A polycrystalline iron loaded porous biochar aerogel catalyst, a preparation method and application thereof

By loading polycrystalline iron nanoparticles onto porous biochar aerogel to form a honeycomb-structured catalyst, the problems of low efficiency and high cost of catalytic ozonation are solved, achieving efficient adsorption and degradation of organic matter, and making it suitable for water and air purification.

CN119259047BActive Publication Date: 2026-11-20WENZHOU UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411440770.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-10-16
Publication Date
2026-11-20
Estimated Expiration
2044-10-16

AI Technical Summary

Technical Problem

Existing catalysts are inefficient in catalytic ozonation, making it difficult to effectively remove structurally complex organic matter. They are also costly, and iron-based materials have poor stress resistance in practical applications.

Method used

Polycrystalline iron nanoparticles are loaded onto porous biochar aerogel via Fe-C bonds to form a honeycomb pore network structure, providing abundant adsorption and reaction active sites and improving the mechanical strength and structural stability of the catalyst.

Benefits of technology

It improves catalytic ozonation efficiency, reduces costs, and achieves efficient adsorption and degradation of organic substances such as antibiotics. It is suitable for water and air purification and has good electron transport capabilities and mechanical stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119259047B_ABST
    Figure CN119259047B_ABST
Patent Text Reader

Abstract

The application discloses a kind of polycrystalline iron supported porous biochar aerogel catalyst and its preparation method and application, it is related to carbon catalyst preparation field.The polycrystalline iron supported porous biochar aerogel catalyst of the application includes porous biochar matrix, polycrystalline iron nanoparticles are supported on biochar sheet layer by Fe-C bond, and the internal structure of the porous biochar aerogel whole is honeycomb-like pore network structure;The preparation method of the catalyst of the application, using the ion exchange of crosslinking agent, crosslinking together iron-based material and carbon-based material, is prepared by freeze drying and high-temperature calcination processing.Formation.The aerogel of the application has abundant pore structure, can adsorb catalytic ozone molecule to generate active atomic oxygen, has stable, efficient catalytic activity when processing new micro-pollutants in tail water, simultaneously polycrystalline iron nanoparticles are supported on the surface of porous biochar by Fe-C bond stability, can effectively improve the mechanical strength and structural stability of catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of wastewater treatment technology, and more specifically, relates to a polycrystalline iron-supported porous biochar aerogel catalyst, its preparation method, and its application. Background Technology

[0002] New pollutants, though present in low concentrations in water bodies, pose significant health risks, impacting the endocrine and genetic systems of humans and other organisms. The potential harm these new pollutants pose to the ecological environment and human health and survival has become a major research topic in water treatment this century. Therefore, there is a need to develop a simple, low-cost, residue-free, and non-polluting method to remove new pollutants from water bodies. Ozone, with its high oxidizing properties, can be used to remove color, odor, and disinfect water, and is widely used in the remediation of organically polluted water bodies.

[0003] Although ozone has strong oxidizing power, it is still difficult to achieve ideal results when treating some structurally complex organic compounds. Moreover, treating some recalcitrant organic compounds often requires the addition of large amounts of ozone or a long time to achieve complete degradation, which undoubtedly increases treatment costs. Therefore, catalytic ozone oxidation is particularly important. The characteristics of the catalyst are the most important factor affecting the efficiency of heterogeneous catalytic ozonation processes. Currently, researchers at home and abroad have conducted extensive research to develop innovative catalysts to improve the efficiency of heterogeneous catalytic ozonation. For example, alumina, natural zeolite, reduced graphene oxide, various metal-supported catalysts, and metal oxides have been used as catalysts in catalytic ozonation processes. Meanwhile, due to the ease of synthesis, good catalytic performance, and availability of iron in nature, iron-based materials are commonly used as catalysts for heterogeneous catalytic ozonation. The synthesis and application of iron-based materials with novel properties and functions in catalytic ozonation systems have been extensively studied, and developing a stable iron-based material to stably promote ozone oxidation is of great significance.

[0004] Therefore, the method of immobilizing transition metals on biochar for treatment has been welcomed and attracted much attention by researchers at home and abroad. For example, Jothinathan et al. (L. Jothinathana, Q. Cai, et al. Fe-Mn doped powdered activated carbon pellet as ozone catalyst for cost-effective phenolic wastewater treatment: Mechanism studies and phenol by-products elimination[J] Journal of Hazardous Materials, 424(2022)127483) prepared a novel bimetallic doped polyaluminum chloride (Fe-Mn / PAC) particle using the sol-gel method and used it as an ozone catalyst for the treatment of phenolic wastewater (PWW). Using the Fe-Mn / PAC particle microbubble ozone oxidation technology, the removal rates of chemical oxygen demand (COD) and phenol in PWW 1h were increased to 79% and 95%, respectively, while Fe-Mn / PAC does not have the ability to adsorb ozone. In her research, Yewen Qiu (Y.Qiu,X.Xu,Z.Xu,J.Liang,Y.Yu,X.Cao, Contribution of different iron species in the iron-biochar composites to sorption and degradation of two dyes with varying properties,[J]Chemical Engineering Journal 389(2020)) found that iron-biochar composites exhibited higher dye removal capabilities compared to raw biochar. The removal efficiencies for methylene blue and Acid Orange 7 increased from 33%-72% to 48%-92% and from 49%-70% to 72%-85%, respectively. This demonstrates that iron-biochar composites can effectively remove dyes, and that iron species play a crucial role in dye removal. However, iron exists primarily in iron oxide forms, resulting in poor resistance to adverse conditions in practical applications.

[0005] For example, Chinese patent CN202211167489 discloses a chitosan-based biochar with a porous structure and high specific surface area, its preparation method, and its application. Chitosan is dispersed in a mixed solvent of potassium hydroxide, urea, and water, then freeze-dried and calcined to obtain a catalyst applicable to the persulfate field. Chinese patent CN202111060989 discloses a highly elastic, high-temperature resistant aerogel and its preparation method. Modified biochar is prepared by sequentially performing low-temperature baking, carbon dioxide microwave heating, ultrasonic treatment, electrostatic directional freeze-drying, and vacuum sublimation to form a porous three-dimensional network structure, endowing the aerogel with oil-absorbing and highly elastic properties.

[0006] The patent applications mentioned above demonstrate the excellent capabilities of aerogels in other fields; however, these catalysts cannot provide effective support for ozone catalysis. Ozone, as one of the most promising advanced oxidation processes for practical engineering applications, is prone to decomposition into oxygen in water due to its gaseous form, resulting in reduced utilization. Therefore, one of the key research focuses on ozone processes is the synthesis of a high-quality ozone catalyst, which can improve ozone utilization while reducing costs, thus providing a green and efficient solution to practical problems. Summary of the Invention

[0007] 1. The technical problem that the invention aims to solve

[0008] One objective of this invention is to provide a polycrystalline iron-supported porous biochar aerogel catalyst. The biochar aerogel has a rich pore structure, which can provide abundant adsorption and reaction active sites and electron transfer channels, thereby effectively improving the catalytic efficiency of the catalyst. In the catalyst, polycrystalline iron nanoparticles are stably supported on the surface of porous biochar through Fe-C bonds, which can effectively improve the mechanical strength and structural stability of the catalyst.

[0009] The second objective of this invention is to provide a method for preparing the above-mentioned polycrystalline iron-supported porous biochar aerogel catalyst, and the preparation process is simple to operate and has low production cost.

[0010] The third objective of this invention is to provide an application of the above-mentioned polycrystalline iron-supported porous biochar aerogel catalyst in water purification, air purification, chemical catalysis, and energy storage. In particular, when applied to an ozone catalytic purification system, it can adsorb ozone to form surface atomic oxygen, enabling it to stably and efficiently play a role in electron transfer in the treatment of new pollutants in wastewater.

[0011] 2. Technical Solution

[0012] To achieve the above objectives, the technical solution provided by the present invention is as follows:

[0013] The first aspect of the present invention provides a polycrystalline iron-supported porous biochar aerogel catalyst, the catalyst having an overall honeycomb-like pore network structure, comprising a porous biochar matrix, wherein polycrystalline iron nanoparticles are supported on biochar sheets via Fe-C bonds.

[0014] The catalyst of this invention uses a porous biochar matrix as a carrier. The biochar matrix has a layered structure with cross-linked layers forming a network structure. The biochar layers also have honeycomb-like channels, resulting in a rich pore structure and significantly increasing the specific surface area of ​​the catalyst. Therefore, when applied to water purification, it can provide more adsorption and reaction active sites and electron migration channels for the adsorption and degradation of organic compounds such as antibiotics, thereby effectively improving the degradation efficiency of these compounds. Simultaneously, the biochar layers in this invention are uniformly loaded with polycrystalline iron nanoparticles. The presence of polycrystalline iron provides more active sites, which is beneficial for improving and ensuring the catalytic effect. Furthermore, the polycrystalline iron nanoparticles are loaded onto the biochar layers through Fe-C bonds, effectively improving their loading stability on the catalyst. This contributes to improving the overall mechanical strength and stability of the catalyst, overcoming the shortcomings of weak surface bonding between iron-based and carbon-based materials in existing technologies.

