A ZrB2-coated zirconium powder, its preparation method and application
By coating zirconium powder with ZrB₂, the problems of high electrostatic sensitivity of zirconium powder and low volumetric calorific value of modified materials are solved, realizing the preparation of high-energy-density solid propellants. The method is simple and easy to scale up.
Patent Information
- Application Number
- CN202311588519.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-27
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-11-27
AI Technical Summary
Existing zirconium powder has high electrostatic sensitivity, which can easily cause safety hazards, and the modified materials have low volumetric calorific value, which limits its application in solid propellants.
Zirconium boride (ZrB₂), an inorganic ceramic phase, is coated onto the surface of zirconium powder. ZrB₂-coated zirconium powder is then prepared by ball milling and high-temperature sintering, which maintains the high density of the zirconium powder and increases its volumetric calorific value.
This method improves the volumetric calorific value of zirconium powder, enhances the energy density of solid propellants, and is simple to prepare and easy to mass-produce.
Smart Images

Figure CN119306556B_ABST
Abstract
Description
Technical Field
[0001] This invention relates generally to the field of energetic materials technology, and specifically to a ZrB2-coated zirconium powder, its preparation method, and its application. Background Technology
[0002] Solid propellants mainly consist of binders, oxidizers, and metallic fuels. The addition of metallic fuels is a crucial way to increase the energy of solid propellants, not only because metallic fuels have high density and release a large amount of heat per unit volume during combustion, but also because metal oxides have high heat of vaporization, providing significant energy to the solid propellant and suppressing combustion instability. The main metallic fuels in solid propellants include Al, Mg, Zr, and Ti. Aluminum and magnesium powders have already been practically applied, while the remaining metallic powders are still under research. Compared to aluminum and magnesium, zirconium powder has higher density, higher bulk calorific value, and superior combustion performance. Studies have shown that 40–70 μm zirconium powder has a burning rate comparable to 10 μm aluminum powder, and the content of 3 μm zirconium particles has a similar effect on the propellant combustion rate as nano-aluminum particles. Therefore, using zirconium powder is a favorable choice for preparing high-energy-density solid propellants.
[0003] However, zirconium powder, as a dense metallic fuel with a high heat of combustion, is limited in its use in solid propellants due to its high electrostatic sensitivity, which can pose safety hazards. When the average particle size of zirconium powder is less than 10 μm and it is in suspension, spontaneous combustion or even explosion can occur. Therefore, zirconium powder must be modified before it can be used in solid propellants. Current literature indicates the use of hydroxyl-terminated butadiene (HTPB, 0.96 g·cm³). -3 43.10 kJ·cm -3 ), Glycidyl azide (GAP, 1.3 g·cm⁻¹) -3 26.67 kJ·cm -3 )), polymethyl methacrylate (PMMA, 1.29 g·cm³), -3 ), azide nitrified cellulose (NC, 1.66 g·cm³) -3 ), aluminum oxide (Al2O3, 3.5 g·cm³) -3 ), zinc oxide (ZnO, 5.6 g·cm³) -3 ), polyimide (PI, 1.59 g·cm³) -3 ), carbon nanofilm (C, 2.26 g·cm⁻¹) -3 74.04 kJ·cm -3 Zirconium powder was modified using substances such as zirconium oxide (Zr, 6.49 g·cm³). However, these coating materials have low volumetric calorific value, resulting in a loss of zirconium powder (Zr, 6.49 g·cm³). -3 78.28 kJ·cm -3 The original advantages of high density and high volumetric calorific value.
[0004] Finding a high-calorific-value material to modify zirconium metal powder is crucial. Zirconium boride, as an inorganic ceramic phase, is inherently insulating and possesses high density and volumetric calorific value (ZrB₂, 6.09 g·cm⁻¹). -3 110.61 kJ·cm -3 Furthermore, the reaction between B and Zr is relatively simple. Therefore, coating the surface of zirconium powder with the inorganic ceramic phase zirconium boride is the key to preparing high-calorific-value zirconium powder composite fuels. Summary of the Invention
[0005] In order to overcome the technical defects of low volumetric calorific value of composite zirconium powder in the prior art, this invention provides a ZrB2-coated zirconium powder, its preparation method and application, wherein the zirconium powder is coated with a ZrB2 coating layer, which ensures the high density of the zirconium powder while ensuring that its volumetric calorific value is not lost.
