A metal pipe inner wall reinforcing device and application thereof
The pulsed current treatment of the metal pipe inner wall strengthening device solves the problems of low efficiency and high energy consumption in the traditional method for processing large-size or irregularly shaped pipes. It achieves simultaneous improvement in wear resistance and corrosion resistance of the inner and outer walls of metal pipes, as well as increased strength and plasticity, significantly shortening processing time and reducing costs.
Patent Information
- Application Number
- CN202411625295.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-14
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-11-14
AI Technical Summary
Existing technologies make it difficult to apply a thick (greater than 0.5 mm) wear-resistant coating to the inner wall of metal pipes at low cost, and it is also difficult to simultaneously improve the wear resistance and corrosion resistance of the inner and outer walls of the pipes. Traditional heat treatment and laser surface treatment methods are inefficient, energy-intensive, and have limited effects on large-size or irregularly shaped pipes.
The device for strengthening the inner wall of metal pipes uses a combination of a displacement control system, a right electrode control system, a stage, a left electrode, a main control device, a main unit and power distribution system, a right electrode, a load control system, an insulation device and a four-jaw chuck to achieve step-by-step, continuous linear or continuous spiral pulse current processing. Combined with the processing methods of different materials, the microstructure of the inner wall of the metal pipe can be controlled.
It achieves simultaneous improvement in wear resistance and corrosion resistance of the inner and outer walls of metal pipes, enhances strength and plasticity, and improves processing efficiency and energy utilization. It breaks through the traditional method to process large-size or irregularly shaped pipes, significantly shortens processing time and reduces costs.
Smart Images

Figure CN119282289B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of pipe processing, and more specifically to a device for strengthening the inner wall of metal pipes and its application. Background Technology
[0002] Metal tubing has wide applications in construction, petrochemicals, energy, and aerospace. According to the requirements of these applications, the tubing needs to possess excellent wear resistance, corrosion resistance, and high strength and toughness. To improve its overall performance, traditional heat treatment, laser surface treatment, and shot peening are commonly used methods. However, these methods are limited by the process and are prone to a series of problems in actual production. Traditional heat treatment can regulate the microstructure of metal materials and improve their properties. However, in practical applications, large-size or irregularly shaped metal tubing requires heat treatment furnaces that are difficult to obtain, making it difficult to process large-size or irregularly shaped metal tubing. Furthermore, heating metal tubing requires long times, consumes a lot of energy, has low energy utilization, and suffers from poor atmosphere protection, making the material prone to oxidation. Meanwhile, during prolonged heat treatment of large-sized metal tubes, the surface area experiences a higher temperature than the core, leading to surface coarsening. The uneven heating temperatures between the surface and core result in inhomogeneities in the microstructure within and outside the tube. Therefore, traditional heat treatment methods struggle to achieve excellent comprehensive mechanical properties in large-sized or irregularly structured metal tubes. Surface treatments such as laser surface heating and shot peening can regulate the surface microstructure and improve surface hardness, corrosion resistance, and wear resistance. However, due to equipment limitations, these methods can only treat tubes with wall thicknesses less than 0.5 mm and can only treat the outer surface of metal tubes, failing to strengthen the inner wall of thick-walled tubes. Therefore, their ability to enhance the comprehensive mechanical properties of thick-walled metal tubes is very limited. Furthermore, existing technologies struggle to cost-effectively clad the inner wall of metal tubes with a thicker (greater than 0.5 mm) wear-resistant coating and significantly improve the wear resistance of both the inner and outer walls. Therefore, how to avoid the influence of pipe size, thick-walled pipes or irregular shapes during the processing of metal pipes, improve processing efficiency, reduce processing costs, and simultaneously achieve rapid and uniform heating of the pipe surface and core, control microstructure, simultaneously strengthen the inner and outer walls of the pipe, improve the wear resistance and corrosion resistance of the inner and outer walls of the pipe, and simultaneously improve the strength and plasticity of the pipe are the technical problems that urgently need to be solved. Summary of the Invention
[0003] To solve the above-mentioned technical problems, the present invention provides a metal pipe inner wall strengthening device, which includes: a displacement control system 1, a right electrode control system 2, a stage 3, a left electrode 4, a central control device 5, a main unit and power distribution system 6, a right electrode 7, a load control system 8, an insulation device 9, a four-jaw chuck 10, and a right electrode rod 11.
[0004] The displacement control system 1 is located at the bottom of the metal pipe inner wall strengthening device. The right electrode control system 2 and the platform 3 are fixed to the upper right and upper left of the displacement control system 1, respectively. The displacement control system 1 can adjust the distance between the right electrode control system 2 and the platform 3. The platform 3 is used to place the metal pipe to be processed. The left electrode 4 is located at the upper left of the platform 3 and on the left side of the metal pipe to be processed. The left electrode 4 can fit against the outer surface of the left end of the metal pipe to be processed. The main control device 5 is located behind the displacement control system 1. The main unit and power distribution system 6 are located behind the main control device 5. The four-jaw chuck 10 is located on the platform. The four-jaw chuck 10 is fixed to the left surface of the right electrode control system 2, located on the upper right side of platform 3 and the right side of the metal tube to be processed. The four-jaw chuck 10 can both clamp the metal tube and allow it to rotate along its central axis. The right electrode control system 2 and the four-jaw chuck 10 have concentric circular holes extending through them. The right electrode rod 11 is connected through these concentric circular holes and is located on the right side of the metal tube to be processed. The load control system 8 is fixed to the left end of the right electrode rod 11 and can move synchronously with it. The right electrode 7 is fixed below the load control system 8. The right electrode 7 is a copper wheel or copper ball. The insulating device 9 is fixed above the load control system 8. The insulating device 9 is an insulating wheel or insulating ball. The centers of the right electrode 7 and the insulating device 9 are on the same vertical line. The right electrode 7 and the insulating device 9 can rotate. The right electrode control system 2 can control the right electrode rod 11 to move left and right. The right electrode rod 11 can extend into the metal pipe. The load control system 8, the right electrode 7, and the insulating device 9 can simultaneously extend into the metal pipe to be processed under the drive of the right electrode rod 11. The load control system 8 can simultaneously apply pressure to the lower right electrode 7 and the upper insulating device 9. Under vertical stress, the right electrode 7 and the insulating device 9 can tightly adhere to the lower and upper surfaces of the inner wall of the metal tube when the load control system 8 applies vertical stress. While the right electrode control system 2 drives the right electrode rod 11 and the load control system 8 to move left and right, the right electrode 7 and the insulating device 9 can roll left and right relative to the inner wall of the metal tube to be treated. The main control device 5 can control the left electrode 4 to move to the right and adhere to the outer surface of the left end of the metal tube to be treated. The left electrode 4, together with the metal tube to be treated on the stage 3 and the right electrode 7, can form a pulse current loop. The main unit and power distribution system 6 can generate pulse current and control the pulse current parameters.The functions of the central control device 5 include: regulating the movement of the right electrode rod 11 by the right electrode control system 2, thereby driving the right electrode 7, load control system 8, and insulation device 9 to move to the left and regulating the speed of leftward movement; controlling the opening or unloading of the load control system 8; controlling the four-jaw chuck 10 to clamp and drive the metal pipe to be processed to rotate along the central axis and its rotation speed; and controlling the right electrode 7, insulation device 9, and load control system 8 to process the inner wall of the metal pipe to be processed.