[0015] It should be noted that in this invention, polycrystalline iron nanoparticles are loaded onto the biochar sheet through Fe-C bonds. This loading can be either direct or indirect, i.e., achieved through a crosslinking agent. Furthermore, the macroscopic shape of the polycrystalline iron-loaded porous biochar aerogel of this invention is not limited and can be varied according to actual conditions and needs. For example, it can adopt a columnar structure (containing interconnected pores), such as spherical, square, columnar, or block shapes, or an irregular shape, or even a thin film.

[0016] As a further improvement to any technical solution of the catalyst in the first aspect of the present invention, the crystal planes of the polycrystalline iron include, but are not limited to, the (220) crystal plane of Fe3O4, the (002) crystal plane of Fe3C, the (211) crystal plane of Fe3C, and the (031) crystal plane of Fe2O3.

[0017] As a further improvement to any technical solution of the catalyst in the first aspect of the present invention, the different crystals of the polycrystalline iron are alternately grown inside the biochar sheet, and the interlaced network lattice stripes can be observed under a transmission electron microscope, thereby providing more sites for catalytic ozone formation.

[0018] As a further improvement to any technical solution of the catalyst in the first aspect of the present invention, the content of the polycrystalline iron accounts for 0.27at% to 37at% of the total catalyst content, wherein Fe(III) accounts for 38at% to 54at% of the total iron content, Fe(II) accounts for 17at% to 31at% of the total iron content, and Fe3C accounts for 17at% to 31at% of the total iron content.

[0019] As a further improvement to any technical solution of the catalyst in the first aspect of the present invention, the loading of the polycrystalline iron nanoparticles accounts for 5 to 15% of the catalyst mass, more preferably 10%.

[0020] As a further improvement to any technical solution of the catalyst in the first aspect of the present invention, the size of the polycrystalline iron nanoparticles is 1-10 nm, more preferably 5-10 nm. The small size and uniform distribution of the polycrystalline iron nanoparticles are beneficial to further improving the catalytic effect of the catalyst.

[0021] As a further improvement to any technical solution of the catalyst in the first aspect of the present invention, the diameter of the pores on the biochar matrix is ​​50 to 100 micrometers, and more preferably 70 to 90 micrometers.

[0022] As a further improvement to any technical solution of the catalyst in the first aspect of the present invention, the biochar aerogel has a contact angle of less than 88° and good hydrophilicity, which is beneficial to further promote the adsorption, migration and degradation of organic pollutants inside the catalyst.

[0023] As a further improvement to any of the technical solutions of the catalyst in the first aspect of the present invention, the biochar aerogel has an impedance value of less than 11Ω and has a fast electron transport capability.

[0024] As a further improvement to any technical solution of the catalyst in the first aspect of the present invention, the biochar aerogel exhibits an ID / IG value greater than 0.85 in its Raman spectrum, and after contact with O3 in water, its in-situ Raman spectrum reaches 877.74 cm⁻¹. -1 935.76cm -1 and 1004.97cm -1 New peaks appeared at all locations. The in-situ Raman spectrum of the catalyst of this invention, after contact with O3, showed a peak at 877.74 cm⁻¹. -1 935.76cm -1 and 1004.97cm -1 New peaks appeared at all locations, corresponding to surface atomic oxygen (O2) respectively. * O * The O3 adsorbed on the surface is mainly due to the formation of O2 after ozone is adsorbed on the material surface. * and O2 * O2 *It is then further converted into singlet oxygen through electron transfer.

[0025] Raman spectroscopy is used to characterize the structural features of carbon material catalysts. The intensity ratio of the D band and the G band (ID / IG) can be used to analyze the degree of defects in the catalyst. The closer the ID / IG value is to 1, the higher the degree of disorder of the biochar sheets. The wrinkles, bumps and defects on the biochar sheets can not only generate redox activity, but also serve as electron transport media and reactive sites.

[0026] A second aspect of the present invention provides a method for preparing any porous biochar aerogel catalyst as described in the first aspect of the present invention, comprising:

[0027] Iron-based biochar and a crosslinking agent are contacted / mixed in an aqueous solution to form an iron-based biochar-crosslinking agent mixture (i.e., iron-based biochar hydrogel); wherein the iron-based biochar includes a biochar matrix and polycrystalline iron nanoparticles loaded on biochar sheets, and the polycrystalline iron nanoparticles and the biochar matrix are physically bonded.

[0028] The iron-based biochar-crosslinking agent mixture was freeze-dried to form honeycomb-like pores in the biochar sheets, resulting in iron-based biochar aerogel. The iron-based biochar-crosslinking agent mixture was first frozen into ice through freeze-drying, and then sublimated to form pores in the biochar sheets.

[0029] The iron-based biochar aerogel is calcined under an inert atmosphere to load polycrystalline iron nanoparticles onto the biochar sheets via Fe-C bonds, thus obtaining the polycrystalline iron-supported porous biochar aerogel catalyst.

[0030] This invention utilizes the ion exchange effect of a crosslinking agent to crosslink iron-based materials with biochar sheets. The overall preparation process is simple, and the porous biochar aerogel, with its tightly bonded iron-carbon structure, possesses a certain mechanical strength. Furthermore, it can adsorb ozone to form surface atomic oxygen, enabling it to stably and efficiently perform electron transfer in treating new pollutants in wastewater, thus improving ozone catalytic efficiency. Simultaneously, the raw materials used in this application are green, pollution-free, readily available, and low-cost, facilitating large-scale production. It can be applied to fields such as the treatment of organically polluted water bodies and the deep purification of drinking water.

[0031] Aerogels obtained directly through freeze-drying are relatively unstable. Low-temperature calcination allows polycrystalline iron to be firmly supported on a porous biochar matrix. The fusion of the two types of carbon helps ensure structural stability and prevents collapse. Specifically, the crosslinking agent and polycrystalline iron are bonded through Fe-C bonds, while the biochar and crosslinking agent are mainly bonded through C=C / CC bonds.

[0032] As a further improvement to any technical solution of the preparation method of the second aspect of the present invention, the specific surface area of ​​the iron-based biochar (polycrystalline iron biochar) is 150-250 m². 2 / g, which can provide abundant active sites for the adsorption and degradation of antibiotic organic pollutants, thus improving the catalytic activity of the catalyst.

[0033] As a further improvement to any technical solution of the preparation method of the second aspect of the present invention, the crosslinking agent includes, but is not limited to, chitosan, carrageenan, and sodium alginate, wherein the mass ratio of iron-based biochar to crosslinking agent is (2-5):(1-5), and more preferably (2-5):3.

[0034] The crosslinking agent is more preferably chitosan. Since chitosan contains a large amount of nitrogen, using it as a crosslinking agent can not only achieve a firm loading of polycrystalline iron nanoparticles, but also provide a nitrogen source to achieve nitrogen doping on the catalyst. Co-doping not only ensures the catalytic stability of the catalyst, but the synergistic effect between the two promotes the adsorption and catalytic degradation of antibiotic organic pollutants, resulting in better catalytic performance than carbon materials doped with a single element.

[0035] As a further improvement to any technical solution of the preparation method of the second aspect of the present invention, the biochar includes, but is not limited to, bamboo charcoal, straw biochar, and coconut shell charcoal, and is more preferably bamboo charcoal. Bamboo charcoal is not only a green and pollution-free raw material that is easy to purchase and has low cost, but also has a large specific surface area, which can provide abundant active sites for the adsorption and degradation of antibiotic organic pollutants, and is conducive to further improving the catalytic activity of the catalyst.

[0036] As a further improvement to any technical solution of the preparation method of the second aspect of the present invention, an organic acid or inorganic acid is added to the aqueous solution to adjust the viscosity of the solution, thereby obtaining a viscous hydrogel; the organic acid or inorganic acid can be, for example, hydrochloric acid, formic acid, acetic acid, lactic acid, malic acid or ascorbic acid, etc., preferably acetic acid, and the ratio of iron-based biochar, crosslinking agent, acetic acid and water is (0.8g~2g):(0.8g~2g):(0.4ml~0.8ml):(38ml~35.2ml), more preferably 1.6g:1.2g:0.8ml:36.4ml.

[0037] As a further improvement to any technical solution of the preparation method of the second aspect of the present invention, the freeze-drying treatment of the iron-based biochar-crosslinking agent mixture includes: first freezing the iron-based biochar-crosslinking agent mixture at -15 to -25°C, and then freeze-drying it at -70 to -85°C to form pores.

[0038] As a further improvement to any technical solution of the preparation method of the second aspect of the present invention, the iron-based biochar aerogel is calcined under an inert atmosphere, comprising: heating the iron-based biochar aerogel to 100°C to 200°C at a rate of 1 to 8°C / min, holding it at that temperature for 1.0 to 2.0 hours, and then cooling it to room temperature. The inert atmosphere is high-purity nitrogen or argon with a purity ≥ 99.99%.

