A low residual stress rare earth microalloyed weathering seamless steel tube for locomotive bogie and a manufacturing method thereof
By adding alloying elements to low-carbon steel and optimizing the production process, the problems of atmospheric corrosion resistance and high residual stress of seamless steel pipes for locomotive bogies have been solved. This has enabled the application of low-cost, high-performance weather-resistant steel pipes suitable for locomotive bogies, thus promoting resource conservation and environmentally friendly social development.
Patent Information
- Application Number
- CN202411253675.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-09-09
AI Technical Summary
In the existing technology, there is a gap in the resistance of seamless steel tubes for locomotive bogies to atmospheric corrosion, and high residual stress leads to material failure and high maintenance costs.
By adding alloying elements such as Cu, Cr, Ni, V, Ti, and Re to low-carbon steel, and combining steelmaking, rolling, and heat treatment processes, Q355NH seamless steel pipes with low residual stress and excellent weather resistance are produced, meeting the GB/T 4171-2008 standard.
It achieves low residual stress, excellent weather resistance and weldability, reduces maintenance costs, extends service life, is suitable for locomotive bogies, and meets the construction requirements of a resource-saving and environmentally friendly society.
Smart Images

Figure CN119307827B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metallurgical materials technology, and in particular relates to a rare earth microalloyed weather-resistant seamless steel pipe for low residual stress locomotive bogies and its manufacturing method. Background Technology
[0002] Residual stress sources encompass all industrial sectors and the natural world, generating, accompanying, and influencing the entire manufacturing process and service life of materials and equipment. Currently, China has put forward new requirements for high-quality development, and residual stress, as a significant factor in the failure of materials and equipment, is closely related to these requirements. Data shows that in Europe, the cost increase due to residual stress distortion accounts for more than 4% of the total manufacturing cost; in the bearing industry alone, the additional costs caused by residual stress distortion are estimated to exceed US$1 billion annually. According to a survey by the Federation of German Industries (VDMA), the annual increase in manufacturing costs for eliminating residual stress distortion in the German power transmission manufacturing sector reaches as high as €850 million. Therefore, the American Society for Metals has made "striving to achieve zero deformation and maximum uniformity in heat-treated parts" its main research and development goal. This invention relates to a method for producing seamless steel pipes with low residual stress.
[0003] Weathering steel refers to low-alloy high-strength structural steel with excellent corrosion resistance achieved by adding small amounts of alloying elements (such as Cu, P, Cr, Ni, Mo, etc.). These alloying elements improve the rust layer structure under atmospheric corrosion, forming a dense internal rust layer that effectively prevents further penetration of corrosive media. Globally, approximately 20% to 40% of annual metal production is scrapped due to corrosion, resulting in over 100 million tons of metal lost annually. Atmospheric corrosion accounts for over 50% of total metal corrosion, and since steel used in the atmosphere typically accounts for over 60% of total steel production, this means that over 30 million tons of steel are scrapped globally each year due to atmospheric corrosion.
[0004] my country's demand for steel will continue to grow for some time to come. With such a large demand and use of steel, the corrosion rate is significant. The experience of industrialized countries worldwide has shown that the peak period of infrastructure investment often coincides with a peak period of frequent corrosion problems. Therefore, the effectiveness of corrosion control directly impacts the long-term development of the nation.
[0005] Weathering steel is used as structural steel in construction facilities such as railways, bridges, and high towers that are exposed to the atmosphere for extended periods. It often serves in environments including industrial atmospheres, marine atmospheres, acid rain, and smog, where corrosion is the primary cause of its damage and failure. With societal progress and technological development, people have placed more and higher demands on weathering steel, shifting from a singular focus on high strength to excellent comprehensive performance, primarily manifested in high strength and toughness, good weldability, and corrosion resistance.