[0005] The present invention also provides an application of a metal pipe inner wall strengthening device in the field of metal pipe processing, the application of which includes step-type, continuous linear or continuous spiral processing methods.
[0006] Furthermore, the step-by-step machining method is as follows:
[0007] (1) Activate the metal pipe inner wall strengthening device, turn on the main control device 5 and the main unit and power distribution system 6, place the metal pipe to be treated horizontally on the stage 3, insert the right electrode 7, load control system 8 and insulation device 9 into the metal pipe to be treated, clamp the metal pipe to be treated with the four-jaw chuck 10, and make the outer surface of the left end of the pipe fit with the left electrode 4. Apply a force of 0.5-2500N to make the right electrode 7 fit with the lower surface of the inner wall of the metal pipe and the insulation device 9 fit with the upper surface of the inner wall of the metal pipe. After the first pulse current treatment of the metal pipe, unload the load control device. The system 8 is then used to move the right electrode rod 11 to the left, causing the right electrode 7, the load control system 8, and the insulation device 9 to move 1-40mm to the left inside the metal tube. The load control system 8 is then activated, applying a force of 0.5-2500N to make the right electrode 7 adhere to the lower surface of the inner wall of the metal tube and the insulation device 9 adhere to the upper surface of the inner wall of the metal tube. After the metal tube is subjected to a second pulse current treatment, the load control system 8 is unloaded. The process is repeated in the aforementioned cycle until the first inner wall surface of the entire length of the metal tube is completed, resulting in the step-processed metal tube 1.
[0008] (2) Using the four-jaw chuck 10 to drive the step-processed metal pipe 1 obtained in step (1) to rotate 5-90° along the central axis, the metal pipe 1 is processed according to the process and process parameters in step (1) until the second inner wall surface of the entire length of the metal pipe to be processed is completed, and then the step-processed metal pipe 2 is obtained.
[0009] (3) The metal pipe 2 is processed in 2-70 cycles according to the processing method in step (2) to complete the processing of the entire inner wall of the metal pipe and finally obtain the step-reinforced metal pipe.
[0010] The pulse current processing in step (1) is as follows: the current magnitude is 0.1-40kA, the voltage magnitude is 1-220V, the frequency is 5-1000Hz, and the processing time is 0.01-20s.
[0011] Furthermore, the continuous linear processing method is as follows:
[0012] (1) Turn on the metal pipe inner wall strengthening device, turn on the main control device 5 and the host and power distribution system 6, place the metal pipe to be processed horizontally on the stage 3, insert the right electrode 7, load control system 8 and insulation device 9 into the metal pipe to be processed, clamp the metal pipe to be processed with the four-jaw chuck 10, the outer surface of the left end of the pipe is in contact with the left electrode 4, the load control system 8 applies a force of 10-2000N to make the right electrode 7 in contact with the lower surface of the inner wall of the metal pipe, and the insulation device 9 in contact with the upper surface of the inner wall of the metal pipe. Then, the right electrode rod 11 drives the right electrode 7, load control system 8 and insulation device 9 to move to the left end of the metal pipe to be processed at a speed of 0.5-50mm / s, and pulse current processing is performed on the metal pipe at the same time. Then unload the load control system 8, and after completing the first inner wall surface of the entire length of the metal pipe to be processed, a continuous linear processed metal pipe 1 is obtained.
[0013] (2) Using the four-jaw chuck 10 to drive the continuous linear processed metal pipe 1 obtained in step (1) to rotate 10-60° along the central axis, the metal pipe 1 is processed according to the process and process parameters in step (1), and the second inner wall surface of the entire length of the metal pipe to be processed is completed to obtain the continuous linear processed metal pipe 2.
[0014] (3) The continuous straight-line processed metal pipe 2 is processed 4-34 times according to the processing method in step (2) to complete the processing of the entire inner wall of the metal pipe and finally obtain the continuous straight-line reinforced metal pipe.
[0015] The pulse current processing in step (1) is as follows: the current magnitude is 0.01-80kA, the voltage magnitude is 0.5-380V, the frequency is 2-2000Hz, and the processing time is 0.5-4000s.
[0016] Furthermore, the continuous linear processing method is as follows:
[0017] (1) Turn on the metal pipe inner wall strengthening device, turn on the main control device 5 and the host and power distribution system 6, place the metal pipe to be processed horizontally on the stage 3, and evenly spread the coating material 0.1-10mm thick on the lower surface of the inner wall of the metal pipe. Insert the right electrode 7, load control system 8 and insulation device 9 into the metal pipe to be processed, clamp the metal pipe to be processed with the four-jaw chuck 10, and the outer surface of the left end of the pipe is in contact with the left electrode 4. The load control system 8 applies a force of 10-2000N to make the right electrode 7 adhere to the lower surface of the inner wall of the metal pipe and the insulation device 9 adhere to the upper surface of the inner wall of the metal pipe. Then, the right electrode rod 11 drives the right electrode 7, load control system 8 and insulation device 9 to move to the left end of the metal pipe to be processed at a speed of 0.5-50mm / s, and simultaneously performs pulse current processing on the metal pipe. Then unload the load control system 8. After completing the first inner wall surface of the entire length of the metal pipe to be processed, a continuous linear processed metal pipe 1 is obtained.
