A laminated cell and a lithium ion secondary battery
By setting a resistive layer on the surface of the positive active layer of the single-sided positive electrode, and optimizing the structure and material composition of the resistive layer, the problem of lithium plating on the single-sided positive electrode in stacked batteries is solved, thereby improving the safety and cycle performance of the battery.
Patent Information
- Application Number
- CN202411600575.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-11
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-11-11
AI Technical Summary
The problem of lithium deposition on a single positive electrode in existing stacked batteries leads to a decline in battery safety and cycle performance.
A resistive layer is set on the surface of the positive active layer of the single-sided positive electrode to increase the resistivity to 0.3kΩ·cm-2kΩ·cm. The structure and material composition of the resistive layer are optimized by adjusting parameters such as the adhesion force between the resistive layer and the positive active layer, the thickness ratio, and the particle size ratio of inorganic particles, so as to reduce the delithiation rate of the single-sided positive electrode during charging.
It effectively reduces the lithium delithiation rate of the single-sided positive electrode, improves the corresponding lithium plating problem of the negative electrode, and enhances the safety and cycle performance of the battery.
Smart Images

Figure CN119340454B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of lithium-ion battery technology, specifically to a stacked cell and a lithium-ion secondary battery. Background Technology
[0002] Battery manufacturing processes are mainly divided into two technical routes: stacking process and winding process. Compared with wound batteries, secondary batteries with stacked structure have great advantages in terms of energy density, safety and cycle life, which has prompted a large number of battery companies to enter the stacking field.
[0003] To improve energy density, the outermost electrode of a laminated battery cell is typically designed as a single-sided positive electrode, meaning the positive active material layer is only placed on one side of the outermost current collector. This results in uneven stress on both sides of the current collector, making it prone to curling. Furthermore, the single-sided electrode is prone to warping during cycling, affecting the battery's safety and cycle performance. To address these issues, the common practice is to increase the thickness of the outermost current collector to overcome stress. However, this introduces new problems: the higher current density on the outermost current collector makes lithium plating more likely on the negative electrode corresponding to the single-sided positive electrode. Summary of the Invention
[0004] In view of this, this application provides a stacked cell and a lithium-ion secondary battery, which aims to solve to some extent the problem of easy lithium deposition on the negative electrode corresponding to the single-sided positive electrode in existing stacked batteries.
[0005] According to an embodiment of this application, in a first aspect, the stacked battery cell provided by this application includes a plurality of positive electrode plates and a plurality of negative electrode plates arranged in alternating layers, a separator is provided between adjacent positive electrode plates and negative electrode plates, and the outermost electrode plate of the stacked battery cell is a single-sided positive electrode plate.
[0006] The single-sided positive electrode includes an outermost current collector, a positive active layer, and a resistive layer stacked in the direction of the interior of the stacked cell. The resistive layer at least covers the surface of the positive active layer away from the outermost current collector, and the resistive layer faces the separator. The resistivity R0 of the single-sided positive electrode is 0.3kΩ·cm-2kΩ·cm.
[0007] In one alternative embodiment, the unit area mm of the resistive layer 2 Within the range, the difference D between the maximum and minimum thickness of the resistive layer satisfies: D ≥ 0.5 μm.
[0008] In one optional embodiment, the adhesion force N1 between the resistive layer and the positive electrode active layer and the adhesion force N2 between the outermost current collector and the positive electrode active layer satisfy the condition: N1 > N2.
[0009] In one optional embodiment, the thickness H1 of the resistive layer and the thickness H2 of the positive electrode active layer satisfy the following condition: H2 / H1≥5.
[0010] In one alternative embodiment, the resistive layer comprises 80%-95% inorganic particles and 5%-20% binder.
[0011] In one optional embodiment, the median particle size Dv501 of the inorganic particles and the median particle size Dv502 of the active particles in the positive electrode active layer satisfy the following relationship: Dv502 / Dv501≥10.
[0012] In one optional embodiment, the inorganic particles are at least one of silicon dioxide, aluminum oxide, calcium oxide, titanium oxide, boehmite, magnesium oxide, and magnesium hydroxide.
[0013] In one alternative implementation, the Dv501 is 0.01μm-1μm.
[0014] In one alternative implementation, the Dv501 is 0.01μm-0.1μm.
[0015] In one alternative implementation, the Dv502 is 10μm-20μm.
[0016] In one alternative implementation, N1 is 1.5 gf / mm to 9 gf / mm.
[0017] In one alternative implementation, the N2 is 0.3 gf / mm to 1 gf / mm.
[0018] In one alternative implementation, H1 is 0.5 μm-6 μm.
[0019] In one alternative implementation, the H2 is 30μm-80μm.
[0020] In one optional embodiment, the inner positive electrode sheet disposed between the two outermost electrode sheets in the laminated cell includes a double-sided positive electrode sheet;
[0021] The surface resistance R1 of the single-sided positive electrode and the surface resistance R2 of the double-sided positive electrode satisfy the condition: R1 > 1 / 2R2.
[0022] In one optional embodiment, the porosity P1 of the single-sided positive electrode and the porosity P2 of the double-sided positive electrode satisfy the condition: P2 > P1.
[0023] In one alternative implementation, R1 is 0.3Ω / cm-2Ω / cm.
[0024] In one alternative implementation, R2 is 0.2Ω / cm to 2Ω / cm.
[0025] In one alternative implementation, P1 is 15%-30%.
[0026] In one alternative implementation, P2 is 20%-40%.
[0027] In one alternative embodiment, the thickness of the outermost current collector is 12μm-25μm.
[0028] In one optional embodiment, the thickness of the current collector of the double-sided positive electrode is 6μm-10μm.
[0029] In one optional embodiment, the diaphragm disposed toward the resistive layer is a thermally composite diaphragm, and the adhesive force N3 between the thermally composite diaphragm and the resistive layer is 0.1 gf / mm-2 gf / mm.
[0030] In one optional embodiment, the negative electrode sheet includes a negative electrode current collector and a negative electrode active layer disposed on the surface of the negative electrode current collector, the negative electrode active layer includes a negative electrode active material, the negative electrode active material includes silicon material; the resistivity R3 of the negative electrode sheet satisfies: 60Ω·cm≥R3≥2Ω·cm.
