A UV type coating material, a preparation method and application thereof

By combining UV-type coating materials, the problems of creases and poor impact resistance that occur in the cover material of foldable screen phones during the folding process are solved, achieving rapid curing and good adhesion, making it suitable for high and low temperature environments of foldable screen phones.

CN119331476BActive Publication Date: 2026-11-24CHENGDU TOMI SHUANG DU OPTOELECTRONICS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310893651.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-19
Publication Date
2026-11-24
Estimated Expiration
2043-07-19

AI Technical Summary

Technical Problem

Existing foldable screen phone cover materials are prone to creases and poor impact resistance during folding. Furthermore, thermosetting resin coatings suffer from slow curing speed, easy contamination, and high shrinkage during application, making it difficult to meet the bending requirements at high and low temperatures.

Method used

The UV-type coating material includes components such as hydroxybutyl acrylate, low-Tg monofunctional UV monomer, low-Tg bifunctional UV monomer, and low-Tg polyurethane acrylate. It achieves rapid curing under UV light through a photoinitiator. The material has a low glass transition temperature, good adhesion and water resistance, and avoids pressure sensitivity.

Benefits of technology

It enables rapid curing and bending of materials at low temperatures, reduces shrinkage, improves adhesion to glass and water resistance, and is suitable for high and low temperature environments of foldable screen phones, avoiding pressure sensitivity issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004355547170000091
    Figure BDA0004355547170000091
  • Figure BDA0004355547170000101
    Figure BDA0004355547170000101
Patent Text Reader

Abstract

The application provides a UV type coating film material, a preparation method and application thereof, and raw materials of the UV type coating film material include the following components: hydroxybutyl acrylate, hexamethylene diisocyanate extended by 1,5-pentanediol or 1,4-butanediol, low-Tg monofunctional UV monomer, low-Tg bifunctional or more UV monomer, low-Tg polyurethane acrylate and photoinitiator. The UV type coating film material has a low glass phase transition temperature, good adhesion to glass, good water resistance, no pressure-sensitive curing, and is not sticky to touch after curing and has excellent high and low temperature resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of ultra-thin glass processing materials technology, specifically relating to a UV-type coating material, its preparation method, and its application. Background Technology

[0002] In the fourth quarter of 2022, shipments of foldable screen products in China reached a new high, exceeding 1.1 million units. Full-year shipments totaled nearly 3.3 million units, representing a year-on-year increase of 118%, exceeding expectations. The share of foldable screen products in the domestic smartphone market rose from 0.5% in 2021 to 1.2%. The global foldable screen market is projected to grow by 52% to reach 22.7 million units in 2023. Against this backdrop, major smartphone manufacturers are launching one to two foldable screen phones per year.

[0003] Currently, the cover plates used in foldable phones are mostly film materials and flexible foldable ultra-thin glass (UTG). Film materials will show obvious creases after being folded for a certain period of time, while flexible foldable ultra-thin glass, although having excellent bending resistance, has poor impact resistance and explosion resistance due to its thinness. There are currently two solutions to address these performance defects: one is to coat the UTG surface with one or more layers of flexible resin material. Flexible resin material can not only protect the ultra-thin glass well, but also does not affect the bending performance; the other is to use center-foldable ultra-thin glass (CFG), where the thickness of the glass in the middle bending area is only 30-50μm, while the thickness in the non-bending area is 70-200μm.

[0004] Because CFG has a flexible central section, it features a groove design. This groove prevents CFG from being directly bonded to the display panel; a flexible resin material is needed to fill it. Thermosetting resin coatings often contain solvents, resulting in significant dry film shrinkage, making it difficult to fill the groove. Furthermore, thermosetting materials cure slowly and are easily contaminated by dust from the environment and equipment during curing, leading to poor appearance. 100% active ingredient UV-curable coatings cure quickly, and their film shrinkage rate is much lower than that of thermosetting materials. However, coating CFG surfaces requires not only specific shrinkage and curing speed but also specific performance characteristics. To withstand bending at high and low temperatures, the material's glass transition temperature (Tg) must be below -20°C, and it must adhere firmly to the glass substrate, necessitating good adhesion. At lower Tg levels, the cured film often exhibits pressure sensitivity, making it easy for dust particles to adhere to the surface and impossible to clean; therefore, the material cannot be pressure-sensitive. Since the application scenario is electronic products, which require waterproofing, good water resistance is required. Summary of the Invention

[0005] To address the shortcomings of existing technologies, the present invention aims to provide a UV-type coating material, its preparation method, and its applications. The UV-type coating material of the present invention exhibits a low glass phase transition temperature, good adhesion to glass, good water resistance, is non-pressure sensitive, and after curing, is not sticky to the touch and possesses excellent high and low temperature resistance.