[0018] (2) Using the four-jaw chuck 10 to drive the continuous linear processed metal pipe 1 obtained in step (1) to rotate 10-60° along the central axis, the metal pipe 1 is processed according to the process and process parameters in step (1), and the second inner wall surface of the entire length of the metal pipe to be processed is completed to obtain the continuous linear processed metal pipe 2.
[0019] (3) The continuous straight-line processed metal pipe 2 is processed 4-34 times according to the processing method in step (2) to complete the processing of the entire inner wall of the metal pipe and finally obtain the continuous straight-line reinforced metal pipe.
[0020] The pulse current processing in step (1) is as follows: the current magnitude is 0.01-80kA, the voltage magnitude is 0.5-380V, the frequency is 2-2000Hz, and the processing time is 0.5-4000s;
[0021] The coating material mentioned in step (1) is one of silicon carbide powder, titanium carbide powder, titanium nitride powder, tungsten nitride powder or tungsten carbide powder.
[0022] Furthermore, the continuous spiral processing method is as follows:
[0023] Activate the metal pipe inner wall strengthening device, turn on the main control device 5 and the main unit and power distribution system 6, place the metal pipe to be treated horizontally on the stage 3, insert the right electrode 7, load control system 8 and insulation device 9 into the metal pipe, clamp the metal pipe with the four-jaw chuck 10, with the outer surface of the left end of the pipe in contact with the left electrode 4, apply a force of 5-3000N to make the right electrode 7 contact the lower surface of the inner wall of the metal pipe, and the insulation device 9 contact the upper surface of the inner wall of the metal pipe, while the four-jaw chuck 10 drives the metal pipe to rotate along the central axis at a speed of 1-60° / s, and at the same time, the right electrode rod 11 drives the right electrode 7 and the load control system 8 to rotate at a speed of 0.1-40mm / s. System 8 and insulation device 9 move to the left end of the metal tube to be processed and perform pulse current treatment on the metal tube to obtain a continuously spiral reinforced metal tube. That is, the right electrode 7, load control device 8 and insulation device 9 move spirally to the left relative to the inner wall of the metal tube while performing pulse current treatment on the metal tube. The continuous spiral processing method is to perform pulse current treatment in a spiral curve with different density in the length direction of the inner wall of the metal tube to achieve reinforcement of the entire inner wall surface of the metal tube. The pulse current treatment is as follows: current magnitude is 0.05-60kA, voltage magnitude is 2-220V, frequency is 10-1500Hz, and processing time is 1-5000s.
[0024] Furthermore, the metal pipe is one of the following: TC4 pipe, TB8 pipe, TC17 pipe, TA0 pipe, TA16 pipe, TA18 pipe, AISI420 stainless steel pipe, AISI430 stainless steel pipe, 35CrMo steel pipe, QT500-7 ductile iron pipe, or QT600-3 ductile iron pipe. Attached Figure Description
[0025] Figure 1 A schematic diagram of the overall device for strengthening the inner wall of metal pipes;
[0026] Figure 2 An optical microscope image of the microstructure of TC4 tubing obtained in Example 1;
[0027] Figure 3 This is a scanning electron microscope image of the microstructure of TC17 pipe obtained in Example 2;
[0028] Figure 4 The image shows the backscattered electron band contrast diagram of the microstructure of the AISI420 stainless steel pipe obtained in Example 3. Detailed Implementation
[0029] The technical solution of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0030] A metal pipe inner wall strengthening device includes: a displacement control system 1, a right electrode control system 2, a stage 3, a left electrode 4, a central control device 5, a main unit and power distribution system 6, a right electrode 7, a load control system 8, an insulation device 9, a four-jaw chuck 10, and a right electrode rod 11.
[0031] The displacement control system 1 is located at the bottom of the metal pipe inner wall strengthening device. The right electrode control system 2 and the platform 3 are fixed to the upper right and upper left of the displacement control system 1, respectively. The displacement control system 1 can adjust the distance between the right electrode control system 2 and the platform 3. The platform 3 is used to place the metal pipe to be processed. The left electrode 4 is located at the upper left of the platform 3 and on the left side of the metal pipe to be processed. The left electrode 4 can fit against the outer surface of the left end of the metal pipe to be processed. The main control device 5 is located behind the displacement control system 1. The main unit and power distribution system 6 are located behind the main control device 5. The four-jaw chuck 10 is located on the platform. The four-jaw chuck 10 is fixed to the left surface of the right electrode control system 2, located on the upper right side of platform 3 and the right side of the metal tube to be processed. The four-jaw chuck 10 can both clamp the metal tube and allow it to rotate along its central axis. The right electrode control system 2 and the four-jaw chuck 10 have concentric circular holes extending through them. The right electrode rod 11 is connected through these concentric circular holes and is located on the right side of the metal tube to be processed. The load control system 8 is fixed to the left end of the right electrode rod 11 and can move synchronously with it. The right electrode 7 is fixed below the load control system 8. The right electrode 7 is a copper wheel or copper ball. The insulating device 9 is fixed above the load control system 8. The insulating device 9 is an insulating wheel or insulating ball. The centers of the right electrode 7 and the insulating device 9 are on the same vertical line. The right electrode 7 and the insulating device 9 can rotate. The right electrode control system 2 can control the right electrode rod 11 to move left and right. The right electrode rod 11 can extend into the metal pipe. The load control system 8, the right electrode 7, and the insulating device 9 can simultaneously extend into the metal pipe to be processed under the drive of the right electrode rod 11. The load control system 8 can simultaneously apply pressure to the lower right electrode 7 and the upper insulating device 9. Under vertical stress, the right electrode 7 and the insulating device 9 can tightly adhere to the lower and upper surfaces of the inner wall of the metal tube when the load control system 8 applies vertical stress. While the right electrode control system 2 drives the right electrode rod 11 and the load control system 8 to move left and right, the right electrode 7 and the insulating device 9 can roll left and right relative to the inner wall of the metal tube to be treated. The main control device 5 can control the left electrode 4 to move to the right and adhere to the outer surface of the left end of the metal tube to be treated. The left electrode 4, together with the metal tube to be treated on the stage 3 and the right electrode 7, can form a pulse current loop. The main unit and power distribution system 6 can generate pulse current and control the pulse current parameters.The functions of the central control device 5 include: regulating the movement of the right electrode rod 11 by the right electrode control system 2, thereby driving the right electrode 7, load control system 8, and insulation device 9 to move to the left and regulating the speed of leftward movement; controlling the opening or unloading of the load control system 8; controlling the four-jaw chuck 10 to clamp and drive the metal pipe to be processed to rotate along the central axis and its rotation speed; and setting the processing method of the inner wall of the metal pipe to be processed by the right electrode 7, insulation device 9, and load control system 8, wherein the processing method includes step-by-step, continuous linear, or continuous spiral processing methods.