[0006] Baotou Steel possesses abundant rare earth reserves, and therefore has vigorously researched and developed rare earth steel in recent years, as rare earth elements play a crucial role in steel. Studies have shown that adding rare earth elements to steel helps purify molten steel, refine grains, increase grain growth resistance, inhibit columnar crystal growth, alter the properties, morphology, and distribution of inclusions, and reduce corrosion initiation points, thereby improving various properties of the steel. Numerous studies, both domestically and internationally, have investigated the effects of rare earth elements on the corrosion resistance of steel. It is generally agreed that adding appropriate amounts of rare earth elements to steel can effectively improve its corrosion resistance. Researchers conducted four years of exposure corrosion tests at test sites in different atmospheric environments, including Qingdao, Jiangjin, Beijing, Wuhan, Qionghai, Guangzhou, and Wanning. They found that the corrosion rate of ordinary carbon steel was higher than that of weathering steel at all test sites, and that weathering steel with added rare earth elements exhibited better corrosion resistance compared to the original weathering steel.
[0007] A search of available literature revealed no relevant reports or literature on weathering-resistant seamless steel tubes for low residual stress locomotive bogies. Q355NH is the steel grade for weathering structural steel in standard GB / T 4171-2008. Developing weathering-resistant structural steel tubes of Q355NH is of great significance. It can not only fill the gap in seamless tubes for locomotive bogies that resist atmospheric corrosion, but also lay the foundation for the next step of developing higher-grade weathering-resistant seamless tubes. At the same time, it can also leverage Baotou Steel's abundant rare earth resources, resulting in good economic benefits.
[0008] The present invention relates to a rare earth microalloyed weather-resistant seamless steel tube for locomotive bogies and its production method, which can fill the gap in the field of atmospheric corrosion resistant seamless tubes for locomotive bogies, and lay the foundation for the next step of developing weather-resistant seamless tubes of higher steel grades. At the same time, it can also take advantage of Baotou Steel's abundant rare earth resources, and has good economic benefits. Summary of the Invention
[0009] The purpose of this invention is to provide a rare earth microalloyed weather-resistant seamless steel tube for locomotive bogies with low residual stress and its manufacturing method. By rationally designing the composition, alloying elements such as Cu, Cr, Ni, V, Ti, and Re are added to low carbon steel. Corrosion-resistant seamless tube Q355NH for locomotive bogies is produced through steelmaking, rolling, and heat treatment processes, and its performance meets the requirements of standard GB / T 4171-2008.
[0010] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:
[0011] This invention discloses a rare-earth microalloyed weather-resistant seamless steel tube for low residual stress locomotive bogies. The chemical elements and their mass percentages of the weather-resistant seamless steel tube are as follows: C 0.12-0.16%; Si 0.30-0.50%; Mn 1.00-1.10%; P≤0.020%; S≤0.010%; Cr 0.45-0.70%; V≤0.10%; Cu≤0.30%; Ni≤0.40%; Ti≤0.04%; Re≤0.002%; the remainder being Fe and unavoidable impurities, with a total mass fraction of 100%.
[0012] Furthermore, the chemical elements and their mass percentages of the weathering seamless steel pipe are as follows: C 0.14%; Si 0.32%; Mn 1.03%; P 0.014%; S 0.005%; Cr 0.47%; V 0.09%; Cu 0.29%; Ni 0.39%; Ti 0.029%; Re 0.0004%; the remainder being Fe and unavoidable impurities, totaling 100% by mass.
[0013] Furthermore, the chemical elements and their mass percentages of the weathering seamless steel pipe are as follows: C 0.14%; Si 0.33%; Mn 1.09%; P 0.013%; S 0.006%; Cr 0.47%; V 0.08%; Cu 0.28%; Ni 0.35%; Ti 0.038%; Re 0.0005%; the remainder being Fe and unavoidable impurities, totaling 100% by mass.
[0014] Furthermore, the chemical elements and their mass percentages of the weathering seamless steel pipe are as follows: C 0.13%; Si 0.32%; Mn 1.05%; P 0.012%; S 0.005%; Cr 0.45%; V 0.08%; Cu 0.27%; Ni 0.39%; Ti 0.035%; Re 0.0005%; the remainder being Fe and unavoidable impurities, totaling 100% by mass.
