Composite photocatalyst, method for preparing the same, and method for producing hydrogen
By combining three-dimensional graphene and two-dimensional MXene, a photocatalyst without semiconductor materials was prepared. By utilizing the photoinduced electron emission mechanism, the problem of low solar energy utilization of existing photocatalysts was solved, and a high-efficiency hydrogen production rate and stability were achieved.
Patent Information
- Application Number
- CN202411424120.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-12
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-10-12
AI Technical Summary
Existing photocatalysts suffer from low solar energy utilization and unsatisfactory photon conversion efficiency due to their large band gap and rapid charge recombination rate, making it difficult to improve hydrogen production rates.
By using three-dimensional graphene as the main catalyst and two-dimensional MXene as the co-catalyst, a composite photocatalyst without semiconductor materials was prepared through the photoinduced electron emission mechanism, and the catalytic performance was enhanced by high-energy heat/free electrons.
Under ultraviolet or visible light irradiation, the prepared composite photocatalyst can achieve a hydrogen production rate of over 1300 μmol·h⁻¹·g⁻¹ through water splitting, and it exhibits high stability, maintaining a hydrogen production rate of over 70% after recycling.
Smart Images

Figure CN119303603B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a composite photocatalyst, its preparation method, and a method for producing hydrogen. Background Technology
[0002] Photocatalytic water splitting for hydrogen production is an important method for converting solar energy into chemical energy. Currently, the most widely used photocatalysts are semiconductor catalysts, such as metal oxides, sulfides, nitrides, and g-C3N4. These catalysts have large band gaps and rapid charge recombination rates, resulting in low solar energy utilization and unsatisfactory photon conversion efficiency. To improve the hydrogen production rate, those skilled in the art have been searching for methods to improve catalyst performance.
[0003] MXene is a novel type of two-dimensional material with excellent electrical conductivity, specific surface area, and surface chemical properties, making it an ideal cocatalyst. Combining MXene with graphene is expected to improve catalyst performance.
[0004] CN111744519A discloses a method for preparing a hydrogen evolution catalyst based on a three-dimensional MXene-based support. This method utilizes a three-dimensional MXene-based material as a catalyst support for the hydrogen evolution reaction in water electrolysis under alkaline conditions, and loads metal particles to prepare a three-dimensional structured catalyst. Graphene or graphene oxide is selected as the carbon material in this method. CN113621989A discloses a method for preparing a nickel-based layered electrocatalyst based on MXene / graphene hydrogel electrodeposition, comprising the following steps: uniformly mixing MXene, graphene oxide (GO), and a dopant, and ultrasonically dispersing them; reacting the dispersion in a hydrothermal reactor under high temperature conditions to obtain a non-metallic element-doped layered MXene / RGO hydrogel; and electrodepositing the hydrogel onto a metal substrate to obtain a structurally controllable three-dimensional nanostructured electrocatalyst. The prepared catalyst consists of MXene / RGO layered material and a three-dimensional layered nickel-based LDH nanosheet array grown on the MXene / RGO substrate. The catalysts obtained by the above methods require hydrogen production under electrolysis conditions.
[0005] CN116889867A discloses a method for creating an MXene-derived porous TiO2 / RGO nanosheet composite photocatalyst. Using MXene as a titanium source, it is composited with graphene oxide (GO). TiO2 and GO serve as self-templates, utilizing their unique thermal conversion properties. The composite is then calcined at high temperature in a muffle furnace under air atmosphere, forming a strong C-Ti bond between TiO2 and graphene, resulting in a porous, hierarchical TiO2 / RGO nanosheet composite photocatalyst. This method uses MXene and graphene to improve the catalytic performance of TiO2, but the main catalyst remains a semiconductor material.