[0032] Example 1
[0033] (1) Activate the metal pipe inner wall strengthening device, turn on the main control device 5 and the main unit and power distribution system 6, place the 400mm long TC4 pipe horizontally on the stage 3, insert the right electrode 7, load control system 8 and insulation device 9 into the TC4 pipe, clamp the TC4 pipe with the four-jaw chuck 10, and make the outer surface of the left end of the pipe fit against the left electrode 4. Set the processing mode to step processing mode, apply a force of 100N to make the right electrode 7 fit against the lower surface of the inner wall of the TC4 pipe, and the insulation device 9 fit against the upper surface of the inner wall of the TC4 pipe, and perform the first pulse current treatment on the TC4 pipe. Then, the load control system 8 is unloaded, and the right electrode rod 11 is moved to the left to drive the right electrode 7, the load control system 8 and the insulation device 9 to move 10mm to the left inside the TC4 pipe. The load control system 8 is activated and applies a force of 100N to make the right electrode 7 adhere to the lower surface of the inner wall of the TC4 pipe and the insulation device 9 adhere to the upper surface of the inner wall of the TC4 pipe. The TC4 pipe is then subjected to a second pulse current treatment and the load control system 8 is unloaded. The above-mentioned cyclic processing is repeated until the first inner wall surface strengthening of the entire length (400mm) of the TC4 pipe is completed to obtain the TC4 pipe 1.
[0034] (2) After the TC4 pipe 1 obtained in step (1) is rotated 15° along the central axis by the four-jaw chuck 10, the TC4 pipe 1 is processed according to the process and process parameters in step (1) until the second inner wall surface of the full length (400mm) of the TC4 pipe 1 is completed to obtain the TC4 pipe 2.
[0035] (3) After processing the TC4 pipe 2 in step (2) for 22 cycles, the processing of the entire inner wall of the metal pipe is completed, and the reinforced TC4 pipe is finally obtained.
[0036] The pulse current processing in step (1) is as follows: the current is 3kA, the voltage is 6V, the frequency is 200Hz, and the processing time is 1s.
[0037] Before processing, the microstructure of the TC4 pipe was an equiaxed α+α' bimorphic structure, with a tensile strength of 970 MPa and an elongation of 11.9%. After conventional heat treatment (950℃ for 2 hours), the microstructure of the TC4 pipe became a lath α+α' basketweave structure, which was coarser, with a tensile strength of 1025 MPa and an elongation of 10.0%. The reinforced TC4 pipe obtained in Example 1 had 960 reinforcing units on its inner wall. Within the reinforcing units, the α+α' bimorphic structure transformed into a refined α' full martensite structure, while retaining a large number of dislocations, resulting in a simultaneous improvement in the strength and plasticity of the pipe. The tensile strength of the reinforced TC4 pipe was 1210 MPa, and the elongation was 15.5%. As shown in Table 1, compared with the TC4 pipe before processing, the tensile strength of the TC4 pipe after heat treatment increased by 55 MPa, while the plasticity decreased by 1.9%. The reinforced TC4 pipe obtained in Example 1, however, showed a 240 MPa increase in tensile strength and a 3.6% increase in plasticity, breaking through the technical bottleneck of simultaneously improving the strength and plasticity of metal pipes. This device overcomes the limitation of existing technologies that can only perform shallow treatment on the outer surface of metal pipes; the treatment depth of this method can reach 10 mm. Simultaneously, the TC4 pipe treated by this device exhibits a refined α' full martensite structure and a large number of dislocations, resulting in a simultaneous improvement in the strength and plasticity of the pipe, as well as enhancing the wear resistance and corrosion resistance of the inner and outer walls. Table 1: Mechanical Properties of TC4 Pipe, Heat-Treated TC4 Pipe, and Reinforced TC4 Pipe Obtained in Example 1
[0038] Processing status tensile strength elongation TC4 pipe before processing 970 11.9% TC4 pipes after heat treatment 1025 10.0% Reinforced TC4 pipes 1210 15.5%
[0039] Example 2
[0040] (1) Activate the metal pipe inner wall strengthening device, turn on the main control device 5 and the main unit and power distribution system 6, place the 500mm long TC17 pipe horizontally on the stage 3, insert the right electrode 7, load control system 8 and insulation device 9 into the TC17 pipe, clamp the TC17 pipe with the four-jaw chuck 10, and make the outer surface of the left end of the pipe fit against the left electrode 4. Apply a force of 50N to make the right electrode 7 fit against the lower surface of the inner wall of the TC17 pipe, and the insulation device 9 fit against the upper surface of the inner wall of the TC17 pipe. The processing method is set as a continuous linear processing method. The right electrode rod 11 drives the right electrode 7, the load control system 8 and the insulation device 9 to move to the left at a speed of 10 mm / s. Then, the right electrode rod 11 drives the right electrode 7, the load control system 8 and the insulation device 9 to move to the left by 500 mm at a speed of 10 mm / s. At the same time, the TC17 pipe is subjected to pulse current treatment. Then, the load control system 8 is unloaded. After completing the first inner wall surface strengthening of the entire length (500 mm) of the TC17 pipe, the TC17 pipe 1 is obtained.
