas barrier performance after cooking, the ratio of (moles of polyvalent metal compounds in the mixture) to (moles of amino groups from polyamine compounds in the mixture) is preferably 0.25 or more, more preferably 0.35 or more, and even more preferably 0.40 or more.

[0907] From the same point of view, the ratio of (moles of polyvalent metal compounds in the mixture) to (moles of amino groups from polyamine compounds in the mixture) is preferably 0.65 or less, more preferably 0.60 or less, and even more preferably 0.55 or less.

[0908] (Phosphorus compounds or their salts)

[0909] Phosphorus compounds or their salts contain one or more -P-OH groups in their molecular structure. Phosphorus compounds can be complexed in mixtures in the form of salts.

[0910] From the viewpoint of further improving the water vapor barrier properties after cooking, the phosphorus compound preferably contains two or more -P-OH groups, more preferably three or more -P-OH groups. Furthermore, from the viewpoint of improving the liquid stability of the gas barrier coating material, the number of -P-OH groups in the phosphorus compound can be, for example, two or less.

[0911] Specific examples of phosphorus compounds include phosphoric acid, phosphorous acid, phosphonic acid, hypophosphoric acid, polyphosphoric acid, and their derivatives.

[0912] Specifically, polyphosphoric acid has a condensation structure of two or more phosphoric acids in its molecular structure. Examples include diphosphoric acid (pyrophosphoric acid), triphosphoric acid, and polyphosphoric acid formed by the condensation of four or more phosphoric acids.

[0913] Specific examples of derivatives include:

[0914] Esters of the aforementioned phosphorus compounds, such as phosphoric acid starch and cross-linked phosphoric acid starch;

[0915] Halides such as chlorides;

[0916] Acid anhydrides such as phosphorus tetraoxide; and

[0917] Compounds such as nitrotri(methylenephosphonic acid) and N,N,N',N'-ethylenediaminetetra(methylenephosphonic acid) have structures in which hydrogen atoms bonded to phosphorus atoms are replaced by alkyl groups.

[0918] From the viewpoint of further improving the balance between barrier properties and productivity, the phosphorus compound is one or more selected from the group consisting of phosphoric acid, phosphorous acid, hypophosphoric acid, polyphosphoric acid, phosphonic acid and their salts, more preferably at least one selected from the group consisting of phosphoric acid and phosphorous acid.

[0919] Furthermore, specific examples of salts in phosphorus compounds include salts of monovalent metals such as sodium and potassium, and ammonium salts. From the viewpoint of improved barrier properties, ammonium salts are preferred for phosphorus compounds.

[0920] In the fourth embodiment, from the viewpoint of improving barrier properties, the ratio of (moles of P atoms from the phosphorus compound or its salt in the mixture) to (moles of -COO- groups from the polycarboxylic acid in the mixture) can be, for example, 0.0001 or more, preferably 0.001 or more, more preferably 0.003 or more, and even more preferably 0.005 or more. In phosphorus compounds containing one P atom in their chemical formula, such as phosphoric acid, the number of moles of P atoms and the number of moles of the phosphorus compound have the same meaning.

[0921] Furthermore, from the viewpoint of improving the liquid stability of the barrier coating material (mixture), the ratio of (moles of P atoms from phosphorus compounds or their salts in the mixture) to (moles of -COO- groups from polycarboxylic acids in the mixture) is preferably 0.3 or less, more preferably 0.1 or less, even more preferably 0.08 or less, and even more preferably 0.005 or less.

[0922] The mixture before curing may contain components other than those mentioned above.

[0923] For example, the mixture preferably also contains ammonium carbonate salts. Ammonium carbonate salts are substances added to improve the solubility of polyvalent metal compounds by converting them into ammonium carbonate complexes, thereby preparing a homogeneous solution containing the polyvalent metal compounds. By including ammonium carbonate salts in the mixture before curing, the solubility of the polyvalent metal compounds can be increased, resulting in a more homogeneous mixture containing the polyvalent metal compounds.

[0924] As a carbonate-based ammonium salt, examples include ammonium carbonate and ammonium bicarbonate. From the perspective of easy volatilization and not easy to remain in the obtained gas barrier layer, ammonium carbonate is preferred.

[0925] From the viewpoint of further improving the solubility of the polyvalent metal compound, the ratio of (moles of ammonium carbonate salt in the mixture) to (moles of polyvalent metal compound in the mixture) is preferably 0.05 or more, more preferably 0.10 or more, even more preferably 0.25 or more, even more preferably 0.50 or more, and even more preferably 0.75 or more.

[0926] Furthermore, from the viewpoint of further improving the coatability of the coating material for gas barrier applications, the ratio of (moles of ammonium carbonate salts in the coating material for gas barrier applications) to (moles of polyvalent metal compounds in the coating material for gas barrier applications) is preferably 10.0 or less, more preferably 5.0 or less, even more preferably 2.0 or less, and even more preferably 1.5 or less.

[0927] Furthermore, from the viewpoint of suppressing depressions when coating as a gas barrier coating material, the mixture before curing preferably also contains a surfactant.

[0928] When the total solid component of the mixture is set to 100% by mass, the amount of surfactant added is preferably 0.01 to 3% by mass, more preferably 0.01 to 1% by mass.

[0929] Examples of surfactants include anionic surfactants, nonionic surfactants, cationic surfactants, and amphoteric surfactants. From the viewpoint of obtaining good coatability, nonionic surfactants are preferred, polyoxyethylene alkyl ethers are more preferred, and polyoxyethylene alkyl ethers are even more preferred.

[0930] Examples of nonionic surfactants include polyoxyalkylene alkyl ethers, polyoxyalkylene alkyl ethers, polyoxyalkylene fatty acid esters, sorbitan fatty acid esters, organosilicon surfactants, alkynyl alcohol surfactants, and fluorinated surfactants.

[0931] Examples of polyoxyethylene alkyl aryl ethers include, for example, polyoxyethylene nonylphenyl ether, polyoxyethylene octylphenyl ether, and polyoxyethylene dodecylphenyl ether.

[0932] Examples of polyoxyethylene alkyl ethers include, for example, polyoxyethylene oil-based ethers and polyoxyethylene lauryl ethers.

[0933] Examples of polyoxyethylene fatty acid esters include, for example, polyoxyethylene oleate, polyoxyethylene laurate, and polyoxyethylene distearate.

[0934] Examples of sorbitan fatty acid esters include, for example, sorbitan laurate, sorbitan monostearate, sorbitan monooleate, sorbitan sesquioleate, polyoxyethylene monooleate, and polyoxyethylene stearate.

[0935] Examples of organosilicon surfactants include, for example, dimethylpolysiloxane.

[0936] Examples of alkynyl alcohol surfactants include 2,4,7,9-tetramethyl-5-decyn-4,7-diol, 3,6-dimethyl-4-octyyn-3,6-diol, and 3,5-dimethyl-1-hexyn-3-ol.

[0937] Examples of fluorinated surfactants include, for example, fluoroalkyl esters.

[0938] The mixture before curing may contain additives other than those mentioned above. For example, various additives such as lubricants, slip agents, anti-caking agents, antistatic agents, anti-fogging agents, pigments, dyes, and inorganic or organic fillers may be added.

[0939] Furthermore, from the viewpoint of improving the coatability when applied as a gas barrier coating material, the concentration of the solid component of the mixture before curing is preferably set to 0.5 to 15% by mass, and more preferably 1 to 10% by mass.