[0031] According to an embodiment of this application, in a second aspect, a lithium-ion secondary battery is provided, including the stacked cells described in the first aspect of this application.
[0032] In one optional embodiment, the lithium-ion secondary battery further includes an electrolyte, wherein the content of a carboxylic acid ester solvent in the electrolyte is A% and 50 ≥ A ≥ 10, and the content of an adhesive in the resistive layer is B% and 20 ≥ B ≥ 5, wherein A and B satisfy: 10 ≥ A / B ≥ 0.5.
[0033] The technical solution of this application has the following advantages:
[0034] The lithium-ion secondary battery provided in this application achieves a resistivity of 0.3kΩ·cm-2kΩ·cm by setting a resistive layer on the surface of the positive active layer of the single-sided positive electrode. The high-impedance resistive layer can reduce the delithiation rate of the single-sided positive electrode during charging and improve the lithium plating problem of the corresponding negative electrode.
[0035] Additional aspects and advantages of the embodiments of this application will be described and shown in part in the following description, or illustrated by practice of the embodiments of this application. Attached Figure Description
[0036] To more clearly illustrate the technical solutions in the specific embodiments of this application or the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of this application. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0037] Figure 1 This is a schematic diagram of the structure of a stacked battery cell in one embodiment of this application.
[0038] Figure 2 This is a SEM image of the cross-section of the outermost positive electrode sheet prepared in Embodiment A of this application.
[0039] The reference numerals in the attached figures are explained as follows:
[0040] 1. Inner positive electrode plate; 2. Negative electrode plate; 3. Outermost positive electrode plate; 101. Inner positive active layer; 102. Inner positive current collector; 103. Negative active layer; 104. Negative current collector; 105. Resistive layer; 106. Positive active layer; 107. Outermost current collector. Detailed Implementation
[0041] The following embodiments are provided to better understand this application and are not limited to the preferred embodiments described herein. They do not constitute a limitation on the content and scope of protection of this application. Any product that is the same as or similar to this application, derived by anyone under the guidance of this application or by combining features of this application with other prior art, falls within the scope of protection of this application.
[0042] It should be noted in the description of this application that the terms "inner" and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation on this application. In addition, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.
[0043] For experiments not specifically described in the examples, the procedures or conditions should be followed according to the conventional experimental procedures described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all commercially available conventional reagent products.
[0044] Furthermore, the technical features involved in the different embodiments of this application described below can be combined with each other as long as they do not conflict with each other.
[0045] To address the problem of lithium deposition on the negative electrode corresponding to the single-sided positive electrode in existing stacked batteries, this application provides the following solution.
[0046] According to a first aspect of this application, a laminated battery cell is provided, comprising a plurality of positive electrode plates and a plurality of negative electrode plates alternately stacked, wherein a separator is disposed between adjacent positive electrode plates and negative electrode plates, and the outermost electrode plate of the laminated battery cell is a single-sided positive electrode plate.
[0047] The single-sided positive electrode includes an outermost current collector, a positive active layer, and a resistive layer stacked in the direction of the interior of the stacked cell. The resistive layer at least covers the surface of the positive active layer away from the outermost current collector, and the resistive layer faces the separator. The resistivity R0 of the single-sided positive electrode is 0.3kΩ·cm-2kΩ·cm.
[0048] It should be noted that conventional single-sided positive electrode sheets (i.e., the outermost positive electrode sheet containing only the current collector and the positive active layer on one side) have relatively thick outer current collector layers, typically 12μm-25μm, resulting in low resistivity, generally less than 0.3kΩ·cm. This leads to a high current density on the single-sided positive electrode sheet, accelerating the lithium-ion insertion / extraction rate. This application addresses this by adding a resistive layer to the surface of the positive active layer of the single-sided positive electrode sheet, achieving a resistivity of 0.3kΩ·cm-2kΩ·cm. This high-impedance resistive layer reduces the lithium extraction rate of the single-sided positive electrode sheet during charging, thus improving the lithium plating problem of the corresponding negative electrode. As an example, the resistivity R0 of a single-sided positive electrode can be, for example, 0.3kΩ·cm, 0.6kΩ·cm, 0.8kΩ·cm, 1kΩ·cm, 1.2kΩ·cm, 1.4kΩ·cm, 1.6kΩ·cm, 1.8kΩ·cm, 2kΩ·cm, or within any two of the above values.
[0049] It is understood that in this application, the laminated cells are stacked in the following order: first electrode - separator - second electrode - separator - first electrode - separator... separator - second electrode - separator - first electrode. Therefore, the first and last stacked first electrode layers are the outermost electrode layers, and the first electrode layers between them are the inner electrode layers. Figure 1 For example, the structure of the laminated battery cell in one embodiment of this application will be further illustrated. Figure 1As shown, in the height direction of the stacked battery cell, from top to bottom, the outermost positive electrode 3, separator (not shown in the figure), negative electrode 2, separator, ... negative electrode 2, separator, inner positive electrode 1, separator, negative electrode 2, separator ... negative electrode 2, separator and outermost positive electrode 3 are stacked sequentially; wherein, the inner positive electrode 1 includes an inner positive current collector 102 and an inner positive active layer 101 disposed on two sides in the thickness direction of the inner positive current collector 102, the negative electrode 2 includes a negative current collector 104 and a negative active layer 103 disposed on two sides in the thickness direction of the negative current collector 104, and the outermost positive electrode 3 includes an outermost current collector 107, a positive active layer 106 and a resistive layer 105 stacked together.
[0050] Furthermore, the positive electrode active layer includes a positive electrode active material. The particle size of the positive electrode active material and the thickness of the positive electrode active layer together determine that the surface of the positive electrode active layer is not a plane. This causes the thickness of the resistive layer covering the surface of the positive electrode active layer to vary. For example, the thickness of the resistive layer is 2.41 μm in the first region, 1.43 μm in the second region, 1.97 μm in the third region, and 0.793 μm in the fourth region. Therefore, it can be concluded that the thickness of the resistive layer per unit area (mm²) is... 2 Within the resistor layer, the difference D between the maximum and minimum thicknesses of the resistor layer satisfies: D ≥ 0.5 μm. This indicates that the resistor layer is partially embedded in the positive electrode active layer. This improves the adhesion between the resistor layer and the positive electrode active layer while avoiding excessive cell thickness due to the addition of a resistor layer, thus preventing energy density loss.