[0039] As a further embodiment of any technical solution of the preparation method of the second aspect of the present invention, the iron-based biochar is prepared by chemical deposition or mechanical ball milling.

[0040] As one implementation of any technical solution of the preparation method of the second aspect of the present invention, the preparation process of the iron-based biochar specifically includes:

[0041] Iron source and biochar are mixed and dispersed in ultrapure water. After mixing at room temperature for a certain period of time, the supernatant is removed, and the mixture is dried, cooled, and ground to obtain iron salt composite biochar material, that is, iron salt is combined to the surface of biochar through electrostatic-complexation.

[0042] Iron-based biochar material is obtained by calcining iron salt composite biochar material at high temperature under air-isolated conditions, followed by cooling and grinding. After calcination, the iron salt decomposes at high temperature, and polycrystalline iron is loaded onto the biochar sheets.

[0043] Furthermore, the iron source is selected from one or more of ferric nitrate, ferric chloride, and ferric citrate.

[0044] Furthermore, the high-temperature calcination of the iron salt composite biochar material under air-isolated conditions includes: heating to 300℃-800℃ at a rate of 1-5℃ / min, and then holding at that temperature for 1-4 hours; more preferably, heating to 700℃ at a rate of 3℃ / min, and then holding at that temperature for 3 hours. The inert atmosphere is preferably high-purity nitrogen or argon with a purity ≥99.99%.

[0045] Furthermore, the process includes: acid washing of the iron-based biochar material synthesized by high-temperature calcination, followed by washing with ultrapure water until the pH is neutral, to remove unstable bound iron and prevent iron leaching during subsequent use. More preferably, sulfuric acid is used for acid washing, with a sulfuric acid concentration preferably of 1 mol / L.

[0046] The third aspect of the present invention also provides the application of any porous biochar aerogel catalyst as described in the first aspect in the fields of water purification, air purification, or chemical catalysis.

[0047] Furthermore, the water purification system includes, but is not limited to, an ozone catalytic oxidation system, the method of use of which includes:

[0048] In the ozone catalytic oxidation system, the porous biochar aerogel catalyst is brought into contact with ozone in the water to be treated to form surface atomic oxygen, which catalyzes the decomposition of ozone to produce singlet oxygen and hydroxyl radicals, thereby enhancing the degradation of pollutants or antibiotics in the water.

[0049] Furthermore, the water to be treated includes both recalcitrant high-concentration antibiotic pharmaceutical wastewater and low-concentration wastewater effluent from wastewater treatment plants, wherein the antibiotic concentration in the high-concentration antibiotic pharmaceutical wastewater is 1-100 mg / L, and the antibiotic concentration in the low-concentration wastewater effluent system is 1-20 μg / L.

[0050] 3. Beneficial effects

[0051] In summary, by adopting the technical solution provided by this invention, the following beneficial effects can be achieved compared with the prior art:

[0052] (1) This invention provides a polycrystalline iron-supported porous biochar aerogel, which comprises a porous biochar matrix and polycrystalline iron nanoparticles supported on the matrix. The aerogel has abundant pores and a large specific surface area, enabling it to adsorb ozone and form surface atomic oxygen. This allows it to stably and efficiently perform electron transfer in treating new pollutants in wastewater, while also providing abundant active sites for the adsorption and degradation of antibiotic organic pollutants, thus improving ozone catalytic efficiency. Furthermore, in this invention, the polycrystalline iron nanoparticles are uniformly supported on the biochar sheets via Fe-C bonds. On the one hand, the presence of various iron-containing crystals is beneficial for providing more reactive sites; on the other hand, the polycrystalline iron nanoparticles are supported via Fe-C bonds rather than simple physical bonding, thus ensuring both stable loading of the polycrystalline iron and stable pore structure of the aerogel. The synergistic effect between the two also enhances the catalytic activation of ozone and the degradation and removal of antibiotic pollutants.

[0053] (2) The polycrystalline iron nanoparticles in this invention have a particle size of 1-10 nm, which is small and thus helps to further improve the ozone catalytic decomposition effect. Compared with porous biochar aerogel materials without polycrystalline iron, polycrystalline iron-supported porous biochar aerogel has a richer pore structure, providing rich adsorption and reactive active sites and electron transfer channels for the adsorption and degradation of antibiotic organic pollutants, thus helping to improve the degradation efficiency of antibiotics and other organic substances.

[0054] (3) Compared with other carbon aerogel materials, the polycrystalline iron-supported porous biochar aerogel of the present invention has better hydrophilicity, which is conducive to further promoting the adsorption, migration and degradation of organic pollutants inside the catalyst; its impedance value is below 11Ω, which has a fast electron transport capability; at the same time, the catalyst has good elasticity and does not deform after multi-stage extrusion; it has a high ID / IG value, so the material is rich in defects, which is conducive to the high-speed adsorption and transformation of pollutants and oxidants inside the material.

[0055] (4) In the preparation of the polycrystalline iron-supported porous biochar aerogel, the present invention adds a certain crosslinking agent. Under the action of the crosslinking agent, after calcination, the polycrystalline iron nanoparticles can be loaded on the biochar sheets in the form of Fe-C bonds, which is beneficial to improve the loading of polycrystalline iron nanoparticles and the stability of the pore structure. The crosslinking agent is preferably chitosan, which can also be used as a nitrogen source to uniformly load N elements on the aerogel. Carbon and nitrogen co-doping promotes the adsorption and catalytic degradation of antibiotic organic pollutants.

[0056] (5) The preparation process of the present invention is simple and low in cost, suitable for large-scale promotion and application, and the prepared aerogel can be processed into various shapes according to actual needs, such as cylindrical, spherical, block, irregular shape, film, etc.

[0057] (6) The aerogel catalyst of the present invention can be applied to water purification, air purification, chemical catalysis or energy storage. When applied to water purification, it can be applied to, but is not limited to, ozone catalytic oxidation systems. It can be used to purify high-concentration antibiotic pharmaceutical wastewater that is difficult to degrade, as well as to purify low-concentration wastewater effluent from sewage treatment plants. Attached Figure Description

[0058] Figure 1 (a) is a scanning electron microscope image of the aerogel prepared in Example 4, (b) is a scanning electron microscope image of the aerogel obtained in Comparative Example 1, and (c), (d), (e), and (f) are transmission electron microscope images of the aerogel obtained in Example 4.

[0059] Figure 2 Scanning electron microscope images of the aerogels obtained in Comparative Example 2 and Examples 2, 3 and 5;

[0060] Figure 3 The image shows the SEM energy dispersive spectroscopy (EDS) analysis of the aerogel prepared in Example 4.

[0061] Figure 4 (a) and (b) are the pressure test results of the aerogels prepared in Example 4 and Comparative Example 1, respectively; (c) to (h) are the contact angles of the aerogels in Comparative Example 1, Comparative Example 2 and Examples 2-5, respectively.

[0062] Figure 5 The X-ray photoelectron spectroscopy (XPS) spectra of the aerogels obtained in Examples 2-5 are shown.

[0063] Figure 6 (a) shows the Raman spectra of the aerogels obtained in Examples 2-5; (b) shows the in-situ Raman spectra of Example 4.

[0064] Figure 7 Impedance diagrams of the aerogels obtained in Comparative Example 1 and Example 4.

[0065] Figure 8 (a) is a schematic diagram of different carbon ratios of the aerogels obtained in Examples 2-5; (b) is a schematic diagram of different nitrogen ratios of the aerogels obtained in Examples 2-5; (c) is a schematic diagram of different oxygen ratios of the aerogels obtained in Examples 2-5; and (d) is a schematic diagram of different iron ratios of the aerogels obtained in Examples 2-5.

[0066] Figure 9 The relationship between different proportions of components in the aerogels obtained in Examples 2-5 and their catalytic efficiency is shown.

[0067] Figure 10 In the figure, (a) shows the kinetic curves of levofloxacin degradation catalyzed by different aerogels, and (b) shows the kinetic fitting of levofloxacin degradation catalyzed by different aerogels.

[0068] Figure 11 (a) shows the free radical quenching experiment results of aerogel degradation of levofloxacin in Example 4; (b) shows the electron paramagnetic resonance spectrum of singlet oxygen during the aerogel degradation of levofloxacin in Example 4; (c) shows the electron paramagnetic resonance spectrum of hydroxyl radicals during the aerogel degradation of levofloxacin in Example 4; and (d) shows the electron paramagnetic resonance spectrum of superoxide ion radicals during the aerogel degradation of levofloxacin in Example 4.

[0069] Figure 12 The results of the repeated use experiment of ozone degradation of levofloxacin by aerogel in Example 4 are shown.