[0006] To achieve this objective, the present invention adopts the following technical solution:

[0007] On one hand, the present invention provides a UV coating material, wherein the raw materials for preparing the UV coating material include the following components: hydroxybutyl acrylate, hexamethylene diisocyanate extended by 1,5-pentanediol or 1,4-butanediol, low Tg monofunctional UV monomer, low Tg difunctional or higher UV monomer, low Tg polyurethane acrylate and photoinitiator.

[0008] The UV-type coating material obtained by reacting the raw materials as described above in this invention has a low glass phase transition temperature, good adhesion to glass, good water resistance, no pressure sensitivity, is not sticky to the touch after curing, and has excellent high and low temperature resistance.

[0009] Low-Tg UV materials are often unbranched long-chain molecular structures with poor adhesion. While hydroxypropyl acrylate in this invention is also an unbranched long-chain molecular structure, its ends have highly polar groups that enhance film adhesion. Furthermore, the addition of low-Tg monomers and resins further lowers the material's Tg point, and since the monomers are all fast-reacting, the material achieves a high degree of curing during curing, resulting in a pressure-sensitive material.

[0010] In this invention, the hydroxybutyl acrylate has a low Tg point and contains hydroxyl groups, and can be reacted with isocyanate to obtain an acrylate prepolymer with a low Tg point. The free hydroxybutyl acrylate or the extra hydroxyl groups provide adhesion of the material to glass.

[0011] In this invention, the hexamethylene diisocyanate chain extended by 1,5-pentanediol or 1,4-butanediol has a very low Tg point and can react with hydroxybutyl acrylate to generate an acrylate prepolymer with a very low Tg point.

[0012] In this invention, low-Tg monofunctional UV monomers can dilute the synthesized acrylate prepolymer and adjust the viscosity of the material.

[0013] In this invention, the low Tg difunctional UV monomer can also play a role in adjusting the viscosity of the material, while also enabling the material to react quickly and not stick to the touch.

[0014] In this invention, low-Tg polyurethane acrylate can be used to adjust the Tg point and viscosity.

[0015] In this invention, the photoinitiator enables the material to polymerize under UV light.

[0016] Preferably, the low Tg monofunctional UV monomer is a fast-reacting low Tg monofunctional monomer selected from any one or a combination of at least two of ethoxyethoxyethyl acrylate, isodecaacrylate, isooctyl acrylate, hydroxybutyl acrylate, isononyl acrylate, methyl laurate, 2-(2-ethoxyethoxy)ethyl acrylate, tridecyl acrylate, or caprolactone acrylate.

[0017] Preferably, the low Tg bifunctional or higher UV monomer includes a low Tg bifunctional UV monomer or a low Tg trifunctional UV monomer.

[0018] Preferably, the low Tg bifunctional UV monomer comprises alkyl oxohexanediol diacrylate and / or ethoxylated trimethylolpropane triacrylate.

[0019] Preferably, the raw materials for preparing the UV-type coating material also include a catalyst.

[0020] Preferably, the catalyst comprises any one or a combination of at least two of dibutyltin dilaurate, stannous octoate, or organobismuth.

[0021] Preferably, the photoinitiator comprises one or a combination of at least two of 1-hydroxy-cyclohexyl-1-phenyl ketone, 2,4,6-(trimethylbenzoyl)diphenylphosphine oxide, 2-hydroxy-2-methyl-1-phenyl-propanone, or phenylbis(4,4,6-trimethylbenzoyl)phosphine oxide.

[0022] Preferably, the photoinitiator further includes a thiol photoinitiator containing a thiol group.

[0023] Preferably, the raw materials for preparing the UV coating material contain hydroxybutyl acrylate and hexamethylene diisocyanate chain extended by 1,5-pentanediol or 1,4-butanediol to form an acrylate prepolymer.

[0024] The acrylate prepolymer of the present invention not only has a low Tg point, good adhesion to glass, and good water resistance, but also reacts rapidly.