[0041] (2) After the TC17 pipe 1 obtained in step (1) is rotated 15° along the central axis by the four-jaw chuck 10, the TC17 pipe 1 is processed according to the process and process parameters in step (1) and the second inner wall surface of the entire length of the TC17 pipe 1 is completed to obtain the TC17 pipe 2.
[0042] (3) After processing the TC17 pipe 2 in step (2) for 22 cycles, the processing of the entire inner wall of the metal pipe is completed, and the reinforced TC17 pipe is finally obtained.
[0043] The pulse current processing in step (1) is as follows: the current is 4kA, the voltage is 20V, the frequency is 100Hz, and the processing time is 50s.
[0044] Before processing, the microstructure of TC17 pipe is coarse-grained equiaxed α+β. t The TC17 pipe exhibits a dual-phase microstructure with a tensile strength of 1130 MPa and an elongation of 9.2%. After conventional heat treatment (840℃ for 4 hours), the microstructure of the TC17 pipe is a coarse-grained equiaxed α+ metastable β microstructure, with a tensile strength of 1155 MPa and an elongation of 8.1%. The reinforced TC17 pipe obtained in Example 2 has 24 axially oriented reinforcing bands on its inner wall. Within these bands, the coarse equiaxed α grains are refined into lamellar α grains, resulting in a refined lamellar α+ β microstructure. t The microstructure retains a large number of dislocations, and the refined microstructure and dislocation retention simultaneously improve the strength and plasticity of the pipe. The tensile strength of the reinforced TC17 pipe is 1280 MPa, and the elongation is 12.8%. As shown in Table 2, compared with the TC17 pipe before processing, the tensile strength of the TC17 pipe after heat treatment increases by 25 MPa, while the plasticity decreases by 1.1%. The reinforced TC17 pipe obtained in Example 2 has a tensile strength increase of 150 MPa and a plasticity increase of 3.6% compared with the TC17 pipe before processing, breaking through the technical bottleneck that it is difficult to simultaneously improve the strength and plasticity of metal pipes. The device obtained by this invention breaks through the barrier of existing technology that can only perform shallow treatment on the outer surface of metal pipes, and the treatment depth can reach 15 mm. At the same time, the TC17 pipe treated by this device has refined lamellar α+β t The structure enhances both the strength and plasticity of the pipe, and also improves the wear resistance and corrosion resistance of the inner and outer walls of the pipe.
[0045] Table 2. Mechanical properties of TC17 tubing, heat-treated TC17 tubing, and reinforced TC17 tubing obtained in Example 2.
[0046] Processing status tensile strength elongation TC17 pipe before processing 1130 9.2% TC17 pipe after heat treatment 1155 8.1% Reinforced TC17 pipe 1280 12.8%
[0047] Example 3
[0048] Activate the metal pipe inner wall strengthening device, turn on the main control device 5 and the main unit and power distribution system 6, and place the 300mm long AISI420 stainless steel pipe horizontally on the stage 3. Insert the right electrode 7, load control system 8, and insulation device 9 into the AISI420 stainless steel pipe. Clamp the AISI420 stainless steel pipe with the four-jaw chuck 10. The outer surface of the left end of the pipe should be in contact with the left electrode 4. Apply a force of 150N to make the right electrode 7 adhere to the lower surface of the inner wall of the AISI420 stainless steel pipe, and the insulation device 9 adhere to the upper surface of the inner wall of the AISI420 stainless steel pipe. Set the processing mode to continuous spiral processing mode. The right electrode rod 11 drives the right electrode 7, load control system 8, and insulation system 9 to the left. The movement speed is 1 mm / s. After the four-jaw chuck 10 drives the AISI420 stainless steel tube to rotate at a speed of 30° / s along the central axis, while the four-jaw chuck 10 drives the AISI420 stainless steel tube to rotate at a speed of 30° / s along the central axis, the right electrode rod 11 drives the right electrode 7, the load control system 8 and the insulation device 9 to move 300 mm to the left at a speed of 1 mm / s and performs pulse current treatment on the AISI420 stainless steel tube. Then, the four-jaw chuck 10 stops rotating, the load control system 8 is unloaded, and the reinforced AISI420 stainless steel tube is obtained. The pulse current treatment is as follows: current magnitude is 6 kA, voltage magnitude is 10 V, frequency is 50 Hz, and treatment time is 300 s.
[0049] Before processing, the microstructure of the AISI420 stainless steel pipe was a coarse-grained full martensite structure with a tensile strength of 1205 MPa and an elongation of 11.2%. After conventional heat treatment (1000℃ for 0.5 hours), a small amount of cementite precipitated in the AISI420 stainless steel pipe, resulting in a tensile strength of 1280 MPa and an elongation of 11.0%. The reinforced AISI420 stainless steel pipe obtained in Example 3 has spiral reinforcing bands distributed along the axial direction on its inner wall. The short-time pulsed current treatment and rapid cooling rate refined the coarse martensite laths and produced fine-grained retained austenite. At the same time, a large number of dislocations were retained within the reinforcing bands, which improved both the strength and plasticity of the pipe. The tensile strength of the reinforced AISI420 stainless steel pipe was 1432 MPa, and the elongation was 15.6%. As shown in Table 3, compared with the untreated AISI420 stainless steel, the heat-treated AISI420 stainless steel pipe exhibits a 75 MPa increase in tensile strength and a 0.2% decrease in plasticity. The strengthened AISI420 stainless steel pipe obtained in Example 3 shows a 227 MPa increase in tensile strength and a 4.4% increase in plasticity compared to the untreated AISI420 stainless steel pipe, breaking through the technical bottleneck of simultaneously improving the strength and plasticity of metal pipes. This device overcomes the limitation of existing technologies that only perform shallow treatment on the outer surface of metal pipes. The device of this invention can process up to 20 mm deep, and the treated AISI420 stainless steel pipe possesses refined martensitic laths and fine-grained retained austenite, resulting in simultaneous improvement in both strength and plasticity, as well as enhanced wear resistance and corrosion resistance of the inner and outer walls. Compared with traditional heat treatment, the processing method provided by this device can complete the strengthening treatment of the entire metal pipe in just 300 seconds, significantly shortening the processing time and reducing processing costs.