[0006] CN111790417A discloses a method for preparing MXene-derived TiO2 nanosheet-graphene gel composite material, comprising: forming a graphene oxide aqueous solution by dissolving graphene oxide in an aqueous solution; adding MXene to the graphene oxide aqueous solution to obtain a first mixed solution; adding a reducing agent to the first mixed solution and forming an MXene-graphene hydrogel under water bath conditions; adding a crystal facet control agent to water to obtain a second mixed solution; placing the MXene-graphene hydrogel in the second mixed solution and carrying out a hydrothermal reaction to obtain a TiO2 nanosheet-graphene hydrogel; and freeze-drying it to obtain a TiO2 nanosheet-graphene aerogel composite material. This method utilizes MXene and graphene to prepare TiO2 nanosheet-graphene, using MXene as a raw material for TiO2 preparation. The photocatalyst prepared by this method is still mainly a semiconductor material. Summary of the Invention
[0007] In view of this, one object of the present invention is to provide a method for preparing a composite photocatalyst, the obtained catalyst exhibiting high hydrogen production rate and stability. Another object of the present invention is to provide a composite photocatalyst obtained by the above method. A further object of the present invention is to provide a method for producing hydrogen by water splitting.
[0008] The present invention achieves the above objectives using the following technical solutions.
[0009] On the one hand, the method for preparing the composite photocatalyst provided by the present invention includes the following steps:
[0010] 1) Graphene oxide dispersion and Ti3C2T were mixed under an inert gas atmosphere. x The dispersions were mixed to obtain a mixture; in the mixture, Ti3C2T x Graphene oxide and Ti3C2T x 8–25 wt% of the total weight;
[0011] 2) The mixture was subjected to a hydrothermal reaction at 100-130℃ for 10-20 hours, and then naturally cooled to room temperature. The colloidal cylindrical product containing water was taken out and freeze-dried to obtain the composite photocatalyst.
[0012] According to the preparation method of the present invention, preferably, in the mixture, Ti3C2T x Graphene oxide and Ti3C2T x It accounts for 9 to 15 wt% of the total weight, more preferably 10 to 11 wt%.
[0013] According to the preparation method of the present invention, preferably, the concentration of graphene oxide in the graphene oxide dispersion is 1-20 mg / mL; Ti3C2T x Ti3C2T in dispersion xThe concentration is 1–20 mg / mL.
[0014] According to the preparation method of the present invention, preferably, the hydrothermal reaction temperature is 110-120°C and the time is 11-15 h.
[0015] According to the preparation method of the present invention, preferably, the XRD pattern of the composite photocatalyst has diffraction peaks of graphene (002) crystal plane and Ti3C2T. x (002) Diffraction peaks of crystal planes.
[0016] According to the preparation method of the present invention, preferably, the composite photocatalyst exhibits Ti3C2T in its Raman spectrum. x Characteristic peaks of graphene and graphene.
[0017] According to the preparation method of the present invention, preferably, the composite photocatalyst has a three-dimensional structure constructed from two-dimensional sheets in the SEM image; and has Ti3C2T in the TEM image. x Image of a graphene sheet loaded onto its surface.
[0018] On the other hand, the present invention also provides a composite photocatalyst prepared by any of the above preparation methods, preferably wherein the hydrogen production rate by water splitting per gram of catalyst is 1350–3000 μmol·h. -1 .
[0019] Furthermore, the present invention also provides a method for producing hydrogen by splitting water, preferably, using the aforementioned composite photocatalyst to split water and produce hydrogen under light irradiation; in the first 0.5 hours, the rate of hydrogen production by splitting water per gram of catalyst is 1350–3000 μmol·h. -1 After five cycles, the hydrogen production rate of the composite photocatalyst remained above 70%.
[0020] The composite photocatalyst of this invention does not contain semiconductor materials and uses three-dimensional graphene as the main catalyst. Based on the photoinduced electron emission mechanism, it emits high-energy hot / free electrons. Two-dimensional MXene acts as a co-catalyst to enhance the catalytic performance of the hot / free electrons, thereby enabling the composite photocatalyst of this invention to produce hydrogen at a high rate. Under ultraviolet or visible light irradiation, the composite photocatalyst prepared by this invention can achieve a water splitting hydrogen production rate of up to 1300 μmol·h⁻¹. -1 ·g cat -1 The above are the results, and the stability is high. Attached Figure Description
[0021] Figure 1 XRD pattern of the composite photocatalyst (3DGraphene / MXene-10) prepared in Example 1;
[0022] Figure 2 Raman image of the composite photocatalyst (3DGraphene / MXene-10) prepared in Example 1;
[0023] Figure 3 SEM image of the composite photocatalyst (3DGraphene / MXene-10) prepared in Example 1;
[0024] Figure 4 TEM image of the composite photocatalyst (3DGraphene / MXene-10) prepared in Example 1;
[0025] Figure 5 The above are the performance test results of the composite photocatalysts prepared in the examples and comparative examples for catalytic water splitting to produce hydrogen.
