A method for producing a t-shaped alloy profile

By using continuous rolling and multi-pass straightening processes in a φ950 tandem 13-strand rolling mill, the production process of T-shaped alloy profiles has been optimized, solving the problems of low efficiency, distortion, and substandard performance in traditional methods, and achieving efficient and low-cost large-scale production.

CN119281811BActive Publication Date: 2026-11-24SHAANXI HUALU GOLD & TITANIUM IND CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411619848.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-11-13
Publication Date
2026-11-24
Estimated Expiration
2044-11-13

Smart Images

  • Figure CN119281811B_ABST
    Figure CN119281811B_ABST
Patent Text Reader

Abstract

This invention provides a method for producing T-shaped alloy profiles, comprising the following steps: S1, selecting a titanium alloy square billet as the raw material and removing the surface oxide layer and impurities; S2, heating the billet to the rolling temperature and then continuously rolling it into a symmetrical T-shaped profile using a φ950 tandem 13-stand rolling mill; S3, utilizing the residual heat of the material after hot rolling, conveying the material to an online tension straightener via roller conveyors for tension straightening, and then performing secondary straightening via a tension straightener; S4, after the semi-finished material cools, cutting it to length using a band saw, and then splitting it lengthwise using water jet cutting to obtain several profiles. This invention provides a method for producing T-shaped alloy profiles, which uses a φ950 tandem 13-stand rolling mill for continuous rolling to produce T-shaped profiles, replacing the traditional extrusion method. This makes the profiles less prone to breakage during processing, results in excellent mechanical properties, and fully utilizes raw materials, greatly reducing material waste.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of non-ferrous metals, and more particularly to a method for producing T-shaped alloy profiles. Background Technology

[0002] T-shaped profiles are named for their cross-section resembling the letter "T". There are two types of T-shaped profiles: 1. T-shaped profiles formed by longitudinally dividing H-shaped profiles, which have advantages such as strong bending resistance, simple construction, cost savings, and light structural weight; 2. Hot-rolled T-shaped profiles formed in one piece, mainly used in machinery, special equipment, and ships.

[0003] Traditional T-shaped profile production involves extruding or welding metal billets to create profiles of a specific shape. Depending on the shape, the corresponding processing methods will also differ. For the preparation process of T-shaped alloy profiles, the traditional production method is to use an extrusion press for extrusion molding.

[0004] In related technologies, extrusion molding using an extruder is employed. Extruded profiles require extremely high power, load pressure, and die specifications from the extrusion equipment. Furthermore, the metal flow after extrusion is poor, resulting in a distorted finished product. The thickness allowance needs to be increased to approximately 30%, making subsequent processing extremely difficult. Currently, only 3-4 meters in length can be produced per piece, with a yield rate of less than 50%, leading to significant waste. Therefore, existing T-shaped profile production methods cannot meet market demand.

[0005] Therefore, it is necessary to provide a production method for T-shaped alloy profiles to solve the above-mentioned technical problems. Summary of the Invention

[0006] This invention provides a method for producing T-shaped alloy profiles, which solves the problems of low production efficiency of T-shaped alloy profiles and the tendency of extrusion methods to cause distortion and substandard material properties.

[0007] To solve the above-mentioned technical problems, the present invention provides a method for producing T-shaped alloy profiles, comprising the following steps:

[0008] S1. Select a titanium alloy square billet as the billet and remove the surface oxide layer and impurities;

[0009] S2. The billet is heated to the rolling temperature and then continuously rolled into a symmetrical T-shaped profile using a φ950 tandem 13-stand rolling mill.

[0010] S3. Utilizing the residual heat of the material after hot rolling, the material is conveyed to an online tension straightener via roller conveyor for tension straightening; then it is straightened a second time via a tension straightener.

[0011] S4. After the semi-finished material has cooled, the band saw cuts the material to the required length and then uses water jet cutting or mechanical cutting to split it in the length direction to obtain several profiles.

[0012] S5. Use the inward stacking method of the flange plates to assemble the cut profiles;

[0013] S6. After the packaged profiles are assembled, they are subjected to stress-relieving annealing. After annealing, they are removed from the furnace and unpacked.

[0014] S7. Sandblasting to remove the oxide scale from the surface of the profile;

[0015] S8. Place the sandblasted profile into an acid bath for pickling and passivation. Pickle the surface until it turns silver-gray, then rinse it clean with water.