[0940] (Manufacturing method of gas barrier layer)

[0941] Specifically, the gas barrier layer 103 can be manufactured by applying a mixture (gas barrier coating material) before curing and then curing it.

[0942] The mixture can be obtained as described below.

[0943] First, a volatile base is appropriately added to the polycarboxylic acid, thereby completely or partially neutralizing the carboxyl groups of the polycarboxylic acid. A polyvalent metal salt compound and a suitable ammonium carbonate salt are then mixed to form a metal salt in all or part of the carboxyl groups of the polycarboxylic acid that has been neutralized by the volatile base, and in the carboxyl groups of the polycarboxylic acid that has not been neutralized by the volatile base.

[0944] Then, a polyamine compound is added, followed by a phosphorus compound or its salt, to obtain a mixture before curing. This forms a salt between the phosphorus compound and the amino group of the polyvalent metal compound or polyamine.

[0945] By mixing polycarboxylic acids, polyvalent metal salts, phosphorus compounds or their salts, appropriate ammonium carbonates, and polyamine compounds through this step, the formation of aggregates can be suppressed, resulting in a more homogeneous mixture. This allows for a more efficient dehydration condensation reaction between the -COO- groups in the polycarboxylic acids and the amino groups in the polyamine compounds.

[0946] More specifically, as described below. The following explanation will take the case of a mixture containing a volatile base and a carbonate-based ammonium salt as an example.

[0947] First, prepare a completely or partially neutralized solution of the carboxyl groups that constitute the polycarboxylic acid.

[0948] Adding a volatile base to a polycarboxylic acid completely or partially neutralizes its carboxyl groups. By neutralizing the carboxyl groups of the polycarboxylic acid, gelation that occurs when polyvalent metal compounds or polyamine compounds are added can be effectively prevented due to the reaction between the carboxyl groups constituting the polycarboxylic acid and the amino groups constituting the polyvalent metal compounds or polyamine compounds, thus obtaining a more homogeneous mixture.

[0949] Next, a polyvalent metal salt compound and a carbonate ammonium salt are added and dissolved. The resulting polyvalent metal ions react with the -COO- group constituting the polycarboxylic acid to form a polyvalent metal salt. Here, the -COO- group that forms the salt with the polyvalent metal ions refers to both the unneutralized carboxyl group and the neutralized -COO- group. In the case of the neutralized -COO- group, the polyvalent metal ions from the aforementioned polyvalent metal compound replace and coordinate to form a -COO- group polyvalent metal salt.

[0950] Then, after forming the polyvalent metal salt, a polyamine compound and a phosphorus compound or their salts are further added, thereby obtaining a mixture. At this point, the polyvalent metal salt located at the -COO- group also coordinates with the -PO- group in the phosphorus compound, forming a -COO-polyvalent metal -OP- structure. Furthermore, an ionic bond is formed between the -NH2 group in the polyamine and the -PO- group in the phosphorus compound.

[0951] The mixture thus manufactured is applied as a gas barrier coating material to the inorganic layer 102 or to an interlayer formed on the inorganic layer 102 between the gas barrier layer 103 and the inorganic layer 102, and then dried and cured to form the gas barrier layer 103. At this time, the polyvalent metal salt constituting the -COO- group of the polycarboxylic acid forms a metal crosslink, the amino group constituting the polyamine forms an amide crosslink, and the -PO- group in the phosphorus compound forms an ionic crosslink with the polyvalent metal or the amino group in the polyamine, thus obtaining a gas barrier layer 103 with excellent gas barrier properties. A more detailed manufacturing method for the gas barrier layer 103 is described later.

[0952] From the viewpoint of improving barrier properties, the thickness of the gas barrier layer 103 after drying and curing is preferably 0.01 μm or more, more preferably 0.05 μm or more, and even more preferably 0.1 μm or more.

[0953] Furthermore, from the viewpoint of reducing the overall thickness of the gas barrier laminate, the thickness of the dried and cured gas barrier layer 103 is preferably 15 μm or less, more preferably 5 μm or less, and even more preferably 1 μm or less.

[0954] (Substrate layer)

[0955] The substrate layer 101 can be a single layer or two or more layers. The shape of the substrate layer 101 is not limited; for example, it can be a sheet or film shape, a shallow dish, a cup, a hollow body, etc.

[0956] As the material for the substrate layer 101, any material capable of stably forming an inorganic layer 102 on the substrate layer 101 and capable of being coated with a solution of a gas barrier coating material on the top of the inorganic layer 102 can be used without limitation. Examples of materials for the substrate layer 101 include, for instance, resins such as thermosetting resins and thermoplastic resins, organic materials such as paper; inorganic materials such as glass, ceramics, silicon dioxide, silicon oxynitride, silicon nitride, concrete, aluminum, alumina, iron, copper, stainless steel, and other metals; and multilayer substrate layers formed by combinations of organic materials or combinations of organic and inorganic materials. Among these, for example, in applications such as packaging materials and panels, plastic films selected from the group consisting of thermosetting resins and thermoplastic resins, or organic materials such as paper, are preferred.

[0957] Known thermosetting resins can be used as thermosetting resins. Examples include epoxy resins, unsaturated polyester resins, phenolic resins, urea-melamine resins, polyurethane resins, silicone resins, and polyimides.

[0958] Known thermoplastic resins can be used as thermoplastic resins. Examples include polyolefins (polyethylene, polypropylene, poly(4-methyl-1-pentene), poly(1-butene), etc.), polyesters (polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, etc.), polyamides (nylon-6, nylon-66, poly(m-phenylene adipamide), etc.), polyvinyl chloride, polyimide, ethylene-vinyl acetate copolymer or its saponification, polyvinyl alcohol, polyacrylonitrile, polycarbonate, polystyrene, ion-crosslinked polymers, fluoropolymers, or mixtures thereof.

[0959] Among them, from the viewpoint of achieving good transparency, one or more resins selected from the group consisting of polypropylene, polyethylene terephthalate (PET), polyethylene naphthalate, polyamide, polyimide and polybutylene terephthalate are preferred.

[0960] Furthermore, from the viewpoint of excellent resistance to pinholes, damage, and heat resistance, it is preferable to use one or more resins selected from the group consisting of polyamide, polyethylene terephthalate, and polybutylene terephthalate. Similarly, from the same viewpoint, the substrate layer 101 is preferably a layer comprising one or more resins selected from the group consisting of polyamide, polyethylene terephthalate, and polybutylene terephthalate, and more preferably a layer comprising one or more of these resins.

[0961] Furthermore, when a hygroscopic material such as polyamide is used in the substrate layer 101, the substrate layer 101 absorbs moisture and swells in the gas barrier laminate, which can easily reduce the gas barrier performance under high humidity, the gas barrier performance after cooking, and the gas barrier performance when filled with acidic contents. However, in the fourth embodiment, even when a hygroscopic material is used as the substrate layer 101, the reduction in the gas barrier performance of the gas barrier laminate under high humidity and the gas barrier performance after cooking can be appropriately suppressed.

[0962] Alternatively, a film formed of thermosetting resin or thermoplastic resin can be stretched along at least one direction, preferably a biaxial direction, to form a substrate layer 101.

[0963] From the viewpoint of excellent transparency, rigidity and heat resistance, the substrate layer 101 is preferably a biaxially stretched film formed of one or more thermoplastic resins selected from the group consisting of polypropylene, polyethylene terephthalate, polyethylene naphthalate, polyamide, polyimide and polybutylene terephthalate, more preferably a biaxially stretched film formed of one or more thermoplastic resins selected from the group consisting of polyamide, polyethylene terephthalate and polybutylene terephthalate.