[0015] Furthermore, the chemical elements and their mass percentages of the weathering seamless steel pipe are as follows: C 0.14%; Si 0.30%; Mn 1.05%; P 0.011%; S 0.004%; Cr 0.46%; V 0.09%; Cu 0.26%; Ni 0.35%; Ti 0.038%; Re 0.0005%; the remainder being Fe and unavoidable impurities, totaling 100% by mass.
[0016] Furthermore, the chemical elements and their mass percentages of the weathering seamless steel pipe are as follows: C 0.13%; Si 0.31%; Mn 1.07%; P 0.014%; S 0.005%; Cr 0.48%; V 0.08%; Cu 0.29%; Ni 0.32%; Ti 0.037%; Re 0.0005%; the remainder being Fe and unavoidable impurities, totaling 100% by mass.
[0017] The role of each element:
[0018] Carbon (C): It is detrimental to the atmospheric corrosion resistance of steel. At the same time, C affects the weldability, cold brittleness and stamping performance of steel. For the present invention, the C content is 0.12-0.16%.
[0019] Silicon (Si): In steel, it mainly exists in a solid solution state, primarily for solid solution strengthening. It does not form carbonitrides and can significantly increase the volume fraction of ferrite and strengthen the ferrite microstructure. For this invention, the Si content is 0.30–0.50%.
[0020] Manganese (Mn): There is no consensus on the effect of manganese on corrosion resistance. Most scholars believe that manganese can improve the corrosion resistance of steel in marine atmospheres, but has almost no effect on corrosion resistance in industrial atmospheres. Typically, the w(Mn) content in weathering steel is 0.5% to 2.0%. Therefore, for the purposes of this invention, the Mn content ranges from 1.00% to 1.10%.
[0021] Chromium (Cr): The alloying element Cr can react with the steel matrix to form a passivation film, making the rust layer on the steel surface denser, increasing its corrosion potential, and reducing the self-corrosion current, thereby achieving the purpose of improving the passivation ability of metallic materials. Therefore, the Cr content is 0.45-0.70%.
[0022] Vanadium (V): V mainly forms stable carbides and nitrides, refines austenite grains, and improves the strength and low-temperature toughness after normalizing, as well as the tempering stability of the material, ensuring a balance between strength and toughness. Therefore, V ≤ 0.10% in this invention.
[0023] Copper (Cu): The most effective alloying element in weathering steel. Cu was first added to weathering steel, and when 0.2%–0.4% Cu is added, it exhibits superior corrosion resistance compared to ordinary carbon steel in rural, industrial, and marine atmospheres. Cu can form secondary precipitation products on the steel surface, acting as a cathode to induce anodic passivation, thereby improving its corrosion resistance. Cu's effect in counteracting the harmful effects of sulfur (S) in steel is significant; the higher the S content in the steel, the more pronounced the relative effect of Cu in reducing the corrosion rate. This is because Cu reacts with S to form insoluble sulfides. Therefore, in this invention, Cu ≤ 0.30%.
[0024] Nickel (Ni): A relatively stable element, the addition of Ni can shift the self-corrosion potential of steel in a positive direction, increasing the steel's stability. Atmospheric exposure tests show that when the Ni content is around 4%, it can significantly improve the atmospheric corrosion resistance of coastal weathering steel. The excellent corrosion resistance of the recently developed Cr-free coastal weathering steel containing 3% Ni in Japan proves that Ni enrichment in the stable rust layer can effectively inhibit the intrusion of chloride ions, promote the formation of a protective rust layer, and reduce the corrosion rate of the steel. Therefore, in this invention, Ni ≤ 0.40%.