[0026] Figure 6 The results show the recycling performance of the composite photocatalyst (3DGraphene / MXene-10) prepared in Example 1 for catalytic water splitting to produce hydrogen. Detailed Implementation
[0027] The present invention will be further described below with reference to specific embodiments, but the scope of protection of the present invention is not limited thereto.
[0028] The "hydrogen production rate" mentioned in this invention refers to the amount of hydrogen produced per gram of catalyst per unit time, expressed in μmol·h⁻¹. -1 ·g cat -1 It is used to measure the rate of photocatalytic hydrogen production.
[0029] <Preparation Methods of Composite Photocatalysts>
[0030] This invention discovers a novel enhanced thermal / free electron photocatalytic water splitting mechanism for hydrogen production and provides a method for preparing a semiconductor-free composite photocatalyst based on this mechanism. This preparation method uses three-dimensional graphene as the main catalyst, emitting high-energy thermal / free electrons based on the photoinduced electron emission mechanism, using two-dimensional MXene (Ti3C2T) as the catalyst. x ,T x The composite catalyst (containing O, OH, and F) enhances the catalytic performance due to heat and free electrons. Under ultraviolet or visible light irradiation, the prepared composite catalyst achieves a high hydrogen production rate in water splitting for hydrogen production.
[0031] The preparation method of the composite photocatalyst of the present invention includes a mixing step and a hydrothermal reaction step. This will be described in detail below.
[0032] Mixing steps
[0033] Under the protection of an inert gas, the graphene oxide dispersion and Ti3C2T were mixed. x The dispersions are mixed to obtain a mixture.
[0034] The graphene oxide dispersion used in this invention and Ti3C2T x The dispersion can be obtained directly from commercially available products or prepared using existing methods according to actual needs.
[0035] According to one embodiment of the present invention, graphene oxide can be prepared by a modified Hummer's method. MXene can be prepared by etching the MAX phase with an etchant. The MAX phase is a known machinable ceramic material in the art, composed of three elements: M, A, and X, and its general chemical formula is M. (n+1) AX n In this system, M represents a transition metal element, A represents a main group element, and X represents carbon or nitrogen.
[0036] In the mixture of the present invention, Ti3C2T x Graphene oxide and Ti3C2T x 8–25 wt% of the total weight. In some technical solutions, Ti3C2T is present in the mixture. x Graphene oxide and Ti3C2T x The total weight is 9–15 wt%. In other technical solutions, the mixture contains Ti3C2T x Graphene oxide and Ti3C2T x The total weight is 10-11 wt%. This invention discovers that combining graphene oxide with Ti3C2T... x By controlling the mass fraction within the above range, both the main catalyst and the co-catalyst can function more stably, ensuring the high efficiency and stability of the composite photocatalyst in hydrogen production.
[0037] According to one embodiment of the present invention, the concentration of graphene oxide in the graphene oxide dispersion can be 1-20 mg / mL, preferably 2-15 mg / mL, and more preferably 5-10 mg / mL. Ti3C2T x Ti3C2T in dispersion x The concentration can be 1 to 20 mg / mL, preferably 2 to 15 mg / mL, and more preferably 5 to 10 mg / mL.
[0038] According to a specific embodiment of the present invention, Ti3C2T x The chemical formula is:
[0039] Ti3C2T x ,T x =O,OH and F.
[0040] In this invention, the inert gas is selected from at least one of helium (He), neon (Ne), and argon (Ar); preferably, the inert gas is selected from at least one of helium (He) and argon (Ar). The inert gas prevents MXene from being oxidized and also prevents the oxidized MXene from further reacting with graphene oxide under oxygen-containing conditions, thus ensuring the stable progress of the subsequent hydrothermal reaction.
[0041] To achieve better reaction results, stirring can be performed during mixing. The stirring time can be 5–30 min, preferably 10–25 min, and more preferably 15–20 min. A reasonable stirring time ensures a more uniform mixture of MXene and graphene oxide, which is beneficial for the subsequent heating reaction and preserves the three-dimensional structure of both three-dimensional graphene and two-dimensional MXene.