[0964] Alternatively, polyvinylidene chloride, polyvinyl alcohol, ethylene-vinyl alcohol copolymer, acrylic resin, urethane resin, etc., can be coated on the surface of the substrate layer 101.

[0965] Furthermore, for the substrate layer 101, in order to improve adhesion to the gas barrier layer 103, a surface-treated substrate layer can be applied. Specifically, the surface of the substrate layer 101 opposite to the gas barrier layer 103 can be subjected to surface activation treatments such as corona treatment, flame treatment, plasma treatment, or primer coating treatment.

[0966] From the viewpoint of obtaining good film properties, the thickness of the substrate layer 101 is preferably 1 μm or more, more preferably 5 μm or more, even more preferably 10 μm or more, and preferably 1000 μm or less, more preferably 500 μm or less, and even more preferably 300 μm or less.

[0967] (Inorganic layer)

[0968] Inorganic materials constituting the inorganic layer 102 may include, for example, metals, metal oxides, metal nitrides, metal fluorides, and metal nitrides, which are capable of forming barrier films.

[0969] As the inorganic material constituting the inorganic layer 102, examples include one or more of the following: elements selected from Group 2A of the periodic table such as beryllium, magnesium, calcium, strontium, and barium; transition elements of the periodic table such as titanium, zirconium, ruthenium, hafnium, and tantalum; elements from Group 2B of the periodic table such as zinc; elements from Group 3A of the periodic table such as aluminum, gallium, indium, and thallium; elements from Group 4A of the periodic table such as silicon, germanium, and tin; and elements from Group 6A of the periodic table such as selenium and tellurium, including their elemental form, oxide, nitride, fluoride, or nitrogen oxide.

[0970] It should be noted that in the fourth embodiment, the group names of the elements in the periodic table for the inorganic layer 102 are represented in the old CAS form.

[0971] Furthermore, among the aforementioned inorganic materials, from the perspective of excellent balance in terms of barrier properties, cost, etc., it is preferable to select one or more inorganic materials selected from the group consisting of silicon oxide, aluminum oxide, and aluminum, and more preferably aluminum oxide.

[0972] It should be noted that, in addition to silicon dioxide, silicon oxide may also contain silicon monoxide and silicon suboxide.

[0973] The inorganic layer 102 is formed from the aforementioned inorganic material. From the perspective of excellent balance between barrier properties and cost, the inorganic layer 102 preferably includes an alumina layer composed of alumina.

[0974] The inorganic layer 102 can be composed of a single inorganic layer or multiple inorganic layers. Furthermore, if the inorganic layer 102 is composed of multiple inorganic layers, they can be composed of inorganic layers of the same type or inorganic layers of different types.

[0975] From the viewpoint of balancing improved barrier properties and improved operability, the thickness of the inorganic layer 102 is usually 1 nm or more, preferably 4 nm or more, and usually 1000 nm or less, preferably 500 nm or less.

[0976] Here, the thickness of the inorganic layer 102 can be determined, for example, using observation images obtained by transmission electron microscopy or scanning electron microscopy.

[0977] The method for forming the inorganic layer 102 is not limited. For example, it can be formed on one or both sides of the substrate layer 101 using vacuum evaporation, ion plating, sputtering, chemical vapor deposition, physical vapor deposition (CVD), plasma CVD, sol-gel methods, etc. Among these, sputtering, ion plating, chemical vapor deposition (CVD), physical vapor deposition (PVD), and plasma CVD are ideal for film formation under reduced pressure. Therefore, it is predicted that silicon-containing chemically active molecules such as silicon nitride and silicon oxynitride will react rapidly, thereby improving the surface smoothness of the inorganic layer 102 and reducing pores. For these bonding reactions to occur rapidly, it is ideal for the inorganic atoms or compounds to be chemically active molecules or atoms.

[0978] Furthermore, from the viewpoint of improving the balance between the barrier properties and productivity of the gas barrier laminate, the inorganic layer 102 is preferably a vapor-deposited film.

[0979] From the viewpoint of improving the balance between the barrier properties and productivity of the gas barrier laminate, the inorganic layer 102 is a vapor-deposited film disposed on the substrate layer 101, or a vapor-deposited film disposed on the interlayer when there is an interlayer between the substrate layer 101 and the inorganic layer 102, and is composed of one or more inorganic substances selected from the group consisting of silicon oxide, aluminum oxide and aluminum.

[0980] (Base coat)

[0981] An undercoat layer 104 may be provided between the substrate layer 101 and the inorganic layer 102. Figure 14 By setting the base coating 104, their adhesion can be further improved, and the barrier properties after cooking can be further improved.

[0982] From the viewpoint of improving the adhesion between the substrate layer 101 and the inorganic layer 102, the material for the base coating layer 104 may be, for example, one or more selected from the group consisting of polyurethane resin, polyester resin, oxazoline resin, and (meth)acrylic resin.

[0983] Examples of polyurethane resins include various polyurethane resins, polyurethane polyurea resins, and their prepolymers. Specific examples of such urethane resins include reactions of diisocyanate components such as toluene diisocyanate, xylene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, cyclohexane diisocyanate, isophorone diisocyanate, and dicyclohexyl diisocyanate with diol components such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, neopentyl glycol, cyclohexanediol, bisphenol, polyester glycol, polyether glycol, polycarbonate glycol, and polyethylene glycol; reactions of urethane prepolymers with isocyanate groups at the ends with amino compounds, aminosulfonates, polyhydroxycarboxylic acids, and acidic sulfurous acid; and so on.

[0984] Furthermore, from the viewpoint of improving barrier properties after cooking and the adhesion between the substrate layer 101 and the inorganic layer 102, it is preferable that the polyurethane resin in the base layer 104 is composed of a polyurethane resin having an aromatic ring structure in its main chain. For example, a polyurethane resin having an aromatic ring structure in its main chain can be obtained as a water-dispersible polyurethane resin through the reaction of a polyol, an organic polyisocyanate, and a chain extender. This allows the introduction of an aromatic ring structure into the main chain of the polyurethane resin.

[0985] As a polyurethane resin having an aromatic ring structure in the main chain, more specifically, the polyurethane resin described in Japanese Patent Application Publication No. 2018-171827 can be used.

[0986] Furthermore, in the aforementioned water-dispersible polyurethane resin, from the viewpoint of improving heat resistance, water resistance, and hydrolysis resistance, a crosslinking agent can be used in conjunction. The crosslinking agent can be an external crosslinking agent added as a third component relative to the water-dispersible polyurethane resin, or it can be an internal crosslinking agent that pre-introduces reaction sites capable of forming a crosslinking structure into the molecular structure of the water-dispersible polyurethane resin.

[0987] As a crosslinking agent, compounds having isocyanate groups, oxazoline groups, carbodiimide groups, epoxy groups, melamine resin groups, and silanol groups can be suitably used, with compounds having carbodiimide groups being more suitable. Furthermore, when using a compound having carbodiimide groups as a crosslinking agent, the amount of the compound added is preferably 0.1 to 3.0 mol of carbodiimide groups relative to 1.0 mol of carboxyl groups in the polyurethane resin, more preferably 0.2 to 2.0 mol, and even more preferably 0.3 to 1.0 mol.