[0006] The technical solution of the present invention is a ZrB2-coated zirconium powder, comprising zirconium powder and a ZrB2 coating layer covering the zirconium powder, wherein the particle size of the zirconium powder is D. 90 The thickness of the coating layer is 0.1 μm-3 μm, and the mass percentage of ZrB2 is 1%-60%.
[0007] The present invention also provides a method for preparing the ZrB2-coated zirconium powder, wherein zirconium powder and boron powder are taken and mixed evenly by ball milling, and then the mixed material is placed in a vacuum tube furnace for high-temperature sintering to obtain the ZrB2-coated zirconium powder.
[0008] Furthermore, the purity of the aforementioned zirconium powder is ≥95%, and the particle size D is... 90 ≤50μm.
[0009] Furthermore, the aforementioned boron powder includes amorphous boron powder and crystalline boron, with a particle size ≤ 1 micrometer.
[0010] Furthermore, the mass ratio of zirconium powder to boron powder is 10:1 to 100:1.
[0011] Furthermore, the above-mentioned ball milling methods include: planetary ball milling or horizontal ball milling, with a ball milling speed of 200 rpm to 400 rpm and a ball milling time of 1 h to 6 h.
[0012] Furthermore, the above-mentioned high-temperature sintering temperature is 700℃~1200℃, and the holding time is 30min~300min.
[0013] Furthermore, the aforementioned vacuum tube furnace is filled with argon or helium.
[0014] The present invention also provides the application of the above-mentioned ZrB2-coated zirconium powder in solid propellant components.
[0015] The beneficial effects of the present invention are: the ZrB2-coated zirconium powder disclosed in the present invention has a high calorific value, which is beneficial to improving the density and energy of solid propellants. At the same time, the preparation method is simple, the experimental results are controllable, and it is easy to achieve batch preparation. Attached Figure Description
[0016] These and / or other aspects and advantages of the present invention will become clearer and more readily understood from the following detailed description of embodiments of the invention taken in conjunction with the accompanying drawings, wherein:
[0017] Figure 1 The XRD patterns of the zirconium powder raw material and the products obtained in Examples 1-5 are shown in the embodiments of the present invention.
[0018] Figure 2 The XRD patterns are of the products obtained in Examples 6-11 of this invention;
[0019] Figure 3 The images shown are SEM images of the products obtained in Examples 1-11 of the present invention, where (a)-(b) correspond to the products of Examples 1-2, and (c) corresponds to the product of Example 9. Detailed Implementation
[0020] To enable those skilled in the art to better understand the present invention, the present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments.
[0021] Example 1:
[0022] Weigh out zirconium powder (D) according to a mass ratio of 10:1. 90 Zirconium powder (≤50μm, the same applies to all subsequent examples) and boron powder (≤1μm particle size, the same applies to all subsequent examples) were ball-milled at 300 rpm for 3 hours. The ball-milled sample was then placed in a vacuum tube furnace and held at 700℃ for 90 minutes under an argon or helium atmosphere to obtain the ZrB2-coated zirconium powder composite material, designated as No. 1#. The XRD patterns of the raw zirconium powder and the obtained product in this example are shown below. Figure 1 As shown: ZrB2 is formed in the zirconium powder, with a ZrB2 content of 4.37%; the SEM image of the product obtained in this example is shown below. Figure 3 As shown, the coating thickness of the sample is 0.68 μm. The volumetric calorific value of the sample is 68.98 kJ·cm⁻¹ for the zirconium powder raw material. -3 Increased to 70.25 kJ·cm -3 .
[0023] Example 2:
[0024] Zirconium powder and boron powder were weighed at a mass ratio of 10:1 and then ball-milled at 300 rpm for 3 hours. The ball-milled sample was then placed in a vacuum tube furnace and held at 800°C for 90 minutes under an argon or helium atmosphere to obtain a ZrB2-coated zirconium powder composite material, designated as #2. The XRD pattern of the product prepared in this embodiment is shown below. Figure 1 As shown: ZrB2 is formed in the zirconium powder, with a ZrB2 content of 18.08%. The SEM image for this example is shown below. Figure 3 As shown, the coating thickness of the sample is 0.92 μm. The volumetric calorific value of the sample is 68.98 kJ·cm⁻¹ for the zirconium powder raw material. -3 Increased to 76.30 kJ·cm -3 .