[0051] Furthermore, the adhesion force between the resistive layer and the positive electrode active layer is defined as N1, and the adhesion force between the outermost current collector and the positive electrode active layer is defined as N2. N1 and N2 satisfy the condition: N1 > N2. This allows for the improvement of the interface impedance between the resistive layer and the positive electrode active layer, thereby enhancing the cell's electrical performance. This is achieved by increasing the impedance of the single-sided positive electrode to reduce the lithium delithiation rate during charging, thus improving lithium plating on the corresponding negative electrode. In some implementations, N1 is 1.5gf / mm-9gf / mm. For example, N1 can be 1.5gf / mm, 3gf / mm, 4.5gf / mm, 6gf / mm, 7.5gf / mm, 9gf / mm, or any value within the range of any two of the above values; N2 is 0.3gf / mm-1gf / mm. For example, N2 can be 0.3gf / mm, 0.4gf / mm, 0.5gf / mm, 0.6gf / mm, 0.7gf / mm, 0.8gf / mm, 0.9gf / mm, 1gf / mm, or any value within the range of any two of the above values.
[0052] To minimize battery energy density loss, the thickness of the resistive layer must be kept as small as possible. Therefore, in this application, the thickness H1 of the resistive layer and the thickness H2 of the positive electrode active layer satisfy the condition: H2 / H1≥5. This ensures that the high impedance of the single-sided positive electrode reduces the lithium delithiation rate of the single-sided positive electrode during charging, thereby improving the lithium plating of the corresponding negative electrode and further reducing battery energy density loss. In some implementations, H1 is 0.5μm-6μm. For example, H1 can be 0.5μm, 1μm, 1.5μm, 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 4.5μm, 5μm, 5.5μm, 6μm, or any two of the above values. H2 is 30μm-80μm. For example, H2 can be 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, or any two of the above values.
[0053] Specifically, the resistive layer described in this application comprises 80%-95% inorganic particles and 5%-20% binder. It should be noted that the binder content in the inner positive electrode layer between the two outermost electrodes of a laminated battery cell is typically around 1%. This application, by increasing the binder content in the resistive layer, not only ensures the adhesion between the resistive layer and the positive active layer and separator, but more importantly, after the resistive layer swells upon contact with the electrolyte, the high binder content can provide greater impedance, helping to improve the resistivity of the single-sided positive electrode. Based on the aforementioned functions of the resistive layer, the resistive layer of this application does not contain conductive agents, and the inorganic particles are also non-conductive. In fact, the inorganic particles in this application should be high-resistivity materials. In some embodiments, the material of the inorganic particles can be, for example, at least one of silicon dioxide, aluminum oxide, calcium oxide, titanium dioxide (molecular formula Ti2O3), boehmite, magnesium oxide, and magnesium hydroxide.
[0054] Furthermore, the particle size Dv501 of the inorganic particles and the particle size Dv502 of the active particles in the positive electrode active layer satisfy the following relationship: Dv502 / Dv501≥10. Small-diameter inorganic particles can be embedded between large-diameter positive electrode active particles. This not only improves the adhesion between the resistive layer and the positive electrode active layer, thereby effectively increasing the resistivity of the single-sided positive electrode sheet, thus reducing the lithium delithiation rate of the single-sided positive electrode sheet during charging and improving the lithium plating effect of the corresponding negative electrode, but also avoids excessive increases in cell thickness, which would lead to a loss of battery energy density. In some implementations, Dv501 is 0.01μm-1μm. For example, Dv501 can be 0.01μm, 0.03μm, 0.05μm, 0.07μm, 0.09μm, 0.1μm, 0.3μm, 0.7μm, 1μm, or any two of the above values. Dv502 is 10μm-20μm. For example, Dv502 can be 10μm, 12μm, 14μm, 16μm, 18μm, 20μm, or any two of the above values.
[0055] To improve battery performance and enhance battery safety, in stacked cells, except for the outermost electrode which is a single-sided positive electrode, the remaining inner electrode layers (i.e., the electrode layers located between the two outermost electrode layers) are all double-sided electrodes. As the name suggests, this means that positive active material is coated on both surfaces of the inner current collector (typically 6μm-10μm thick) to form a double-sided positive electrode, or negative active material is coated on both surfaces to form a double-sided negative electrode. In this application, the surface resistance R1 of the single-sided positive electrode and the surface resistance R2 of the double-sided positive electrode satisfy the condition: R1 > 1 / 2R2. This indicates that the increased surface resistance of the single-sided positive electrode reduces the lithium stripping rate during charging, preventing lithium deposition on the corresponding negative electrode. In some implementations, R1 is 0.3Ω / cm-2Ω / cm. For example, R1 can be 0.3Ω / cm, 0.7Ω / cm, 1.0Ω / cm, 1.3Ω / cm, 1.7Ω / cm, 2.0Ω / cm, or any two of the above values. R2 is 0.2Ω / cm-2Ω / cm. For example, R2 can be 0.2Ω / cm, 0.5Ω / cm, 1.0Ω / cm, 1.5Ω / cm, 2.0Ω / cm, or any two of the above values.
[0056] Furthermore, the porosity P1 of the single-sided positive electrode sheet and the porosity P2 of the double-sided positive electrode sheet satisfy the condition: P2 > P1. Reducing the porosity of the single-sided positive electrode sheet, on the one hand, helps to increase the adhesion between the resistive layer and the positive electrode active layer, not only reducing the interfacial impedance between them but also increasing the resistivity of the single-sided positive electrode sheet, thereby solving the lithium plating problem of the corresponding negative electrode. On the other hand, it also avoids excessive cell thickness, thus helping to reduce the energy density loss of the battery. In some embodiments, P1 is 15%-30%, for example, P1 can be 15%, 18%, 20%, 23%, 26%, 30%, etc., or within any two of the above values; P2 is 20%-40%, for example, P2 can be 20%, 25%, 30%, 35%, 40%, etc., or within any two of the above values.