[0050] Table 3 Mechanical properties of AISI 420 stainless steel tubing and pulsed current-strengthened AISI 420 stainless steel tubing
[0051] Processing status tensile strength elongation AISI420 stainless steel pipe before processing 1205 11.2% AISI420 stainless steel pipes after heat treatment 1280 11.0% Strengthened AISI420 stainless steel pipe 1432 15.6%
[0052] Example 4
[0053] (1) Activate the metal pipe inner wall strengthening device, turn on the main control device 5 and the main unit and power distribution system 6, place the 600mm long QT600-3 ductile iron pipe horizontally on the stage 3, evenly spread about 0.5mm thick tungsten carbide powder on the lower surface of the inner wall of the cast iron pipe, insert the right electrode 7, load control system 8 and insulation device 9 into the inside of the cast iron pipe, clamp the cast iron pipe with the four-jaw chuck 10, and make the outer surface of the left end of the pipe fit with the left electrode 4. Apply a force of 200N to the load control system 8 to make the right electrode 7 fit with the lower surface of the inner wall of the cast iron pipe. The insulating device 9 is attached to the upper surface of the inner wall of the cast iron pipe. The processing method is set to continuous linear processing. The right electrode rod 11 drives the right electrode 7, the load control system 8 and the insulating device 9 to move to the left at a speed of 20 mm / s. Then, the right electrode rod 11 drives the right electrode 7, the load control system 8 and the insulating device 9 to move to the left at a speed of 20 mm / s, while the cast iron pipe is subjected to pulse current processing. Then, the load control system 8 is unloaded. After the first inner wall surface of the cast iron pipe is clad for the entire length (600 mm), the cast iron pipe 1 is obtained.
[0054] (2) After the cast iron pipe 1 obtained in step (1) is rotated 10° along the central axis by the four-jaw chuck 10, the cast iron pipe 1 is processed according to the process and process parameters in step (1) and the second inner wall surface of the entire length of the cast iron pipe 1 is clad to obtain the cast iron pipe 2.
[0055] (3) After processing the cast iron pipe 2 in step (2) for 34 cycles, the processing of the entire inner wall of the metal pipe is completed, and the reinforced cast iron pipe is finally obtained.
[0056] The pulse current processing in step (1) is as follows: the current is 8kA, the voltage is 5V, the frequency is 500Hz, and the processing time is 30s.
[0057] After the inner wall surface of QT600-3 ductile iron pipe is coated with a wear-resistant tungsten carbide coating, the surface hardness increases from 272 HV to 1201 HV, while the wear resistance is also significantly improved. This device breaks through the barrier of existing technology, which can only coat the outer surface of metal pipes with wear-resistant coatings. It can quickly and efficiently coat the inner surface of metal pipes within seconds, achieving a significant improvement in the pipe's hardness, wear resistance, and plasticity.
[0058] Comparative Example 1
[0059] This comparative example is adapted from the paper "Influence of Heat Treatment on the Microstructure and Properties of Cold-Rolled TC4 Titanium Alloy Tubes" by Chen Hongmei of Jiangsu University of Science and Technology, published in the journal *Heat Treatment Technology* in 2012. In this comparative example, the cold-rolled TC4 titanium alloy tubes underwent conventional heat treatment: annealing at 920℃ for 1 hour, furnace cooling to 500℃, and then air cooling to room temperature. After annealing, the tensile strength was 1119 MPa, and the elongation was 14.9%.
[0060] The TC4 pipe treated in Example 1 has a tensile strength of 1210 MPa and an elongation of 15.5%. Compared with Example 1 of the present invention, the cold-rolled TC4 pipe in Comparative Example 1 underwent recrystallization and grain coarsening after annealing at 920°C for 1 hour and furnace cooling to 500°C. However, the method used in Example 1 of the present invention causes the TC4 pipe to undergo rapid phase transformation and martensitic lath refinement, achieving a simultaneous improvement in strength and plasticity. Its processing time (within seconds) is shorter than that of traditional heat treatment, but the tensile strength is 91 MPa higher and the plasticity is improved by 0.6%. At the same time, the method used in the present invention is more efficient and energy-saving. Therefore, compared with Comparative Example 1, Example 1 of the present invention has achieved an unexpectedly significant improvement in technical effect.
[0061] Comparative Example 2
[0062] This comparative example is taken from the paper "Influence of Heat Treatment Process on Microstructure and Mechanical Properties of Large-Size TC17 Titanium Alloy Bars" by Guo Ping of the Northwest Institute of Nonferrous Metals, published in the journal "Advances in Titanium Industry" in 2024. In this comparative example, the TC17 bars were subjected to conventional heat treatment. The optimal heat treatment process was to hold at 800℃ for two hours, then water quench, and then hold at 630℃ for eight hours before air cooling. The tensile strength was 1154 MPa and the elongation was 12.0%.
[0063] The TC17 tubing treated in Example 2 has a tensile strength of 1280 MPa and an elongation of 12.8%. Compared to Example 2 of this invention, the TC17 bar in Comparative Example 2, after prolonged conventional heat treatment, exhibits coarsened microstructure and reduced dislocation density. In contrast, the method employed in Example 2 of this invention results in coarse equiaxed α+β dislocations in the TC17 tubing. t The bimorphic tissue is refined into lamellar α+β t The structure achieves both enhanced plasticity and improved tensile strength, with a 126 MPa increase and a 0.8% improvement in plasticity. Furthermore, its processing time (within seconds) is shorter than that of traditional heat treatment. Therefore, compared with Comparative Example 2, Embodiment 2 of the present invention achieves an unexpectedly significant improvement in technical effect.
