A photochromic polystyrene film, and a preparation method and application thereof
By introducing azobenzene UV-responsive groups onto the polystyrene molecular chain and combining this with electrospinning technology, a photochromic polystyrene film was prepared. This solved the problems of the complexity in preparing existing photostimulation-responsive films and the difficulty in utilizing waste polystyrene, enabling efficient anti-counterfeiting, information encryption, and oil-water separation applications.
Patent Information
- Application Number
- CN202411386355.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-09-30
AI Technical Summary
Existing photostimulation-responsive membranes are cumbersome to prepare, have complex processes, and exhibit unstable performance. Waste expanded polystyrene is difficult to utilize at a high value, and the material is difficult to degrade in the environment, leading to environmental pollution and resource waste.
Photochromic polystyrene films were prepared by introducing azobenzene UV-responsive groups onto the polystyrene molecular chain through chemical modification and electrospinning technology. Photoresponsive smart film materials were prepared using waste expanded polystyrene as raw material and combined with electrospinning technology.
A simple preparation method for photochromic polystyrene films has been achieved, which exhibit UV light response, color reversibility, and stability. These films are suitable for anti-counterfeiting and information encryption, and can also be used for the efficient separation of oily wastewater, enabling the multifunctional reuse of polystyrene materials.
Smart Images

Figure CN119332414B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the fields of anti-counterfeiting and information encryption, and in particular to a photochromic polystyrene film, its preparation method, and its application. Background Technology
[0002] Expanded polystyrene (EPS) is lightweight, moisture-proof, heat-insulating, shock-absorbing, impact-resistant, and easy to process and mold, making it widely used in construction, packaging, electronics, and automobile manufacturing. However, EPS generates a large amount of waste, and due to its stable chemical properties, it is difficult to degrade in nature, posing a significant threat to the environment. Currently used incineration and landfill methods not only pollute the environment but also result in a serious waste of resources.
[0003] Stimulus-responsive membranes can react to environmental stimuli (such as light, heat, and mechanical force) with visual color or shape changes, and the development of advanced smart materials based on stimulus-responsive membranes has attracted widespread attention. Photostimulus-responsive membranes possess advantages such as non-contact operation, remote control, and fast response speed, making them highly promising for applications in sensing, optics, security and anti-counterfeiting, data storage, and intelligent robotics. However, most existing photostimulus-responsive membranes suffer from problems such as cumbersome preparation processes, complex manufacturing techniques, and unstable performance.
[0004] Polystyrene possesses good solubility and spinnability, allowing for the fabrication of fibrous membranes using electrospinning technology. Electrospinning offers advantages such as simplicity, energy efficiency, and functionalization, making it a mature and effective technology for preparing functional polymer membranes. Furthermore, the benzene ring structure of polystyrene exhibits strong nucleophilicity, enabling the introduction of various active groups onto the benzene ring through common unit reactions such as alkylation, sulfonation, and nitration. This provides active reaction sites for the introduction of photoresponsive functional groups. Therefore, by combining common chemical reactions with simple electrospinning technology, photoresponsive smart membrane materials with significant application value can be designed and developed from waste expanded polystyrene. On the other hand, polystyrene membrane materials possess hydrophobic / oleophilic surface wettability, a unique property that makes them promising for applications in oil-water separation. The treatment of industrial oily wastewater is also a significant environmental challenge; therefore, photoresponsive membrane materials based on waste expanded polystyrene hold promise for treating oily wastewater, enabling the multifunctional reuse of plastic waste. Summary of the Invention
[0005] The excellent reactivity of the benzene ring structure in polystyrene molecules allows for the introduction of various active groups (such as sulfonic acid groups, nitro groups, and chloromethyl groups) onto the benzene ring through common unit reactions, providing active reaction sites for the introduction of photoresponsive groups. Simultaneously, polystyrene itself possesses good solubility and spinnability, enabling the fabrication of functional fiber membranes using electrospinning technology. The azophenyl group exhibits ultraviolet (UV) light responsiveness, meaning it can undergo trans- and cis-isomerization under UV and visible light, resulting in color changes in azobenzene materials.
[0006] This application combines the UV light response characteristics of azobenzene with the excellent reactivity and film-forming properties of polystyrene. By chemically modifying and electrospinning a large amount of waste expanded polystyrene, a photochromic polystyrene-based functional film can be designed and developed for anti-counterfeiting or information encryption, thereby achieving the goal of high-value utilization of waste expanded polystyrene.