[0042] Hydrothermal reaction steps
[0043] Graphene oxide dispersion and Ti3C2T x The mixture of dispersions undergoes a hydrothermal reaction, followed by natural cooling to room temperature. The water-containing colloidal cylindrical product is then removed and freeze-dried to obtain the composite photocatalyst.
[0044] According to one embodiment of the present invention, the hydrothermal reaction can be carried out in a high-pressure reactor, and the pressure inside the high-pressure reactor during the reaction is 0.1 to 3 MPa.
[0045] In this invention, preferably, the hydrothermal reaction temperature can be 100–130°C, more preferably 110–120°C, and even more preferably 115–120°C. The hydrothermal reaction time can be 10–20 h, preferably 11–15 h, and even more preferably 12–13 h. Reasonable hydrothermal temperature and time can achieve the reduction of graphene oxide to graphene, while also facilitating the formation of the three-dimensional / two-dimensional structure of the three-dimensional graphene / Mxene photocatalyst, ensuring the stable loading of two-dimensional Mxene on three-dimensional graphene, and improving the stability of the catalyst.
[0046] According to one embodiment of the present invention, freeze drying is preferably vacuum freeze drying. Vacuum freeze drying can be carried out using a vacuum freeze dryer, which is selected from one of the following: capping freeze dryer, manifold freeze dryer, bell-type freeze dryer, in-situ freeze dryer, rotary dynamic freeze dryer, and vibrating dynamic freeze dryer, with a preference for one of the following: bell-type freeze dryer, in-situ freeze dryer, and rotary dynamic freeze dryer.
[0047] According to another embodiment of the present invention, the freeze-drying conditions of the present invention are as follows:
[0048] The cold trap temperature can be -80 to -10°C, preferably -75 to -20°C, and more preferably -70 to -45°C;
[0049] The vacuum degree can be 0.1 to 50 Pa, preferably 1 to 30 Pa, and more preferably 5 to 20 Pa;
[0050] The drying time can be 10 to 300 hours, preferably 50 to 250 hours, and more preferably 80 to 150 hours.
[0051] In addition to removing moisture, freeze-drying is more conducive to the formation and stabilization of three-dimensional graphene and two-dimensional MXene structures. At the same time, freeze-drying can prevent graphene from being oxidized and degraded, which is beneficial to maintaining the original properties of MXene.
[0052] According to one embodiment of the present invention, the composite photocatalyst prepared by the method of the present invention exhibits diffraction peaks of graphene (002) crystal planes and Ti3C2T in its XRD pattern. x (002) Diffraction peaks of the crystal plane. The Raman spectrum of the composite photocatalyst shows Ti3C2T x Characteristic peaks of both α and β and graphene. The SEM image of the composite photocatalyst shows a three-dimensional structure constructed from two-dimensional sheets; the TEM image shows Ti3C2T... x Images of graphene sheets loaded onto the surface of graphene sheets. In composite photocatalysts with the above characteristics, two-dimensional MXene is loaded onto three-dimensional graphene to form a stable three-dimensional structure, which is beneficial to improving the catalytic hydrogen production rate and stability.
[0053] <Composite photocatalyst>
[0054] The composite photocatalyst of the present invention can be obtained by using the above method.
[0055] In the composite photocatalyst of this invention, two-dimensional MXene is stably supported on three-dimensional graphene. Two-dimensional MXene possesses excellent conductivity, specific surface area, and surface chemical properties. Using two-dimensional MXene as a co-catalyst, its high conductivity facilitates the rapid transfer of hot electrons generated by the three-dimensional graphene; its excellent surface chemical properties, especially its hydrophilicity, promote the enrichment of water molecules, thereby accelerating water decomposition, enhancing the catalytic performance of the main catalyst, three-dimensional graphene, and significantly increasing the hydrogen production rate. Furthermore, the composite photocatalyst of this invention does not contain semiconductor materials, making it environmentally friendly and cost-effective.