[0057] It should be noted that this application does not specifically limit the type of positive electrode active material. Any positive electrode active material used in lithium-ion secondary batteries can be used in this application. For example, it can be at least one of lithium manganese oxide, lithium nickel oxide, lithium nickel manganese oxide, lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium manganese iron phosphate, and lithium-rich manganese-based materials.
[0058] The lithium-ion secondary battery of this application can use conventional polyethylene or polypropylene separators. During the stacking process, the separator and electrode are preheated and pressed before stacking. The separator after this step is called a thermally composite separator. In particular, when the separator facing the resistive layer of the single-sided positive electrode is a thermally composite separator, the adhesion between the resistive layer and the separator adhesive layer can be further enhanced, reducing the interfacial impedance. In some embodiments, the adhesive force N3 between the thermally composite separator and the resistive layer is 0.1 gf / mm-2 gf / mm. As an example, N3 can be 0.1 gf / mm, 0.3 gf / mm, 0.5 gf / mm, 0.7 gf / mm, 1 gf / mm, 1.2 gf / mm, 1.5 gf / mm, 1.8 gf / mm, 2 gf / mm, etc., or within any two of the above values.
[0059] According to a second aspect of this application, a lithium-ion secondary battery is provided, comprising the stacked cells described in the first aspect of this application.
[0060] The space between the positive and negative electrodes of a lithium-ion secondary battery is filled with an electrolyte. The main components of the electrolyte include organic solvents and lithium salt electrolyte. These components create an environment inside the battery that can conduct ions, allowing lithium ions to move freely between the positive and negative electrodes, thus enabling the battery to charge and discharge. To improve the kinetic performance of battery cells, carboxylic acid ester solvents are often used. However, these solvents can affect the bonding effect of the single-sided positive electrode and easily deteriorate the furnace temperature. Therefore, it is necessary to control the content A% of carboxylic acid ester solvents in the electrolyte to meet the following conditions: 50 ≥ A ≥ 10 and 10 ≥ A / B ≥ 0.5, where B is the content of binder in the resistive layer. According to the aforementioned value of B, which is 5-20, a high binder content can not only ensure the bonding effect between the resistive layer and the positive electrode active layer and the separator, but more importantly, it can also provide more impedance after the resistive layer swells upon contact with the electrolyte, thereby increasing the resistivity of the single-sided positive electrode and solving the lithium plating problem of the corresponding negative electrode. At the same time, the content of carboxylic acid ester solvents in the electrolyte also needs to be controlled within an appropriate range. This can further ensure the bonding effect between the single-sided positive electrode and the adjacent separator while ensuring the kinetic balance of the battery cell, thus helping to improve the safety performance of the battery cell. In some embodiments, the content A% of carboxylic acid ester solvent in the electrolyte can be, for example, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, or within any two of the above values. The content B% of adhesive in the resistive layer can be 5%, 7.5%, 10%, 12.5%, 15%, 17.5%, 20%, or within any two of the above values. Then the value of A / B can be 0.5, 1, 2, 4, 6, 8, 9, 10, or within any two of the above values.
[0061] As an example, the carboxylic acid ester solvent in this application may be at least one of methyl formate (MF), ethyl acetate (EA), ethyl propionate (EP), methyl acetate (MA), methyl butyrate (MB), methyl propyl carbonate (MP), propyl propionate (PP), ethyl butyrate (EB), or their fluorinated derivatives, wherein the fluorinated carboxylic acid ester may be, for example, methyl fluoroformate, ethyl difluoroformate, ethyl 2-fluoropropionate, methyl fluoroacetate, methyl 4-fluorobutyrate, propyl 2-fluoropropionate, or ethyl 4-fluorobutyrate.
[0062] It is understood that the negative electrode sheet includes a negative electrode current collector and a negative electrode active layer disposed on the surface of the negative electrode current collector. The negative electrode active layer includes a negative electrode active material. In some embodiments of this application, the negative electrode active material may be silicon, such that the resistivity R3 of the negative electrode sheet satisfies: 60Ω·cm ≥ R3 ≥ 2Ω·cm. As an example, R3 may be 2Ω·cm, 6Ω·cm, 10Ω·cm, 20Ω·cm, 30Ω·cm, 40Ω·cm, 50Ω·cm, 60Ω·cm, etc., or within any two of the above values. This is because silicon negative electrodes have advantages such as high energy density, good safety performance, excellent fast charging performance, and low cost. When applied to the lithium-ion secondary battery of this application, it can significantly improve the energy density of the cell. Furthermore, the resistive layer of the single-sided positive electrode sheet, in addition to having high impedance, also has elastic characteristics, which can alleviate the thickness expansion of the silicon negative electrode.
[0063] As an example, the silicon material in this application may be at least one of elemental silicon, silicon alloy, silicon-carbon, and silicon-oxygen, and the amount of silicon material incorporated may be, for example, 5%, 6%, 7%, 8%, 9%, 10%, or within any two of the above values.
[0064] The present application is further described in detail below with reference to specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in this application. Where specific experimental steps or conditions are not specified in the embodiments and comparative examples, they can be performed according to the conventional experimental steps or conditions described in the literature in the art. Where the manufacturers of reagents or instruments are not specified, they are all commercially available conventional reagent products. In all embodiments and comparative examples of this application, the unit % represents mass percentage content.
[0065] Example A
[0066] Step 1: Fabrication of the inner positive electrode layer
[0067] Conductive carbon black and carbon nanotubes in a 1:1 mass ratio were added to a PVDF adhesive and stirred until homogeneous. Then, lithium cobalt oxide (particle size Dv502 of 15 μm) was added and stirred until homogeneous again to prepare a positive electrode active material slurry. This slurry was coated onto both sides of a positive electrode current collector (i.e., an 8 μm thick aluminum foil). After baking and rolling, an inner positive electrode sheet was obtained. In the positive electrode active layer of this inner positive electrode sheet, the mass fraction of lithium cobalt oxide was 97.6%, the mass fraction of PVDF was 1.05%, and the mass fraction of conductive carbon black and carbon nanotubes was 1.35%.