[0007] Based on this, the present invention provides a photochromic polystyrene film with a simple preparation process, its preparation method and application, which can solve the problems of cumbersome process, complex process and unstable performance of existing photochromic film preparation technology.
[0008] The application of photochromic polystyrene film in anti-counterfeiting or information encryption, wherein the photochromic polystyrene film is an electrospun fiber film of modified polystyrene, and the structural formula of the modified polystyrene is as follows:
[0009]
[0010] Where m is an integer between 100 and 800, and n is an integer between 20 and 200.
[0011] This application also provides a photochromic polystyrene film, wherein the photochromic polystyrene film is an electrospun fiber film of modified polystyrene, and the structural formula of the modified polystyrene is shown below:
[0012]
[0013] Where m is an integer between 100 and 800, and n is an integer between 20 and 800.
[0014] For example, the number average molecular weight of the modified polystyrene polymer ranges from 30,000 to 100,000.
[0015] The photochromic polystyrene film has UV light responsive properties. The film is mustard gold in color. Under UV light, the film color changes from mustard gold to yellowish-brown. When the film is yellowish-brown, after being exposed to visible light, the film changes from yellowish-brown to mustard gold. This change is reversible and can be repeated multiple times. Therefore, it can be used for anti-counterfeiting and information encryption.
[0016] Optionally, the diameter of the fibers in the modified polystyrene electrospun fiber membrane is 1.0 to 12.0 μm.
[0017] This application also provides a method for preparing the photochromic polystyrene film, comprising:
[0018] (1) Polystyrene was treated with a chloromethylating agent to obtain chloromethylated polystyrene;
[0019] (2) Add a modifying agent to the chloromethylated polystyrene obtained in step (1) to introduce an azobenzene structure into the polystyrene structure to obtain modified polystyrene; the modifying agent is 4-hydroxyazophenol;
[0020] (3) The modified polystyrene obtained in step (2) is dissolved in a first organic solvent to prepare a spinning solution, and a photochromic polystyrene film is prepared by electrospinning.
[0021] In step (1):
[0022] Optionally, the reaction process between the chloromethylating agent and polystyrene includes:
[0023] The polystyrene is dissolved in a second organic solvent, a first catalyst is added, and then a chloromethylation reagent is added to react and obtain a first reaction solution. The chloromethylated polystyrene is then separated from the first reaction solution.
[0024] Optionally, the second organic solvent is dichloromethane, trichloromethane, or carbon tetrachloride.
[0025] Optionally, the first catalyst is anhydrous tin tetrachloride.
[0026] Optionally, the chloromethylating agent is 1,4-dichloromethoxybutane and the molar ratio of the chloromethylating agent to the polystyrene is 1.5:1 to 10:1.
[0027] Optionally, the reaction temperature is room temperature and the reaction time is 12 to 24 hours.
[0028] Optionally, the polystyrene is waste polystyrene foam.
[0029] Optionally, the mass ratio of the first catalyst to polystyrene is 3:1 to 1:1.
[0030] In step (2):
[0031] Optionally, the reaction process between the modifying agent and the chloromethylated polystyrene includes:
[0032] The modifying reagent and the chloromethylated polystyrene are dissolved in the first organic solvent, and a second catalyst is added to react and obtain a second reaction solution. The modified polystyrene is then separated from the second reaction solution.
[0033] Optionally, the molar ratio of the modifying agent to the chloromethylated polystyrene is 1:1 to 4:1.
[0034] Optionally, the second catalyst is potassium carbonate and potassium iodide.
[0035] Optionally, the molar ratio of potassium carbonate to chloromethylated polystyrene is 1:1 to 3:1.
[0036] Optionally, the potassium iodide accounts for 5 to 20 wt% of the potassium carbonate; preferably, the potassium iodide accounts for 7 to 12 wt% of the potassium carbonate.
[0037] Optionally, the reaction conditions are: a reaction temperature of 50–90°C and a reaction time of 5–10 h. Preferably, the reaction conditions are: a reaction temperature of 60–80°C and a reaction time of 6–8 h.
[0038] Optionally, the first organic solvent used in this step is the same as the first organic solvent in step (3).
[0039] In step (3):
[0040] Optionally, the first organic solvent is N,N-dimethylformamide or N,N-dimethylacetamide.