[0064] In summary, compared with the prior art, the advantages of this invention are:
[0065] The device obtained by this invention can perform step-by-step, continuous linear, and continuous spiral processing methods, and can quickly apply pulsed current treatment to the inner wall of metal pipes, avoiding pipe disassembly and welding, improving processing efficiency and energy utilization. It can complete processing within seconds, saving processing time and reducing processing costs. After processing, the microstructure of the metal pipe is significantly refined, with a large number of dislocations retained, and the strengthened area and matrix are coordinated in deformation. Strength, plasticity, wear resistance, hardness, and corrosion resistance are simultaneously improved, achieving short-time and efficient microstructure control and toughening of metal pipes. This device can also quickly and efficiently coat the inner wall of metal pipes with a relatively thick (greater than 0.5 mm) wear-resistant coating at low cost, significantly improving the hardness, wear resistance, and strength of the inner wall of the metal pipe. This device can process pipes of various shapes and sizes, overcoming the technical difficulties of traditional heat treatment in processing large, irregularly shaped, and thick-walled pipes and simultaneously improving their strength and plasticity. It also overcomes the limitations of laser surface treatment and shot peening, which can only treat the outer surface of pipes, have a shallow depth (less than 0.5 mm), and provide limited strengthening for large, thick-walled metal pipes. This invention breaks through the technical bottleneck of simultaneously improving the strength, plasticity, wear resistance, and corrosion resistance of metal pipes, and overcomes the barrier of existing technologies that can only perform shallow treatments on the outer surface of metal pipes. Furthermore, each embodiment of this invention uses different components, processes, and process parameters, resulting in different properties of the strengthened pipes. This demonstrates that the superior effects achieved by this invention are due to the synergistic control of the metal pipe to be processed, the device, and the device's process parameters, and that the optimal strengthening effect can only be achieved within the scope of the claims of this invention.
Claims
1. A device for reinforcing the inner wall of a metal pipe, comprising: Displacement control system, right electrode control system, stage, left electrode, main control device, main unit and power distribution system, right electrode, load control system, insulation device, four-jaw chuck, right electrode rod; The displacement control system is located at the bottom of the metal pipe inner wall strengthening device. The right electrode control system and the platform are fixed to the upper right and upper left of the displacement control system, respectively. The displacement control system can adjust the distance between the right electrode control system and the platform. The platform is used to place the metal pipe to be processed. The left electrode is located at the upper left of the platform and on the left side of the metal pipe to be processed. The left electrode can fit against the outer surface of the left end of the metal pipe to be processed. The main control device is located behind the displacement control system. The main unit and power distribution system are located behind the main control device. The four-jaw chuck is located at the upper right of the platform and on the right side of the metal pipe to be processed. The four-jaw chuck is fixed to the right electrode control system. On the left side surface of the system, the four-jaw chuck can both clamp the metal tube and rotate it along the central axis. The right electrode control system and the four-jaw chuck have concentric circular holes that pass through from left to right. The right electrode rod passes through and connects to the concentric circular holes of the right electrode control system and the four-jaw chuck. The right electrode rod is located on the right side of the metal tube to be processed. The load control system is fixed to the left end of the right electrode rod and can move synchronously with the right electrode rod. The right electrode is fixed below the load control system and is a copper wheel or copper ball. The insulating device is fixed above the load control system and is an insulating wheel or insulating ball. The centers of the right electrode and the insulating device are on the same vertical line. The right electrode and insulating device are rotatable. The right electrode control system controls the right electrode rod to move left and right, allowing it to extend into the metal tube. The load control system, right electrode, and insulating device simultaneously extend into the metal tube under the influence of the right electrode rod. The load control system applies vertical stress to both the lower right electrode and the upper insulating device. When the load control system applies vertical stress, the right electrode and insulating device fit tightly against the lower and upper surfaces of the metal tube's inner wall. While the right electrode control system drives the right electrode rod and load control system to move left and right, the right electrode and insulating device simultaneously move against the inner wall of the metal tube. The control device can control the left electrode to move to the right and fit against the outer surface of the left end of the metal tube to be processed. The left electrode can form a pulse current loop with the metal tube to be processed on the platform and the right electrode. The host and power distribution system can generate pulse current and control the pulse current parameters. The functions of the control device include: adjusting the right electrode control system to move the right electrode rod and drive the right electrode, load control system and insulation device to move to the left and adjusting the speed of leftward movement; controlling the load control system to open or unload; controlling the four-jaw chuck to clamp and drive the metal tube to be processed to rotate along the central axis and the rotation speed; and controlling the right electrode, insulation device and load control system to process the inner wall of the metal tube to be processed.
2. The application of the metal pipe inner wall strengthening device according to claim 1 in the field of metal pipe processing, wherein the application includes step-type, continuous linear or continuous spiral processing methods.
3. The application of the metal pipe inner wall strengthening device according to claim 2 in the field of metal pipe processing, characterized in that: The step-by-step machining method is as follows: (1) Turn on the metal pipe inner wall strengthening device, turn on the main control device, host and power distribution system, place the metal pipe to be treated horizontally on the platform, insert the right electrode, load control system and insulation device into the metal pipe to be treated, clamp the metal pipe to be treated with a four-jaw chuck, the outer surface of the left end of the pipe is in contact with the left electrode, the load control system applies a force of 0.5-2500N to make the right electrode contact the lower surface of the inner wall of the metal pipe, and the insulation device contact the upper surface of the inner wall of the metal pipe. After the first pulse current treatment of the metal pipe, unload the load control system, and then move the right electrode rod to the left to drive the right electrode, load control system and insulation device to move to the left 1-40 mm inside the metal pipe. Start the load control system, the load control system applies a force of 0.5-2500N. The force of N causes the right electrode to adhere to the lower surface of the inner wall of the metal pipe, and the insulating device adheres to the upper surface of the inner wall of the metal pipe. After the metal pipe is subjected to a second pulse current treatment, the load control system is unloaded. The process is repeated in the above-mentioned cycle until the first inner wall surface of the entire length of the metal pipe to be processed is completed, and then the step-processed metal pipe is obtained. (2) After the metal pipe obtained in step (1) is rotated 5-90° along the central axis by the four-jaw chuck, the metal pipe is processed according to the process and process parameters in step (1) until the second inner wall surface of the entire length of the metal pipe is completed, and then the metal pipe is processed in step (2). (3) Perform 2-70 cycles of processing on the step-by-step metal pipe according to the processing method in step (2) to complete the processing of the entire inner wall of the metal pipe and finally obtain the step-by-step reinforced metal pipe. The pulse current processing in step (1) is as follows: the current magnitude is 0.1-40 kA, the voltage magnitude is 1-220 V, the frequency is 5-1000 Hz, and the processing time is 0.01-20 s.
