Composite metal foil and cable
By chemically or physically treating the composite metal foil support layer and setting a transition layer, the problems of poor tinning effect and insufficient elongation of the composite metal foil are solved, achieving efficient welding and stable connection of cable shielding effect.
Patent Information
- Application Number
- CN202411511104.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-28
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-10-28
AI Technical Summary
Existing composite metal foils have poor tinning effect and insufficient elongation during welding, which makes the shielding layer prone to breakage, affecting the connection stability and electromagnetic shielding performance of cables.
By chemically or physically treating the support layer to increase its dyne value to 54-58, and setting a transition layer between the support layer and the shielding layer, the affinity and bonding force between the support layer and the molten solder are enhanced. The surface of the support layer is modified by immersion in an alkaline solution or by high-frequency, high-voltage plasma treatment, and a transition layer is formed by vacuum sputtering to improve the tinning effect and elongation.
It improves the tinning rate and elongation of composite metal foil, enhances the welding reliability and electromagnetic shielding performance of cable joints, reduces the risk of shielding layer breakage, and meets the requirements for stable cable connection.
Smart Images

Figure CN119314727B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of cable technology, and more specifically to a composite metal foil and cable. Background Technology
[0002] Wires and cables are the medium for energy and information transmission, playing a vital role in economic and social development. In recent years, with the development of the information age, cables used to transmit information and data signals support the communication needs of modern society. To reduce external electromagnetic interference and achieve accurate and stable signal transmission, a shielding layer is generally added to the cable. Currently, metal braided layers, metal foil layers, combined shielding layers, or semiconductor layers are generally selected as shielding layers depending on the application scenario. To improve the performance of the shielding layer, it is often combined with high-performance thermoplastic engineering plastics. Among them, composite copper foil is widely used in the electronics industry because it combines the excellent mechanical properties of polymers with the excellent conductivity of metal materials. However, when welding composite copper foil, the substrate needs to be melted for welding. Thinner composite materials can melt quickly, but this will lead to a decrease in the elongation of the shielding layer, causing the shielding layer to break when the cable is wound, and the shielding effect to fail. If a thicker substrate is used to form composite copper foil, the overall elongation can be guaranteed, but it is not easy to melt when making joints, resulting in high difficulty in tinning and poor welding effect. Therefore, it hinders the application of composite copper foil in cable shielding materials. Summary of the Invention
[0003] Therefore, the technical problem to be solved by the present invention is to overcome the defect of poor tin effect on the surface of composite metal foil in the prior art, thereby providing a composite metal foil and cable.
[0004] Another technical problem to be solved by the present invention is to overcome the defect of poor elongation of composite metal foil in the prior art, thereby providing a composite metal foil and cable.
[0005] The present invention provides a composite metal foil for cable shielding, comprising a support layer and a shielding layer stacked together, wherein the dyne value of the surface of the support layer away from the shielding layer is 54 to 58.
[0006] In this invention, when the dyne value of the surface of the support layer of the composite metal foil furthest from the shielding layer is 54-58, the affinity between the support layer and the molten solder is improved during tinning, reducing the difficulty of contact between the molten solder and the support layer, increasing the tinning rate on the support layer, and thus improving the tinning effect. Simultaneously, the composite metal foil exhibits strong electromagnetic shielding performance. For example, the dyne value of the surface of the support layer furthest from the shielding layer is 54, 55, 56, 57, 58, or any range of two values.
[0007] Specifically, in this invention, the surface of the support layer of the composite metal foil is treated by chemical or physical methods, such as immersion in acidic solution, immersion in alkaline solution, plasma treatment, corona treatment, etc.
[0008] In some embodiments, the chemical treatment method specifically involves immersing the support layer in an alkaline solution for 20-40 seconds. During this immersion, hydroxide ions in the alkaline solution attack the ester bonds of ethylene glycol in the support layer, causing a hydrolysis reaction that breaks the surface molecular chains. This transforms the surface portion of the material from polyester to sodium terephthalate and ethylene glycol, softening the surface and causing slight expansion. On one hand, this reduces the surface strength of the support layer, allowing the alloy layer to penetrate better during sputtering, improving the adhesion between the sputtered layer and the support layer, and increasing the peel strength between the metal layer and the support layer after copper plating. The damaged surface of the support layer allows it to dissolve more quickly in the molten solder when welding cable connectors, thus improving the tinning effect of the shielding layer. On the other hand, immersion in the alkaline solution increases the dyne value of the support layer, enhancing its affinity with the molten solder during tinning. This helps the molten solder to contact the support layer more fully during welding, melting the support layer, increasing the tinning rate, and improving the reliability of the composite metal foil during connector welding.