[0041] Optionally, the concentration of the spinning solution is 10–60 wt%. Preferably, the concentration of the spinning solution is 20–40 wt%.
[0042] Optionally, the electrospinning conditions are: positive voltage of 10–15 kV, negative voltage of 2–6 kV, syringe advance speed of 0.1–0.8 mm / min, receiving distance of 15–40 cm, and receiver rotation speed of 3000–6000 r / h. Preferably, the electrospinning conditions are: positive voltage of 12–14 kV, negative voltage of 2–4 kV, syringe advance speed of 0.2–0.4 mm / min, receiving distance of 20–30 cm, and receiver rotation speed of 4200–5400 r / h.
[0043] Optionally, separating the chloromethylated polystyrene from the first reaction solution and separating the modified polystyrene from the second reaction solution respectively include: adding the first reaction solution or the second reaction solution to ethanol or water to precipitate and obtaining a precipitate, and taking the precipitate for vacuum drying.
[0044] Optionally, the vacuum drying process conditions for the precipitate are: temperature 50–100°C, time 8–12 h. Preferably, the vacuum drying process conditions are: temperature 60–70°C, time 10–12 h.
[0045] The photochromic polystyrene film, its preparation method, and its application described in this application have at least one of the following technical advantages compared to existing technologies:
[0046] (1) This invention uses waste polystyrene foam as raw material and utilizes a chemical reaction to bond 4-hydroxyazophenol containing UV-responsive groups (azobenzene) to the polystyrene macromolecular chain. Finally, a photochromic polystyrene film is prepared by electrospinning technology. Specifically, the prepared photochromic polystyrene film can be stimulated by UV light to change its surface color from mustard gold to yellowish-brown, and this transformation is reversible, flexible, and stable.
[0047] (2) The membrane can be used for intelligent anti-counterfeiting or information encryption, and can also be used for efficient separation of oily wastewater in various systems (such as oil-water mixtures and water-in-oil emulsions). The membrane has good recycling performance.
[0048] (3) The photochromic polystyrene film of this application has a simple preparation process, low raw material cost, wide applicability and multiple uses, and is suitable for industrial application. Attached Figure Description
[0049] Figure 1 The image shows the 1H NMR spectrum of the modified polystyrene prepared in Example 1 of this invention.
[0050] Figure 2 Photograph of the photochromic polystyrene film sample prepared in Example 2 of the present invention.
[0051] Figure 3 Scanning electron microscope image of the photochromic polystyrene film prepared in Example 2 of the present invention.
[0052] Figure 4 This is a photograph of the polystyrene fiber membrane sample prepared in Comparative Example 1 of this invention.
[0053] Figure 5 The UV-Vis absorption spectra of the modified polystyrene N-methyl-2-pyrrolidone solution prepared in Example 2 of this invention under UV light (a) and visible light (b) irradiation for different times.
[0054] Figure 6 The kinetic curves of trans-cis (a) and cis-trans (b) isomerization of N-methyl-2-pyrrolidone solution of modified polystyrene prepared in Example 2 of this invention are shown.
[0055] Figure 7The diagram shows the reversible changes in the absorption peak intensity at 350 nm and 440 nm of the photochromic polystyrene N-methyl-2-pyrrolidone solution prepared in Example 2 of this invention under alternating irradiation with ultraviolet and visible light.
[0056] Figure 8 The color change of the photochromic polystyrene film prepared in Example 2 of this invention under alternating irradiation with ultraviolet and visible light.
[0057] Figure 9 The color change of the polystyrene fiber membrane prepared in Comparative Example 1 of this invention under alternating irradiation with ultraviolet and visible light.
[0058] Figure 10 A schematic diagram (a) and an anti-counterfeiting label (b) are shown for the process of making an anti-counterfeiting label using the photochromic polystyrene film prepared in Example 2 of the present invention.
[0059] Figure 11 The ASCII binary code is prepared using the photochromic polystyrene film prepared in Example 2 of this invention.
[0060] Figure 12 A QR code made using the photochromic polystyrene film prepared in Example 2 of this invention.
[0061] Figure 13 The results of the contact angle test of the photochromic polystyrene film prepared in Example 2 of the present invention with water (a) and oil (b) in air.
[0062] Figure 14 The results of the contact angle test of water (a) and oil (b) in air for the polystyrene fiber membrane prepared in Comparative Example 1 of the present invention are shown.