4. The application of the metal pipe inner wall strengthening device according to claim 2 in the field of metal pipe processing, characterized in that: The continuous linear machining method is as follows: (1) Turn on the metal pipe inner wall strengthening device, turn on the main control device, host and power distribution system, place the metal pipe to be processed horizontally on the platform, insert the right electrode, load control system and insulation device into the metal pipe to be processed, clamp the metal pipe to be processed with a four-jaw chuck, the outer surface of the left end of the pipe is in contact with the left electrode, the load control system applies a force of 10-2000 N to make the right electrode in contact with the lower surface of the inner wall of the metal pipe, and the insulation device in contact with the upper surface of the inner wall of the metal pipe. Then, the right electrode rod drives the right electrode, load control system and insulation device to move to the left end of the metal pipe to be processed at a speed of 0.5-50 mm / s, and pulse current processing is performed on the metal pipe. Then unload the load control system. After completing the first inner wall surface of the entire length of the metal pipe to be processed, a continuous linear processed metal pipe is obtained. (2) After the continuous linear processing metal pipe obtained in step (1) is rotated 10-60° along the central axis by the four-jaw chuck, the metal pipe is processed according to the process and process parameters in step (1) and the second inner wall surface of the entire length of the metal pipe is completed to obtain the continuous linear processing metal pipe. (3) The continuous straight-line processed metal pipe is processed 4-34 times according to the processing method in step (2) to complete the processing of the entire inner wall of the metal pipe and finally obtain the continuous straight-line reinforced metal pipe. The pulse current processing in step (1) is as follows: the current magnitude is 0.01-80 kA, the voltage magnitude is 0.5-380 V, the frequency is 2-2000 Hz, and the processing time is 0.5-4000 s.
5. The application of the metal pipe inner wall strengthening device according to claim 4 in the field of metal pipe processing, characterized in that: The continuous linear machining method is as follows: (1) Turn on the metal pipe inner wall strengthening device, turn on the main control device, host and power distribution system, place the metal pipe to be processed horizontally on the platform, spread a 0.1-10 mm thick coating material evenly on the lower surface of the inner wall of the metal pipe, insert the right electrode, load control system and insulation device into the metal pipe to be processed, clamp the metal pipe to be processed with a four-jaw chuck, the outer surface of the left end of the pipe is in contact with the left electrode, the load control system applies a force of 10-2000 N to make the right electrode in contact with the lower surface of the inner wall of the metal pipe, and the insulation device in contact with the upper surface of the inner wall of the metal pipe. Then, the right electrode rod drives the right electrode, load control system and insulation device to move to the left end of the metal pipe to be processed at a speed of 0.5-50 mm / s, and pulse current processing is performed on the metal pipe at the same time. Then unload the load control system, and after completing the first inner wall surface of the entire length of the metal pipe to be processed, a continuous linear processed metal pipe is obtained. (2) After the continuous linear processing metal pipe obtained in step (1) is rotated 10-60° along the central axis by the four-jaw chuck, the metal pipe is processed according to the process and process parameters in step (1) and the second inner wall surface of the entire length of the metal pipe is completed to obtain the continuous linear processing metal pipe. (3) The continuous straight-line processed metal pipe is processed 4-34 times according to the processing method in step (2) to complete the processing of the entire inner wall of the metal pipe and finally obtain the continuous straight-line reinforced metal pipe. The pulse current processing in step (1) is as follows: the current magnitude is 0.01-80 kA, the voltage magnitude is 0.5-380 V, the frequency is 2-2000 Hz, and the processing time is 0.5-4000 s; The coating material mentioned in step (1) is one of silicon carbide powder, titanium carbide powder, titanium nitride powder, tungsten nitride powder or tungsten carbide powder.
6. The application of the metal pipe inner wall strengthening device according to claim 2 in the field of metal pipe processing, characterized in that: The continuous spiral processing method is as follows: Activate the metal pipe inner wall strengthening device, turn on the main control device, host, and power distribution system. Place the metal pipe to be treated horizontally on the platform. Insert the right electrode, load control system, and insulation device into the metal pipe. Clamp the metal pipe with a four-jaw chuck, ensuring the outer surface of the left end of the pipe is in contact with the left electrode. Apply a force of 5-3000 N to ensure the right electrode is in contact with the lower surface of the inner wall of the metal pipe, and the insulation device is in contact with the upper surface of the inner wall of the metal pipe. Simultaneously, the four-jaw chuck rotates the metal pipe at a speed of 1-60° / s along the central axis, while the right electrode rod rotates at a speed of 0.1-40° / s. The right electrode, load control system, and insulation device are moved to the left at a speed of mm / s to the left end of the metal tube to be processed. After pulse current treatment, a continuously spiral reinforced metal tube is obtained. That is, the right electrode, load control system, and insulation device move spirally to the left relative to the inner wall of the metal tube while pulse current treatment is performed on the metal tube. The continuous spiral processing method is to perform pulse current treatment in a spiral curve with different density in the length direction of the inner wall of the metal tube to strengthen the entire inner wall surface of the metal tube. The pulse current treatment is as follows: current magnitude is 0.05-60 kA, voltage magnitude is 2-220 V, frequency is 10-1500 Hz, and processing time is 1-5000 s.
7. The application of the metal pipe inner wall strengthening device according to any one of claims 2-6 in the field of metal pipe processing, characterized in that: The metal pipe is one of the following: TC4 pipe, TB8 pipe, TC17 pipe, TA0 pipe, TA16 pipe, TA18 pipe, AISI420 stainless steel pipe, AISI430 stainless steel pipe, 35CrMo steel pipe, QT500-7 ductile iron, or QT600-3 ductile iron.
Citation Information
Patent Citations
High-strength or low-plasticity material hollow member low pressure thermoforming apparatus and method thereof
CN104162948A
Electrolytic deburring device of air cylinder body
CN109570667A