[0016] S9. Use an ultrasonic flaw detector to perform flaw detection. If the flaw detection is qualified, it is a finished product; if the flaw detection is unqualified, it is a scrap product. After the flaw detection is completed, the finished product is placed in a drying chamber for drying to obtain the T-shaped alloy profile finished product. In S2, the rolling mill is used to sequentially pass through the K13-K12-K11-K10-K9-K8-K7-K6-K5-K4-K3-K2-K1 pass. The rolling mill working speed is 1.2-1.5 m / s. The K13-K12-K11-K10-K9 pass is a double-support symmetrical pass for billet opening. K8, K6, K4, and K2 are finished by a universal rolling mill. K7, K5, K3, and K1 are edged by a two-roll horizontal rolling mill.

[0017] Preferably, in S2, K13 has dimensions of 430×220mm, K12 has dimensions of 420×200mm, K11 has dimensions of 380×190mm, K10 has dimensions of 350×180mm, K9 has dimensions of 280×160mm, K8 has dimensions of 220×150mm, K7 has dimensions of 210×140mm, K6 has dimensions of 205×130mm, K5 has dimensions of 200×125mm, K4 has dimensions of 200×120mm, K3 has dimensions of 200×115mm, K2 has dimensions of 200×105mm, and K1 has dimensions of 200×100mm; wherein K13-K9 are pre-forming holes for initial rolling, and K8-K1 are finishing rolling holes.

[0018] Preferably, in step S5, the specific method of packaging is as follows: use 10 profiles to package, stack them facing each other, and tie the package with steel strips, with each bundle tied 5-8 times.

[0019] Preferably, in step S6, the annealing process is as follows: after the temperature of the annealing furnace rises to 550-750℃, annealing begins and is maintained at a constant temperature for 2-4 hours. After cooling in the furnace to 180-220℃, the furnace is removed from the furnace, and the straightness is controlled to 2mm / m after unpacking.

[0020] Preferably, in step S8, the acid solution used comprises the following components by weight percentage:

[0021] 15% nitric acid, 5% hydrofluoric acid, and the remainder is water;

[0022] The pickling soaking time is 10-30 minutes.

[0023] Preferably, in step S9, the flaw detection standard is Class A, the medium is water, and the drying temperature is 60-80℃.

[0024] Preferably, in S1, the dimensions of the titanium alloy square billet are δ450×230×2000mm, and in S2, the dimensions of the rolled profile are 200×100×6000mm.

[0025] Preferably, a processing device is used when processing the T-shaped profile in step S4. The processing device includes a processing table, inside which a cutting device is installed. The cutting device includes a rotating rod, with a cutting wheel positioned at the center of the rotating rod's surface. A driving component is located on one side of the rotating rod. Filter screens are installed on the surface of the processing table and on both sides of the cutting wheel. A positioning device is installed on the side of the processing table, comprising four fixing blocks. The four fixing blocks are grouped in pairs, and a fixing rod connects the two groups of fixing blocks. The center of the surface of the fixing rod is... A connecting frame is provided, and a double-headed hydraulic telescopic rod is installed inside the connecting frame. Both ends of the double-headed hydraulic telescopic rod are connected to rectangular blocks. One end of each rectangular block is connected to a movable sleeve, which is fitted onto the surface of the fixed rod. A push rod is connected to one side of each rectangular block, and one end of the push rod is connected to a positioning plate. A collection box is provided inside the processing table, and a disassembly assembly is provided at one end of the processing table. The disassembly assembly includes a disassembly plate, and mounting blocks are connected to both sides of the disassembly plate. Mounting sleeves are fitted onto the surface of each mounting block, and the mounting sleeves are connected to the side of the processing table.

[0026] Preferably, a suction assembly is provided above the processing table. The suction assembly includes a mounting frame, one end of which is connected to a suction cover. A conveying device is provided on one side of the processing table. The conveying device includes a housing. A pump body is installed on the top of the housing. Both the input and output ends of the pump body are connected to conveying pipes. One end of each of the two conveying pipes is connected to the suction cover and the housing, respectively. A bottom plate is provided inside the housing, and the bottom plate is connected to the side of the processing table.

[0027] Compared with related technologies, the production method of T-shaped alloy profiles provided by this invention has the following beneficial effects:

[0028] This invention provides a method for producing T-shaped alloy profiles. The method uses a φ950 tandem 13-stand rolling mill to continuously roll the T-shaped profiles, replacing the traditional extrusion method. This makes the profiles less prone to breakage during processing, results in superior mechanical properties, and allows for full utilization of raw materials, greatly reducing material waste.