[0988] Various polyester resins and their modifiers can be cited as examples of the polyester resin used in the primer layer 104. Specific examples of such polyester resins include reaction products of polycarboxylic acid components such as terephthalic acid, phthalic acid, isophthalic acid, trimellitic acid, pyromellitic acid, 2-sulfonic isophthalic acid, 5-sulfonic isophthalic acid, adipic acid, sebacic acid, succinic acid, and dodecanoic acid with diol components such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, neopentyl glycol, cyclohexanediol, and bisphenol, as well as modifiers based on acrylic resins, epoxy resins, etc.

[0989] When an oxazoline resin is used in the base coating 104, the base coating 104 is preferably composed of an oxazoline-based resin composition comprising an aqueous polymer containing an oxazoline group, an aqueous (meth)acrylic resin, and an aqueous polyester resin.

[0990] The oxazoline-based resin composition is, for example, composed of an aqueous polymer containing oxazoline groups with an oxazoline group content of 6.0 to 9.0 mmol / g, an aqueous (meth)acrylic resin with a carboxyl group content of 0.5 to 3.5 mmol / g, and an aqueous polyester resin with a carboxyl group content of 0.5 to 2.0 mmol / g.

[0991] In addition, the total amount of the aqueous polymer containing oxazoline, the aqueous (meth)acrylic resin and the aqueous polyester resin is set to 100% by mass. For example, the oxazoline resin composition contains 10 to 55% by mass of the aqueous polymer containing oxazoline, 10 to 80% by mass of the aqueous (meth)acrylic resin and 10 to 80% by mass of the aqueous polyester resin.

[0992] Furthermore, in the oxazoline resin composition, for example, the ratio of the molar number of oxazoline groups to the molar number of carboxyl groups [expressed as the ratio of the molar number of oxazoline groups (x mmol) to the molar number of carboxyl groups (y mmol) (x / y) × 100 [mol%]] is 150–420 mol%.

[0993] As the oxazoline resin used in the base coating 104, more specifically, the oxazoline resin described in International Publication No. 2016 / 186074 may be used.

[0994] From the viewpoint of obtaining good adhesion, the thickness of the base coating 104 is preferably 0.001 μm or more, more preferably 0.005 μm or more, even more preferably 0.01 μm or more, even more preferably 0.05 μm or more, even more preferably 0.1 μm or more, and even more preferably 0.2 μm or more.

[0995] Furthermore, from an economic point of view, the thickness of the base coating 104 is preferably 1.0 μm or less, more preferably 0.6 μm or less, even more preferably 0.5 μm or less, and may also be, for example, 0.1 μm or less or 0.05 μm or less.

[0996] (Adhesive layer)

[0997] In gas barrier laminates, an adhesive layer may also be provided. It should be noted that the primer layer 104 is excluded from the adhesive layer.

[0998] An adhesive layer may be disposed, for example, between the gas barrier layer 103 and the upper layer of the gas barrier layer 103. Alternatively, when the upper layer is formed of multiple layers, an adhesive layer may be disposed between the multiple layers. Here, the upper layer of the gas barrier layer 103 refers to the layer stacked on the side of the gas barrier layer 103 opposite to the side facing the inorganic layer 102.

[0999] The adhesive layer may contain a known adhesive. Examples of adhesives include laminated adhesives composed of organotitanium resins, polyethyleneimine resins, urethane resins, epoxy resins, acrylic resins, polyester resins, resins containing oxazoline groups, modified silicone resins and alkyl titanates, polyester polybutadiene, etc.; or one-component and two-component polyols and polyisocyanates, aqueous urethanes, ion-crosslinked polymers, etc. Alternatively, water-based adhesives with acrylic resins, vinyl acetate resins, urethane resins, polyester resins, etc., as the main raw materials may be used.

[1000] Furthermore, depending on the intended use of the gas barrier laminate 100, other additives such as curing agents and silane coupling agents can be added to the adhesive. When the gas barrier laminate is intended for use in hot water treatment such as boiling, from the viewpoint of heat resistance and water resistance, a dry lamination adhesive, represented by a polyurethane adhesive, is preferred, and a solvent-based two-component curing polyurethane adhesive is more preferred.

[1001] (Method for manufacturing gas barrier laminates)

[1002] In the fourth embodiment, the method for manufacturing the gas barrier laminate 100 includes, for example, the following steps: preparing a substrate layer 101; forming an inorganic layer 102 on the substrate layer 101; and forming a gas barrier layer 103 on the upper part of the substrate layer 101 on which the inorganic layer 102 is formed. Furthermore, after the step of forming the inorganic layer 102 and before the step of forming the gas barrier layer 103, a step of forming an undercoat layer 104 on the inorganic layer 102 may also be included.

[1003] In the process of forming the inorganic layer 102 on the substrate layer 101, the aforementioned method for forming the inorganic layer 102 may be used, for example.

[1004] The process of forming the gas barrier layer 103 includes, for example, the following steps: applying the mixture before curing as a gas barrier coating material to the inorganic layer 102, followed by drying, thereby obtaining the coating layer; and heating the coating layer to cause the carboxyl groups contained in the polycarboxylic acid to undergo a dehydration condensation reaction with the amino groups contained in the polyamine compound, thereby forming the gas barrier layer 103 having amide bonds.

[1005] There is no limitation on the method of coating the gas barrier coating material onto the inorganic layer 102; conventional methods can be used. For example, methods can be described using known coating machines such as Mayer bar coaters, air knife coaters, direct gravure coaters, gravure offset coaters, curved gravure coaters, reverse gravure coaters, and jet nozzle type gravure coaters; reverse roller coaters such as top-feed reverse coaters, bottom-feed reverse coaters, and nozzle-feed reverse coaters; five-roll coaters; lip coaters; bar coaters; bar reverse coaters; and die coaters.

[1006] From the viewpoint of achieving better barrier properties in the resulting gas barrier laminate, the coating amount (wet thickness) is preferably 0.05 μm, more preferably 1 μm or more.

[1007] Furthermore, from the viewpoint of suppressing warping of the obtained gas barrier laminate and from the viewpoint of more effectively carrying out the dehydration condensation reaction between the -COO- group contained in the polycarboxylic acid and the amino group contained in the polyamine compound, the wet thickness is preferably 300 μm or less, more preferably 200 μm or less, and even more preferably 100 μm or less.

[1008] For drying and heat treatment, heat treatment can be performed after drying, or drying and heat treatment can be performed simultaneously.

[1009] The method for drying and heating is not limited as long as the effects of the present invention are achieved; it can be a method for curing the gas barrier coating material or a method for heating the cured gas barrier coating material. Examples include ovens and dryers based on convective heat transfer; heating rollers based on conductive heat transfer; infrared, far-infrared, and near-infrared heaters based on radiative heat transfer using electromagnetic waves; and microwaves based on internal heating. From a manufacturing efficiency perspective, an apparatus capable of performing both drying and heating is preferred for the drying and heating process. Specifically, from the viewpoint of being usable for various purposes such as drying, heating, and annealing, a hot air oven is preferred; and from the viewpoint of excellent heat transfer efficiency to the film, a heating roller is preferred. Furthermore, the methods for drying and heating can be appropriately combined. Specifically, a hot air oven and a heating roller can be used together. For example, when the gas barrier coating material is dried using a hot air oven and then heated using a heating roller, the heating process time is shortened, which is preferable from a manufacturing efficiency perspective. In addition, it is preferable to use only a hot air oven for drying and heating.