[0063] Figure 15 The process and results of the separation experiment of the oil-water mixture (a) and water-in-oil emulsion (b) of the photochromic polystyrene film prepared in Example 2 of the present invention.
[0064] Figure 16 This is a flowchart of the photochromic polystyrene film preparation method of this application. Detailed Implementation
[0065] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0066] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the application.
[0067] Figure 16 This is a flowchart of the method for preparing photochromic polystyrene films; the following describes the corresponding steps in detail with reference to each embodiment.
[0068] All chemical reagents used in the following examples are commercially available.
[0069] Example 1
[0070] Preparation of modified polystyrene:
[0071] Dissolve 0.500g of waste polystyrene foam fragments in 15.00mL of carbon tetrachloride, add 0.375mL of anhydrous tin tetrachloride, and then add 1.50mL of 1,4-dichloromethoxybutane. Stir the reaction at room temperature for 16h, then precipitate in ethanol, filter, wash, and vacuum dry at 60℃ for 12h to obtain chloromethylated polystyrene.
[0072] 0.200 g of chloromethylated polystyrene was dissolved in 8.00 mL of N,N-dimethylformamide, followed by the addition of 0.400 g of 4-hydroxyazophenol, 0.400 g of anhydrous potassium carbonate, and 0.040 g of potassium iodide. The mixture was heated to 70 °C and stirred for 7 h. The mixture was then allowed to settle in water, filtered, washed with acetonitrile, and dried under vacuum at 60 °C for 12 h to obtain modified polystyrene.
[0073] Figure 1 The above is the 1H NMR spectrum of the modified polystyrene prepared in Example 1. The peaks at 7.03 ppm and 6.57 ppm are attributed to the chemical shifts of hydrogen protons on the benzene ring of polystyrene, the peaks at 1.81 ppm and 1.40 ppm are attributed to the chemical shifts of hydrogen protons in the polystyrene skeleton structure, the peak at 4.94 ppm is attributed to the chemical shifts of hydrogen protons in the methylene group, and the peaks at 7.47 ppm and 7.89 ppm are attributed to the chemical shifts of hydrogen protons on the benzene ring of azobenzene. The above results confirm that the azobenzene UV-responsive group was successfully introduced into the polystyrene molecular structure, and modified polystyrene was prepared from waste polystyrene foam.
[0074] Example 2
[0075] Preparation of photochromic polystyrene film:
[0076] 1.000 g of the modified polystyrene prepared in Example 1 was dissolved in 3.70 mL of N,N-dimethylformamide and stirred until homogeneous to prepare a spinning solution. The spinning solution was injected into a spinneret, and electrospinning was performed using an electrospinning machine to obtain a photochromic polystyrene film. The positive voltage was 13 kV, the negative voltage was 2 kV, the syringe advance speed was 0.3 mm / min, the receiving distance was 20 cm, and the receiver rotation speed was 4800 r / h.
[0077] Figure 2 This is a photograph of the photochromic polystyrene film sample prepared in Example 2. The film has a mustard-gold appearance, and the fibers on the film surface are uniform and dense. Figure 3 This is a scanning electron microscope image of the photochromic polystyrene film prepared in Example 2. It can be seen that the fibers in the film are of uniform thickness and have smooth surfaces, and the fibers are interwoven to form a network structure.
[0078] Comparative Example 1
[0079] Preparation of polystyrene fiber membranes:
[0080] Weigh 2.000g of waste polystyrene foam fragments and dissolve them in 40.00mL of dichloromethane. The mixture is then settled in ethanol, filtered, and dried under vacuum at 60℃ for 12h to obtain recycled polystyrene.
[0081] Compared with Example 2, only the modified polystyrene in Example 2 was replaced with recycled polystyrene to obtain a polystyrene fiber membrane.
[0082] Figure 4 This is a photograph of the polystyrene fiber membrane sample prepared in Comparative Example 1. The membrane is white in appearance, which is clearly different from the photoluminescent polystyrene membrane prepared in Example 2.
