Humidifying stacked body and humidifier
By using a porous reinforcing material and a non-porous membrane laminate structure, the problems of miniaturization and insufficient moisture permeability of permeable membrane humidifiers are solved, achieving high efficiency and economy in humidifiers.
Patent Information
- Application Number
- CN202380045957.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-06-15
- Filing Date
- 2023-06-12
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-06-12
AI Technical Summary
Existing permeable membrane humidifiers are limited in terms of miniaturization and cost reduction, resulting in reduced permeability and increased permeability resistance.
By employing a porous reinforcing material and a non-porous membrane laminate structure, the high moisture permeability and high water retention of the non-porous membrane are utilized, avoiding the need for uneven shapes on the laminate and improving moisture permeability.
This technology has enabled the miniaturization of humidifiers and improved moisture permeability, while reducing moisture permeability resistance and enhancing both permeability and economy.
Smart Images

Figure CN119343233B_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to a humidifying laminate and a humidifier. Furthermore, this application claims priority to Japanese Patent Application No. 2022-096876, filed on June 15, 2022, the contents of which are incorporated herein by reference. Background Technology
[0002] As a humidifier, a permeable membrane humidifier is known to be able to perform both ventilation and humidification. However, compared with a natural evaporation humidifier that supplies water to the surface of the evaporation plate and humidifies the air, such a permeable membrane humidifier has a higher humidification performance, but it also has the problem of increased cost.
[0003] In order to reduce costs, research is being conducted on reducing and miniaturizing the components. For example, research is being conducted on a permeable membrane humidifier with an uneven shape on the membrane surface in order to increase the surface area of the permeable membrane, as in Patent Document 1.
[0004] Existing technical documents
[0005] Patent documents
[0006] Patent Document 1: Japanese Patent Application Publication No. 2001-174008 Summary of the Invention
[0007] The problem that the invention aims to solve
[0008] However, in the invention described in Patent Document 1, the thickness of the permeable membrane needs to be increased according to the size of the component used to give the permeable membrane an uneven shape, so there is a limit to the miniaturization of the humidifier, and consequently, the cost reduction is not sufficient.
[0009] Furthermore, the following problems exist: the membrane thickness needs to be increased according to the shape of the unevenness, which generates moisture permeability resistance and reduces the moisture permeability performance itself.
[0010] Therefore, the purpose of this disclosure is to provide a humidifying laminate that improves moisture permeability and enables miniaturization of the humidifier.
[0011] Solution for solving the problem
[0012] The inventors of this disclosure conducted in-depth research to achieve the aforementioned objectives and discovered that a humidifying laminate can improve moisture permeability and enable miniaturization of the humidifier by comprising: a porous reinforcing material; and a non-porous membrane laminated on at least one surface of the porous reinforcing material to function as a moisture-permeable membrane, wherein the moisture permeability of the laminate is greater than or equal to the moisture permeability of a single porous reinforcing material. This disclosure relates to substances made based on these insights.
[0013] That is, this disclosure provides a humidifying laminate, which is a laminate having: a porous reinforcing material; and a non-porous membrane laminated on at least one side of the porous reinforcing material to function as a moisture-permeable membrane, wherein the moisture permeability of the laminate is greater than or equal to the moisture permeability of the porous reinforcing material monomer.
[0014] By using a non-porous membrane with a porous reinforcing material monomer or higher, the humidifier laminate described above can achieve sufficient moisture permeability even without providing an uneven shape on the humidifier laminate, thus enabling miniaturization of the humidifier.
[0015] The aforementioned non-porous membrane preferably possesses the property that the thicker the membrane, the higher the moisture permeability. By using such a non-porous membrane, the aforementioned humidification laminate can more easily achieve moisture permeability.
[0016] The adsorption isotherm of the aforementioned porous reinforcing material is preferably any one of types I to VI shown in IUPAC.
[0017] Furthermore, the adsorption isotherm of the aforementioned porous reinforcing material is preferably Type III as shown in IUPAC.