[0025] Example 3:
[0026] Zirconium powder and boron powder were weighed at a mass ratio of 10:1 and then ball-milled at 300 rpm for 3 hours. The ball-milled sample was then placed in a vacuum tube furnace and held at 900°C for 90 minutes under an argon or helium atmosphere to obtain a ZrB2-coated zirconium powder composite material, designated as #3. The XRD pattern of the product prepared in this embodiment is shown below. Figure 1 As shown, ZrB2 was formed in the zirconium powder, with a ZrB2 content of 35.25%. The sample coating thickness was 1.82 μm, and the volumetric calorific value was 77.55 kJ·cm⁻¹. -3 .
[0027] Example 4:
[0028] Zirconium powder and boron powder were weighed at a mass ratio of 10:1, and then ball-milled at 300 rpm for 3 hours. The ball-milled sample was placed in a vacuum tube furnace and held at 1200℃ for 90 minutes under an argon or helium atmosphere to obtain a ZrB2-coated zirconium powder composite material, designated as No. 4#. The XRD pattern of the product prepared in this embodiment is shown below. Figure 1 As shown, ZrB2 was formed in the zirconium powder, with a ZrB2 content of 59.33%. The sample coating thickness was 2.14 μm, and the volumetric calorific value was 81.06 kJ·cm⁻¹. -3 .
[0029] Example 5:
[0030] Zirconium powder and boron powder were weighed at a mass ratio of 10:1, and then ball-milled at 300 rpm for 3 hours. The ball-milled sample was placed in a vacuum tube furnace and held at 900°C for 30 minutes under an argon or helium atmosphere to obtain a ZrB2-coated zirconium powder composite material, designated as No. 5#. The XRD pattern of the product prepared in this embodiment is shown below. Figure 1As shown, ZrB2 was formed in the zirconium powder, with a ZrB2 content of 22.65%. The sample coating thickness was 1.16 μm, and the volumetric calorific value was 76.98 kJ·cm⁻¹. -3 .
[0031] Example 6:
[0032] Zirconium powder and boron powder were weighed at a mass ratio of 10:1 and then ball-milled at 300 rpm for 3 hours. The ball-milled sample was then placed in a vacuum tube furnace and held at 900°C for 150 minutes under an argon or helium atmosphere to obtain a ZrB2-coated zirconium powder composite material, designated as No. 6#. The XRD pattern of the product prepared in this embodiment is shown below. Figure 2 As shown, ZrB2 was formed in the zirconium powder, with a ZrB2 content of 41.29%. The sample coating thickness was 1.95 μm, and the volumetric calorific value was 79.80 kJ·cm⁻¹. -3 .
[0033] Example 7:
[0034] Zirconium powder and boron powder were weighed at a mass ratio of 10:1 and then ball-milled at 300 rpm for 3 hours. The ball-milled sample was then placed in a vacuum tube furnace and held at 900°C for 300 minutes under an argon or helium atmosphere to obtain a ZrB2-coated zirconium powder composite material, designated as No. 7#. The XRD pattern of the product prepared in this embodiment is shown below. Figure 2 As shown, ZrB2 was formed in the zirconium powder, with a ZrB2 content of 43.83%. The sample coating thickness was 2.03 μm, and the volumetric calorific value was 80.58 kJ·cm⁻¹. -3 .
[0035] Example 8:
[0036] Zirconium powder and boron powder were weighed at a mass ratio of 20:1, and then ball-milled at 300 rpm for 3 hours. The ball-milled sample was placed in a vacuum tube furnace and held at 900°C for 90 minutes under an argon or helium atmosphere to obtain a ZrB2-coated zirconium powder composite material, designated as No. 8#. The XRD pattern of the product prepared in this embodiment is shown below. Figure 2 As shown, ZrB2 was formed in the zirconium powder, with a ZrB2 content of 19.70%. The sample coating thickness was 1.03 μm, and the volumetric calorific value was 76.31 kJ·cm⁻¹. -3 .