[0029] The production process is simple and controllable, and the finished product yield can reach over 90%. The continuous rolling mill operates fully automatically, eliminating the need for manual operation. This achieves the important conditions for low-cost and large-scale production, resulting in high production efficiency. It can also meet all performance indicators of key industries such as marine engineering equipment, navigation, and ships, thus effectively satisfying the market demand for profiles. Attached Figure Description

[0030] Figure 1 This is a schematic diagram of the structure of a first embodiment of a method for producing T-shaped alloy profiles provided by the present invention;

[0031] Figure 2 This is a schematic diagram of the structure of a second embodiment of a method for producing T-shaped alloy profiles provided by the present invention;

[0032] Figure 3 for Figure 2 A schematic diagram of the overall three-dimensional structure of the device shown;

[0033] Figure 4 for Figure 3 The enlarged schematic diagram of part A shown below;

[0034] Figure 5 for Figure 2 A three-dimensional structural diagram of the overall external structure of the device shown;

[0035] Figure 6 This is a structural schematic diagram of a third embodiment of a method for producing T-shaped alloy profiles provided by the present invention.

[0036] Numbered in the diagram: 1. Processing table

[0037] 2. Cutting device; 21. Rotating rod; 22. Cutting wheel; 23. Driving component.

[0038] 3. Filter screen

[0039] 4. Positioning device; 41. Fixing block; 42. Fixing rod; 43. Connecting frame; 44. Double-headed hydraulic telescopic rod; 45. Rectangular block; 46. Movable sleeve; 47. Push rod; 48. Positioning plate.

[0040] 5. Collection box,

[0041] 6. Disassembly components; 61. Disassembly plate; 62. Mounting block; 63. Mounting sleeve; 7. Suction assembly; 71. Mounting bracket; 72. Suction cover.

[0042] 7. Conveying device; 81. Box body; 82. Pump body; 83. Conveying pipe; 84. Base plate. Detailed Implementation

[0043] The present invention will be further described below with reference to the accompanying drawings and embodiments.

[0044] First Embodiment

[0045] Please refer to the following: Figure 1 ,in, Figure 1 This is a schematic diagram of the structure of a first embodiment of a method for producing a T-shaped alloy profile provided by the present invention. A method for producing a T-shaped alloy profile includes the following steps:

[0046] S1. Select a titanium alloy square billet as the billet and remove the surface oxide layer and impurities;

[0047] S2. The billet is heated to the rolling temperature and then continuously rolled into a symmetrical T-shaped profile using a φ950 tandem 13-stand rolling mill.

[0048] S3. Utilizing the residual heat of the material after hot rolling, the material is conveyed to the online tension straightener via roller conveyor for tension straightening, and then straightened a second time via a tension straightener.

[0049] S4. After the semi-finished material has cooled, the band saw cuts the material to the required length, and then uses water jet cutting to split it in the length direction to obtain several profiles.

[0050] S5. Use the inward stacking method of the flange plates to assemble the cut profiles;

[0051] S6. After the packaged profiles are assembled, they are subjected to stress-relieving annealing. After annealing, they are removed from the furnace and unpacked.

[0052] S7. Sandblasting to remove the oxide scale from the surface of the profile;

[0053] S8. Place the sandblasted profile into an acid bath for pickling and passivation. Pickle the surface until it turns silver-gray, then rinse it clean with water.

[0054] S9. Use an ultrasonic flaw detector to perform flaw detection. If the flaw detection is qualified, it is a finished product; if the flaw detection is unqualified, it is a scrap product. After flaw detection, the finished product is placed in a drying chamber for drying to obtain the T-shaped alloy profile finished product. In S2, the rolling mill is used to sequentially pass through the K13-K12-K11-K10-K9-K8-K7-K6-K5-K4-K3-K2-K1 passes. The rolling mill working speed is 1.2-1.5 m / s. The K13-K12-K11-K10-K9 passes are double-support symmetrical passes for billet opening. K8, K6, K4, and K2 are finished using a universal rolling mill, and K7, K5, K3, and K1 are edge-finished using a two-roll horizontal rolling mill.