[0068] Step 2: Preparing the outermost positive electrode sheet
[0069] The positive electrode active material slurry prepared in the first step was coated onto one side of a 15 μm thick aluminum foil and baked to obtain a single-sided positive electrode active layer. Vaporized SiO2 particles (particle size Dv501 of 0.1 μm) at a mass ratio of 95:5 were mixed with PVDF adhesive and stirred until homogeneous to obtain a resistive layer slurry. This resistive layer slurry was coated onto the surface of the single-sided positive electrode active layer away from the aluminum foil, and after baking and rolling, the outermost positive electrode sheet was obtained.
[0070] Figure 2 This is a SEM image of the cross-section of the outermost positive electrode sheet prepared in this embodiment. As can be seen from the image, the resistive layer is partially embedded in the positive electrode active layer. The resistive layer has a unit area of [missing information - likely mm]. 2 The difference D between the maximum and minimum thickness of the internal resistance layer is 1.617 μm.
[0071] Step 3: Preparation of the negative electrode sheet
[0072] 97.3% silicon-carbon (containing 5% silicon), 0.5% conductive carbon black, 1.3% PVDF and 0.9% CMC are mixed evenly, and then an appropriate amount of deionized water is added to disperse evenly to prepare a negative electrode active material slurry. The negative electrode active material slurry is coated on both sides of a carbon-coated copper foil, and the negative electrode sheet is obtained after baking and rolling.
[0073] Step 4: Fabrication of lithium-ion secondary batteries
[0074] Stacked cells are obtained by stacking and pressing the outermost positive electrode sheet, separator, first negative electrode sheet, separator, first inner positive electrode sheet, separator, ... separator, Nth negative electrode sheet, separator, and outermost positive electrode sheet. The cells are then packaged, baked, injected with electrolyte, formed, resealed, sorted, and subjected to OCV to obtain lithium-ion secondary batteries.
[0075] The separator comprises a first adhesive layer, a substrate layer, a ceramic layer, and a second adhesive layer, which are sequentially stacked. The first adhesive layer is bonded to the negative electrode, and the second adhesive layer is bonded to the positive electrode. A commercially available conventional electrolyte is used, with a carboxylic acid ester solvent content of 25%.
[0076] Example 1-1
[0077] Except for the following, the rest is the same as in Example A.
[0078] The mass ratio of gaseous SiO2 particles to PVDF adhesive in the resistive layer slurry is 90:10.
[0079] Examples 1-2
[0080] Except for the following, the rest is the same as in Example A.
[0081] The mass ratio of gaseous SiO2 particles to PVDF adhesive in the resistive layer slurry is 85:15.
[0082] Examples 1-3
[0083] Except for the following, the rest is the same as in Example A.
[0084] The mass ratio of gaseous SiO2 particles to PVDF adhesive in the resistive layer slurry is 80:20.
[0085] Example 2-1
[0086] Except for the following, the rest is the same as in Example A.
[0087] The particle size Dv501 of the gaseous SiO2 particles is 0.01 μm.
[0088] Example 2-2
[0089] Except for the following, the rest is the same as in Example A.
[0090] The particle size Dv501 of the gaseous SiO2 particles is 0.2 μm, and the particle size Dv502 of lithium cobalt oxide is 10 μm.
[0091] Example 2-3
[0092] Except for the following, the rest is the same as in Example A.
[0093] The particle size Dv501 of the gaseous SiO2 particles is 1 μm, and the particle size Dv502 of lithium cobalt oxide is 20 μm.
[0094] Example 3-1
[0095] Except for the following, the rest is the same as in Example A.
[0096] The thickness H1 of the resistive layer is 6 μm.
[0097] Example 3-2
[0098] Except for the following, the rest is the same as in Example A.
[0099] The thickness H1 of the resistive layer is 0.5 μm.
[0100] Example 3-3
[0101] Except for the following, the rest is the same as in Example A.
[0102] The thickness H2 of the positive electrode active layer is 55 μm.
[0103] Examples 3-4
[0104] Except for the following, the rest is the same as in Example A.
[0105] The thickness H2 of the positive electrode active layer is 80 μm.
[0106] Example 4-1
[0107] Except for the following, the rest is the same as in Example A.
[0108] The electrolyte contains 50% carboxylic acid ester solvents.
[0109] Example 4-2
[0110] Except for the following, the rest is the same as in Example A.
[0111] The electrolyte contains 10% carboxylic acid ester solvents.
[0112] Example 4-3
[0113] Except for the following, the rest is the same as in Example A.
[0114] The electrolyte contains 30% carboxylic acid ester solvent, and the resistive layer slurry contains 20% PVDF adhesive.
[0115] Example 4-4
[0116] Except for the following, the rest is the same as in Example A.
[0117] The electrolyte contains 10% carboxylic acid ester solvent, and the resistive layer slurry contains 20% PVDF adhesive.
[0118] Example 5-1
[0119] Except for the following, the rest is the same as in Example A.
[0120] The particle size Dv501 of the gaseous SiO2 particles is 0.9 μm.
[0121] Example 5-2
[0122] Except for the following, the rest is the same as in Example A.
[0123] The mass ratio of gaseous SiO2 particles to PVDF adhesive in the resistive layer slurry is 96:4.
[0124] Example 5-3
[0125] Except for the following, the rest is the same as in Example A.
[0126] The particle size Dv501 of the gaseous SiO2 particles is 2 μm.
[0127] Example 5-4
[0128] Except for the following, the rest is the same as in Example A.
[0129] The thickness H2 of the positive electrode active layer is 14.5 μm.
[0130] Example 5-5
[0131] Except for the following, the rest is the same as in Example A.
[0132] The electrolyte contains 40% carboxylic acid ester solvents, and the resistive layer slurry contains 4.8% PVDF adhesive.
[0133] Example B
[0134] Step 1: Fabrication of the inner positive electrode layer
[0135] Conductive carbon black and carbon nanotubes in a 1:1 mass ratio were added to a PVDF adhesive and stirred until homogeneous. Then, lithium manganese iron phosphate (particle size Dv502 of 10 μm) was added and stirred until homogeneous to prepare a positive electrode active material slurry. This slurry was coated onto both sides of a positive electrode current collector (i.e., a 10 μm thick aluminum foil). After baking and rolling, an inner positive electrode sheet was obtained. In the positive electrode active layer of this inner positive electrode sheet, the mass fraction of lithium manganese iron phosphate was 97%, the mass fraction of PVDF was 1%, and the mass fractions of conductive carbon black and carbon nanotubes were 2%.