[0025] Preferably, the weight ratio of hydroxybutyl acrylate to hexamethylene diisocyanate extended by 1,5-pentanediol or 1,4-butanediol is 38:22-33. Too much hydroxybutyl acrylate will result in incomplete polymerization, excessive oxygen inhibition, and a sticky feel. Too little hydroxybutyl acrylate will increase the heat transfer temperature (Tg), making it prone to breakage when bent at low temperatures.

[0026] Preferably, the acrylate prepolymer accounts for 60-85% by weight in the raw materials used for preparation, for example, 60%, 65%, 68%, 70%, 75%, 78%, 80%, or 85%.

[0027] Preferably, in the preparation raw materials, the weight percentage of the low Tg monofunctional UV monomer is 10-30%, for example 10%, 13%, 15%, 18%, 20%, 23%, 25%, 28% or 30%.

[0028] Preferably, in the raw materials for preparation, the weight percentage of the UV monomer with low Tg and above dual functionality is 0-20%, for example, 0%, 1%, 3%, 5%, 8%, 10%, 13%, 15%, 18% or 20%.

[0029] Preferably, in the raw materials for preparation, the low-Tg polyurethane acrylate accounts for 0-10% by weight, for example, 0%, 1%, 3%, 5%, 8% or 10%.

[0030] Preferably, the amount of catalyst used is 0.03%-0.1% of the total weight of hydroxybutyl acrylate and hexamethylene diisocyanate extended by 1,5-pentanediol or 1,4-butanediol, for example 0.03%, 0.05%, 0.08% or 0.1%.

[0031] Preferably, the initiator accounts for 2-7% by weight in the raw materials used for preparation, for example, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5% or 7%.

[0032] In this invention, "low Tg" in low Tg monofunctional UV monomers, low Tg multifunctional UV monomers, and low Tg polyurethane acrylates refers to a Tg below -40°C.

[0033] On the other hand, the present invention provides a method for preparing the UV-type coating material as described above, the method comprising the following steps:

[0034] (1) Hydroxybutyl acrylate reacts with hexamethylene diisocyanate extended by 1,5-pentanediol or 1,4-butanediol to obtain acrylate prepolymer;

[0035] (2) Add low Tg monofunctional UV monomer, low Tg bifunctional or higher UV monomer, low Tg polyurethane acrylate and photoinitiator to the reactants in step (1), mix them, and obtain the UV type coating material.

[0036] Preferably, the reaction in step (1) is carried out in the presence of a catalyst.

[0037] Preferably, the catalyst comprises dibutyltin dilaurate.

[0038] Preferably, the reaction temperature in step (1) is 70-110℃ (e.g., 70℃, 73℃, 75℃, 78℃, 80℃, 85℃, 90℃, 95℃, 100℃, 105℃ or 110℃), and the reaction time is 2-4 hours (e.g., 2 hours, 2.5 hours, 2.8 hours, 3 hours, 3.5 hours, 3.8 hours or 4 hours).

[0039] Preferably, the viscosity of the UV coating material is 200-500 cps, for example 200 cps, 250 cps, 300 cps, 350 cps, 400 cps, 450 cps or 500 cps.

[0040] On the other hand, the present invention provides the application of the UV-type coating material as described above as a non-uniform thickness ultrathin glass coating material.

[0041] On the other hand, the present invention provides an ultra-thin glass with non-uniform thickness, the ultra-thin glass with non-uniform thickness comprising a foldable ultra-thin glass with non-uniform thickness and a coating covering the surface of the foldable ultra-thin glass with non-uniform thickness, the coating being obtained by curing a UV-type coating material as described above.

[0042] Compared with the prior art, the present invention has the following beneficial effects:

[0043] The UV-type coating material described in this invention uses all resins and monomers with low Tg points. The material has a very low Tg point, and its cured product can be bent at low temperatures. It is 100% solid component with very low shrinkage, making it suitable for CFG coating. It uses hydroxybutyl acrylate to synthesize a prepolymer, which not only has a very low Tg point, but also has good adhesion to glass due to the presence of polar groups. No primer is required, reducing the difficulty of the process. It uses fast-reacting monomers and resins, resulting in fast curing speed, relatively complete crosslinking, and no pressure sensitivity of the material. Detailed Implementation

[0044] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.

[0045] All raw materials described in this invention are available on the domestic chemical market.

[0046] HDI chain extension reaction:

[0047] (1) Preparation of HDI via 1,5-pentanediol:

[0048] 84 parts by weight of HDI (hexamethylene diisocyanate) were added to a sealed container equipped with a reflux condenser. The mixture was stirred at 1000 RPM and heated to 60°C. 45 parts by weight of 1,5-pentanediol were added to the container at a rate of 3 g / min. The reaction was carried out for 80 min to obtain the final product.