[0083] Application Example 1
[0084] UV light responsiveness of photochromic polystyrene films:
[0085] Figure 5 Part (a) shows the UV-Vis absorption spectra of the N-methyl-2-pyrrolidone solution of modified polystyrene prepared in Example 1 after irradiation with 365 nm UV light for different times. It can be seen that the absorption band at 350 nm (attributed to the π-π* transition of the azobenzene structure) gradually weakens with increasing UV irradiation time, while the absorption band at 440 nm (attributed to the n-π* transition) gradually strengthens with increasing UV irradiation time, reaching a photostable state after 30 s of UV irradiation. This is because the azobenzene structure in the modified polystyrene gradually changes from the trans configuration to the cis configuration under UV irradiation. Figure 5Part (b) shows the UV-Vis absorption spectra of the above solution after being irradiated with visible light for different times. It can be seen that as the irradiation time with visible light increases, the absorption band at 350 nm gradually strengthens, while the absorption band at 440 nm gradually weakens. After 20 min of visible light irradiation, the absorption peak intensity basically returns to the state before UV irradiation. This is because the azo structure gradually changes from the cis configuration to the trans configuration under visible light.
[0086] Figure 6 Parts (a) and (b) show the trans-cis and cis-trans isomerization kinetics of the N-methyl-2-pyrrolidone solution of modified polystyrene prepared in Example 1, respectively. It can be seen that the isomerization of modified polystyrene follows first-order kinetics. The rate constants for the trans-cis and cis-trans isomerization reactions of modified polystyrene, as shown in the figure, are 0.20017 s⁻¹. -1 and 0.12655s -1 This confirms that the modified polystyrene prepared in Example 1 has a rapid UV-stimulated response, and that this rapid response is reversible. Figure 7 ).
[0087] Figure 8 The images shown are of the photochromic polystyrene film prepared in Example 2 before and after irradiation with 365nm UV light. Before UV irradiation, the film appears mustard gold, and after UV irradiation, the film turns yellowish-brown. The CIE color coordinate values L of the film before and after UV irradiation are also shown. * a * b * The values are 52.59, 13.34, 73.82 and 41.26, 24.71, 70.05 respectively. According to the formula... The calculated color difference value ΔE is 16.49. The above results confirm that the photochromic polystyrene film prepared in Example 2 has reversible photoresponse properties; that is, the film's color changes from mustard gold to yellowish-brown under UV light, and when the film is further irradiated with visible light, the color changes back from yellowish-brown to mustard gold. This is because the azobenzene structure in the modified polystyrene changes from trans to cis configuration under UV light and then from cis to trans configuration under visible light. Utilizing this reversible cis-trans isomerism process, by changing the light source (UV light and visible light), the film surface color can switch between mustard gold and yellowish-brown multiple times. Furthermore, because the color difference between the two colors is quite significant (ΔE>12), this color change is easily distinguishable to the naked eye and is suitable for anti-counterfeiting applications.
[0088] Appendix Figure 9 To compare the polystyrene fiber membrane prepared in Example 1 under UV and visible light irradiation, it was found that the color of the membrane surface did not change significantly after changing the light source.
[0089] The above results show that, unlike the photochromic polystyrene film prepared from modified polystyrene, the fiber film prepared from recycled polystyrene without the introduction of azobenzene structure has no UV responsiveness. This confirms that the azobenzene structure in modified polystyrene is the key to the reversible light-responsive color change of the photochromic polystyrene film.
[0090] Application Example 2
[0091] Brand anti-counterfeiting:
[0092] Figure 10 Part (a) is a schematic diagram of the process of making anti-counterfeiting labels using the photochromic polystyrene film prepared in Example 2, and part (b) is the prepared anti-counterfeiting label. It can be seen that under 365nm UV light irradiation, the brand pattern on the anti-counterfeiting label gradually appears; with continued irradiation with visible light, the brand pattern gradually disappears. This change is visible to the naked eye, and the process can be repeated multiple times. Therefore, brand anti-counterfeiting can be achieved by switching the light source. This confirms that the photochromic polystyrene film prepared in this invention can be used in the field of anti-counterfeiting.
[0093] Application Example 3
[0094] Information encryption and information transmission:
[0095] Figure 11 and Figure 12 Application of the photochromic polystyrene film prepared in Example 2 in information encryption and transmission. (See attached document.) Figure 10 In the production process of section (a), the brand pattern cutout template was replaced with an ASCII binary code cutout template and a QR code cutout template, respectively. Binary codes with information encryption and transmission functions were then created using photochromic polystyrene film. Figure 11 ) and QR code ( Figure 12 ).like Figure 11 As shown, the binary code can be displayed under 365nm UV light and can be converted into the English word "OK" to achieve information transmission, while the binary code gradually disappears under visible light. Figure 12 The QR code produced is an upgraded encryption model. It is visible under 365nm UV light and can be scanned by a smartphone to access the "Jiaxing University" website. However, it gradually disappears under visible light. These results demonstrate that the photochromic polystyrene film prepared using this invention can be used to design various complex information encryption modes, applicable to advanced information encryption and transmission fields.