[0055] In S2, the dimensions of K13 are 430×220mm, K12 is 420×200mm, K11 is 380×190mm, K10 is 350×180mm, K9 is 280×160mm, K8 is 220×150mm, K7 is 210×140mm, K6 is 205×130mm, K5 is 200×125mm, K4 is 200×120mm, K3 is 200×115mm, K2 is 200×105mm, and K1 is 200×100mm; among them, K13-K9 are the pre-forming holes for initial rolling, and K8-K1 are the finishing rolling holes.

[0056] In S5, the specific method of packaging is as follows: use 10 profiles to package, stack them facing each other, and tie the package with steel strips, with each bundle tied 5-8 times.

[0057] In S6, the annealing process is as follows: after the temperature of the annealing furnace rises to 550-750℃, annealing begins and is maintained at a constant temperature for 2-4 hours. After cooling in the furnace to 180-220℃, the furnace is removed from the furnace and the straightness is controlled to 2mm / m after unpacking.

[0058] In step S8, the acid solution used comprises the following components by weight percentage:

[0059] 15% nitric acid, 5% hydrofluoric acid, and the remainder is water;

[0060] The pickling soaking time is 10-30 minutes.

[0061] In S9, the flaw detection standard is Class A, the medium is water, and the drying temperature is 60-80℃.

[0062] In S1, the dimensions of the titanium alloy square billet are δ450×230×2000mm, and in S2, the dimensions of the rolled profile are 200×100×6000mm.

[0063] S1. Select a titanium alloy square billet of grade TA15 as the billet, with dimensions of δ450×230×2500mm, and remove the surface oxide layer and impurities.

[0064] S2. The selected billet is heated to 950℃ in a box-type electric furnace, and then continuously rolled in a 13-roll tandem rolling mill, passing through the K13-K12-K11-K10-K9-K8-K7-K6-K5-K4-K3-K2-K1 passes in sequence to form a 200×100×6000mm T-shaped alloy profile in one pass. The mill operating speed is 1.2 m / s. Among them, the K13-K12-K11-K10-K9 passes are double-support symmetrical passes for billet opening, K8, K6, K4, and K2 are finished by a universal mill, and K7, K5, K3, and K1 are edged by a two-roll horizontal mill. The universal rolling mill and the two-roll horizontal rolling mill are arranged in a longitudinal row to form a finishing rolling mill. The number of universal rolling mills and the number of two-roll horizontal rolling mills are 4. The universal rolling mill is designated as U and the two-roll horizontal rolling mill as E. The rolling mill arrangement is U-E-U-E-U-E-U-E.

[0065] Specifically, the billet used is a square billet of 450×230mm. The dimensions of K13 are 430×220mm, K12 are 4020×200mm, K11 are 380×190mm, K10 are 350×180mm, K9 are 280×160mm, K8 are 220×150mm, K7 are 210×140mm, K6 are 205×130mm, K5 are 200×125mm, K4 are 200×120mm, K3 are 200×115mm, K2 are 200×105mm, and K1 are 200×100mm.

[0066] S3. Utilizing the residual heat of the material after hot rolling, the equilateral material is conveyed to the online tension straightener via roller conveyor for tension straightening, and then straightened a second time via a tension straightener.

[0067] S4. After the semi-finished material has cooled, cut it into profiles with a length of 6 meters / piece; then use water jet cutting to split it in the length direction.

[0068] S5. Use the staggered stacking method to pack the cut profiles. The specific packing method is as follows: use 10 profiles to pack, stack them in staggered positions, and tie them with two δ30mm steel strips. Each bundle is tied with 5 knots, and each knot is 1 meter apart.

[0069] S6. After the packaged profiles are loaded into the annealing furnace, the temperature is raised to 750℃ and annealing begins. The temperature is maintained for 2 hours. After cooling to about 200℃ in the furnace, the material is taken out of the furnace and transported to the straightening machine. After straightening, the straightness can reach 2mm / m.

[0070] S7. Use a through-type sandblasting machine to sandblast and remove the surface oxide scale of the profile;

[0071] S8. Place the sandblasted profile into an acid bath for pickling and passivation. The acid solution ratio is 15% nitric acid, 5% hydrofluoric acid, and the remainder is water. Soak for about 15 minutes, pickle the surface until it turns silver-gray, and then rinse it clean with water.

[0072] S9. Use an ultrasonic flaw detector to perform flaw detection. The flaw detection standard is Class A, and the medium is water. If the flaw detection is qualified, it is a finished product; if the flaw detection is unqualified, it is a scrap product. After the flaw detection is completed, the finished product is placed in the drying room to dry, and T-shaped alloy profile finished product is obtained. The drying temperature is 60℃.