[0070] Figure 13 The results are from the experiment in Example 4 on the degradation of antibiotics in wastewater by ozone catalysis using aerogel. Detailed Implementation

[0071] This invention provides a polycrystalline iron-supported porous biochar aerogel catalyst. The catalyst comprises a porous biochar matrix and polycrystalline iron nanoparticles uniformly distributed on the biochar matrix. The porous biochar matrix and polycrystalline iron nanoparticles together constitute a polycrystalline iron biochar material. The catalyst exhibits a honeycomb-like porous network structure (i.e., the biochar sheets are cross-linked to form a three-dimensional network structure with interconnected pores). This abundant pore structure results in a large specific surface area, allowing for the adsorption of ozone to form surface atomic oxygen and providing abundant active sites for the adsorption and degradation of organic pollutants such as antibiotics, thereby improving the degradation efficiency of antibiotics and other organic compounds. The polycrystalline iron nanoparticles are uniformly supported on the biochar sheets through Fe-C bonds, which not only promotes the adsorption and catalytic degradation of organic pollutants such as antibiotics, further improving catalytic efficiency, but also effectively ensures the robustness of the polycrystalline iron nanoparticle support, thus improving the overall mechanical strength of the catalyst and ensuring its catalytic stability.

[0072] As a further preferred embodiment of the polycrystalline iron-supported porous biochar aerogel catalyst of the present invention, the specific surface area of ​​the polycrystalline iron biochar material is 150-250 m². 2 / g, the diameter of the pores in the biochar matrix is ​​50-100 micrometers, more preferably 70-90 micrometers. In some embodiments, the size (particle size) of the polycrystalline iron nanoparticles is 1-10 nm, more preferably 5-10 nm.

[0073] The crystal planes of the polycrystalline iron include, but are not limited to, the (220) crystal plane of Fe3O4, the (002) crystal plane of Fe3C, the (211) crystal plane of Fe3C, and the (031) crystal plane of Fe2O3. As a further preferred embodiment of the polycrystalline iron supported porous biochar aerogel catalyst of the present invention, the loading of polycrystalline iron nanoparticles accounts for 5 to 15% of the catalyst mass or the content of polycrystalline iron accounts for 0.27 at% to 37 at% of the total catalyst mass, wherein Fe(III) accounts for 38 at% to 54 at% of the total iron content, Fe(II) accounts for 17 at% to 31 at% of the total iron content, and Fe3C accounts for 17 at% to 31 at% of the total iron content.

[0074] To further understand the content of this invention, a detailed description of the invention is now provided in conjunction with specific embodiments. Some of the equipment and instruments used in the experiments of each embodiment are shown in Table 1-1 below.

[0075] Table 1-1 List of instruments

[0076]

[0077]

[0078] The detection experiments and their operation instructions involved in the embodiments of this invention are as follows:

[0079] 1. Transmission electron microscopy (TEM) analysis

[0080] This invention involves passing uniformly ground aerogel powder through a 100-mesh sieve, dispersing it in an ethanol solution, and then sonicating it until the material particles are invisible to the naked eye. The treated sample is then dropped onto a copper grid and irradiated with an infrared lamp to rapidly evaporate the ethanol solution, drying the sample. This experiment observed the lamellar structure on the surface of the biochar aerogel and the transition metal iron nanoparticles within the aerogel at different magnifications. Furthermore, the crystal structure of iron was identified by observing the diffraction rings formed by the polycrystalline iron structure and the lattice fringes of the iron metal nanoparticles.

[0081] 2. X-ray diffraction analysis (XRD)

[0082] The X-ray diffraction analysis of this invention uses a Cu target with an angle set in the range of 20 to 80° and a scanning speed of 10° / min. The CS, Fe-BC, 4BC / 3CS, 2Fe-BC / 3CS, 3Fe-BC / 3CS, 4Fe-BC / 3CS and 5Fe-BC / 3CS materials are pressed into uniform thin sheets using a small pellet press before testing.

[0083] 3. Micro FTIR spectroscopy

[0084] The functional groups and chemical structure inside the catalyst are qualitatively identified by micro-infrared spectroscopy, and the types of chemical elements and the purity of the substances are semi-quantitatively analyzed. In this invention, CS, 4BC / 3CS, 2Fe-BC / 3CS, 3Fe-BC / 3CS, 4Fe-BC / 3CS and 5Fe-BC / 3CS materials are pressed evenly with a small tablet press and then cut into small pieces for observation.

[0085] 4. X-ray photoelectron spectroscopy (XPS) analysis

[0086] This invention uses a small tablet press to uniformly compress 4BC / 3CS, 2Fe-BC / 3CS, 3Fe-BC / 3CS, 4Fe-BC / 3CS, and 5Fe-BC / 3CS materials, then cuts them into small pieces for observation. The effect of different amounts of powdered biochar added on the ratio of C, N, O, and Fe elements in the aerogel material is analyzed.

[0087] 5. Impedance Analysis (EIS)

[0088] Electrochemical impedance spectroscopy (EIS) studies the relationship between AC impedance and frequency by applying a small-amplitude sinusoidal AC excitation signal to an electrochemical cell in equilibrium or under stable DC polarization conditions. The electron transport capability of a catalyst can be reflected by analyzing its impedance value (EIS). A dispersion was obtained by mixing 5 mg of aerogel catalyst powder, 400 μL of ultrapure water, 400 μL of ethanol, and 5 μL of Nafion, followed by ultrasonic treatment for 30 min. 200 μL of the suspension was then added dropwise to a 1.5 cm × 1.5 cm FTO conductive glass plate and dried under infrared light. A three-electrode system (counter electrode: platinum electrode; reference electrode: Ag / AgCl; working electrode: FTO) was used, with a 0.5 mol / L Na₂SO₄ solution as the electrolyte.

[0089] 6. In-situ Raman analysis (IS-Raman)

[0090] In-situ Raman spectroscopy characterizes ongoing reactions using a high-resolution laser Raman spectrometer, comprising an in-situ electrochemical Raman cell and a Raman spectroscopy analyzer. Before the experiment, a 532 nm green laser was vertically aligned with the side of a dual-channel quartz cuvette (7.5 × 12.5 × 45 mm, capacity: 1.75 mL), allowing the laser to pass through the cuvette. At the start of the experiment, a certain amount of aerogel catalyst was added to the quartz cuvette, and an ozone solution was added using a syringe. The cuvette was then sealed with a lid and gently shaken to ensure uniform suspension of the solid catalyst. After the reaction was complete, the Raman laser was activated, with an emission scanning range of 200 to 1200 cm⁻¹. -1 The resolution is 2cm. -1 In the experiment, laser irradiation did not cause ozone decomposition. For comparison, ultrapure water and an aqueous solution saturated with oxygen were added to replace the ozone solution in the same procedure.

[0091] 7. Electron Paramagnetic Resonance (EPR)

[0092] EPR is a magnetic resonance technique based on the unpaired electron magnetic moment, which can be used to qualitatively and quantitatively detect unpaired electrons in materials, thereby enabling in-depth research into the structural properties of materials. At the start of the reaction, an unsaturated diamagnetic functional group (such as 5,5-dimethyl-1-pyrrolline-N-oxide) is added to the reaction system. Combined with EPR spectroscopy and the specific peak shape of free radicals, the generated ·OH is detected, with a peak shape of 1:2:2:1. In this experiment, TEMP (2,2,6,6-tetramethyl-4-piperidinone hydrochloride), DMPO (5,5-dimethyl-1-pyrrolline-N-oxide), and MeOH (methanol) are used at 30 seconds and 60 seconds after the start of the degradation reaction. 1 O2, ·OH and ·O2 -The reactive oxygen species generated by the 4Fe-BC / 4CS&O3 system were captured and detected.

[0093] Example 1

[0094] This embodiment presents a polycrystalline iron-supported porous biochar aerogel catalyst. The catalyst comprises a porous biochar matrix and polycrystalline iron nanoparticles uniformly distributed on the biochar matrix. The porous biochar matrix and the polycrystalline iron nanoparticles together constitute a polycrystalline iron biochar material. The catalyst as a whole exhibits a honeycomb-like pore network structure, and the polycrystalline iron nanoparticles are uniformly supported on the biochar sheets via Fe-C bonds. Compared to porous carbon materials without polycrystalline iron doping, the polycrystalline iron-supported porous biochar aerogel possesses a richer pore structure, providing more adsorption and reactive active sites and electron migration channels for the adsorption and degradation of organic compounds such as antibiotics.

[0095] Specifically, in this embodiment, the macroscopic shape of the polycrystalline iron-supported porous biochar aerogel is a black columnar object (different shapes can be produced by changing the production mold according to actual needs), and the specific surface area of ​​the polycrystalline iron biochar material is 150-250 m² / g. 2 / g, the diameter of the pores on the biochar matrix is ​​70-90 micrometers, the size (particle size) of the polycrystalline iron nanoparticles is 5-10nm, and the crystal planes of the polycrystalline iron include but are not limited to the (220) crystal plane of Fe3O4, the (002) crystal plane of Fe3C, the (211) crystal plane of Fe3C and the (031) crystal plane of Fe2O3.

[0096] The loading of the polycrystalline iron nanoparticles accounts for 5-15% of the catalyst mass or the content of polycrystalline iron accounts for 0.27at%-37at% of the total catalyst mass, wherein Fe(III) accounts for 38at%-54at% of the total iron content, Fe(II) accounts for 17at%-31at% of the total iron content, and Fe3C accounts for 17at%-31at% of the total iron content.