[0025] Titanium (Ti): Ti in steel is characterized by its extremely strong affinity for oxygen, nitrogen, sulfur, and carbon, exhibiting significant deoxidizing, denitrifying, and sulfur-binding properties, and a significant carbide-forming effect. It acts as a carbide-forming agent, providing stability and resistance to intergranular corrosion. It also possesses the characteristic of refining grain size. Therefore, in this invention, Ti ≤ 0.04%.
[0026] Rare earth elements (Re): Adding appropriate amounts of rare earth elements to steel helps purify the molten steel, refine grains, increase grain growth resistance, inhibit columnar crystal growth, alter the properties, morphology, and distribution of inclusions, and reduce corrosion initiation points, thereby improving various properties of the steel. Adding appropriate amounts of rare earth elements to steel can effectively improve its corrosion resistance. Therefore, in this invention, Re ≤ 0.002%.
[0027] A method for manufacturing rare-earth microalloyed weather-resistant seamless steel tubes for low residual stress locomotive bogies includes:
[0028] Steelmaking process flow: Blast furnace hot metal → Hot metal pretreatment → Converter smelting → LF ladle refining → VD vacuum treatment → Continuous casting → Slow cooling of billets → Warehousing; where:
[0029] Desulfurized hot metal is used, and the final slag basicity of converter smelting is ≥3.0. Final carbon control is crucial to prevent over-oxidation and ultra-low carbon tapping. The tapping temperature is 1615–1635℃. Ferrosilicon and ferromanganese are used for deoxidation and alloying, with aluminized deoxidation for final deoxidation. An appropriate amount of quicklime is added during tapping. In the LF refining process, argon is blown normally throughout as required, and the temperature is increased gradually from low to high argon charge to create white slag. Copper and nickel alloys are added during the converter process, while other alloys are added in the later stages of refining. Composition is fine-tuned in the later stages of refining, with rare earth alloys added proportionally. A suitable amount of high-calcium wire is fed before the end of refining. The VD deep vacuum degree is ≤0. 0.12 kPa, deep vacuum time ≥ 10 minutes. During the vacuuming process, the boiling of the molten steel should be monitored at all times and the argon pressure should be adjusted in a timely manner. After vacuum treatment, the soft blowing time should be ≥ 10 minutes. At the same time, attention should be paid to the weak stirring effect, and the molten steel should not be exposed. Electromagnetic stirring technology is used in the continuous casting process. The superheat of the continuously cast steel is controlled within the range of 20℃~30℃ to ensure constant casting speed. The nozzles of the secondary cooling water should ensure uniform spraying, and no interruption or water jet is allowed. The billet should be sent to the slow cooling pit for slow cooling in a timely manner. The slow cooling time should be greater than 48 hours. The billet temperature should be reduced to below 100℃ before it can be removed from the pit. This method can obtain high-quality round billets with low P, low S and uniform composition.
[0030] Tube manufacturing process: Continuous casting billet → sawing → ring furnace heating → piercing → PQF three-roll limiting mandrel continuous rolling → tube removal → tension reduction → cooling → sawing → heat treatment → straightening; where:
[0031] Before loading the tube billet into the furnace, an inspection should be carried out. The surface quality of the tube billet should meet the requirements of Q / BG 524. Severe slag pits and scale should be ground. The quality of the sawed end face should be checked, and tube billets with defects exceeding the standard, such as central cracks and central shrinkage cavities, should be rejected in time. The temperature of the ring furnace holding section is 1260±20℃. During piercing, the center lines of the piercing mill body and the front and rear rolling lines must be kept consistent. The mandrel extension should be strictly controlled according to the requirements. The temperature of the round billet after piercing is 1200±20℃. The continuous rolling inlet temperature is 1110±20℃. During the rolling process, the surface quality of the rough tube and mandrel should be checked. High-pressure water descaling should be turned on. The pressure range of high-pressure descaling water is 9~12MPa. The temperature after tension reduction is 940±20℃. The spray direction of the roller table cooling water should be adjusted to ensure that it does not spray onto the inner surface of the tube body. High-precision, high-quality tube bodies of different sizes can be obtained by combining the PQF of the three-roll limited-movement mandrel continuous rolling mill with high-end hot rolling control technology.