[0073] This invention employs a double-sided symmetrical die rolling method, which splits the material after rolling to obtain two T-shaped profiles simultaneously, thereby solving the problem of turtleback and sickle-shaped curves occurring during rolling.

[0074] The roll diameter ratio used in step S2 is shown in the table below:

[0075] Serial Number Road name upper roller diameter (mm) lower roller diameter (mm) Roller speed 1 K13 Φ1050 Φ950 Different hearts, same speed 2 K12 Φ1050 Φ950 Different hearts, same speed 3 K11 Φ1050 Φ950 Different hearts, same speed 4 K10 Φ950 Φ850 Different hearts, same speed 5 K9 Φ950 Φ850 Different hearts, same speed

[0076] The mechanical properties of the 200×100×6000mm T-shaped alloy profile prepared using the method of Example 1 are as follows:

[0077]

[0078] The profile dimensions and thickness tolerances meet ±0.1mm, the profile surface is glossy, free of cracks and inclusions, with uniform structure and no segregation, and ultrasonic testing meets the Class A standard.

[0079] Example 2

[0080] Please combine Figure 1 A method for producing a T-shaped alloy profile includes the following steps:

[0081] S1. Select a titanium alloy square billet of grade TC4 as the billet, with dimensions of 450×230×2500mm, and remove the surface oxide layer and impurities.

[0082] S2. The selected billet is heated to 1050℃ in a box-type electric furnace, and then continuously rolled using a φ950 tandem 13-stand rolling mill. The billet is opened using a double-support symmetrical pass pattern (K13-K12-K11-K10-K9). K8, K6, K4, and K2 are finished using a universal mill, while K7, K5, K3, and K1 are edge-finished using a two-roll horizontal mill. The universal mill and the two-roll horizontal mill are arranged in a tandem configuration to form the finishing mill. There are 4 stands for both the universal mill and the two-roll horizontal mill. The universal mill is designated as U, and the two-roll horizontal mill as E. The mill arrangement is U-E-U-E-U-E-U-E.

[0083] Specifically, the billet used is a square billet of 450×230mm. The dimensions of K13 are 430×220mm, K12 are 420×200mm, K11 are 380×190mm, K10 are 350×180mm, K9 are 280×160mm, K8 are 220×150mm, K7 are 210×140mm, K6 are 205×130mm, K5 are 200×125mm, K4 are 200×120mm, K3 are 200×115mm, K2 are 200×105mm, and K1 are 200×100mm.

[0084] S3. Utilizing the residual heat of the material after hot rolling, the material is conveyed to the online tension straightener via roller conveyor for tension straightening, and then straightened a second time via a tension straightener.

[0085] S4. After the semi-finished material has cooled, use a band saw to cut the blank into profiles with a length of 6 meters / piece; then use water jet cutting to divide the length into several profiles.

[0086] S5. Use the staggered stacking method to pack the cut profiles. The specific packing method is as follows: use 10 profiles to pack, stack them in staggered positions, and tie them with two δ30mm steel strips. Each bundle is tied with 5 knots, and each knot is 1 meter apart.

[0087] S6. After the packaged profiles are loaded into the annealing furnace, the temperature is raised to 750℃ and annealing begins. The temperature is kept constant for 2 hours. After cooling to about 200℃ in the furnace, the material is taken out of the furnace and conveyed to the straightening machine. After straightening, the straightness can reach 2mm / m.

[0088] S7. Use a through-type sandblasting machine to sandblast and remove the surface oxide scale of the profile;

[0089] S8. Place the sandblasted profile into an acid bath for pickling and passivation. The acid solution ratio is 15% nitric acid, 5% hydrofluoric acid, and the remainder is water. Soak for about 15 minutes, pickle the surface until it turns silver-gray, and then rinse it clean with water.

[0090] S9. Use an ultrasonic flaw detector to perform flaw detection. The flaw detection standard is Class A, and the medium is water. If the flaw detection is qualified, it is a finished product; if the flaw detection is unqualified, it is a scrap product. After the flaw detection is completed, the finished product is placed in the drying room to dry, and T-shaped alloy profile finished product is obtained. The drying temperature is 80℃.