[1010] Regarding the heat treatment conditions, for example, the heat treatment temperature is 80–250°C, and the heat treatment time is 1 second–10 minutes; preferably, the heat treatment temperature is 120–240°C, and the heat treatment time is 1 second–1 minute; more preferably, the heat treatment temperature is 170°C–230°C, and the heat treatment time is 1 second–30 seconds; even more preferably, the heat treatment temperature is 200°C–220°C, and the heat treatment time is 1 second–10 seconds. Furthermore, by using a heating roller as described above, heat treatment can be performed in a short time.

[1011] It should be noted that, from the viewpoint of effectively carrying out the dehydration condensation reaction between the -COO- group contained in polycarboxylic acids and the amino group contained in polyamine compounds, it is important to adjust the heat treatment temperature and time according to the wet thickness of the coating material used for gas barrier. By selecting appropriate heat treatment temperature and time, a suitable cross-linked structure can be formed.

[1012] By drying and heat-treating the coating material for gas barrier, the carboxyl groups of polycarboxylic acids react with polyamines and polyvalent metal compounds to form covalent bonds and ionic crosslinks, thereby forming a gas barrier layer 103 that also has good gas barrier properties after cooking.

[1013] In the fourth embodiment, the gas barrier laminate has excellent gas barrier properties and can be appropriately used as a packaging material for various purposes, such as packaging materials, especially food packaging materials for contents requiring high gas barrier properties, medical applications, industrial applications, and everyday grocery applications.

[1014] Furthermore, the gas barrier laminate in the fourth embodiment can be suitably used, for example, as a vacuum insulation film requiring high barrier performance; a sealing film for sealing electroluminescent elements, solar cells, etc.; and so on.

[1015] In the fourth embodiment, a specific example of a laminated structure comprising a gas barrier laminate is shown below.

[1016] (Example of laminated structure 1) Substrate layer 101 (PET substrate) / Inorganic layer 102 (alumina vapor deposition layer) / Gas barrier layer 103 / Adhesive layer / Polyolefin layer

[1017] (Example of laminated structure 2) Substrate layer 101 (PET substrate) / base coating 104 / inorganic layer 102 (alumina vapor deposition layer) / gas barrier layer 103 / adhesive layer / polyolefin layer

[1018] (Example of laminated structure 3) Substrate layer 101 (PET substrate) / Inorganic layer 102 (alumina vapor deposition layer) / Gas barrier layer 103 / Adhesive layer / Polyamide layer / Adhesive layer / Polyolefin layer

[1019] (Example of laminated structure 4) Substrate layer 101 (PET substrate) / Base coating 104 / Inorganic layer 102 (alumina vapor deposition layer) / Gas barrier layer 103 / Adhesive layer / Polyamide layer / Adhesive layer / Polyolefin layer

[1020] Here, by including a polyolefin layer composed of polyolefins such as polyethylene, polypropylene, poly(4-methyl-1-pentene), and poly(1-butene) in the laminated structure, the gas barrier laminate can achieve good resistance to pinholes, damage, and heat, and further suppress the reduction of gas barrier performance under high humidity and after cooking treatment.

[1021] <Fifth Implementation>

[1022] Figure 15 A cross-sectional view illustrating an example of the configuration of the gas barrier laminate in the fifth embodiment. Figure 15 The gas barrier laminate 100 shown includes a substrate layer 101, a gas barrier layer 103 disposed on at least one side of the substrate layer 101, and an inorganic layer 102 disposed between the substrate layer 101 and the gas barrier layer 103. Moreover, the gas barrier layer 103 is composed of a cured product comprising a mixture of polycarboxylic acids, polyamine compounds, and polyvalent metal compounds.

[1023] The specific composition of each layer will be described later.

[1024] In the gas barrier laminate 100, a substrate layer 101, an inorganic layer 102, and a gas barrier layer 103 are stacked sequentially. Furthermore, the gas barrier layer 103 is composed of a cured product of the aforementioned mixture. Therefore, it exhibits an excellent balance between barrier properties and productivity.

[1025] More specifically, the gas barrier laminate 100 exhibits excellent barrier properties, such as oxygen barrier and water vapor barrier, after being subjected to a boiling treatment. Furthermore, since the gas barrier layer 103 in the gas barrier laminate 100 is composed of a cured product of the aforementioned mixture, even if, for example, the curing time (specifically, the heat treatment time) for obtaining the gas barrier layer 103 is short, a gas barrier laminate 100 with excellent barrier properties can still be obtained.

[1026] Figure 16 A cross-sectional view is shown schematically to illustrate other configurations of the gas barrier laminate. Figure 16 The basic structure and reference of the gas barrier laminate 110 shown Figure 15 The gas barrier laminate 100 described above is similar, but differs in that it also includes an undercoat layer 104 disposed between the substrate layer 101 and the inorganic layer 102.

[1027] The same effect as that of the gas barrier laminate 100 can be obtained in the gas barrier laminate 110. Furthermore, in the gas barrier laminate 110, by providing an undercoat layer 104 between the substrate layer 101 and the inorganic layer 102, the adhesion between the substrate layer 101 and the inorganic layer 102 can be further improved.

[1028] The composition of the layers contained in the gas barrier laminate will be explained in more detail below. First, the gas barrier layer 103 will be explained.

[1029] (Gas barrier layer)

[1030] The gas barrier layer 103 is composed of a cured material comprising a mixture of polycarboxylic acids, polyamine compounds, and polyvalent metal compounds. More specifically, the gas barrier layer 103 is a film (gas barrier film 10) composed of the aforementioned cured material.

[1031] More specifically, the gas barrier layer 103 can be obtained, for example, by coating a mixture before curing, i.e., a gas barrier coating material, onto a layer such as an inorganic layer 102 disposed immediately below the gas barrier layer 103, followed by drying and heat treatment to cure the gas barrier coating material.

[1032] In the infrared absorption spectrum of the gas barrier layer 103, at a depth of 1300 cm⁻¹ -1 The above 1490cm -1The maximum peak height of absorbance within the following range is set as α, and 1690 cm⁻¹ is used. -1 The above 1780cm -1 When the maximum peak height of absorbance within the following range is set as γ, from the viewpoint of the liquid stability of the gas barrier coating material before coating, the ratio of free carboxyl groups, expressed as γ / α, to the NH3 complex is preferably 0.00 or more, more preferably 0.01 or more, and even more preferably 0.02 or more.

[1033] Furthermore, from the viewpoint of improving the barrier properties of the gas barrier layer 103 obtained after coating, the above-mentioned γ / α is preferably 1.00 or less, more preferably 0.80 or less, even more preferably 0.60 or less, even more preferably 0.40 or less, even more preferably 0.20 or less, and even more preferably 0.10 or less.

[1034] Furthermore, in the infrared absorption spectrum of the gas barrier layer 103, 1493 cm⁻¹ -1 The above 1780cm -1 Let the total peak area within the following absorption band range be A, and let 1598 cm⁻¹ be the peak area. -1 The above 1690cm -1 Let the total peak area within the following absorption band range be B, and set 1690 cm⁻¹ as the maximum area. -1 The above 1780cm -1 Let the total peak area within the following absorption band range be C, and set 1493 cm⁻¹ as the maximum peak area. -1 The above is 1598cm -1 When the total peak area within the following absorption band range is set to D, the following shows a preferred example of the area ratio.

[1035] In the infrared absorption spectrum of the gas barrier layer 103, from the viewpoint of further improving the gas barrier performance after cooking, the area ratio of the amide bonds represented by B / A is preferably 0.200 or more, more preferably 0.250 or more, even more preferably 0.270 or more, even more preferably 0.290 or more, and even more preferably 0.310 or more.