[0032] Heat treatment process: normalizing + air cooling; the heating temperature for normalizing is usually 30-50℃ above AC3, the normalizing temperature is 930℃±10℃, and the holding time is 70±5 minutes; after normalizing, straightening is necessary. During straightening, the straightening force should be strictly controlled to ensure the bending requirements of the steel pipe, and there should be no straightening concavity, straightening ellipse, or straightening crack.
[0033] Compared with the prior art, the beneficial technical effects of the present invention are as follows:
[0034] The rational selection of alloying elements and appropriate element content ratios in this invention result in a steel grade with a low carbon equivalent. This provides excellent weather resistance while also exhibiting good weldability and low cost. The rational smelting, continuous casting, rolling, and heat treatment processes ensure high dimensional accuracy of the steel pipe. This invention allows for paint-free use, significantly reducing maintenance costs and environmental pollution associated with painting. Furthermore, it lowers the maintenance requirements for steel structures during service, greatly reducing direct maintenance costs and traffic interruption costs, and extending service life. This has significant implications for the promotion of steel structures. This invention marks the first application of seamless weathering steel pipes in locomotive bogies in China. It features high strength, high toughness, low-temperature resistance, easy welding, and good atmospheric corrosion resistance, making a significant contribution to building a resource-saving and environmentally friendly society and achieving carbon peaking and carbon neutrality. Attached Figure Description
[0035] The present invention will be further described below with reference to the accompanying drawings.
[0036] Figure 1 The metallographic structure of the finished steel pipe in Example 1 is shown. Detailed Implementation
[0037] A rare-earth microalloyed weather-resistant seamless steel tube for low residual stress locomotive bogies
[0038] The chemical composition of the steel pipe obtained according to the present invention, taking a production specification of Φ307×13mm as an example, is shown in Table 1:
[0039] Table 1. Statistical results of the chemical composition (wt%) of the steel pipe of the present invention
[0040]
[0041] As can be seen from Table 1, the chemical composition of the steel pipe has a very small deviation, which fully meets the design requirements of this invention for the steel grade. The stable composition content is conducive to temperature control during heat treatment, thus providing a prerequisite for the pipe to have good structure and performance.
[0042] Steelmaking process: For producing steel pipes with a specification of Φ307×13mm, the continuous casting machine is inspected before production to ensure good arc and center alignment; the pressure of the straightening machine is reduced to ensure normal straightening of the billet; the nozzles blocking the secondary cooling zone are replaced to ensure uniform billet size in the secondary cooling zone; the casting speed is appropriately increased, and if the casting speed cannot be guaranteed, the flow is shut off in a tight sequence to maintain the pouring speed; the billet straightening temperature is increased to not lower than 930℃; the superheat of the molten steel is controlled at 30℃ to ensure good melting of the mold flux and uniform slag discharge. Copper tubes are selected for the early and middle stages of the mold to ensure the inverted taper of the mold. After the billet exits the secondary cooling zone, it is covered with asbestos board for insulation to increase the billet straightening temperature. The billet should be promptly sent to the slow cooling pit for slow cooling for more than 48 hours. Through these measures, high-quality round billets are obtained.
[0043] Pipe rolling process: The round billet is heated in an annular furnace at 1280℃. Whether the temperature range of the billet during hot rolling is within the plastic deformation zone of the steel grade is crucial, affecting the inner and outer surface quality of the steel pipe and the load on the rolling mill. During production, the heating temperature of the annular furnace is strictly controlled to not exceed 1270℃. The billet is placed within the optimal temperature range and plastic deformation zone. The time in the furnace should not be too long. Piercing adopts a low-speed bite and high-speed rolling process. The temperature after piercing is 1200℃, the temperature entering the continuous rolling mill is 1100℃, the temperature after sizing is 925℃, followed by cooling and sawing.