[0091] This invention employs a double-sided symmetrical die rolling method. After rolling, the material is split in half to obtain two T-shaped profiles, thereby solving the problem of turtle back and sickle-shaped bends occurring during rolling.

[0092] The roll diameter ratio used in step S2 is shown in the table below:

[0093]

[0094]

[0095] The mechanical properties of the 200×100×6000mm T-shaped alloy profile prepared using the method of Example 2 are as follows:

[0096]

[0097] The profile dimensions and thickness tolerances meet ±0.1mm, the profile surface is glossy, free of cracks and inclusions, with uniform structure and no segregation, and ultrasonic testing meets the Class A standard.

[0098] Compared with related technologies, the production method of T-shaped alloy profiles provided by this invention has the following beneficial effects:

[0099] This invention provides a method for producing T-shaped alloy profiles. The method uses a φ950 tandem 13-stand rolling mill to continuously roll the T-shaped profiles, replacing the traditional extrusion method. This makes the profiles less prone to breakage during processing, results in superior mechanical properties, and allows for full utilization of raw materials, greatly reducing material waste.

[0100] The production process is simple and controllable, and the finished product yield can reach over 90%. The continuous rolling mill operates fully automatically, eliminating the need for manual operation. This achieves the important conditions for low-cost and large-scale production, resulting in high production efficiency. It can also meet all performance indicators of key industries such as marine engineering equipment, navigation, and ships, thus effectively satisfying the market demand for profiles.

[0101] Second Embodiment

[0102] Please refer to the following: Figure 2 , Figure 3 , Figure 4 and Figure 5 Based on the first embodiment of this application providing a method for producing T-shaped alloy profiles, the second embodiment of this application proposes another method for producing T-shaped alloy profiles. The second embodiment is merely a preferred embodiment of the first embodiment, and the implementation of the second embodiment will not affect the separate implementation of the first embodiment.

[0103] Specifically, the difference in the production method of a T-shaped alloy profile provided in the second embodiment of this application lies in that, in the production method of the T-shaped alloy profile, a processing device is used when processing the T-shaped profile in step S4. The processing device includes a processing table 1, and a cutting device 2 is provided inside the processing table 1. The cutting device 2 includes a rotating rod 21, and a cutting wheel 22 is provided at the center of the surface of the rotating rod 21. A driving member 23 is provided on one side of the rotating rod 21. Filter screens 3 are provided on the surface of the processing table 1 and on both sides of the cutting wheel 22. A positioning device 4 is provided on the side of the processing table 1. The positioning device 4 includes four fixing blocks 41, which are arranged in groups of two, and a fixing rod connects the two groups of fixing blocks 41. 42. A connecting frame 43 is provided at the center of the surface of the fixed rod 42. A double-headed hydraulic telescopic rod 44 is provided inside the connecting frame 43. A rectangular block 45 is connected to both ends of the double-headed hydraulic telescopic rod 44. A movable sleeve 46 is connected to one end of the rectangular block 45. The movable sleeve 46 is fitted onto the surface of the fixed rod 42. A push rod 47 is connected to one side of the rectangular block 45. A positioning plate 48 is connected to one end of the push rod 47. A collection box 5 is provided inside the processing table 1. A disassembly assembly 6 is provided at one end of the processing table 1. The disassembly assembly 6 includes a disassembly plate 61. Mounting blocks 62 are connected to both sides of the disassembly plate 61. Mounting sleeves 63 are fitted onto the surface of the mounting blocks 62. The mounting sleeves 63 are connected to the side of the processing table 1.

[0104] The drive unit 23 consists of a motor, two pulleys and a belt. The two ends of the rotating rod 21 are rotatably connected to the left and right sides of the inner wall of the processing table 1 through the rotating shaft. A rectangular through groove adapted to the cutting wheel 23 is opened at the center of the surface of the processing table 1 to facilitate the rotation of the cutting wheel 23. Two sets of fixing blocks 41 are connected to the left and right sides of the two ends of the processing table 1. The use of the connecting frame 43 can divide the fixing rod 42 evenly, and also facilitates the installation of the double-headed hydraulic telescopic rod 44. The use of the filter screen 3 facilitates the collection of debris generated during cutting into the collection box 5 for centralized treatment.