[0009] In some embodiments, when the support layer is chemically treated, the concentration of the alkaline substance in the alkaline solution is 5 wt% to 10 wt%. Exemplarily, the alkaline substance is at least one selected from sodium hydroxide, potassium hydroxide, calcium hydroxide, and barium hydroxide.
[0010] The concentration of alkaline substances in the alkaline solution should not be too high, otherwise it will cause excessive damage to the support layer and reduce the elongation at break after copper plating. Conversely, a concentration that is too low will result in poor treatment performance. For example, the concentration of alkaline substances in the alkaline solution can be 5 wt%, 6 wt%, 8 wt%, and 10 wt%, or any range of two such values. Furthermore, to improve the efficiency of chemical treatment, when the concentration of alkaline substances in the alkaline solution is low, an ultrasonic treatment step can be added during the chemical treatment process. This can accelerate the reaction rate and improve the uniformity of surface treatment, thereby improving the tinning effect of the composite metal foil and simultaneously increasing its elongation.
[0011] In one embodiment, the support layer is treated on both sides simultaneously using an alkaline solution to modify both surfaces of the support layer. This not only improves the bonding force between the support layer and the shielding layer, but also increases the elongation and tinning efficiency of the composite metal foil, further improving the processing efficiency. It is highly operable, as only the surface material is treated, and sodium hydroxide will not attack the interior of the material.
[0012] Taking sodium hydroxide as an alkaline substance as an example, and polyethylene terephthalate as the main material of the support layer, the reaction equation of sodium hydroxide and polyethylene terephthalate is shown in equation (Ⅰ).
[0013]
[0014] In formula (Ⅰ), the value of n is between 50 and 200, preferably between 50 and 100.
[0015] In some embodiments, the physical processing method specifically involves using high-frequency, high-voltage corona discharge on the surface of the support layer away from the shielding layer. The generated low-temperature plasma produces a free radical reaction on the surface of the support layer, causing the polymer in the support layer to crosslink. This results in a rough, granular surface on the support layer, while simultaneously enhancing the wettability of the support layer surface to polar solvents. The generated plasma enters the support layer under the action of electric shock and penetration, destroying the molecular structure of the support layer and oxidizing and polarizing the surface molecules to be treated, thereby modifying the surface material of the support layer.
[0016] To further improve the modification effect of the support layer, enhance the cross-linking reaction of the polymer in the support layer, and improve the tinning effect of the composite metal foil, the voltage during corona discharge of the support layer is 5000-15000V / m. 2 For example, the voltage is 5000V / m. 2 6500V / m 2 7000V / m 2 7500V / m 2 8000V / m 2 12000V / m 2 13500V / m 2 15000V / m 2 Or an interval consisting of any two values.
[0017] In some embodiments, the two sides of the support layer are treated separately using different powers. The copper-plated side is electroplated with a lower power to achieve a dyne value of 44-50. The support layer is treated before electroplating to improve the adhesion between the sputtered metal layer and the support layer. The non-plated side is treated with a higher power corona or plasma after copper plating to achieve a surface dyne value of 54 or higher to increase surface energy and improve wettability with molten solder, which helps dissolve the support layer before soldering.
[0018] For details, please refer to [link / reference]. Figure 1As shown, in order to further enhance the peel strength of the shielding layer and the support layer, a transition layer is provided between the support layer and the shielding layer. More specifically, the transition layer is a metal layer formed on the support layer by means of vacuum sputtering, evaporation plating, spraying, chemical plating, etc. In this invention, the support layer is made conductive by the metal layer, and the shielding layer is subsequently formed by electroplating, which enhances the peel strength between the shielding layer and the support layer and improves the shielding effectiveness.
[0019] The maximum depth of the transition layer extending into the support layer is 0.01–0.1 μm, as detailed in the reference document. Figure 2 , Figure 2 In this context, H represents the distance between the plane containing the farthest point of the transition layer facing away from the support layer and the lowest point of the side of the support layer facing the transition layer, indicating the maximum depth of the transition layer penetrating the support layer. For example, the maximum depth of the transition layer penetrating the support layer is 0.01 μm, 0.02 μm, 0.04 μm, 0.07 μm, 0.9 μm, and 0.1 μm, or any two of these values. By limiting the maximum depth of the transition layer penetrating the support layer to 0.01–0.1 μm, this invention not only enhances the peel strength between the shielding layer and the support layer, but also accelerates the dissolution rate of the support layer in the molten solder after the support layer is damaged, resulting in better tinning. Furthermore, the composite metal foil provided in this embodiment exhibits strong electromagnetic shielding performance.