[0044] Heat Treatment: The production of seamless steel tubes for locomotive bogies, resistant to atmospheric corrosion, requires normalizing. However, when producing large-diameter, thick-walled steel tubes, lower strength can easily occur. The normalizing process is 930℃ + holding for 70 minutes. Insufficient holding time negatively impacts the temperature uniformity during heating; therefore, a minimum of 70 minutes is recommended. The normalizing furnace process involves a heating section at 930℃, a holding section at 920℃ for 70 minutes, followed by air cooling.
[0045] The mechanical properties of the steel pipe of this invention are shown in Table 2. As can be seen from Table 2, the steel pipe with specifications of Φ307×13mm produced by the method of this invention can well meet the requirements of Q355NH steel grade in the national standard GB / T 4171-2008, exhibiting excellent low-temperature impact toughness, with a longitudinal impact strength greater than 27J at -40℃. Generally, structural steel undergoes a transition from ductile to brittle as the temperature decreases. If structural steel is used in the transition temperature or brittle state, low-stress failure is inevitable even at low stress levels. For materials used at low temperatures, in addition to requiring a certain strength, sufficient toughness is essential. Seamless Q355NH pipe has very high requirements for low-temperature impact; the full-size impact energy (-40℃) of the steel pipe is required to be KV2≥27J. As can be seen from Table 2, the low-temperature impact performance of the steel pipe is excellent, far exceeding the standard requirement of 27J, reaching 230J, demonstrating very excellent toughness.
[0046] Table 2 Mechanical properties of the steel pipe of the present invention
[0047]
[0048] The steel pipe samples of this invention were taken for laboratory analysis. After grinding and polishing, the samples were etched with 4% nitric acid alcohol and the microstructure was observed under an optical microscope. The grain size was rated according to the requirements of GB / T 6394-2002 standard, and the grade was not lower than 8.5. Non-metallic inclusions were rated according to A in GB / T 10561-2005. The results are shown in Table 3.
[0049] Table 3. Steel pipe of the present invention, including impurities and grain size.
[0050]
[0051] Note: F represents ferrite, and P represents pearlite.
[0052] After heat treatment, the metallographic structure of the steel pipe in Example 1 is as follows. Figure 1 .from Figure 1 As can be seen, the steel pipe has a microstructure of ferrite and pearlite, which is uniform and fine with a grain size of grade 10. The steel pipe contains appropriate amounts of V and Ti. When austenite transforms into ferrite, precipitates will be formed. The precipitates can inhibit the growth of ferrite grains and improve the strength of the matrix, as well as inhibit the transformation of bainite, making the microstructure more uniform. Heat treatment further refines the grains. The uniform and fine microstructure gives the steel pipe good strength and toughness.
[0053] The presence of residual stress reduces the material's strength and fatigue resistance. In corrosive environments, it can lead to stress corrosion and material failure. Furthermore, during processing or use, the release of internal stress can cause changes in the material's shape and dimensions, even resulting in cracking. Using the residual stress circumferential displacement measurement method in GB / T 43898-2024, the residual stress of the steel pipes in Examples 1 to 5 of this invention was measured to be 75–95 MPa, lower than the recommended minimum limit of 100 MPa in this standard, effectively improving the corrosion resistance of the steel pipe. Therefore, the weather-resistant seamless steel pipe for bogies produced using this invention is a low-residual-stress seamless steel pipe.
[0054] Cyclic immersion tests simulate the real service conditions of metallic materials in the atmosphere, allowing for the simulation of different industrial environments and the acquisition of corrosion resistance data for the test steel within a short period. The patented finished steel pipe underwent cyclic immersion tests according to the standard "Cyclic Immersion Corrosion Test Method for Weathering Steel for Railways" TB / T 2375-93. The simulated environment was an industrial atmosphere, and the control steel was Q345B seamless structural steel pipe of the same strength grade. The 72-hour cyclic immersion test results showed that the relative corrosion rate of the patented finished steel pipe was 18% lower than that of Q345B seamless structural steel pipe. This indicates that under the same corrosive environment, the atmospheric corrosion resistance of the patented finished steel pipe is superior to that of Q345B.