[1036] Furthermore, from the viewpoint of further improving the balance between barrier properties and productivity, the area ratio of the amide bond represented by B / A is preferably 0.370 or less, more preferably 0.360 or less, and even more preferably 0.350 or less.

[1037] In the infrared absorption spectrum of the gas barrier layer 103, from the viewpoint of further improving the gas barrier performance after cooking, the area ratio of carboxylic acid expressed as C / A is preferably 0.150 or less, more preferably 0.100 or less, even more preferably 0.080 or less, and even more preferably 0.060 or less.

[1038] Furthermore, the lower limit of the area ratio of carboxylic acids represented by C / A is not limited, for example, it can be 0.000 or more, or it can be 0.0001 or more.

[1039] In the infrared absorption spectrum of the gas barrier layer 103, from the viewpoint of further improving the balance between barrier properties and productivity, the area ratio of the carboxylate, expressed as D / A, is preferably 0.580 or more, and more preferably 0.600 or more.

[1040] Furthermore, from the viewpoint of further improving the gas barrier performance after cooking, the D / A ratio is preferably 0.800 or less, more preferably 0.720 or less, even more preferably 0.700 or less, and even more preferably 0.680 or less.

[1041] Furthermore, from the viewpoint of achieving a more ideal balance between productivity and barrier properties in gas barrier laminates, it is also preferable that the area ratio of amide bonds represented by B / A is 0.200 or more and 0.370 or less, the area ratio of carboxylic acids represented by C / A is 0.150 or less, and the area ratio of carboxylate represented by D / A is 0.580 or more and 0.800 or less.

[1042] In the infrared absorption spectrum of the gas barrier layer 103, from the viewpoint of improving barrier properties, the area ratio of the carboxylate (represented by D / A) relative to the area ratio of the amide bond (represented by B / A) is preferably 1.2 or more, more preferably 1.6 or more, and even more preferably 1.8 or more.

[1043] Furthermore, from the viewpoint of improved barrier properties after cooking, the area ratio of the carboxylate represented by D / A relative to the area ratio of the amide bond represented by B / A is preferably 4.0 or less, more preferably 3.5 or less, even more preferably 3.0 or less, and even more preferably 2.5 or less.

[1044] Here, in the gas barrier layer 103, at 1700cm -1 The absorption of unreacted carboxylic acids based on the νC=O of the nearby visible infrared absorption spectrum, in the range of 1630–1685 cm⁻¹. -1 Absorption based on νC=O, which is a cross-linking structure, is visible in the vicinity at 1540–1560 cm⁻¹. -1 Nearby absorption based on carboxylates at νC=O is visible in the 1300–1490 cm⁻¹ region. -1 The absorption of δN-H based on ammonia that has formed a complex is visible nearby.

[1045] The 1300 cm⁻¹ in the infrared absorption spectrum is considered to be... -1 The above 1490cm -1The maximum peak height α of absorbance in the following range indicates the amount of ammonia present in the complex, 1690 cm⁻¹. -1 The above 1780cm -1 The maximum peak height γ in the following range is an indicator of the amount of free, i.e., unreacted carboxylic acid present.

[1046] In the fifth embodiment, specifically, the maximum peak heights α and γ can be measured by the following steps: A 1cm × 3cm sample is cut from the gas barrier layer 103. Then, the infrared absorption spectrum of the surface of the gas barrier layer 103 is obtained using total infrared reflectance (ATR) measurement. In the obtained infrared absorption spectrum, the peak heights α and γ are connected by a straight line at 900cm. -1 absorbance and 1900cm -1 Using the absorbance as a baseline, the maximum peak height within each absorbance range is calculated.

[1047] In addition, the 1493 cm⁻¹ in the infrared absorption spectrum is considered to be... -1 The above 1780cm -1 The total peak area A within the following absorption band range represents an indicator of the total stoichiometry of carboxylic acid, amide bond, and carboxylate, 1598 cm⁻¹. -1 The above 1690cm -1 The total peak area B within the following absorption band range represents an indicator of the amount of amide bonds present. Furthermore, it is believed that 1690 cm⁻¹... -1 The above 1780cm -1 The total peak area C within the following absorption band range represents an indicator of the amount of unreacted carboxylic acid present, 1493 cm⁻¹. -1 The above is 1598cm -1 The total peak area D within the absorption band below represents an indicator of the amount of carboxylate present.

[1048] In the fifth embodiment, specifically, the total peak areas A to D can be measured by the following steps.

[1049] First, a 1cm × 3cm sample for measurement is cut from the gas barrier layer 103. Next, the infrared absorption spectrum of the surface of the gas barrier layer 103 is obtained by infrared total reflectance measurement (ATR method). Based on the obtained infrared absorption spectrum, the total peak areas A to D are calculated by the following steps (1) to (4).

[1050] (1) 1780cm -1 With 1493cm -1 The absorbance values ​​are connected by a straight line (N), and the values ​​from 1493 cm⁻¹ will be represented by the absorbance values. -1 The above 1780cm -1The absorption spectrum within the following absorption band range and the area enclosed by N are taken as the total peak area A.

[1051] (2) From 1690cm -1 Draw a straight line (O) perpendicular to the absorbance (Q), and take the intersection of N and O as P, starting from 1598cm. -1 Draw a straight line (S) perpendicular to the absorbance (R), and take the intersection of N and S as T. Then, from 1598 cm⁻¹... -1 The above 1690cm -1 The area enclosed by the absorption spectrum within the following absorption band range and the lines S, T, N, P, O, absorbance Q, and R is taken as the total peak area B.

[1052] (3) The height of 1690cm -1 The above 1780cm -1 The area enclosed by the absorption spectrum and absorbance Q, line O, point P, and line N within the following absorption band range is taken as the total peak area C.

[1053] (4) The 1493cm -1 The above is 1598cm -1 The area enclosed by the absorption spectrum and absorbance R, the line S, the point T, and the line N within the following absorption band range is taken as the total peak area D.

[1054] Next, the area ratios B / A, C / A, and D / A are calculated from the areas obtained using the above method.

[1055] It should be noted that, in the fifth embodiment, for the measurement of infrared absorption spectra (infrared total internal reflection measurement: ATR method), for example, an IRT-5200 device manufactured by Nippon Spectrophotometer Co., Ltd. can be used, equipped with a PKM-GE-S (germanium) crystal, at an incident angle of 45 degrees, room temperature, and a resolution of 4 cm⁻¹. -1 The test was conducted under the condition of a cumulative total of 100 tests.

[1056] The maximum peak heights α and γ of the gas barrier layer 103, as well as the area ratio of amide bonds (represented by B / A), the area ratio of carboxylic acids (represented by C / A), and the area ratio of carboxylate salts (represented by D / A), can be controlled by appropriately adjusting the manufacturing conditions of the gas barrier layer 103. Specifically, factors for controlling the maximum peak heights α and γ of the gas barrier layer 103, as well as the area ratio of amide bonds (represented by B / A), the area ratio of carboxylic acids (represented by C / A), and the area ratio of carboxylate salts (represented by D / A), include the proportions of polycarboxylic acids, polyamine compounds, and polyvalent metal compounds, the preparation method of the mixture before curing, and the method, temperature, and time of heat treatment of the mixture.

[1057] Next, the components contained in the mixture (gas barrier coating material) before curing will be explained.