[0105] The working principle of the T-shaped alloy profile production method provided by this invention is as follows:

[0106] In use, the entire T-shaped alloy profile is first placed on the surface of the processing table 1. Then, the double-headed hydraulic telescopic rod 44 is activated to drive the push rods 47 at both ends to move. When the push rods 47 move, the positioning plate 48 moves on the surface of the processing table 1. When the double-headed hydraulic telescopic rod 44 moves, the movable sleeve 46 moves on the surface of the fixed rod 42 through the rectangular block 45. When the positioning plate 48 moves to contact and fix with both sides of the T-shaped alloy profile on the surface of the processing table 1, the operation of the double-headed hydraulic telescopic rod 44 is stopped. Then, the rotating rod 21 with the cutting wheel 23 is driven to rotate through the driving component 23. When the rotating rod 21 drives the cutting wheel 23 to rotate, the T-shaped alloy profile can be moved on the surface of the processing table 1 to cut the entire T-shaped alloy profile in half.

[0107] Compared with related technologies, the production method of T-shaped alloy profiles provided by this invention has the following beneficial effects:

[0108] This invention provides a method for producing T-shaped alloy profiles. A cutting device 2 is set at the center of the processing table 1 to work with a positioning device 4. This facilitates the production of multiple T-shaped alloy profiles by cutting the produced T-shaped alloy profiles after processing.

[0109] Third Embodiment

[0110] Please refer to the following: Figure 6 Based on the first embodiment of this application providing a method for producing T-shaped alloy profiles, the third embodiment of this application proposes another method for producing T-shaped alloy profiles. The third embodiment is merely a preferred embodiment of the first embodiment, and the implementation of the third embodiment will not affect the separate implementation of the first embodiment.

[0111] Specifically, the difference in the production method of a T-shaped alloy profile provided in the third embodiment of this application is that, in the production method of a T-shaped alloy profile, a suction assembly 7 is provided above the processing table 1, the suction assembly 7 includes a mounting frame 71, one end of the mounting frame 71 is connected to a suction cover 72, a conveying device 8 is provided on one side of the processing table 1, the conveying device 8 includes a housing 81, a pump body 82 is installed on the top of the housing 81, the input end and the output end of the pump body 82 are both connected to conveying pipes 83, one end of the two conveying pipes 83 is respectively connected to the suction cover 72 and the housing 81, and a bottom plate 84 is provided inside the housing 81, the bottom plate 84 is connected to the side of the processing table 1.

[0112] Mounting bracket 71 is connected to the side of processing table 1.

[0113] The working principle of the T-shaped alloy profile production method provided by this invention is as follows:

[0114] When the cutting device 2 generates dust and fumes while cutting the T-shaped alloy profile, the pump body 82 is activated to transport the external dust and fumes into the interior of the housing 81 through two conveying pipes 83 and the suction hood 72.

[0115] Compared with related technologies, the production method of T-shaped alloy profiles provided by this invention has the following beneficial effects:

[0116] This invention provides a method for producing T-shaped alloy profiles. A suction assembly 7 is provided above the processing table 1 in conjunction with a conveying device 8 to facilitate the collection of dust and fumes generated when the cutting device 2 cuts the T-shaped alloy profiles.

[0117] The above description is merely an embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent structural or procedural transformations made based on the content of the present invention specification and drawings, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of the present invention.

Claims

1. A method for producing a T-shaped alloy profile, characterized in that, Includes the following steps: S1. Select a titanium alloy square billet as the billet and remove the surface oxide layer and impurities; S2. The billet is heated to the rolling temperature and then continuously rolled into a symmetrical T-shaped profile using a φ950 tandem 13-stand rolling mill. S3. Utilizing the residual heat of the material after hot rolling, the material is conveyed to an online tension straightener via roller conveyor for tension straightening; then it is straightened a second time via a tension straightener. S4. After the semi-finished material has cooled, the band saw is used to cut the material to the specified length. Then, the length is split in half using water cutting or mechanical cutting to obtain several profiles; S5. Use the inward stacking method of the flange plates to assemble the cut profiles; S6. After the packaged profiles are assembled, they are subjected to stress-relieving annealing. After annealing, they are removed from the furnace and unpacked. S7. Sandblasting to remove the oxide scale from the surface of the profile; S8. Place the sandblasted profile into an acid bath for pickling and passivation. Pickle the surface until it turns silver-gray, then rinse it clean with water. S9. Use an ultrasonic flaw detector to perform flaw detection. Products that pass the flaw detection are considered finished products; those that fail are considered scrap. After flaw detection, the finished products are placed in a drying chamber to dry, obtaining the T-shaped alloy profile. In S2, a rolling mill is used to sequentially pass through passes K13-K12-K11-K10-K9-K8-K7-K6-K5-K4-K3-K2-K1. The rolling mill operating speed is 1.2-1.5 m / s. Passes K13-K12-K11-K10-K9 are double-sided symmetrical passes. Passes K8, K6, K4, and K2 are rolled using a universal finishing mill. K7, K5, K3, and K1 are edge-finished using a two-roll horizontal mill; in S2, K13 has dimensions of 430×220mm, K12 has dimensions of 420×200mm, K11 has dimensions of 380×190mm, K10 has dimensions of 350×180mm, K9 has dimensions of 280×160mm, K8 has dimensions of 220×150mm, K7 has dimensions of 210×140mm, K6 has dimensions of 205×130mm, K5 has dimensions of 200×125mm, K4 has dimensions of 200×120mm, K3 has dimensions of 200×115mm, K2 has dimensions of 200×105mm, and K1 has dimensions of 200×100mm; among them, K13-K9 are pre-forming holes for initial rolling, and K8-K1 are forming holes for finishing rolling.