[0020] Specifically, the maximum depth of the transition layer penetrating the support layer refers to the maximum value of the depth of the transition layer penetrating the support layer. In some embodiments, the depth of the transition layer penetrating the support layer can be measured by slicing using scanning electron microscopy, optical electron microscopy, or focused ion beam, or other measurement methods can be used. This invention does not limit this, as long as the depth of the transition layer penetrating the support layer can be accurately measured and the maximum depth can be obtained.
[0021] In some embodiments, the transition layer comprises a conductive metal, polyethylene terephthalate, sodium terephthalate, and ethylene glycol. The conductive metal is made of at least one of the same materials as the shielding layer. Specifically, if the shielding layer is made of copper or aluminum, the conductive metal may be copper, aluminum, or a mixture of copper and aluminum.
[0022] To improve the bonding strength between the support layer and the shielding layer, in the transition layer, the content of polyethylene terephthalate is 2wt% to 30wt%, the content of sodium terephthalate is 2wt% to 15wt%, and the content of ethylene glycol is 5wt% to 25wt%. For example, the content of polyethylene terephthalate in the transition layer is 2wt%, 5wt%, 10wt%, 12wt%, 20wt%, 25wt%, 30wt%, or any two of these values; the content of sodium terephthalate is 2wt%, 5wt%, 10wt%, 12wt%, 13wt%, 15wt%, or any two of these values; and the content of ethylene glycol is 5wt%, 8wt%, 15wt%, 20wt%, 25wt%, or any two of these values.
[0023] To improve the elongation and tinning effect of the composite metal foil, the support layer has a hybrid layer on the side opposite to the shielding layer, the hybrid layer comprising polyethylene terephthalate, sodium terephthalate and ethylene glycol.
[0024] Optionally, the blending layer and the transition layer can be set as separate layers or as blended layers.
[0025] To further improve the elongation of the composite metal foil, the polyethylene terephthalate (PET) content in the mixed layer is 50 wt% to 70 wt%. For example, the PET content in the mixed layer is 50 wt%, 57 wt%, 58 wt%, 59 wt%, 60 wt%, 68 wt%, 70 wt%, or any range of two values. Simultaneously, to enhance the tinning effect of the composite metal foil, the sodium terephthalate (NDT) content in the mixed layer is 15 wt% to 25 wt%. For example... The sodium terephthalate content in the mixed layer is 15wt%, 16wt%, 19wt%, 20wt%, 22wt%, 25wt%, or any two of these values. To further improve the elongation of the composite metal foil and the tinning effect, the ethylene glycol content in the mixed layer is 15wt% to 25wt%. For example, the ethylene glycol content in the mixed layer is 15wt%, 16wt%, 17wt%, 20wt%, 23wt%, and 25wt%, or any two of these values.
[0026] To improve the elongation of the composite metal foil, the support layer provided by the present invention comprises at least one of polyethylene terephthalate, polyimide, polyethylene terephthalate copolymer, polyethylene naphthalate, polyethylene terephthalate (PET), polypropylene (PP), polyimide (PI), polyvinyl chloride (PVC), polyethylene (PE), ethylene-vinyl acetate copolymer (EVA), and polycarbonate (PC). Specifically, the support layer is preferably polyethylene terephthalate, which has good gloss, high strength, wear resistance, chemical corrosion resistance, and dimensional stability. In particular, PET has good elongation and tensile strength, making it more suitable as a support layer for composite metal foil. More preferably, by combining polyethylene terephthalate with polyethylene terephthalate... PET films are made by blending materials such as ethylene glycol copolymers, neopentyl glycol (NPG) copolymers, and polyethylene naphthalate. Adding appropriate amounts of other components lowers the melting point of the PET film, increases its hardness and tensile strength, and is more conducive to improving the performance of composite metal foils. More specifically, by copolymerizing polyethylene terephthalate and neopentyl glycol, and using neopentyl glycol to modify polyethylene terephthalate, a series of copolyesters with different glycol ratios are synthesized. The melting point and crystallinity of the resulting copolyesters are inversely proportional to the amount of neopentyl glycol added. Simultaneously, the impact resistance and processing properties of the formed copolyesters are greatly improved. Specifically, when the molar fraction of neopentyl glycol is 2%–15% of polyethylene terephthalate, the copolymerized copolyester exhibits superior impact resistance and processing properties.