[0037] Example 9:
[0038] Zirconium powder and boron powder were weighed at a mass ratio of 100:1 and then ball-milled at 300 rpm for 3 hours. The ball-milled sample was then placed in a vacuum tube furnace and held at 900°C for 90 minutes under an argon or helium atmosphere to obtain a ZrB2-coated zirconium powder composite material, designated as No. 9#. The XRD pattern of the product prepared in this embodiment is shown below. Figure 2 As shown: ZrB2 is formed in the zirconium powder, with a ZrB2 content of 10.46%. The SEM image for this example is shown below. Figure 3 As shown, the sample coating thickness is 1.71 μm, and the surface is dotted. The sample volumetric calorific value is 72.99 kJ·cm⁻¹. -3 .
[0039] Example 10:
[0040] Zirconium powder and boron powder were weighed at a mass ratio of 10:1 and then ball-milled at 400 rpm for 1 hour. The ball-milled sample was placed in a vacuum tube furnace and held at 900°C for 90 minutes under an argon or helium atmosphere to obtain a ZrB2-coated zirconium powder composite material, designated as number 10#. The XRD pattern of the product prepared in this embodiment is shown below. Figure 2 As shown, ZrB2 was formed in the zirconium powder, with a ZrB2 content of 36.78%. The sample coating thickness was 1.87 μm, and the volumetric calorific value was 78.13 kJ·cm⁻¹. -3 .
[0041] Example 11:
[0042] Zirconium powder and boron powder were weighed at a mass ratio of 10:1 and then ball-milled at 200 rpm for 6 hours. The ball-milled sample was placed in a vacuum tube furnace and held at 900°C for 90 minutes under an argon or helium atmosphere to obtain a ZrB2-coated zirconium powder composite material, designated as No. 11#. The XRD pattern of the product prepared in this embodiment is shown below. Figure 2 As shown, ZrB2 was formed in the zirconium powder, with a ZrB2 content of 33.21%. The sample coating thickness was 1.55 μm, and the volumetric calorific value was 77.53 kJ·cm⁻¹. -3 .
[0043] The various embodiments of the present invention have been described above. These descriptions are exemplary and not exhaustive, nor are they limited to the disclosed embodiments. Many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.
Claims
1. A ZrB2-coated zirconium powder, characterized in that, It includes zirconium powder and a ZrB2 coating layer covering the zirconium powder, wherein the particle size of the zirconium powder is D. 90 The thickness of the coating layer is 0.1 μm-3 μm, and the mass percentage of ZrB2 is 1%-60%.
2. A method for preparing ZrB2-coated zirconium powder according to claim 1, characterized in that, Zirconium powder and boron powder are mixed evenly by ball milling, and then the mixed material is placed in a vacuum tube furnace for high-temperature sintering to obtain the ZrB2-coated zirconium powder.
3. The method for preparing ZrB2-coated zirconium powder according to claim 2, characterized in that, The zirconium powder has a purity of ≥95% and a particle size D90 ≤50μm.
4. The method for preparing ZrB2-coated zirconium powder according to claim 2, characterized in that, The boron powder includes amorphous boron powder and crystalline boron, with a particle size ≤ 1 micrometer.
5. The method for preparing ZrB2-coated zirconium powder according to claim 2, characterized in that, The mass ratio of zirconium powder to boron powder is 10:1-100:
1.
6. The method for preparing ZrB2-coated zirconium powder according to claim 2, characterized in that, The ball milling method includes: planetary ball milling or horizontal ball milling, with a ball milling speed of 200 rpm to 400 rpm and a ball milling time of 1 h to 6 h.
7. The method for preparing ZrB2-coated zirconium powder according to claim 2, characterized in that, The high-temperature sintering temperature is 700℃~1200℃, and the holding time is 30min~300min.
8. The method for preparing ZrB2-coated zirconium powder according to claim 2, characterized in that, The vacuum tube furnace is filled with argon or helium.
9. An application of the ZrB2-coated zirconium powder according to claim 1, characterized in that, It is used in solid propellant components.
Citation Information
Patent Citations
Method for reducing electrostatic spark sensitivity of zirconium powder by utilizing ALD (Atomic Layer Deposition) coating layer
CN105750541A
Preparation method of core-shell carbon-coated micro-nano zirconium powder
CN107297496A