2. The method for producing T-shaped alloy profiles according to claim 1, characterized in that, In S5, the specific method of packaging is as follows: use 10 profiles to package, stack them facing each other, and tie the package with steel strips, with each bundle tied 5-8 times.

3. The method for producing T-shaped alloy profiles according to claim 1, characterized in that, In S6, the annealing process is as follows: after the temperature of the annealing furnace rises to 550-750℃, annealing begins and is maintained at a constant temperature for 2-4 hours. After cooling in the furnace to 180-220℃, the furnace is removed from the furnace. After unpacking, the straightness is controlled to 2mm / m.

4. The method for producing T-shaped alloy profiles according to claim 1, characterized in that, In step S8, the acid solution used comprises the following components by weight percentage: 15% nitric acid, 5% hydrofluoric acid, and the remainder is water; The pickling soaking time is 10-30 minutes.

5. The method for producing T-shaped alloy profiles according to claim 1, characterized in that, In S9, the flaw detection standard is Class A, the medium is water, and the drying temperature is 60-80℃.

6. The method for producing T-shaped alloy profiles according to claim 1, characterized in that, In S1, the dimensions of the titanium alloy square billet are 450×230×2000mm, and in S2, the dimensions of the rolled profile are 200×100×6000mm.

7. The method for producing T-shaped alloy profiles according to claim 1, characterized in that, In step S4, a processing device is used when processing the T-shaped profile. This processing device includes a processing table, inside which a cutting device is installed. The cutting device includes a rotating rod, with a cutting wheel positioned at the center of the rotating rod's surface. A driving component is located on one side of the rotating rod. Filter screens are installed on the surface of the processing table and on both sides of the cutting wheel. A positioning device is installed on the side of the processing table, comprising four fixing blocks. The four fixing blocks are grouped in pairs, and a fixing rod connects the two groups of fixing blocks. A cutting wheel is positioned at the center of the surface of the fixing rod. The system includes a connecting frame with a double-headed hydraulic telescopic rod inside. Rectangular blocks are connected to both ends of the double-headed hydraulic telescopic rod. A movable sleeve is connected to one end of each rectangular block and fits onto the surface of a fixed rod. A push rod is connected to one side of each rectangular block, and a positioning plate is connected to one end of the push rod. A collection box is installed inside the processing table, and a disassembly assembly is installed at one end of the processing table. The disassembly assembly includes a disassembly plate, and mounting blocks are connected to both sides of the disassembly plate. Mounting sleeves are fitted onto the surfaces of the mounting blocks and connect to the sides of the processing table.

8. The method for producing T-shaped alloy profiles according to claim 7, characterized in that, A suction assembly is provided above the processing table. The suction assembly includes a mounting frame, one end of which is connected to a suction hood. A conveying device is provided on one side of the processing table. The conveying device includes a housing, and a pump body is installed on the top of the housing. Both the input and output ends of the pump body are connected to conveying pipes. One end of each of the two conveying pipes is connected to the suction hood and the housing, respectively. A bottom plate is provided inside the housing, and the bottom plate is connected to the side of the processing table.

Citation Information

Patent Citations

  • Preparation method of zirconium or zirconium alloy extruded and rolled thin-wall profile

    CN112708790A

  • Method for producing industrial pure titanium wire rod on high-speed wire rod production line

    CN116000085A