[0049] (2) Preparation of HDI with chain extension of 1,4-butanediol

[0050] 84 parts by weight of HDI (hexamethylene diisocyanate) were added to a sealed container equipped with a reflux condenser. The mixture was stirred at 1300 RPM and heated to 70°C. 45 parts by weight of 1,4-butanediol were added to the container at a rate of 5 g / min. The reaction was carried out for 100 min to obtain the final product.

[0051] Example 1

[0052] This embodiment provides a UV-type coating material, the preparation method of which includes the following steps:

[0053] 38 parts by weight of hydroxybutyl acrylate, 33 parts by weight of HDI chain-extended with 1,5-pentanediol, and 0.03 parts by weight of dibutyltin dilaurate were added to a reaction vessel equipped with a reflux condenser. The mixture was stirred and heated to 90°C, and reacted for 3 hours to obtain a bifunctional acrylate prepolymer. This acrylate prepolymer not only has a low Tg point (-45°C), good adhesion to glass (GB / T9286-1998 paint film adhesion test standard, 5B), and good water resistance (paint film adhesion test after boiling in water at 85°C for 1 hour, >4B), but also reacts rapidly (360 mW / cm²). 2 3000mJ / cm 2 (This will allow it to fully cure). Add 70% (by weight) of the above acrylate prepolymer, 27% ethoxyethoxyethyl acrylate, 1.5% 1-hydroxy-cyclohexyl-1-phenyl ketone, and 1.5% 2,4,6-(trimethylbenzoyl)diphenylphosphine oxide to a container and stir until homogeneous to obtain a material with a viscosity of approximately 320 cps.

[0054] Example 2

[0055] This embodiment provides a UV-type coating material, the preparation method of which includes the following steps:

[0056] 38 parts of hydroxybutyl acrylate, 22 parts of HDI chain-extended with 1,4-butanediol, and 0.03 parts of dibutyltin dilaurate were added to a reaction vessel equipped with a reflux condenser. The mixture was stirred and heated to 110°C, and reacted for 2 hours to obtain a trifunctional acrylate prepolymer. This acrylate prepolymer not only has a low Tg point (-52°C), good adhesion to glass (GB / T9286-1998 paint film adhesion test standard, 5B), and good water resistance (paint film adhesion test after boiling in water at 85°C for 1 hour, >4B), but also reacts rapidly (360mW / cm²). 2 3000mJ / cm 2 (This will allow it to fully cure). Add 70% of the above-mentioned acrylate prepolymer, 20% of 2-(2-ethoxyethoxy)ethyl acrylate, 5% alkylhexanediol diacrylate, 2.5% of 1-hydroxy-cyclohexyl-1-phenyl ketone, and 2.5% of 2,4,6-(trimethylbenzoyl)diphenylphosphine oxide to a container and stir until homogeneous to obtain a material with a viscosity of approximately 260 cps.

[0057] Example 3

[0058] This embodiment provides a UV-type coating material, the preparation method of which includes the following steps:

[0059] 38 parts by weight of hydroxybutyl acrylate, 33 parts by weight of HDI chain-extended with 1,5-pentanediol, and 0.05 parts by weight of dibutyltin dilaurate were added to a reaction vessel equipped with a reflux condenser. The mixture was stirred and heated to 70°C, and reacted for 4 hours to obtain a trifunctional acrylate prepolymer. This acrylate prepolymer not only has a low Tg point (-45°C), good adhesion to glass (GB / T9286-1998 paint film adhesion test standard, 5B), and good water resistance (paint film adhesion test after boiling in water at 85°C for 1 hour, >4B), but also reacts rapidly (360 mW / cm²). 2 3000mJ / cm 2 (This allows for complete curing). Add 60% of the above-mentioned acrylate prepolymer, 20% of 2(2-ethoxyethoxy)ethyl acrylate, 10% alkylhexanediol diacrylate, 5% low-Tg polyurethane acrylate, 2.5% of 1-hydroxy-cyclohexyl-1-phenyl ketone, and 2.5% of 2,4,6-(trimethylbenzoyl)diphenylphosphine oxide to a container, and stir until homogeneous to obtain a material with a viscosity of 240 cps.