[0097] In this embodiment, the biochar aerogel has a contact angle of less than 88° and an impedance value below 11Ω. The Raman spectrum of this biochar aerogel shows an ID / IG value greater than 0.85. After contacting O3 in water, its in-situ Raman spectrum reaches 877.74 cm⁻¹. -1 935.76cm -1 and 1004.97cm -1 New peaks have appeared in all areas.

[0098] Example 2

[0099] This embodiment provides a method for preparing a polycrystalline iron-supported porous biochar aerogel catalyst, comprising the following steps:

[0100] (1) Using bamboo charcoal as the biochar source, weigh 5g, and using nonahydrate and ferric nitrate as the iron source, weigh 160g. After weighing, mix with 200ml of ultrapure water and add 10ml of 1M nitric acid to prevent iron hydrolysis. Mix at room temperature for 8 hours, remove the supernatant, dry in an oven overnight, then grind and pass through a 100-mesh sieve. Under the protection of inert gas, place in a tube furnace for calcination. During the calcination process, heat up to 700℃ at a rate of 3℃ / min and hold for 3.0 hours to obtain polycrystalline iron biochar material, denoted as Fe-BC.

[0101] (2) Weigh 0.8g of polycrystalline iron biochar, and weigh 1.2g of chitosan as a nitrogen source and binder. After weighing, put it into a beaker, add 37.2ml of deionized water, add 0.8ml of glacial acetic acid, and then place the beaker on a magnetic stirrer and stir for 60min. After mixing evenly, sonicate for 10min.

[0102] (3) Take 1 ml of the sample from (2), drop it into a cryovial, and freeze it at -20°C until it is non-flowing; then freeze it in a freeze dryer at -80°C for 24 hours.

[0103] (4) Take a certain amount of the sample from step (3) above and put it into a custom crucible. Place it in a high-temperature tube furnace under N2 atmosphere and heat it to 150°C at a heating rate of 5°C / min. Hold it at 150°C for 80 minutes and then let it cool naturally to room temperature. This will produce a polycrystalline iron-supported porous biochar aerogel, denoted as 2Fe-BC / 3CS.

[0104] Example 3

[0105] The preparation method of the polycrystalline iron supported porous biochar aerogel catalyst in this embodiment is basically the same as that in Example 2. The main difference is that in step (2) of this embodiment, the amount of polycrystalline iron biochar added is 1.2g and the amount of deionized water added is 36.8ml. The polycrystalline iron porous biochar aerogel finally prepared is denoted as 3Fe-BC / 3CS.

[0106] Example 4

[0107] The preparation method of the polycrystalline iron supported porous biochar aerogel catalyst in this embodiment is basically the same as that in Example 2. The main difference is that in step (2) of this embodiment, the amount of polycrystalline iron biochar added is 1.6g and the amount of deionized water added is 36.4ml. The polycrystalline iron porous biochar aerogel finally prepared is denoted as 4Fe-BC / 3CS.

[0108] Example 5

[0109] The preparation method of the polycrystalline iron supported porous biochar aerogel catalyst in this embodiment is basically the same as that in Example 2. The main difference is that in step (2) of this embodiment, the amount of polycrystalline iron biochar added is 2g, the amount of deionized water added is 36ml, and the polycrystalline iron porous biochar aerogel finally prepared is denoted as 5Fe-BC / 3CS.

[0110] Comparative Example 1

[0111] (1) Weigh 1.2g of chitosan and put it into a beaker. Add 38ml of deionized water and 0.8ml of glacial acetic acid. Then place the beaker on a magnetic stirrer and stir for 60min. After mixing evenly, sonicate for 10min.

[0112] (2) Take 1 ml of the sample from step (1), drop it into a cryovial, freeze it at -20°C until it is non-flowing, and then freeze it at -80°C for 24 hours in a freeze dryer.

[0113] (3) Take a certain amount of the sample from step (2) above and put it into a crucible. Place it in a high-temperature tube furnace under N2 atmosphere and heat it to 150°C at a rate of 5°C / min. Keep it at 150°C for 80 minutes. Then let it cool down naturally to room temperature to obtain chitosan porous aerogel, denoted as CS.

[0114] Comparative Example 2

[0115] (1) Weigh 1.6g of bamboo charcoal and 1.2g of chitosan and put them into a beaker. Add 36.4ml of deionized water and 0.8ml of glacial acetic acid. Then place the beaker on a magnetic stirrer and stir for 60min. After mixing evenly, sonicate for 10min.

[0116] (2) Take 1 ml of the sample from step (1), drop it into a cryovial, freeze it at -20°C until it is non-flowing, and then freeze it at -80°C for 24 hours in a freeze dryer.

[0117] (3) Take a certain amount of the sample from step (2) above and put it into a crucible. Place it in a high-temperature tube furnace under N2 atmosphere and heat it to 150°C at a rate of 5°C / min. Keep it at 150°C for 80 minutes. Then let it cool down to room temperature naturally to obtain biochar porous aerogel, denoted as 4BC / 3CS.

[0118] Comparative Example 3

[0119] The main difference between this comparative example and Example 4 is that in step (1) of this comparative example, straw is used as the biochar source and ferrocene is used as the iron source to first prepare ferrocene biochar material, denoted as Ferrocene-BC; then chitosan is used as the nitrogen source and binder, and after freeze drying and calcination, ferrocene biochar aerogel is obtained, denoted as 4Ferrocene-BC / 3CS. Other preparation processes are basically the same as in Example 4.

[0120] Comparative Example 4

[0121] The main difference between this comparative example and Example 4 is that in step (1) of this comparative example, straw is used as the biochar source and ferric chloride is used as the iron source to first prepare ferric chloride biochar material, denoted as 4Ferric chloride-BC; then chitosan is used as the nitrogen source and binder, and after freeze drying and calcination, ferric chloride biochar aerogel is obtained, denoted as 4Ferric chloride-BC / 3CS. Other preparation processes are basically the same as in Example 4.

[0122] like Figure 2 Images (a), (b), (c), and (d) show SEM images of the aerogels obtained in Comparative Example 2, Example 2, Example 3, and Example 5, respectively. Figure 1 Image (a) shows an SEM image of the product from Example 4. Comparison revealed that the biochar aerogel doped with polycrystalline iron had more uniform pores, while the pores formed by the direct composite of iron-free biochar and chitosan were larger and stretched into uneven shapes, failing to achieve a stable form. Figure 2 (a)). The biochar aerogel formed by the combination of iron-based biochar and chitosan has uniform pores, and as the amount of iron-based biochar added increases, the biochar sheets gradually become rougher and the degree of defects increases.

[0123] like Figure 1 Image (b) shows a scanning electron microscope (SEM) image of undoped chitosan porous aerogel CS (Comparative Example 1). Low-viscosity chitosan was dispersed in an acetic acid aqueous solution to form a colloid, which was then freeze-dried to create a porous honeycomb structure with a pore size of approximately 80 micrometers. However, the CS sheets were smooth and flat with low defect levels, providing fewer catalytic reaction active sites. In contrast, adding chitosan as a crosslinking agent to iron-based biochar materials allows for stable connection of biochar sheets and polycrystalline iron particles through crosslinking, forming a loose, porous, and water-stable biochar porous aerogel material. Its relatively coarse pore structure effectively improves electron transfer efficiency, providing abundant reaction sites for ozone catalysis.

[0124] Figure 1 Image (c) shows a TEM scan of the prepared 4Fe-BC / 3CS, revealing iron particles with sizes ranging from 5 to 7 nm. Meanwhile, as... Figure 1 As shown in (d) and (e), TEM also confirmed the presence of polycrystalline iron. The alternating growth of multiple crystals within the biochar sheets provides more catalytic sites for ozone formation. Furthermore, due to the presence of multiple grains within the material's crystal structure, each with a different crystal plane, multiple diffraction rings appear in the diffraction pattern, which... Figure 1(a) Diffraction ring calibration in the middle region shows that ( Figure 1 f), the diffraction radii from the inside out are the (220) crystal plane of Fe3O4, the (002) crystal plane of Fe3C, and the F… e3 The (211) crystal plane of C and the (031) crystal plane of Fe2O3.

[0125] like Figure 3 The image shown is a SEM energy dispersive spectroscopy (EDS) image of the aerogel from Example 4. Figure 3 As can be seen from d and e, chitosan acts as an adhesive, forming the main framework of the pores, while iron ( Figure 3 f) indicates that the iron is evenly distributed throughout the material, demonstrating the uniform distribution of iron within the catalyst and the formation of a 3D porous structure by the chitosan-bonded biochar. In other words, the addition of a crosslinking agent allows the polycrystalline iron to be firmly supported on the porous biochar matrix via Fe-C bonds, while simultaneously using the crosslinking agent to bond the porous biochar sheets together to form a 3D porous framework structure.