[0136] Step 2: Preparing the outermost positive electrode sheet
[0137] The positive electrode active material slurry prepared in the first step was coated onto one side of a 20 μm thick aluminum foil, and after baking, a single-sided positive electrode active layer was obtained. Calcium oxide (particle size Dv501 of 0.1 μm) at a mass ratio of 82:18 was mixed with PVDF adhesive and stirred until homogeneous to obtain a resistive layer slurry. This resistive layer slurry was coated onto the surface of the single-sided positive electrode active layer away from the aluminum foil, and after baking and rolling, the outermost positive electrode sheet was obtained. The thickness H2 of the positive electrode active layer was 40 μm, the thickness H1 of the resistive layer was 2 μm, and the resistive layer was partially embedded in the positive electrode active layer. The resistive layer had a unit area of [missing information - likely a unit area measurement]. 2 The difference D between the maximum and minimum thickness of the internal resistance layer is 1.1 μm.
[0138] Step 3: Preparation of the negative electrode sheet
[0139] 97.3% silicon-carbon (containing 10% silicon), 0.5% conductive carbon black, 1.3% PVDF and 0.9% CMC are mixed evenly, and then an appropriate amount of deionized water is added to disperse evenly to prepare a negative electrode active material slurry. The negative electrode active material slurry is coated on both sides of a carbon-coated copper foil, and the negative electrode sheet is obtained after baking and rolling.
[0140] Step 4: Fabrication of lithium-ion secondary batteries
[0141] Stacked cells are obtained by stacking and pressing the outermost positive electrode sheet, separator, first negative electrode sheet, separator, first inner positive electrode sheet, separator, ... separator, Nth negative electrode sheet, separator, and outermost positive electrode sheet. The cells are then packaged, baked, injected with electrolyte, formed, resealed, sorted, and subjected to OCV to obtain lithium-ion secondary batteries.
[0142] The separator comprises a first adhesive layer, a substrate layer, a ceramic layer, and a second adhesive layer, which are sequentially stacked. The first adhesive layer is bonded to the negative electrode, and the second adhesive layer is bonded to the positive electrode. A commercially available conventional electrolyte is used, and the content of carboxylic acid ester solvent in the electrolyte is 15%.
[0143] Example C
[0144] Step 1: Fabrication of the inner positive electrode layer
[0145] Conductive carbon black was added to the PVDF adhesive and stirred until homogeneous. Then, lithium nickel cobalt manganese oxide (NCM811) with a particle size of 12 μm (Dv502) was added and stirred until homogeneous to prepare a positive electrode active material slurry. This positive electrode active material slurry was coated onto both sides of the positive electrode current collector (i.e., an 8 μm thick aluminum foil). After baking and rolling, the inner positive electrode sheet was obtained. In the positive electrode active layer of this inner positive electrode sheet, the mass fraction of NCM811 was 98%, the mass fraction of PVDF was 1.1%, and the mass fraction of conductive carbon black was 0.9%.
[0146] Step 2: Preparing the outermost positive electrode sheet
[0147] The positive electrode active material slurry prepared in the first step was coated onto one side of an 18 μm thick aluminum foil, and after baking, a single-sided positive electrode active layer was obtained. Alumina (particle size Dv501 of 0.08 μm) at a mass ratio of 88:12 was mixed with PVDF adhesive and stirred evenly to obtain a resistive layer slurry. This resistive layer slurry was coated onto the surface of the single-sided positive electrode active layer away from the aluminum foil, and after baking and rolling, the outermost positive electrode sheet was obtained. The thickness H2 of the positive electrode active layer was 60 μm, and the thickness H1 of the resistive layer was 4 μm. The resistive layer was partially embedded in the positive electrode active layer, with a unit area of mm² of resistive layer. 2 The difference D between the maximum and minimum thickness of the internal resistance layer is 1.8 μm.
[0148] Step 3: Preparation of the negative electrode sheet
[0149] 98% silicon-carbon (containing 7% silicon), 0.5% conductive carbon black, 1% PVDF and 0.5% CMC are mixed evenly, and then an appropriate amount of deionized water is added to disperse evenly to prepare a negative electrode active material slurry. The negative electrode active material slurry is coated on both sides of a carbon-coated copper foil, and the negative electrode sheet is obtained after baking and rolling.
[0150] Step 4: Fabrication of lithium-ion secondary batteries
[0151] Stacked cells are obtained by stacking and pressing the outermost positive electrode sheet, separator, first negative electrode sheet, separator, first inner positive electrode sheet, separator, ... separator, Nth negative electrode sheet, separator, and outermost positive electrode sheet. The cells are then packaged, baked, injected with electrolyte, formed, resealed, sorted, and subjected to OCV to obtain lithium-ion secondary batteries.
[0152] The separator comprises a first adhesive layer, a substrate layer, a ceramic layer, and a second adhesive layer stacked sequentially. The first adhesive layer is bonded to the negative electrode, and the second adhesive layer is bonded to the positive electrode. A commercially available conventional electrolyte is used, with a carboxylic acid ester solvent content of 30%.
[0153] Example D
[0154] Step 1: Fabrication of the inner positive electrode layer
[0155] Conductive carbon black and carbon nanotubes in a 1:1 mass ratio were added to a PVDF adhesive and stirred until homogeneous. Then, lithium nickelate (particle size Dv502 of 18 μm) was added and stirred until homogeneous again to prepare a positive electrode active material slurry. This slurry was coated onto both sides of a positive electrode current collector (i.e., a 9 μm thick aluminum foil). After baking and rolling, an inner positive electrode sheet was obtained. In the positive electrode active layer of this inner positive electrode sheet, the mass fraction of lithium nickelate was 97.2%, the mass fraction of PVDF was 1.2%, and the mass fraction of conductive carbon black and carbon nanotubes was 1.6%.