[1058] (Polycarboxylic acids)

[1059] Polycarboxylic acids are compounds having two or more carboxyl groups within their molecules. Specifically, examples include homopolymers or copolymers of α,β-unsaturated carboxylic acids such as (meth)acrylic acid, itaconic acid, fumaric acid, crotonic acid, cinnamic acid, 3-hexenoic acid, and 3-hexenediaic acid. Alternatively, they can be copolymers of the aforementioned α,β-unsaturated carboxylic acids with esters such as ethyl esters, olefins such as ethylene, etc.

[1060] Among them, the preferred polymers are homopolymers or copolymers of acrylic acid, methacrylic acid, itaconic acid, fumaric acid, crotonic acid, and cinnamic acid; more preferably, one or more polymers selected from the group consisting of polyacrylic acid, polymethacrylic acid, and copolymers of acrylic acid and methacrylic acid; further preferably, at least one polymer selected from polyacrylic acid and polymethacrylic acid; and even more preferably, at least one polymer selected from homopolymers of acrylic acid and homopolymers of methacrylic acid.

[1061] In this fifth embodiment, the term "polyacrylic acid" includes both homopolymers of acrylic acid and copolymers of acrylic acid with other monomers. In the case of copolymers of acrylic acid with other monomers, for polyacrylic acid, 100% by mass of the polymer contains structural units derived from acrylic acid, typically 90% by mass or more, preferably 95% by mass or more, and more preferably 99% by mass or more.

[1062] Furthermore, in the fifth embodiment, the term "polymethacrylic acid" includes both homopolymers of methacrylic acid and copolymers of methacrylic acid with other monomers. In the case of copolymers of methacrylic acid with other monomers, for polymethacrylic acid, 100% by mass of the polymer contains structural units derived from methacrylic acid, typically 90% by mass or more, preferably 95% by mass or more, and more preferably 99% by mass or more.

[1063] Polycarboxylic acids are polymers formed by the polymerization of carboxylic acid monomers. From the viewpoint of excellent balance between gas barrier properties and operability, the molecular weight of polycarboxylic acids is preferably 500 to 2,500,000, more preferably 5,000 to 2,000,000, even more preferably 10,000 to 1,500,000, and even more preferably 100,000 to 1,200,000.

[1064] In this fifth embodiment, the molecular weight of the polycarboxylic acid is the weight-average molecular weight converted from polyethylene oxide, which can be determined using gel permeation chromatography (GPC).

[1065] At least a portion of a polycarboxylic acid can be neutralized using a volatile base. By neutralizing the polycarboxylic acid with a volatile base, gelation can be suppressed when polyvalent metal compounds or polyamine compounds are mixed with the polycarboxylic acid. Therefore, from the viewpoint of preventing gelation, it is preferable to prepare a partially or completely neutralized carboxyl group using a volatile base. The neutralized product can be obtained by partially or completely neutralizing the carboxyl group of the polycarboxylic acid with a volatile base, that is, by partially or completely preparing a carboxylate of the polycarboxylic acid. This prevents gelation when polyamine compounds or polyvalent metal compounds are added.

[1066] Partial neutralization can be prepared by adding a volatile base to an aqueous solution of a polycarboxylic acid polymer. The desired degree of neutralization can be achieved by adjusting the molar ratio of the polycarboxylic acid to the volatile base. In the fifth embodiment, from the viewpoint of sufficiently suppressing gelation caused by the neutralization reaction with the amino group of the polyamine compound, the degree of neutralization of the polycarboxylic acid obtained using the volatile base is preferably 70 to 300 equivalents, more preferably 90 to 250 equivalents, and even more preferably 100 to 200 equivalents.

[1067] As a volatile base, any water-soluble base can be used.

[1068] Examples of volatile bases include, for example, tertiary amines such as ammonia, morpholine, alkylamines, 2-dimethylaminoethanol, N-methylmorpholine, ethylenediamine, triethylamine, or aqueous solutions of these, or mixtures thereof. From the viewpoint of obtaining good gas barrier properties, aqueous ammonia solutions are preferred.

[1069] (Polyamine compounds)

[1070] The mixture before curing contains polyamine compounds. By including polyamine compounds, the barrier properties of the resulting gas barrier material can be improved.

[1071] Polyamine compounds are compounds having two or more amino groups on their main chain, side chain, or terminal, and are preferably polymers. Specifically, examples include aliphatic polyamines such as polyallylamine, polyvinylamine, polyethyleneimine, and poly(propyleneimine); polyamides such as polylysine and polyarginine, which have amino groups on their side chains; and so on. Alternatively, polyamines can be formed by modifying a portion of the amino groups.

[1072] From the viewpoint of obtaining good gas barrier properties, the polyamine compound preferably contains polyethyleneimine, and more preferably polyethyleneimine.

[1073] From the viewpoint of achieving a good balance between gas barrier properties and operability, the number average molecular weight of the polyamine compound is preferably 50 to 2,000,000, more preferably 100 to 1,000,000, even more preferably 1,500 to 500,000, even more preferably 1,500 to 100,000, even more preferably 1,500 to 50,000, even more preferably 3,500 to 20,000, even more preferably 5,000 to 15,000, and even more preferably 7,000 to 12,000.

[1074] In this fifth embodiment, the molecular weight of the polyamine compound can be determined using the boiling point elevation method or the viscosity method.

[1075] From the viewpoint of further improving the gas barrier performance after cooking, the ratio of (moles of amino groups in the polyamine compound in the mixture) to (moles of -COO- groups in the polycarboxylic acid in the mixture) is preferably 0.20 or more, more preferably 0.25 or more, even more preferably 0.30 or more, even more preferably 0.35 or more, and even more preferably 0.40 or more.

[1076] From the same point of view, the ratio of (moles of amino groups contained in the polyamine compound in the mixture) to (moles of -COO- groups contained in the polycarboxylic acid in the mixture) is preferably 0.90 or less, more preferably 0.85 or less, even more preferably 0.80 or less, even more preferably 0.75 or less, and even more preferably 0.70 or less.

[1077] Although the detailed reasons are unclear, it is believed that by achieving a good balance between amide crosslinking (which is formed by amino groups constituting polyamine compounds) and metal crosslinking (which is formed by polyvalent metals constituting polycarboxylic acids and polyvalent metal salts) to form a dense structure, a gas barrier layer 103 with excellent gas barrier performance after cooking and a gas barrier laminate having the same can be obtained.

[1078] (Polyvalent metal compounds)

[1079] Polyvalent metal compounds specifically refer to metals and metal compounds belonging to groups 2 to 13 of the periodic table. More specifically, examples include metals with a valence of divalent or higher, such as magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), and aluminum (Al), as well as their oxides, hydroxides, halides, carbonates, phosphates, phosphites, hypophosphites, sulfates, or sulfites. From the viewpoint of water resistance and impurities, metal oxides or metal hydroxides are preferred.

[1080] From the viewpoint of further improving the gas barrier performance after cooking, the metal with a valence of 2 or higher in the polyvalent metal compound is preferably one or more metals selected from the group consisting of Zn, Ca, Mg, Ba and Al, and more preferably Zn.

[1081] From the same point of view, the polyvalent metal compound is preferably a compound of one or more metals with a divalent or higher valence selected from the group consisting of Zn, Ca, Mg, Ba and Al, and more preferably a compound of Zn.