[0055] The seamless steel pipe for weathering locomotive bogies with specifications of Φ307×13mm produced using this invention features a rational selection of alloying elements and an appropriate element content ratio, making the steel easy to produce and cost-effective. The rational smelting, continuous casting, rolling, and heat treatment processes result in steel pipes with low residual stress, high strength, excellent low-temperature impact toughness, and high dimensional accuracy. The product of this invention exhibits good corrosion resistance, low residual stress, high dimensional accuracy, good internal and external surface quality, high strength, and uniform and stable overall pipe performance. In particular, it possesses excellent low-temperature toughness, meeting the requirements for use in low-temperature environments. Furthermore, the low-carbon equivalent composition design provides excellent weldability, improving user production efficiency and fully meeting the requirements of the national standard GB / T4171-2008.
[0056] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.
Claims
1. A rare-earth microalloyed weather-resistant seamless steel tube for low residual stress locomotive bogies, characterized in that, The chemical elements and their mass percentages of the weather-resistant seamless steel pipe are as follows: C 0.12~0.16%; Si 0.30~0.50%; Mn 1.00~1.10%; P≤0.020%; S≤0.010%; Cr 0.45~0.70%; V ≤0.10%; Cu ≤0.30%; Ni≤0.40%; Ti≤0.04%; Re≤0.002%; the remainder is Fe and unavoidable impurities, with a total mass fraction of 100%; its manufacturing method includes: Steelmaking process flow: Blast furnace hot metal → Hot metal pretreatment → Converter smelting → LF ladle refining → VD vacuum treatment → Continuous casting → Slow cooling of billets → Warehousing; where: Desulfurized hot metal is used, and the final slag basicity of converter smelting is ≥3.
0. Final carbon control is crucial to prevent over-oxidation and ultra-low carbon tapping. The tapping temperature is 1615–1635℃. Ferrosilicon and ferromanganese are used for deoxidation and alloying, with aluminized deoxidation for final deoxidation. An appropriate amount of quicklime is added during tapping. In the LF refining process, argon is blown normally throughout as required, and the temperature is increased gradually from low to high argon charge to create white slag. Copper and nickel alloys are added during the converter process, while other alloys are added in the later stages of refining. Composition is fine-tuned in the later stages of refining, with rare earth alloys added proportionally. A suitable amount of high-calcium wire is fed before the end of refining. The VD deep vacuum degree is ≤0. 0.12 kPa, deep vacuum time ≥ 10 minutes. During the vacuuming process, the boiling of the molten steel should be monitored at all times and the argon pressure should be adjusted in a timely manner. After vacuum treatment, the soft blowing time should be ≥ 10 minutes. At the same time, attention should be paid to the weak stirring effect, and the molten steel should not be exposed. Electromagnetic stirring technology is used in the continuous casting process. The superheat of the continuously cast steel is controlled within the range of 20℃~30℃ to ensure constant casting speed. The nozzles of the secondary cooling water should ensure uniform spraying, and no interruption or water jet is allowed. The billet should be sent to the slow cooling pit for slow cooling in a timely manner. The slow cooling time should be greater than 48 hours. The billet temperature should be reduced to below 100℃ before it can be removed from the pit. This method can obtain high-quality round billets with low P, low S and uniform composition. Tube manufacturing process: Continuous casting billet → sawing → ring furnace heating → piercing → PQF three-roll limiting mandrel continuous rolling → tube removal → tension reduction → cooling → sawing → heat treatment → straightening; where: Before loading the tube billet into the furnace, an inspection should be carried out. The surface quality of the tube billet should meet the requirements of