[0060] Example 4

[0061] This embodiment provides a UV-type coating material, the preparation method of which includes the following steps:

[0062] 38 parts by weight of hydroxybutyl acrylate, 33 parts by weight of 1,5-pentanediol chain-extended HDI, and 0.03 parts by weight of dibutyltin dilaurate were added to a reaction vessel equipped with a reflux condenser. The mixture was stirred and heated to 90°C, and reacted for 3 hours to obtain a trifunctional acrylate prepolymer. This acrylate prepolymer not only has a low Tg point (-45°C), good adhesion to glass (GB / T9286-1998 paint film adhesion test standard, 5B), and good water resistance (paint film adhesion test after boiling in water at 85°C for 1 hour, >4B), but also reacts rapidly (360 mW / cm²). 2 3000mJ / cm 2 (This will allow for complete curing). Add 85% of the above-mentioned acrylate prepolymer, 5% ethoxyethoxyethyl acrylate, 5% 2(2-ethoxyethoxy)ethyl acrylate, 1.5% 1-hydroxy-cyclohexyl-1-phenyl ketone, 1.5% 2,4,6-(trimethylbenzoyl)diphenylphosphine oxide, and 2% dodecyl mercaptan to a container, and stir until homogeneous to obtain a material with a viscosity of approximately 440 cps.

[0063] Comparative Example 1

[0064] The only difference between this comparative example and Example 1 is that hydroxybutyl acrylate and hexamethylene diisocyanate do not react to form a trimer.

[0065] The preparation method includes the following steps:

[0066] 38 parts by weight of hydroxybutyl acrylate, 33 parts by weight of HDI chain-extended with 1,5-pentanediol, and 0.03 parts by weight of dibutyltin dilaurate were added to a reaction vessel equipped with a reflux condenser and mixed to obtain a mixture. Then, 70% (by weight) of the above mixture, 27% ethoxyethoxyethyl acrylate, 1.5% 1-hydroxy-cyclohexyl-1-phenyl ketone, and 1.5% 2,4,6-(trimethylbenzoyl)diphenylphosphine oxide were added to the vessel and stirred until homogeneous, yielding a material with a viscosity of 10 cps. Because it did not undergo a polymerization reaction, its average molecular weight is relatively small, resulting in a low viscosity. Most of the chain-extended HDI failed to participate in the reaction and will exist as a liquid. During the photocuring process, the material will remain liquid and will not form a coating.

[0067] Comparative Example 2

[0068] The only difference between this comparative example and Example 3 is that all monomers in the material are low-Tg bifunctional monomers.

[0069] The preparation method includes the following steps:

[0070] 38 parts by weight of hydroxybutyl acrylate, 33 parts by weight of HDI chain-extended with 1,5-pentanediol, and 0.05 parts by weight of dibutyltin dilaurate were added to a reaction vessel equipped with a reflux condenser and mixed at room temperature to obtain a mixture. Then, 70% of the above mixture, 27% of alkylhexanediol diacrylate, 5% of low-Tg polyurethane acrylate, 2.5% of 1-hydroxy-cyclohexyl-1-phenyl ketone, and 2.5% of 2,4,6-(trimethylbenzoyl)diphenylphosphine oxide were added to the vessel and stirred until homogeneous to obtain a material with a viscosity of approximately 350 cps. Because all monomers are difunctional, the material has relatively high hardness and the finished paint film is prone to breakage when bent.

[0071] The material performance test results of Examples 1-4 and Comparative Examples 1-2 are shown in Table 1.

[0072] Table 1

[0073]

[0074]

[0075] The applicant declares that the present invention is illustrated by the above embodiments to demonstrate the UV-type coating material, its preparation method, and its application. However, the present invention is not limited to the above embodiments, that is, it does not mean that the present invention must rely on the above embodiments to be implemented. Those skilled in the art should understand that any improvements to the present invention, equivalent substitutions of the raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A UV-type coating material, characterized in that, The raw materials for preparing the UV coating material include the following components: hydroxybutyl acrylate, hexamethylene diisocyanate extended by 1,5-pentanediol or 1,4-butanediol, low Tg monofunctional UV monomer, low Tg difunctional or higher UV monomer, low Tg polyurethane acrylate and photoinitiator. In the raw materials for preparing the UV-type coating material, hydroxybutyl acrylate and hexamethylene diisocyanate chain extended by 1,5-pentanediol or 1,4-butanediol form an acrylate prepolymer. In the raw materials used for preparation, the acrylate prepolymer accounts for 60-85% by weight; The term "low Tg" in the context of low Tg monofunctional UV monomers, low Tg multifunctional UV monomers, and low Tg polyurethane acrylates refers to a Tg below -40°C.