[1082] From the same point of view, the polyvalent metal compound is preferably one or more compounds selected from the group consisting of oxides such as magnesium oxide, calcium oxide, barium oxide, zinc oxide, and magnesium hydroxide, and hydroxides such as calcium hydroxide, barium hydroxide, and zinc hydroxide, more preferably at least one of zinc oxide and zinc hydroxide, and even more preferably zinc oxide.

[1083] In the fifth embodiment, from the viewpoint of further improving the gas barrier performance after cooking, the ratio of (moles of polyvalent metal compounds in the mixture) to (moles of -COO- groups contained in the polycarboxylic acid in the mixture) is preferably 0.10 or more, more preferably 0.13 or more, even more preferably 0.15 or more, even more preferably 0.18 or more, even more preferably 0.20 or more, even more preferably 0.25 or more, and even more preferably 0.28 or more.

[1084] From the same point of view, the ratio of (moles of polyvalent metal compounds in the mixture) to (moles of -COO- groups contained in the polycarboxylic acid in the mixture) is preferably 0.80 or less, more preferably 0.70 or less, even more preferably 0.60 or less, even more preferably 0.55 or less, and even more preferably 0.50 or less.

[1085] In the fifth embodiment, from the viewpoint of further improving the gas barrier performance after cooking, the ratio of (moles of polyvalent metal compounds in the mixture) to (moles of amino groups from polyamine compounds in the mixture) is preferably 0.25 or more, more preferably 0.35 or more, and even more preferably 0.40 or more.

[1086] From the same point of view, the ratio of (moles of polyvalent metal compounds in the mixture) to (moles of amino groups from polyamine compounds in the mixture) is preferably 0.75 or less, more preferably 0.65 or less, even more preferably 0.60 or less, and even more preferably 0.55 or less.

[1087] The mixture before curing may contain components other than those mentioned above.

[1088] For example, the mixture preferably also contains ammonium carbonate salts. Ammonium carbonate salts are substances added to improve the solubility of polyvalent metal compounds by converting them into ammonium carbonate complexes, thereby preparing a homogeneous solution containing the polyvalent metal compounds. By including ammonium carbonate salts in the mixture before curing, the solubility of the polyvalent metal compounds can be increased, resulting in a more homogeneous mixture containing the polyvalent metal compounds.

[1089] As a carbonate-based ammonium salt, examples include ammonium carbonate and ammonium bicarbonate. From the perspective of easy volatilization and not easy to remain in the obtained gas barrier layer, ammonium carbonate is preferred.

[1090] From the viewpoint of further improving the solubility of the polyvalent metal compound, the ratio of (moles of ammonium carbonate salt in the mixture) to (moles of polyvalent metal compound in the mixture) is preferably 0.05 or more, more preferably 0.10 or more, even more preferably 0.25 or more, even more preferably 0.50 or more, and even more preferably 0.75 or more.

[1091] Furthermore, from the viewpoint of further improving the coatability of the coating material for gas barrier applications, the ratio of (moles of ammonium carbonate salts in the coating material for gas barrier applications) to (moles of polyvalent metal compounds in the coating material for gas barrier applications) is preferably 10.0 or less, more preferably 5.0 or less, even more preferably 2.0 or less, and even more preferably 1.5 or less.

[1092] Furthermore, from the viewpoint of suppressing depressions when coating as a gas barrier coating material, the mixture before curing preferably also contains a surfactant.

[1093] When the total solid component of the mixture is set to 100% by mass, the amount of surfactant added is preferably 0.01 to 3% by mass, more preferably 0.01 to 1% by mass.

[1094] Examples of surfactants include anionic surfactants, nonionic surfactants, cationic surfactants, and amphoteric surfactants. From the viewpoint of obtaining good coatability, nonionic surfactants are preferred, polyoxyethylene alkyl ethers are more preferred, and polyoxyethylene alkyl ethers are even more preferred.

[1095] Examples of nonionic surfactants include polyoxyalkylene alkyl ethers, polyoxyalkylene alkyl ethers, polyoxyalkylene fatty acid esters, sorbitan fatty acid esters, organosilicon surfactants, alkynyl alcohol surfactants, and fluorinated surfactants.

[1096] Examples of polyoxyethylene alkyl aryl ethers include, for example, polyoxyethylene nonylphenyl ether, polyoxyethy...

Claims

1. A gas barrier laminate comprising a substrate layer, a gas barrier layer disposed on at least one side of the substrate layer, and an inorganic layer disposed between the substrate layer and the gas barrier layer. The Zn composition of the gas barrier layer, as determined by X-ray photoelectron spectroscopy analysis, is 1-10 atomic%. The data were determined by time-of-flight secondary ion mass spectrometry analysis of the gas barrier layer. 64 ZnPO4H - The mass peak intensity is set as I ( 64 ZnPO4H - ) and C3H3O2 - Let the mass peak intensity be I(C3H3O2) - )hour, I ( 64 ZnPO4H - ) / I(C3H3O2 - The value of ) is 6 × 10 -4 Above 5×10 -2 the following, The composition ratio of N, as determined by X-ray photoelectron spectroscopy analysis of the gas barrier layer, is greater than 0 atomic% and less than 12 atomic%. The CN content was determined by time-of-flight secondary ion mass spectrometry analysis of the gas barrier layer. - The mass peak intensity is set as I (CN) - )hour, I (CN) - ) / I(C3H3O2 - The value of ) is greater than 0 and less than 2.

2. The gas barrier laminate as described in claim 1, wherein, The PO2 content was determined by time-of-flight secondary ion mass spectrometry analysis of the gas barrier layer. - Let the mass peak intensity be I(PO2) - ) and PO3 - The mass peak intensity is set as I(PO3). - )hour, (I(PO2)) - ) + I (PO3) - )) / I(C3H3O2 - The value is above 0.02 and below 5.

3. The gas barrier laminate as described in claim 1 or 2, wherein, The PO2 content was determined by time-of-flight secondary ion mass spectrometry analysis of the gas barrier layer. - Let the mass peak intensity be I(PO2) - ) and PO3 - The mass peak intensity is set as I(PO3). - When ), the I (PO2) - ) and the I (PO3) - The intensity ratio of I(PO2) - ) / I(PO3) - The value is above 0.05 and below 1.

4. The gas barrier laminate as described in claim 1 or 2, wherein, The gas barrier layer is composed of a cured material comprising at least a polycarboxylic acid, Zn, and a phosphorus compound or its salt containing one or more -P-OH groups.

5. The gas barrier laminate as described in claim 4, wherein, The concentration of P atoms of the phosphorus compound or its salt in the mixture is 5 × 10⁻⁶ per mol of the polycarboxylic acid. -4 Above 0.3 mol and below 0.3 mol.

6. The gas barrier laminate as described in claim 4, wherein, The mixture also contains polyamines.

7. The gas barrier laminate as described in claim 6, wherein, The polyamine is polyethyleneimine.

8. The gas barrier laminate as described in claim 4, wherein, The polycarboxylic acid comprises one or more polymers selected from the group consisting of polyacrylic acid, polymethacrylic acid, and copolymers of acrylic acid and methacrylic acid.

9. The gas barrier laminate as described in claim 1 or 2, wherein, The thickness of the gas barrier layer is between 0.05 μm and 10 μm.

Citation Information

Patent Citations

  • Gas barrier film

    JP2005225940A

  • Gas barrier film and manufacturing method

    JP2013010857A

  • Barrier laminate film

    JP2018171827A

  • Film and process for producing the same

    WO2003091317A1

  • Composite structure, packaging material and molded article each produced using same, process for production of composite structure, and coating solution

    WO2011122036A1