[0126] like Figure 4 As shown in (a) and (b), compared to the undoped chitosan porous aerogel CS (Comparative Example 1), the expansion factor of the polycrystalline iron biochar-doped aerogel 4Fe-BC / 3CS (Example 4) increased from 1.05 times to 1.3 times, and it maintained its original morphology after multiple compressions without particle peeling, indicating that the material has good softness, resilience, and plasticity, and the connection between the biochar sheets is relatively strong. This may be because the incorporation of biochar results in a more stable structure through surface complexation, π-π interactions, and hydrogen bonding, while the elasticity and plasticity provide greater possibilities for practical applications.

[0127] Figure 4 The figures (ch) represent the contact angle and absorption time of the aerogels obtained in Comparative Examples 1, 2, and 2-5, respectively. As can be seen from the figures, the absorption time was reduced to 0.34 s after the introduction of biochar. This is likely because the O and C functional groups on the surface of the biochar material improve its water absorption rate, but the contact angle remained almost unchanged (89.8°). However, after the introduction of polycrystalline iron biochar, both the contact angle and water absorption time of the composite material decreased significantly, indicating that the hydrophilicity and water absorption performance of the aerogel were greatly improved after the introduction of iron-based biochar. This may be related to the change in the amount of oxygen-containing functional groups on the surface of the iron-based biochar aerogel after calcination heat treatment, which can improve the hydrophilicity of the biochar material. The increased hydrophilicity and water absorption rate allow pollutants to react rapidly with the material inside the pores while passing through them, effectively increasing the exchange rate and providing conditions for high-speed ion reactions.

[0128] like Figure 5 As shown, the X-ray photoelectron spectroscopy (XPS) spectra of the aerogels obtained in Examples 2-5 show peaks of C1s (around 283.60 eV), N1s (around 400.00 eV), O1s (around 531.93 eV), and Fe2p (around 722.02 and 710.81 eV), without any other impurity peaks. This confirms that Fe was successfully incorporated into the C framework without any other products. The intensity of the peaks indicates the elemental content in the material to some extent. XPS spectra provide a better understanding of the surface composition, chemical state, and molecular structure of the catalyst. XPS spectra with different doping ratios further confirm that Fe, C, O, and N are the main components of Example 4. Pure biochar has an extremely low nitrogen content. After the introduction of chitosan, the abundant nitrogen content within chitosan provides an opportunity for the aggregation of nitrogen functional groups, while also fixing a large number of reactive oxygen functional groups.

[0129] like Figure 6 (b) shows that Raman spectroscopy is used to characterize the structural features of carbon catalysts, in the D band (~1350 cm⁻¹). -1 ) and G band (~1580cm) -1 The defects and crystallinity of sp3 hybrid carbon were characterized, respectively. Therefore, the intensity ratio of the D and G bands (ID / IG) can be used to analyze the degree of catalyst defects. The test results in the figure show that the ID / IG values ​​follow the order of Example 4 (0.99) > Example 2 (0.951) > Example 3 (0.92) > Example 5 (0.87). The closer the ID / IG value is to 1, the higher the degree of disorder of the biochar sheets. This can not only generate redox activity, but also serve as an electron transport medium and reactive site. With the increase of polycrystalline iron biochar, the ID / IG value first increases and then decreases, indicating that the iron doping amount needs to be within a suitable limit to achieve the maximum catalytic effect.

[0130] In-situ Raman spectroscopy further revealed the dissociation process of O3 at the Fe sites on the surface, such as... Figure 6 As shown in (a), after adding O3, the diameter is 877.74 cm. -1 935.76cm -1 and 1004.97cm -1 New peaks appeared, corresponding to surface atomic oxygen (O2*, O*) and surface adsorbed O3, respectively. Conversely, this phenomenon was not observed in suspensions containing O2 and ultrapure water, mainly due to the formation of O3 from ozone adsorbed on the material surface. * and O2 * O2 * It is then further converted into singlet oxygen through electron transfer.

[0131] like Figure 7The figure shows the impedance diagrams of the aerogels prepared in Example 4 and Comparative Example 1, as well as the polycrystalline iron biochar material Fe-BC. As can be seen from the figure, the Nyquist distribution of the EIS of different materials was measured experimentally, and the diameter of the extrapolated semicircle obtained by the algorithm was used as the accurate value of the impedance. Among the four materials, Rct from largest to smallest is: CS (15.28Ω) > 4BC / 3CS (11.91Ω) > Fe-BC (12.96Ω) > 4Fe-BC / 3CS (10.29Ω). This may be because biochar itself has good conductivity, and the conductivity is enhanced after incorporating iron ions into the biochar. Furthermore, incorporating iron-based biochar into chitosan forms a continuous network structure, establishing electron transport channels with good conductivity between molecules. These channels provide pathways for electron movement, thereby promoting charge transport and conduction. Therefore, this is also why 4Fe-BC / 3CS can efficiently catalyze the ozone degradation of new organic pollutants.

[0132] like Figure 8 As shown, pure biochar has an extremely low nitrogen content. After the introduction of chitosan, the abundant nitrogen content inside chitosan provides an opportunity for the aggregation of nitrogen functional groups, while also fixing a large number of reactive oxygen functional groups. Figure 8 The detailed N1s plot in (b) classifies the doped N types as: pyridine N (398.2 eV), Co-Nx (399.0 eV), pyrrole N (399.9 eV), graphite N (401.1 eV), and N oxide (402.7 eV). With increasing doping concentration in the polycrystalline iron biochar, the pyridine nitrogen content reaches 65% (Example 4). Furthermore, from... Figure 8 (d) It can be seen that the Fe inside the polycrystalline iron biochar is... X -C has a lower peak, and after being fixed on the chitosan surface, Fe... X -C begins to increase, and as the amount of iron-based biochar doping increases, the Fe content of the aerogel obtained in Example 4 increases. X -C content remained stable at around 22%, and ferrous iron reached 31% of the total iron content. Figure 8 (a) It can be seen that the chitosan aerogel after freeze-drying-secondary calcination has Fe X -C peak height begins to increase significantly, and Fe increases with increasing iron-based biochar content. X -C peak height gradually increases, reaching 36%-39%, which is not found in Fe-BC. Figure 8 (c) shows that the ratio of iron to oxygen is stable at 18%-26% under different iron-based biochar ratios, and reaches the maximum at 4Fe-BC / 3CS.

[0133] To further analyze the reasons for the improved catalytic performance, the logarithm of the degradation rate (log(k)) and the catalyst structural properties were fitted and analyzed (e.g., Figure 9As shown in the figure), the results indicate that the pyridine nitrogen content log(k)(R) 2 =0.998) shows a good linear correlation ( Figure 9 (a)), and the k value increases with increasing pyridine nitrogen content, which is consistent with previous experiments, indicating that pyridine nitrogen is the catalytic site for ozone formation. Furthermore, the Fe-C group content shows a positive linear relationship with log(k) (R0). 2 =0.974)( Figure 9 (c) indicates that Fe-C on the catalyst can effectively adsorb ozone to form surface atomic oxygen, and the direct reaction between O3 molecules and Fe3C produces surface atomic oxygen species. The Fe-O groups on the catalyst surface are rich in electrons and show a positive linear correlation with log(k) (R0). 2 =0.911)( Figure 9 (b) This drives the electron transfer pathway and promotes 1 The formation of O2 and ·OH.

[0134] like Figure 10 As shown in (a), the ozone activation efficiency of different systems was evaluated. Using levofloxacin (LEV) as a model pollutant, comparative experiments were conducted on multiple systems. Furthermore, based on the established pseudo-first-order reaction kinetics... Figure 10 (b) The apparent rate constant K was calculated. The results showed that Comparative Example 1 had no ability to adsorb or remove LEV; after the introduction of biochar, the adsorption capacity of the aerogel in Comparative Example 2 was improved, but it could not catalyze the degradation of LEV by ozone; in the aerogel and ozone system of Example 4, the reaction rate was 0.0929 min. -1 Under the specified conditions, levofloxacin could be completely removed in just 40 seconds. This represents a 1.75-fold improvement over Fe-BC alone, indicating that the abundant pores within the aerogel provide feasible reaction sites. The results show that the non-metallic biochar aerogel framework has almost no catalytic effect on ozone, while pure iron-based biochar has limited activation ability for ozone catalysis. This may be because the formation of a stable three-dimensional structure provides additional doping centers for the active components, accelerating the electron transfer rate within the material. Furthermore, the iron ion dissolution in the Fe-BC and ozone system was 0.07 mg / L, approximately 35 times higher than the system in Example 4 (2.1 μg / L), which would pose a serious ecological risk if used long-term.