[0027] In some embodiments, the thickness of the support layer is 3-10 μm. For example, the thickness of the support layer is 3 μm, 5 μm, 8 μm, and 10 μm, or any range of two such values.
[0028] In some embodiments, the shielding layer includes at least one of copper, aluminum, gold, silver, iron, nickel, chromium, and zinc.
[0029] The thickness of the shielding layer is 0.5-5 μm. For example, the thickness of the shielding layer is 0.5 μm, 1 μm, 3 μm and 5 μm or any range of two values.
[0030] An adhesive layer is further disposed between the shielding layer and the substrate, the thickness of the adhesive layer being 0.1-2 μm. For example, the thickness of the adhesive layer is 0.1 μm, 0.5 μm, 0.8 μm, 1.2 μm, and 2 μm, or any range of two such values.
[0031] Preferably, the adhesive layer includes at least one of the following resins: vinyl acetate, polyester, polyethylene, polyamide, rubber, acrylate, phenolic, epoxy, polyimide, urethane, melamine, alkyd, ABF, etc.
[0032] Meanwhile, the present invention also provides a cable comprising the above-mentioned composite metal foil, wherein the cable has high elongation, good tinning effect and strong shielding performance. Attached Figure Description
[0033] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0034] Figure 1 This is a schematic diagram of the composite metal foil structure provided in Embodiment 1 of the present invention;
[0035] Figure 2 yes Figure 1 Enlarged view of point A in the middle;
[0036] Figure 3 This is a schematic diagram of the composite metal foil structure provided in Embodiment 5 of the present invention;
[0037] Figure 4 This is a schematic diagram of the composite metal foil structure provided in Embodiment 6 of the present invention;
[0038] Figure label:
[0039] 1-Shielding layer; 2-Transition layer; 3-Supporting layer; 4-Hybrid layer. Detailed Implementation
[0040] The following embodiments are provided to better understand the present invention and are not limited to the preferred embodiments described. They do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the protection scope of the present invention.
[0041] For experiments not specifically described in the examples, the procedures or conditions should be followed according to the conventional experimental procedures described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all commercially available conventional reagent products.
[0042] Example 1
[0043] This embodiment provides a composite metal foil, the structure of which is described below. Figure 1It includes a support layer 3 and a shielding layer 1 stacked together, with a transition layer 2 between the support layer and the shielding layer. The support layer is made of polyethylene terephthalate and has a thickness of 5 μm. The shielding layer is made of copper foil and has a thickness of 2 μm. The transition layer is made of copper. The dyne value of the surface of the support layer away from the shielding layer is 54.
[0044] Example 2
[0045] This embodiment provides a composite metal foil. The composite metal foil structure, the material and thickness of each structure are the same as those in Embodiment 1. The difference is that the dyne value of the surface of the support layer away from the shielding layer is 58.
[0046] Example 3
[0047] See Figure 1 and Figure 2 This embodiment provides a composite metal foil. The composite metal foil structure, the materials and thicknesses of each structure are the same as in Embodiment 1, except that the maximum depth of the transition layer extending into the support layer is 0.01 μm. Figure 2 In the middle, H represents the maximum depth into which the transition layer penetrates the support layer.
[0048] Example 4
[0049] See Figure 1 and Figure 2 This embodiment provides a composite metal foil. The composite metal foil structure, the materials and thicknesses of each structure are the same as in Embodiment 1, except that the maximum depth of the transition layer extending into the support layer is 0.1 μm. Figure 2 In the middle, H represents the maximum depth into which the transition layer penetrates the support layer.
[0050] Example 5
[0051] This embodiment provides a composite metal foil, the structure of which is described below. Figure 3 ,include,
[0052] The support layer 3 and the shielding layer 1 are stacked together.
[0053] A transition layer 2 is provided between the support layer and the shielding layer.
[0054] The support layer has a hybrid layer 4 on the side facing away from the shielding layer.
[0055] The support layer is made of polyethylene terephthalate and has a thickness of 3 μm.
[0056] The shielding layer is made of copper foil and has a thickness of 1.2μm.
[0057] The transition layer is made of copper.
[0058] The mixed layer material includes polyethylene terephthalate, sodium terephthalate, and ethylene glycol.
[0059] The support layer was immersed in a 5 wt% sodium hydroxide solution for 20 seconds, and the dyne value of the surface of the support layer away from the shielding layer was 56.