[0056] <Methods for producing hydrogen by water splitting>
[0057] This invention also provides a method for producing hydrogen by water splitting, wherein the above-mentioned composite photocatalyst is used to split water to produce hydrogen under illumination. Specific illumination conditions are as follows: the xenon lamp spectral range is 200–1000 nm. The light power incident on the reaction liquid surface can be 50–500 mW, preferably 100–350 mW, and more preferably 150–300 mW;
[0058] In the first 0.5 hours, the rate of hydrogen production from water splitting per gram of catalyst was 1350–3000 μmol·h⁻¹. -1 It exhibited excellent hydrogen production performance; after 5 cycles, the hydrogen production rate of the composite photocatalyst remained above 70%, demonstrating good cycle stability.
[0059] <Testing Method>
[0060] The test was conducted using an online photocatalytic reaction system equipped with a gas chromatograph, following standard procedures.
[0061] <Raw Material Preparation>
[0062] The raw materials used in the following examples and comparative examples are described below:
[0063] Ti3C2T x The dispersion, with a concentration of 8.6 mg / mL, was prepared by etching the Ti3AlC2 phase with LiF / HCl.
[0064] The graphene oxide dispersion, with a concentration of 6.57 mg / mL, was prepared by a modified Hummer's method.
[0065] Examples 1-3 and Comparative Examples 1-3
[0066] A dispersion containing 70 mg of graphene oxide and Ti3C2T x The dispersions were mixed to a total volume of 70 mL. The mixture was stirred for 10 min under argon protection to obtain the final mixture.
[0067] The mixture was transferred to a 100 mL polytetrafluoroethylene-lined high-pressure reactor and heated to 120 °C for hydrothermal reaction for 12 h. After natural cooling to room temperature, the water-containing colloidal cylindrical product was removed from the high-pressure reactor. The colloidal cylindrical product was then freeze-dried to obtain the composite photocatalyst. Freeze-drying was performed using a freeze dryer with a cold trap temperature of -60 °C, a vacuum degree of 10 Pa, and a drying time of 100 h. Detailed parameters and performance of the obtained composite photocatalyst are shown in Table 1.
[0068] In Comparative Example 1, Example 1, Example 2, and Example 3, the Ti3C2T content in the mixture was controlled respectively. x Graphene oxide and Ti3C2Tx Composite photocatalysts were prepared by using 5%, 10%, 15%, and 20% of the total weight, respectively, and the corresponding composite photocatalysts are designated as 3DGraphene / MXene-5, 3DGraphene / MXene-10, 3DGraphene / MXene-15, and 3DGraphene / MXene-20.
[0069] Table 1
[0070]
[0071] As shown in Table 1, Ti3C2T x A high hydrogen production rate can only be obtained by controlling the weight within a suitable range.
[0072] The phase and crystal structure of the composite photocatalyst (3DGraphene / MXene-10) prepared in Example 1 were characterized and analyzed by X-ray diffraction (XRD). Figure 1 As shown in the XRD pattern, the graphene (002) crystal plane and the Ti3C2T plane are clearly visible. x (002) All diffraction peaks of the crystal planes can be observed.
[0073] Raman spectra of 3DGraphene / MXene-10 are as follows Figure 2 As shown, Ti3C2T x Characteristic peaks of the α and D and G peaks of graphene were observed.
[0074] SEM characterization results of 3DGraphene / MXene-10 are as follows: Figure 3 As shown, a three-dimensional structure constructed from two-dimensional sheets was observed. In the TEM results of 3DGraphene / MXene-10 ( Figure 4 ), observed Ti3C2T x The sheet is loaded onto the surface of the graphene sheet (marked with a white dashed circle).
[0075] The composite photocatalysts prepared in Examples 1-3 and Comparative Example 3 were tested for their catalytic performance in the water splitting to hydrogen production reaction under illumination. The xenon lamp spectral range was 200-1000 nm, and the incident light power on the reaction liquid surface was 260 mW. Using the same preparation method as in Example 1, MXene-free 3D graphene and graphene-free pure MXene (Con-MXene) were prepared as Comparative Examples 1 and 2. The test results are as follows. Figure 5As shown, Con-MXene produces almost no hydrogen, indicating that pure MXene has no photocatalytic activity. 3D Graphene exhibits photocatalytic activity under illumination, further confirming the catalytic ability of three-dimensional graphene to generate hot / free electrons. Furthermore, the composite photocatalysts prepared in Examples 1-3 significantly improved the hydrogen production rate during water splitting.