Q / BG 524. Severe slag pits and scale should be ground. The quality of the sawed end face should be checked, and tube billets with defects exceeding the standard, such as central cracks and central shrinkage cavities, should be rejected in time. The temperature of the ring furnace holding section is 1260±20℃. During piercing, the center lines of the piercing mill body and the front and rear rolling lines must be kept consistent. The mandrel extension should be strictly controlled according to the requirements. The temperature of the round billet after piercing is 1200±20℃. The continuous rolling inlet temperature is 1110±20℃. During the rolling process, the surface quality of the rough tube and mandrel should be checked. High-pressure water descaling should be turned on. The pressure range of high-pressure descaling water is 9~12MPa. The temperature after tension reduction is 940±20℃. The spray direction of the roller table cooling water should be adjusted to ensure that it does not spray onto the inner surface of the tube body. High-precision, high-quality tube bodies of different sizes can be obtained by combining the PQF of the three-roll limited-movement mandrel continuous rolling mill with high-end hot rolling control technology. Heat treatment process: normalizing + air cooling; the heating temperature for normalizing is usually 30-50℃ above AC3, the normalizing temperature is 930℃±10℃, and the holding time is 70±5 minutes; after normalizing, straightening is necessary. During straightening, the straightening force should be strictly controlled to ensure the bending requirements of the steel pipe, and there should be no straightening concavity, straightening ellipse, or straightening crack.
2. The rare-earth microalloyed weather-resistant seamless steel tube for low residual stress locomotive bogies according to claim 1, characterized in that, The chemical elements and their mass percentages of the weathering seamless steel pipe are as follows: C 0.14%; Si 0.32%; Mn 1.03%; P 0.014%; S 0.005%; Cr 0.47%; V 0.09%; Cu 0.29%; Ni 0.39%; Ti 0.029%; Re 0.0004%; the remainder is Fe and unavoidable impurities, with a total mass fraction of 100%.
3. The rare-earth microalloyed weather-resistant seamless steel tube for low residual stress locomotive bogies according to claim 1, characterized in that, The chemical elements and their mass percentages of the weathering seamless steel pipe are as follows: C 0.14%; Si 0.33%; Mn 1.09%; P 0.013%; S 0.006%; Cr 0.47%; V 0.08%; Cu 0.28%; Ni 0.35%; Ti 0.038%; Re 0.0005%; the remainder is Fe and unavoidable impurities, with a total mass fraction of 100%.
4. The rare-earth microalloyed weather-resistant seamless steel tube for low residual stress locomotive bogies according to claim 1, characterized in that, The chemical elements and their mass percentages of the weathering seamless steel pipe are as follows: C 0.13%; Si 0.32%; Mn 1.05%; P 0.012%; S 0.005%; Cr 0.45%; V 0.08%; Cu 0.27%; Ni 0.39%; Ti 0.035%; Re 0.0005%; the remainder is Fe and unavoidable impurities, with a total mass fraction of 100%.
5. The rare-earth microalloyed weather-resistant seamless steel tube for low residual stress locomotive bogies according to claim 1, characterized in that, The chemical elements and their mass percentages of the weathering seamless steel pipe are as follows: C 0.14%; Si 0.30%; Mn 1.05%; P 0.011%; S 0.004%; Cr 0.46%; V 0.09%; Cu 0.26%; Ni 0.35%; Ti 0.038%; Re 0.0005%; the remainder is Fe and unavoidable impurities, with a total mass fraction of 100%.
6. The rare-earth microalloyed weather-resistant seamless steel tube for low residual stress locomotive bogies according to claim 1, characterized in that, The chemical elements and their mass percentages of the weathering seamless steel pipe are as follows: C 0.13%; Si 0.31%; Mn 1.07%; P 0.014%; S 0.005%; Cr 0.48%; V 0.08%; Cu 0.29%; Ni 0.32%; Ti 0.037%; Re 0.0005%; the remainder is Fe and unavoidable impurities, with a total mass fraction of 100%.
Citation Information
Patent Citations
Rare earth microalloyed Q345qDNH-grade weather-proof seamless steel pipe for bridge and manufacturing method thereof
CN115323286A