2. The UV-type coating material according to claim 1, characterized in that, The low-Tg monofunctional UV monomer is a fast-reacting low-Tg monofunctional monomer selected from any one or a combination of at least two of ethoxyethoxyethyl acrylate, isodecaacrylate, isooctyl acrylate, hydroxybutyl acrylate, isononyl acrylate, methyl laurate, tridecyl acrylate, or caprolactone acrylate.

3. The UV-type coating material according to claim 1, characterized in that, The low-Tg bifunctional or higher UV monomers include low-Tg bifunctional UV monomers or low-Tg trifunctional UV monomers.

4. The UV-type coating material according to claim 3, characterized in that, The low-Tg, bifunctional or higher UV monomers include alkyl oxyhexanediol diacrylate and / or ethoxytrimethylolpropane triacrylate.

5. The UV-type coating material according to claim 1, characterized in that, The raw materials for preparing the UV-type coating material also include a catalyst.

6. The UV-type coating material according to claim 5, characterized in that, The catalyst comprises any one or a combination of at least two of dibutyltin dilaurate, stannous octoate, or organobismuth.

7. The UV-type coating material according to claim 1, characterized in that, The photoinitiator includes one or a combination of at least two of 1-hydroxy-cyclohexyl-1-phenyl ketone, 2,4,6-(trimethylbenzoyl)diphenylphosphine oxide, 2-hydroxy-2-methyl-1-phenyl-propanone, or phenylbis(4,4,6-trimethylbenzoyl)phosphine oxide.

8. The UV-type coating material according to claim 7, characterized in that, The photoinitiator also includes thiol photoinitiators containing thiol groups.

9. The UV-type coating material according to claim 1, characterized in that, The weight ratio of the hydroxybutyl acrylate and the hexamethylene diisocyanate extended by 1,5-pentanediol or 1,4-butanediol is 38:22-33.

10. The UV-type coating material according to claim 1, characterized in that, In the raw materials for preparation, the low Tg monofunctional UV monomer accounts for 10-30% by weight.

11. The UV-type coating material according to claim 1, characterized in that, In the raw materials for preparation, the UV monomer with low Tg and above dual functionality accounts for 0-20% by weight.

12. The UV-type coating material according to claim 1, characterized in that, In the raw materials used for preparation, the low-Tg polyurethane acrylate accounts for 0-10% by weight.

13. The UV-type coating material according to claim 5, characterized in that, The amount of catalyst used is 0.03%-0.1% of the total weight of hydroxybutyl acrylate and hexamethylene diisocyanate extended by 1,5-pentanediol or 1,4-butanediol.

14. The UV-type coating material according to claim 1, characterized in that, In the raw materials for preparation, the initiator accounts for 2-7% by weight.

15. A method for preparing a UV-type coating material according to any one of claims 1-14, characterized in that, The preparation method includes the following steps: (1) Hydroxybutyl acrylate reacts with hexamethylene diisocyanate extended by 1,5-pentanediol or 1,4-butanediol to obtain acrylate prepolymer; (2) Add low Tg monofunctional UV monomer, low Tg bifunctional or higher UV monomer, low Tg polyurethane acrylate and photoinitiator to the reactants in step (1), mix them, and obtain the UV type coating material.

16. The preparation method according to claim 15, characterized in that, The reaction described in step (1) is carried out in the presence of a catalyst.

17. The preparation method according to claim 16, characterized in that, The catalyst includes dibutyltin dilaurate.

18. The preparation method according to claim 15, characterized in that, The reaction temperature in step (1) is 70-110℃, and the reaction time is 2-4 hours.

19. The preparation method according to claim 15, characterized in that, The viscosity of the UV-type coating material is 200-500 cps.

20. The application of a UV-type coating material according to any one of claims 1-14 as a non-uniform thickness ultrathin glass coating material.

21. A non-uniform thickness ultrathin glass, characterized in that, The non-uniform thickness ultra-thin glass includes foldable non-uniform thickness ultra-thin glass and a coating applied to the surface of the foldable non-uniform thickness ultra-thin glass, the coating being cured from a UV-type coating material as described in any one of claims 1-14.

Citation Information

Patent Citations

  • Preparation method and applications of low Tg polyurethane acrylate prepolymer

    CN108341922A

  • Flexible UV photocureable coating, and preparation method and application thereof

    CN111138966A