[0135] To investigate the catalytic performance of catalysts with different iron-based biochar doping ratios, ozone catalysis experiments were conducted using biochar aerogels with different iron-based biochar doping ratios. The results are as follows: Figure 10 As shown in (c), according to pseudo-first-order reaction kinetics ( Figure 10 The apparent rate constant K was calculated (as shown in Figure d). As the doping concentration of iron-based biochar gradually increased, the reaction rate also increased from 0.050 min / min.-1 Gradually increased to 0.056 min -1 The value increased to 0.093 min at 4Fe-BC / 3CS. -1 However, the reaction rate of 5Fe-BC / 3CS decreased to 0.060 min. -1 This may be due to the dilution effect of continuously increasing the doping amount on the active sites. That is, the introduction of dopants increases the distance between active sites, reducing the density of active sites and catalytic activity. XPS results also confirm this view, with the actual iron doping amounts of 4Fe-BC / 3CS and 5Fe-BC / 3CS being similar. Figure 8 However, the content of pyridine nitrogen and divalent iron in 5Fe-BC / 3CS decreased, and it was also found during the material preparation that the chitosan surface in 5Fe-BC / 3CS aerogel could not coat the iron-based biochar powder. This indicates that the covalent bond between the iron-based biochar powder and chitosan has reached a certain degree of saturation. Further addition of iron-based biochar is not very meaningful and will instead block the pores in the aerogel, leading to lattice distortion and unstable crystal phase structure of the catalyst material, which in turn affects the exposure and activity of active sites.

[0136] To understand the contributions of different oxidizing agents in the examples, a free radical quenching experiment was conducted using the aerogel in Example 4 as an example to explore the mechanism of ozone degradation of levofloxacin by the aerogel of this invention. Commonly used quenchers furfuryl alcohol (FFA), p-chlorobenzoic acid (pCBA), potassium iodide (KI), and chloroform (CHCl3) were used as... 1 O2, ·OH, electrons, O2 ·- Quenching agents, such as Figure 11 As shown in (a), only 10.1% of LEV was degraded within 60 seconds after the addition of FFA, indicating a significant inhibition of the reaction, with the reaction rate decreasing to 0.002 min. -1 Furthermore, pCBA, as a scavenger of ·OH in the ozone system, significantly inhibited the reaction by degrading only 19.7% of LEV within 60 seconds. Considering that iron can promote electron transfer through polymorphic transformation, KI was introduced as a chemical probe to block the electron transfer pathway. Consistent with the FFA quenching experiment, only 10% of LEV was degraded, indicating that blocking the electron transfer process significantly affected the degradation of LEV. 1 The generation of O2 was observed. Finally, the addition of CHCl3 to the system only slightly inhibited the experiment, indicating that O2 generation... ·- It is not a major active species in the 4Fe-BC / 3CS&O3 system.

[0137] EPR was used to visually verify the ROS (reactive oxygen species) involved in the levofloxacin system of Example 4. No different types of ROS were detected in either the pure Example 4 or O3 systems, indicating that the pure ozone system was a homogeneous system catalyzed by pure ozone. However, the Example 4 & O3 system generated a large amount of ROS. 1 O2 was captured by TEMP (2,2,6,6-tetramethylpiperidine oxide), exhibiting a typical (1:1:1) EPR spectrum with three lines of equal intensity. Figure 11 (b) The ·OH group was captured by DMPO (5,5-dimethyl-1-pyrrolidone-N-oxide), showing a distinct 1:2:2:1 signal peak. Figure 11 (c) In addition, DMPO is added to methanol to capture O2. ·- Only a mild signal peak was produced. Figure 11 (d) Therefore, it can be concluded that the Example 4 & O3 system can generate a large amount of ROS, which promotes the effective degradation of levofloxacin, while neither Example 4 nor the O3 system alone can generate enough ROS to be captured in a short period of time.

[0138] One of the important evaluation criteria for practical applications is the reusability and stability of materials. The aerogel obtained in Example 4 exhibited excellent reusability, maintaining a 100% degradation rate after ten cycles. Figure 12 (a)). And as Figure 12 As shown in (b), the iron ion leaching concentration was 2.14 μg / L, which is far below the 0.3 mg / L requirement of the Chinese Drinking Water Standard (GB 5749-2022). Furthermore, the average reaction rate after 10 cycles was 0.076 min. -1 Therefore, compared with earlier studies, 4Fe-BC / 3CS is a more stable material that can be reused multiple times, and the above findings demonstrate the potential of this catalytic material in practical wastewater treatment.

[0139] Furthermore, to demonstrate the feasibility of practical application, actual rural wastewater was used as a background. Sixteen antibiotics in the water were measured and classified according to standard (DB37 / T3738—2019) to investigate the feasibility of the aerogel-catalyzed ozone degradation of different types of antibiotics in this invention. For example... Figure 13 As shown, after ozone catalysis by the material of this invention, the levels of sulfonamides, macrolides, tetracyclines, and Group III carcinogens listed in the World Health Organization's International Agency for Research on Cancer decreased to below 10 ng / L. The levels of fluoroquinolones were significantly affected by actual root exudates, but the overall levels showed a downward trend.

[0140] Example 6

[0141] The preparation method of the polycrystalline iron-supported porous biochar aerogel catalyst in this embodiment includes the following steps:

[0142] (1) Bamboo charcoal is used as the biochar source and ferric chloride is used as the iron source. The mixture is mixed and dispersed in ultrapure water, and hydrochloric acid is added to prevent iron hydrolysis. The mixture is mixed at room temperature for 10 hours, the supernatant is removed, and the mixture is dried in an oven overnight. Then it is ground and passed through a 100-mesh sieve. Under the protection of inert gas, it is placed in a tube furnace for calcination. The calcination process is carried out at a rate of 5℃ / min to 800℃ and held for 1.0 hour to obtain polycrystalline iron biochar material.

[0143] (2) Weigh 1.4g of polycrystalline iron biochar, and weigh 1.2g of chitosan as a nitrogen source and binder. After weighing, put it into a beaker, add 36.6ml of deionized water, add 1ml of glacial acetic acid, and then place the beaker on a magnetic stirrer and stir for 50min. After mixing evenly, sonicate for 12min.

[0144] (3) Take 1 ml of the sample from step (2), drop it into a cryovial, and freeze it at -20°C until it is non-flowing; then freeze it in a freeze dryer at -80°C for 22 hours.

[0145] (4) Take a certain amount of the sample from step (3) above and place it in a crucible. Place the crucible in a high-temperature tube furnace under N2 atmosphere and heat it to 100°C at a heating rate of 1°C / min. Hold the temperature for 120 min and then allow it to cool naturally to room temperature to obtain polycrystalline iron-supported porous biochar aerogel. In this example, due to the high solubility of ferric chloride, it can be combined with biochar at a high concentration. After high-temperature oxidation, magnetic iron oxide is formed. Therefore, compared with Example 4, the iron clusters are larger and the catalytic performance is slightly reduced.

[0146] Example 7

[0147] The preparation method of the polycrystalline iron-supported porous biochar aerogel catalyst in this embodiment includes the following steps:

[0148] (1) Bamboo charcoal was used as the biochar source and iron citrate was used as the iron source. They were mixed and dispersed in ultrapure water, and 15 ml of citric acid was added to prevent iron hydrolysis. The mixture was mixed at room temperature for 12 hours, the supernatant was removed, and the mixture was dried in an oven overnight. Then it was ground and passed through a 100-mesh sieve. Under the protection of inert gas, it was placed in a tube furnace for calcination. The calcination process was carried out at a rate of 1℃ / min to 300℃ and held for 4.0 hours to obtain polycrystalline iron biochar material.

[0149] (2) Weigh 1.5g of polycrystalline iron biochar, and use chitosan as a nitrogen source and binder. Weigh 1.5g of the biochar and put it into a beaker. Add 35.8ml of deionized water and 0.7ml of glacial acetic acid. Place the beaker on a magnetic stirrer and stir for 70min. After mixing evenly, sonicate for 8min.

[0150] (3) Take 1.5 ml of the sample from step (2), drop it into a cryovial, and freeze it at -20°C until it is non-flowing; then freeze it in a freeze dryer at -80°C for 24 hours.

[0151] (4) Take a certain amount of the sample from step (3) above and place it in a crucible. Place the crucible in a high-temperature tube furnace under N2 atmosphere and heat it to 200°C at a heating rate of 8°C / min. Hold the temperature at 200°C for 60 min and then allow it to cool naturally to room temperature to obtain polycrystalline iron-supported porous biochar aerogel. The biochar aerogel prepared in this example has almost the same catalytic performance for single use as that in Example 4, but its reusability is worse than that in Example 4.

[0152] Example 8

[0153] The preparation method of the polycrystalline iron-supported porous biochar aerogel catalyst in this embodiment includes the following steps:

[0154] (1) Coconut shell carbon is used as the biochar source, and nonahydrate and ferric nitrate are used as the iron source. They are mixed and dispersed evenly in ultrapure water, and 10 ml of 1M nitric acid is added to prevent iron hydrolysis. The mixture is mixed at room temperature for 9 hours, the supernatant is removed, and the mixture is dried in an oven overnight. Then it is ground and passed through a 100-mesh sieve. Under the protection of inert gas, it is placed in a tube furnace for calcination. During the calcination process, the temperature is raised to 600℃ at a rate of 4℃ / min and held for 2.5 hours to obtain polycrystalline iron biochar material.