[0060] The mixed layer contains 50 wt% polyethylene terephthalate, 15 wt% sodium terephthalate, and 20 wt% ethylene glycol, with the remainder being unavoidable impurities.
[0061] Example 6
[0062] This embodiment provides a composite metal foil, the structure of which is described below. Figure 4 ,include,
[0063] The support layer 3 and the shielding layer 1 are stacked together.
[0064] A transition layer 2 is provided between the support layer and the shielding layer.
[0065] The hybrid layer 4 is present on both opposite sides of the support layer.
[0066] The support layer is made of polyethylene terephthalate and has a thickness of 3 μm.
[0067] The shielding layer is made of copper foil and has a thickness of 1.2μm.
[0068] The transition layer is made of copper.
[0069] The mixed layer material includes polyethylene terephthalate, sodium terephthalate, and ethylene glycol.
[0070] The support layer was immersed in a 5 wt% sodium hydroxide solution for 20 seconds, and the dyne value of the surface of the support layer away from the shielding layer was 56.
[0071] The mixed layer contains 55 wt% polyethylene terephthalate, 18 wt% sodium terephthalate, and 25 wt% ethylene glycol, with the remainder being unavoidable impurities.
[0072] Comparative Example 1
[0073] This comparative example provides a composite metal foil with the same structure, material, and thickness as in Example 1, except that the dyne value of the surface of the support layer away from the shielding layer is 52.
[0074] Comparative Example 2
[0075] This comparative example provides a composite metal foil with the same structure, material, and thickness as in Example 1, except that the dyne value of the surface of the support layer away from the shielding layer is 60.
[0076] Experimental Example
[0077] The elongation and tinning area ratio of the composite metal foils provided in Examples 1-6 and Comparative Examples 1-2 were tested, and the results are shown in Table 1.
[0078] The elongation of the composite metal foil was determined by a tensile test using a tensile testing machine.
[0079] A tin-immersion test was conducted on a 50×50mm composite metal foil sample at 270℃ for 3s. The tinning area ratio of the composite metal foil was calculated using imageJ image processing software or MATLAB image processing program. The tinning area ratio (%) = tinning area / surface area of composite metal foil × 100.
[0080] Table 1 Performance of Composite Metal Foil
[0081]
[0082]
[0083] As shown in Table 1, the composite metal foil provided by this invention exhibits good elongation and tinning effect, ensuring the connection stability between the composite metal foil and the connector during cable manufacturing. Furthermore, while ensuring electromagnetic shielding performance, it meets elongation requirements, reduces the probability of breakage, and improves the operational reliability of the cable.
[0084] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.
Claims
1. A composite metal foil for electromagnetic shielding in cables, characterized in that, It includes a support layer and a shielding layer stacked together, wherein the dyne value of the surface of the support layer away from the shielding layer is 54 to 58; A transition layer is provided between the support layer and the shielding layer, and the maximum depth of the transition layer extending into the support layer is 0.02~0.1μm; The support layer has a mixing layer on the side opposite to the shielding layer. The mixing layer includes polyethylene terephthalate, sodium terephthalate, and ethylene glycol. The content of polyethylene terephthalate is 50wt%~70wt%, the content of sodium terephthalate is 15wt%~25wt%, and the content of ethylene glycol is 15wt%~25wt%.
2. The composite metal foil according to claim 1, characterized in that, The transition layer comprises a conductive metal, polyethylene terephthalate, sodium terephthalate, and ethylene glycol, wherein the conductive metal is made of at least one of the same materials as the shielding layer.
3. The composite metal foil according to claim 1, characterized in that, The hybrid layer is present on both opposite sides of the support layer.
4. The composite metal foil according to any one of claims 1-3, characterized in that, The support layer comprises at least one of polyethylene terephthalate, polyimide, polyethylene terephthalate copolymer, and polyethylene naphthalate, and / or, The thickness of the support layer is 3-10 μm.
5. The composite metal foil according to claim 4, characterized in that, The shielding layer includes at least one of copper foil, aluminum foil, and a metal braided layer, and / or, The thickness of the shielding layer is 0.5-5 μm.
6. The composite metal foil according to claim 1, characterized in that, An adhesive layer is also provided between the shielding layer and the support layer, and the thickness of the adhesive layer is 0.1-2μm.
7. A cable, characterized in that, Includes the composite metal foil according to any one of claims 1-6.
Citation Information
Patent Citations
Flexible weldable antioxidant electromagnetic shielding film and preparation method thereof
CN113412043A