[0076] The hydrogen production rate during the first 0.5 hours of catalytic water splitting for hydrogen production under light irradiation was measured. The composite photocatalysts prepared in Examples 1-3 exhibited a hydrogen production rate of 1300 μmol·h⁻¹. -1 ·g cat -1 The hydrogen production rate described above is significantly higher than that of Comparative Example 1 (3D Graphene, 392 μmol·h⁻¹). -1 ·g cat -1 ), and significantly higher than the control group 3.
[0077] The photocatalytic cycle stability of the composite photocatalyst (3DGraphene / MXene-10) prepared in Example 1 was tested. A total of 5 cycles were performed, with each cycle lasting 4 hours of hydrogen production. The test results are as follows: Figure 6 As shown, the hydrogen production rate decreases slightly with increasing cycle number, but remains at 71% after 5 cycles, indicating that the composite photocatalyst of the present invention has good cycle stability.
[0078] Comparative Examples 4-5
[0079] By changing the hydrothermal reaction temperature, while keeping other conditions the same as in Example 1, a composite photocatalyst was obtained. Detailed parameters and performance are shown in Table 2.
[0080] Table 2
[0081]
[0082] As can be seen from Table 2, a lower hydrothermal reaction temperature is not conducive to obtaining composite photocatalysts with stable three-dimensional / two-dimensional structures, and reduces the hydrolysis hydrogen production rate of the composite photocatalyst.
[0083] This invention is not limited to the above-described embodiments. Any modifications, improvements, or substitutions that can be conceived by those skilled in the art without departing from the essential content of this invention fall within the scope of this invention.
Claims
1. A method for producing hydrogen by splitting water using a composite photocatalyst, characterized in that, Under illumination, a composite photocatalyst was used to decompose water to produce hydrogen. In the first 0.5 hours, the hydrogen production rate per gram of catalyst was 1350–3000 µmol·h⁻¹. -1 After five cycles, the hydrogen production rate of the composite photocatalyst remained above 70%. The composite photocatalyst is prepared by a method comprising the following steps: 1) Under the protection of an inert gas, the graphene oxide dispersion and Ti3C2T were mixed. x The dispersions were mixed to obtain a mixture; in the mixture, Ti3C2T x Graphene oxide and Ti3C2T x The total weight is 8–11 wt%; the concentration of graphene oxide in the graphene oxide dispersion is 5–10 mg / mL; Ti3C2T x Ti3C2T in dispersion x The concentration is 5–10 mg / mL; 2) The mixture was subjected to a hydrothermal reaction at 100-130℃ for 10-20 hours, and then naturally cooled to room temperature. The colloidal cylindrical product containing water was taken out and freeze-dried to obtain the composite photocatalyst.
2. The method according to claim 1, characterized in that, In the mixture, Ti3C2T x Graphene oxide and Ti3C2T x 10 to 11 wt% of the total weight.
3. The method according to claim 1, characterized in that, The hydrothermal reaction temperature is 110–120℃, and the time is 11–15 hours.
4. The method according to any one of claims 1 to 3, characterized in that, The XRD pattern of the composite photocatalyst shows diffraction peaks of the graphene (002) crystal plane and Ti3C2T. x (002) Diffraction peaks of crystal planes.
5. The method according to any one of claims 1 to 3, characterized in that, The composite photocatalyst exhibits Ti3C2T in its Raman spectrum. x Characteristic peaks of graphene and graphene.
6. The method according to any one of claims 1 to 3, characterized in that, The SEM image of the composite photocatalyst shows a three-dimensional structure constructed from two-dimensional sheets; the TEM image shows Ti3C2T. x Image of a graphene sheet loaded onto its surface.
Citation Information
Patent Citations
Preparation method of hydrogen evolution catalyst of three-dimensional MXene-based carrier
CN111744519A
Mxene derived TiO2 nano sheet-graphene gel composite material as well as preparation method and application thereof
CN111790417A
Synthesis method for preparing nickel-based layered structure electrocatalyst based on Mxene / graphene hydrogel electrodeposition
CN113621989A
Graphene quantum dot / MXene nanosheet two-dimensional composite material as well as preparation method and application thereof
CN113718281A