[0155] (2) Weigh 1.0g of polycrystalline iron biochar, and use carrageenan as a nitrogen source and binder. Weigh 1.2g of the biochar and put it into a beaker. Add 37ml of deionized water and 0.8ml of glacial acetic acid. Place the beaker on a magnetic stirrer and stir for 50min. After mixing evenly, sonicate for 15min.

[0156] (3) Take 1 ml of the sample from step (2), drop it into a cryovial, and freeze it at -15°C until it is non-flowing; then freeze it in a freeze dryer at -70°C for 24 hours.

[0157] (4) Take a certain amount of the sample from step (3) above and put it into a crucible. Place it in a high-temperature tube furnace under N2 atmosphere and heat it to 150°C at a heating rate of 5°C / min. Hold it at that temperature for 80 minutes and then let it cool naturally to room temperature to obtain polycrystalline iron-supported porous biochar aerogel. Although the binding ability between coconut shell and iron is relatively weak, it has strong resistance due to its high self-hardness and is suitable for engineering conditions. Compared with Example 4, it has higher hardness, but its catalytic performance is slightly reduced.

[0158] Example 9

[0159] The preparation method of the polycrystalline iron-supported porous biochar aerogel catalyst in this embodiment includes the following steps:

[0160] (1) Using straw biochar as the biochar source and ferric chloride as the iron source, they are mixed and dispersed evenly in ultrapure water, and a certain amount of hydrochloric acid is added to prevent iron hydrolysis. The mixture is mixed at room temperature for 10 hours, the supernatant is removed, and the mixture is dried in an oven overnight. Then it is ground and passed through a 100-mesh sieve. Under the protection of inert gas, it is placed in a tube furnace for calcination. During the calcination process, the temperature is raised to 400℃ at a rate of 4℃ / min and held for 2.0 hours to obtain polycrystalline iron biochar material.

[0161] (2) Weigh 1.6g of polycrystalline iron biochar, and weigh 1.2g of sodium alginate as a nitrogen source and binder. After weighing, put it into a beaker, add 36.4ml of deionized water, add 0.8ml of glacial acetic acid, and then place the beaker on a magnetic stirrer and stir for 60min. After mixing evenly, sonicate for 10min.

[0162] (3) Take 1 ml of the sample from (2), drop it into a cryovial, and freeze it at -25°C until it is non-flowing; then freeze it in a freeze dryer at -85°C for 20 hours.

[0163] (4) Take a certain amount of the sample from step (3) above and put it into a custom crucible. Place it in a high-temperature tube furnace under N2 atmosphere and heat it to 130°C at a heating rate of 4°C / min. Hold it at 130°C for 90 minutes and then let it cool naturally to room temperature to obtain polycrystalline iron-supported porous biochar aerogel.

[0164] Straw, as an agricultural waste, has relatively low collection and processing costs. After being converted into carbon, straw biochar has low density and small particle size. When combined with iron, the resulting particles have a small diameter, thus forming a fine iron-based biochar catalyst. However, compared with Example 4, its hardness is lower and its performance is slightly worse.

[0165] In summary, the aerogel prepared by this invention has abundant pores and a large specific surface area. At the same time, by utilizing the ion exchange of the crosslinking agent, iron-based materials and carbon-based materials are crosslinked together, resulting in a relatively strong loading of polycrystalline iron nanoparticles. This can effectively improve the mechanical strength and structural stability of the catalyst. Furthermore, the preparation process of this catalyst is simple, the required raw materials are green and pollution-free, low in cost, and easy to mass-produce. It can be used in fields such as treating organic pollutants in wastewater and deep purification of drinking water.

Claims

1. A polycrystalline iron-supported porous biochar aerogel catalyst, characterized in that, The catalyst has an overall honeycomb-like porous network structure, which includes a porous biochar matrix and polycrystalline iron nanoparticles loaded on the biochar sheets through Fe-C bonds; the crystal faces of the polycrystalline iron include the (220) crystal face of Fe3O4, the (002) crystal face of Fe3C, the (211) crystal face of Fe3C, and the (031) crystal face of Fe2O3; The preparation method of the porous biochar aerogel catalyst includes the following steps: Iron-based biochar and a crosslinking agent are mixed in an aqueous solution to form an iron-based biochar-crosslinking agent mixture; wherein the iron-based biochar comprises a biochar matrix and polycrystalline iron nanoparticles supported on biochar sheets; and the crosslinking agent comprises chitosan. The iron-based biochar-crosslinking agent mixture was freeze-dried to form honeycomb-like pores in the biochar sheets, thus obtaining iron-based biochar aerogel. The iron-based biochar aerogel is calcined under an inert atmosphere. Specifically, the iron-based biochar aerogel is heated to 150°C to 200°C at a rate of 1 to 8°C / min, held at that temperature for 1.0 to 2.0 hours, and then cooled to room temperature, so that polycrystalline iron nanoparticles are loaded onto the biochar sheets through Fe-C bonds, thus obtaining the polycrystalline iron-supported porous biochar aerogel catalyst.

2. The porous biochar aerogel catalyst according to claim 1, characterized in that, Different crystals of the polycrystalline iron grow alternately within the biochar sheets, and interlaced mesh-like lattice stripes can be observed under a transmission electron microscope. And / or the loading of the polycrystalline iron nanoparticles accounts for 5-15% of the catalyst mass; And / or the content of the polycrystalline iron accounts for 0.27 at% to 37 at% of the total catalyst, wherein Fe 3+ Fe accounts for 38 at %~54 at % of the total iron content. 2+ Fe3C accounts for 17 at %~31 at % of the total iron content.

3. The porous biochar aerogel catalyst according to claim 1 or 2, characterized in that, The polycrystalline iron nanoparticles have a size of 1~10 nm; and / or the pores on the biochar matrix have a diameter of 50~100 micrometers.

4. The porous biochar aerogel catalyst according to claim 1 or 2, characterized in that, The contact angle of the biochar aerogel is less than 88°; And / or the impedance value of the biochar aerogel is below 11Ω; And / or the Raman spectrum of the biochar aerogel shows an ID / IG value greater than 0.85, and its in-situ Raman spectrum after contact with O3 in water reaches 877.74 cm⁻¹. -1 935.76cm -1 and 1004.97cm -1 New peaks have appeared in all areas.

5. A method for preparing a porous biochar aerogel catalyst as described in any one of claims 1-4, characterized in that, include: Iron-based biochar and a crosslinking agent are mixed in an aqueous solution to form an iron-based biochar-crosslinking agent mixture; wherein the iron-based biochar comprises a biochar matrix and polycrystalline iron nanoparticles supported on biochar sheets; The iron-based biochar-crosslinking agent mixture was freeze-dried to form honeycomb-like pores in the biochar sheets, thus obtaining iron-based biochar aerogel. Iron-based biochar aerogel is calcined under an inert atmosphere to load polycrystalline iron nanoparticles onto the biochar sheets via Fe-C bonds. Specifically, the iron-based biochar aerogel is heated to 150°C to 200°C at a rate of 1 to 8°C / min, held at that temperature for 1.0 to 2.0 hours, and then cooled to room temperature to obtain the polycrystalline iron-supported porous biochar aerogel catalyst.

6. The method for preparing the porous biochar aerogel catalyst according to claim 5, characterized in that, The specific surface area of ​​the iron-based biochar is 150~250 m². 2 / g; And / or the mass ratio of the iron-based biochar to the crosslinking agent is (2-5):(1-5); And / or the biochar includes bamboo charcoal, straw biochar, and coconut shell charcoal; And / or the aqueous solution contains organic or inorganic acids, and the ratio of iron-based biochar, crosslinking agent, organic or inorganic acid, and water is (0.8g~2g): (0.8g~2g): (0.4ml~0.8ml): (38ml~35.2ml); And / or the freeze-drying treatment of the iron-based biochar-crosslinking agent mixture includes: first freezing the iron-based biochar-crosslinking agent mixture at -15~-25°C, and then freeze-drying it at -70~-85°C.

7. The method for preparing the porous biochar aerogel catalyst according to claim 5 or 6, characterized in that, The iron-based biochar was prepared by chemical deposition or mechanical ball milling.

8. The application of a porous biochar aerogel catalyst as described in any one of claims 1-4 in a water purification system.

9. The application according to claim 8, characterized in that, The water purification system includes an ozone catalytic oxidation system, and its usage method includes: In the ozone catalytic oxidation system, the porous biochar aerogel catalyst is brought into contact with ozone in the water to be treated to form surface atomic oxygen, which catalyzes the decomposition of ozone to generate singlet oxygen and hydroxyl radicals, thereby enhancing the degradation of pollutants in the water.

Citation Information

Patent Citations

  • A high-elasticity, high-temperature-resistant aerogel and a preparation method thereof

    CN113750917B

  • Chitosan-based biochar with porous structure and high specific surface area as well as preparation method and application of chitosan-based biochar

    CN115634679A

  • Modified biochar and preparation method and application thereof

    CN110217772A

  • Modified biochar catalyst and preparation method thereof

    CN116943704A