[0156] Step 2: Preparing the outermost positive electrode sheet
[0157] The positive electrode active material slurry prepared in the first step was coated onto one side of a 25 μm thick aluminum foil, and after baking, a single-sided positive electrode active layer was obtained. Titanium oxide (particle size Dv501 of 0.01 μm) at a mass ratio of 93:7 was mixed with PVDF adhesive and stirred until homogeneous to obtain a resistive layer slurry. This resistive layer slurry was coated onto the surface of the single-sided positive electrode active layer away from the aluminum foil, and after baking and rolling, the outermost positive electrode sheet was obtained. The thickness H2 of the positive electrode active layer was 70 μm, and the thickness H1 of the resistive layer was 1 μm. The resistive layer was partially embedded in the positive electrode active layer, with a unit area of mm² of resistive layer. 2 The difference D between the maximum and minimum thickness of the internal resistance layer is 0.2 μm.
[0158] Step 3: Preparation of the negative electrode sheet
[0159] 97.3% silicon-carbon (containing 8% silicon), 0.5% conductive carbon black, 1.3% PVDF and 0.9% CMC are mixed evenly, and then an appropriate amount of deionized water is added to disperse evenly to prepare a negative electrode active material slurry. The negative electrode active material slurry is coated on both sides of a carbon-coated copper foil, and the negative electrode sheet is obtained after baking and rolling.
[0160] Step 4: Fabrication of lithium-ion secondary batteries
[0161] Stacked cells are obtained by stacking and pressing the outermost positive electrode sheet, separator, first negative electrode sheet, separator, first inner positive electrode sheet, separator, ... separator, Nth negative electrode sheet, separator, and outermost positive electrode sheet. The cells are then packaged, baked, injected with electrolyte, formed, resealed, sorted, and subjected to OCV to obtain lithium-ion secondary batteries.
[0162] The separator comprises a first adhesive layer, a substrate layer, a ceramic layer, and a second adhesive layer stacked sequentially. The first adhesive layer is bonded to the negative electrode, and the second adhesive layer is bonded to the positive electrode. A commercially available conventional electrolyte is used, with a carboxylic acid ester solvent content of 36%.
[0163] Comparative Example 1
[0164] Except for the following, the rest is the same as in Example A.
[0165] The outermost positive electrode does not contain a resistive layer.
[0166] Comparative Example 2
[0167] Except for the following, the rest is the same as in Example A.
[0168] Titanium dioxide was used to replace fumed SiO2 in the preparation of the resistive layer paste.
[0169] Comparative Example 3
[0170] Except for the following, the rest is the same as in Example A.
[0171] Magnesium oxide was used instead of fumed SiO2 to prepare the resistive layer paste.
[0172] Test case
[0173] 1. Particle size test
[0174] Ultrapure water was selected as the dispersion medium. 1g of the sample to be tested was added to 1L of dispersion medium, and the sample was sonicated for 60 minutes to fully disperse the sample and form a uniform suspension or dispersion. The prepared sample suspension or dispersion was poured into the sample cell, and the laser particle size analyzer was turned on for testing. After the test was completed, the computer generated a particle size distribution map and related data report.
[0175] 2. Coating thickness test
[0176] This was derived from the SEM image of the coating cross-section.
[0177] 3. Adhesion test
[0178] Testing equipment: Tensile testing machine. Cut the rolled positive electrode sheet into 25mm widths. Prepare a flat, thin steel plate and attach a strip of double-sided tape to its center. Attach the electrode sheet to the tape, ensuring a perfect fit between the electrode sheet and the tape to avoid testing errors. Insert the steel plate with the attached electrode sheet into the lower clamp of the tensile testing machine and fix it vertically. Clamp the electrode sheet without tape onto the upper clamp, fixing it at a 90° angle to the electrode sheet in the lower clamp. Set parameters such as test width, peel length, and peel speed on the tensile testing machine. Start the test program; the tensile testing machine will apply tensile force according to the set parameters and record the force changes during the peeling process. After the test, the peel strength curve and average value data will be obtained.
[0179] 4. Surface resistance test
[0180] Discharge the battery to the lower limit voltage, then disassemble it in a drying room, take out the positive electrode sheet and let it air dry naturally in the drying room, and then place the positive electrode sheet on a surface resistance tester for testing.
[0181] 5. Resistivity test
[0182] Discharge the battery to the lower limit voltage, then disassemble it in a drying room, take out the positive electrode and let it air dry naturally in the drying room, and then place the positive / negative electrode on a resistivity tester for testing.
[0183] 6. Porosity test
[0184] The positive electrode is placed in a true density meter, using helium as the medium. The pressure in the measuring chamber is gradually increased to a specified value, and then the helium expands into the expansion chamber. The equilibrium pressure of the two processes is automatically recorded by the instrument. According to the law of conservation of mass, after calibrating the volumes of the measuring chamber and the expansion chamber using a standard sphere, the difference between the two is the true volume of the electrode. The porosity is then calculated using the formula: porosity = (electrode volume - true electrode volume) / electrode volume.
[0185] 7. Energy density retention rate test
[0186] The prepared battery was charged to full capacity under constant current and constant voltage at 25℃, and then discharged to 3.0V at 0.5C. The discharged capacity was recorded as the battery capacity.
[0187] The prepared finished battery was charged to 50% SOC at 25°C, and the battery thickness was tested using 600g PPG.
[0188] Calculate the volumetric energy density (ED) = battery capacity * platform voltage / battery length / width / thickness.
[0189] Calculate the ED loss rate as follows: (Energy density of Comparative Example 1 - Energy density of Example) / Energy density of Comparative Example 1.
[0190] 8. Loop Testing
[0191] The prepared batteries were subjected to 2C / 4C charge-discharge cycles at 25°C for 800 cycles to confirm the battery capacity retention and expansion rate.
[0192] After 800 cycles of charging at 3C and discharging at 1C, the electrode was dissected to observe whether the outermost current collector was curled and whether lithium plating occurred on the corresponding negative electrode. Specifically: if the entire surface of the negative electrode was golden yellow after dissection, it was considered no lithium plating; if 2-5 gray spots appeared on the surface, it was considered slight lithium plating; and if more than 5 gray spots appeared, it was considered lithium plating.
[0193] The test results are shown in Tables 1 and 2. In Table 1, " / " indicates that the sample does not exist; R0 represents the resistivity of a single-sided positive electrode; and D is the area per unit area (mm²). 2 The difference between the maximum and minimum thickness of the resistive layer within the resistive layer; N1 is the adhesive force between the resistive layer and the positive electrode active layer; N2 is the adhesive force between the outermost current collector and the positive electrode active layer; N3 is the adhesive force between the resistive layer and the thermal composite separator; R1 is the sheet resistance of the single-sided positive electrode; R2 is the sheet resistance of the double-sided positive electrode; R3 is the resistivity of the negative electrode; P1 is the porosity of the single-sided positive electrode; and P2 is the porosity of the double-sided positive electrode.