[0096] Application Example 4
[0097] Surface wettability of photochromic polystyrene films:
[0098] Figure 13The results of the contact angle test for the photochromic polystyrene membrane prepared in Example 2 are shown. It can be seen that the contact angle of the membrane with water in air is 123.3°, and the contact angle with oil is 0°. This indicates that the prepared membrane has good hydrophobic / oleophilic properties and can be applied to oil-water separation.
[0099] Figure 14 The results show the contact angle test results of the polystyrene fiber membrane prepared in Comparative Example 1. It can be seen that the membrane has a water contact angle of 117.6° and an oil contact angle of 0° in air, exhibiting good hydrophobic / oleophilic properties.
[0100] The above results indicate that the photochromic polystyrene membrane prepared from modified polystyrene in Example 2 and the polystyrene fiber membrane prepared from recycled polystyrene in Comparative Example 1 both exhibit hydrophobic / oleophilic properties. This confirms that the surface wettability of the membrane is mainly based on the properties of polystyrene itself, and the introduction of the azobenzene structure did not affect the wettability of the membrane surface. Therefore, the prepared photochromic polystyrene membrane exhibits dual functionality, namely, photoresponsiveness and hydrophobic / oleophilic properties. Thus, the photochromic polystyrene membrane prepared by this invention can be applied not only to anti-counterfeiting and information encryption fields, but also to oil-water separation fields.
[0101] Application Example 5
[0102] Separation of oil-water mixtures:
[0103] 30.00 mL of oil (n-hexane) and 30.00 mL of methylene blue-stained deionized water were mixed to obtain an oil-water mixture. The oil-water mixture was separated using a photochromic polystyrene membrane prepared in Example 2. The separation process and results are as follows. Figure 15 As shown in part (a), the membrane exhibits hydrophobic / lipophilic properties, allowing oil to pass through while water is retained. Based on experimental results, the oil separation flux was calculated to be as high as 6790.88 L·m⁻¹. -2 ·h -1 The separation efficiency is as high as 99.82%, and the separation flux is still 6520.00 L·m after 10 cycles. -2 ·h -1 The separation efficiency remains above 99.60%. These results confirm that the photochromic polystyrene membrane prepared by this invention can efficiently separate oil-water mixtures and has excellent recyclability.
[0104] Application Example 6
[0105] Separation of water-in-oil emulsions:
[0106] 2 mg of Span 80 was added to 49.00 mL of oil (n-hexane), followed by 1.00 mL of deionized water. After thorough stirring, a water-in-oil emulsion was obtained. The water-in-oil emulsion was separated using a photochromic polystyrene membrane prepared in Example 2. The separation process and results are as follows. Figure 15 As shown in section (b), the water-in-oil emulsion before separation is an opaque emulsion, while after separation it is a clear and transparent oil. Based on the experimental results, the oil separation flux was calculated to be as high as 7073.55 L·m⁻¹. -2 ·h -1 The separation efficiency reached 99.60%, and the separation flux remained at 6520.00 L·m after 10 cycles. -2 ·h -1 The separation efficiency remains above 99.00%. This confirms that the photochromic polystyrene membrane prepared by this invention can efficiently separate water-in-oil emulsions and has excellent recyclability.
[0107] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims.
Claims
1. The application of photochromic polystyrene film in anti-counterfeiting or information encryption, characterized in that, The photochromic polystyrene film is a modified polystyrene electrospun fiber film, wherein the fiber diameter in the modified polystyrene electrospun fiber film is 1.0 to 12.0 μm; The structural formula of the modified polystyrene is as follows: ; Where m is an integer between 100 and 800, and n is an integer between 20 and 200; The photochromic polystyrene film has UV light responsive properties. The film color is mustard gold. Under UV light, the color of the photochromic polystyrene film changes from mustard gold to yellowish-brown. When the photochromic polystyrene film is yellowish-brown, after being exposed to visible light, the photochromic polystyrene film changes from yellowish-brown to mustard gold, and this change is reversible.
Citation Information
Patent Citations
PH / UV dual-response oil-water separation membrane as well as preparation method and application thereof
CN117138609A