[0194] Table 1
[0195]
[0196]
[0197] Table 2
[0198]
[0199]
[0200] As shown in Tables 1 and 2, the resistivity R0 of the single-sided positive electrode in all embodiments is between 0.3 and 2 kΩ·cm, which can significantly improve the lithium plating problem of the corresponding negative electrode. However, Comparative Example 1 did not have a resistive layer, Comparative Example 2 used titanium dioxide to prepare the resistive layer, which resulted in a lower resistivity of the single-sided positive electrode. Comparative Example 3 used magnesium oxide to prepare the resistive layer, resulting in a higher resistivity of the single-sided positive electrode. None of the above comparative examples can solve the lithium plating problem of the negative electrode.
[0201] Compared to other embodiments, Embodiment 5-1 has a smaller unit area (mm) of resistive layer. 2 The difference between the maximum and minimum thickness of the internal resistance layer is less than 0.5 μm, increasing the battery thickness and resulting in significant energy density loss. In Example 5-4, the thickness of the positive active layer in the single-sided positive electrode is too small, while in Example 3-1, the thickness of the resistance layer is too large, leading to substantial energy density loss. In Examples 5-2 and 5-5, the binder content in the resistance layer is too low, resulting in low impedance of the single-sided positive electrode and high local current density, leading to slight lithium plating and affecting battery cycle performance. In Example 5-3, the inorganic particles in the resistance layer are too large, resulting in poor adhesion between the single-sided positive electrode and the separator, also affecting battery cycle performance.
[0202] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this application.
Claims
1. A laminated battery cell, comprising a plurality of positive electrode plates and a plurality of negative electrode plates alternately stacked, wherein a separator is disposed between adjacent positive electrode plates and negative electrode plates, and the outermost electrode plate of the laminated battery cell is a single-sided positive electrode plate; characterized in that, The single-sided positive electrode sheet includes an outermost current collector, a positive active layer, and a resistive layer stacked in the direction of the interior of the stacked cell. The resistive layer at least covers the surface of the positive active layer away from the outermost current collector, and the resistive layer faces the separator. The resistivity R0 of the single-sided positive electrode sheet is 0.3kΩ·cm-2kΩ·cm. The resistive layer comprises 80%-95% inorganic particles and 5%-20% binder. The inorganic particles include at least one of fumed silica, alumina, calcium oxide, and titanium oxide. % represents the mass percentage content. The inner positive electrode sheet disposed between the two outermost electrode sheets in the stacked cell includes a double-sided positive electrode sheet. The double-sided positive electrode sheet is formed by coating both surfaces of the inner current collector with a positive active material. The double-sided positive electrode sheet does not contain the resistive layer. The sheet resistance R1 of the single-sided positive electrode sheet and the sheet resistance R2 of the double-sided positive electrode sheet satisfy the following condition: R1>1 / 2R2. The porosity P1 of the single-sided positive electrode sheet and the porosity P2 of the double-sided positive electrode sheet satisfy the following condition: P2>P1.
2. The laminated cell according to claim 1, characterized in that, The unit area mm of the resistive layer 2 Within the range, the difference D between the maximum and minimum thickness of the resistive layer satisfies: D ≥ 0.5 μm; And / or, the adhesion force N1 between the resistive layer and the positive electrode active layer, and the adhesion force N2 between the outermost current collector and the positive electrode active layer satisfy the following condition: N1 > N2; And / or, the thickness H1 of the resistive layer and the thickness H2 of the positive electrode active layer satisfy the following condition: H2 / H1≥5.
3. The laminated cell according to claim 2, characterized in that, The N1 is 1.5 gf / mm-9 gf / mm; And / or, the N2 is 0.3 gf / mm-1 gf / mm; And / or, the H1 is 0.5μm-6μm; And / or, the H2 is 30μm-80μm.
4. The laminated cell according to claim 1, characterized in that, The median particle size Dv501 of the inorganic particles and the median particle size Dv502 of the active particles in the positive electrode active layer satisfy the following condition: Dv502 / Dv501≥10.
5. The laminated cell according to claim 4, characterized in that, The Dv501 is 0.01μm-1μm; And / or, the Dv502 is 10μm-20μm.
6. The laminated cell according to claim 4 or 5, characterized in that, The Dv501 is 0.01μm-0.1μm.
7. The laminated cell according to claim 1, characterized in that, The P1 is 15%-30%; And / or, the P2 is 20%-40%; And / or, the thickness of the outermost current collector is 12μm-25μm; And / or, the thickness of the current collector in the double-sided positive electrode is 6μm-10μm.
8. The laminated cell according to claim 1 or 2, characterized in that, The diaphragm disposed toward the resistive layer is a thermally composite diaphragm, and the adhesion force N3 between the thermally composite diaphragm and the resistive layer is 0.1gf / mm-2gf / mm.
9. The laminated cell according to claim 1 or 2, characterized in that, The negative electrode sheet includes a negative electrode current collector and a negative electrode active layer disposed on the surface of the negative electrode current collector. The negative electrode active layer includes a negative electrode active material, and the negative electrode active material includes silicon material. The resistivity R3 of the negative electrode sheet satisfies: 60Ω·cm ≥ R3 ≥ 2Ω·cm.
10. A lithium-ion secondary battery, characterized in that, Includes the laminated battery cell as described in any one of claims 1-9.
11. The lithium-ion secondary battery according to claim 10, characterized in that, The lithium-ion secondary battery also includes an electrolyte, wherein the content of carboxylic acid ester solvent in the electrolyte is A% and 50≥A≥10, and the content of binder in the resistive layer is B% and 20≥B≥5, wherein A and B satisfy: 10≥A / B≥0.5; In A% and B%, the % represents the percentage content by mass.
Citation Information
Patent Citations
Positive pole piece and preparation method thereof, secondary battery and electronic device
CN116111045A
Positive pole piece, electrode assembly, battery monomer, battery and electric equipment
CN118843951A