[0018] The adsorption isotherm of the above-mentioned non-porous membrane is preferably any one of type I to VI shown in IUPAC.
[0019] Furthermore, the adsorption isotherm of the aforementioned non-porous membrane is preferably of type III as shown in IUPAC.
[0020] Furthermore, the moisture content of the non-porous membrane at 100% relative humidity is preferably 10 times or more than that of the porous reinforcing material. By making the moisture content of the non-porous membrane at 100% relative humidity 10 times or more than that of the porous reinforcing material, the humidification laminate can easily achieve moisture permeability.
[0021] Furthermore, the non-porous membrane is preferably disposed on the water side of the liquid relative to the porous reinforcing material, for absorbing water from the liquid and releasing it into the air.
[0022] The aforementioned cation portion preferably contains a group that includes ammonium ions or a group that can form ammonium ions. By containing a group that includes ammonium ions or a group that can form ammonium ions, the aforementioned non-porous membrane can exert a bactericidal effect, thereby inhibiting the adhesion / accumulation of bacteria and the like.
[0023] Preferably, the thermoplastic resin has a hydrophilic portion containing a structural unit as shown in formula (1). The non-porous membrane, through the hydrophilic portion having the structural unit, can form water-conducting pathways within the non-porous membrane, easily achieving moisture permeability.
[0024] [Chemical Formula 1]
[0025]
[0026] (R1 and R2 independently represent a hydrogen atom or a methyl group.)
[0027] Furthermore, preferably, the thermoplastic resin has a hydrophobic portion containing structural units represented by formula (2) and / or formula (3). Through the hydrophobic portion having the aforementioned structural units, the non-porous membrane can form water-conducting pathways, easily achieving moisture permeability.
[0028] [Chemical Formula 2]
[0029]
[0030] (R1 represents a hydrogen atom or a methyl group, and R3 represents a hydrogen atom or an alkyl group having 1 to 2 carbon atoms.)
[0031] [Chemical Formula 3]
[0032]
[0033] (R1 represents a hydrogen atom or a methyl group, and R4 represents a branched alkyl group with 3 or more carbon atoms.)
[0034] Furthermore, the aforementioned humidifying laminate is preferably coated with the non-porous membrane in such a way that it covers at least one surface of the porous reinforcing material.
[0035] Furthermore, the present invention provides a humidifier having a plurality of bag-shaped water-retaining containers formed by bonding the aforementioned humidifying laminate with a frame.
[0036] In addition, this disclosure provides an air conditioner equipped with the aforementioned humidifier.
[0037] In addition, this disclosure provides an air exchange device equipped with the above-mentioned humidifier.
[0038] In addition, this disclosure provides an air purifier equipped with the aforementioned humidifier.
[0039] Beneficial effects
[0040] The humidification laminate disclosed herein can improve moisture permeability and enable miniaturization of humidifiers. Therefore, the humidification laminate disclosed herein is preferably used in permeable membrane type humidifiers. Attached Figure Description
[0041] Figure 1 This is a cross-sectional schematic diagram illustrating one embodiment of the humidification laminate of this disclosure. Detailed Implementation
[0042] [Hydraulic laminate]
[0043] One embodiment of this disclosure provides a humidifying laminate comprising at least: a porous reinforcing material; and a non-porous membrane disposed on at least one side of the porous reinforcing material. The non-porous membrane may be disposed on one side or both sides of the reinforcing material. Furthermore, the humidifying laminate may also be a structure in which the non-porous membrane is sandwiched between two porous reinforcing materials. That is, the porous reinforcing material may also be disposed on both sides of the non-porous membrane. In this case, the two porous reinforcing materials may be the same porous reinforcing material, or they may be porous reinforcing materials with different materials, thicknesses, etc.
[0044] Figure 1 This is a cross-sectional schematic diagram showing one embodiment of the humidifying laminate of the present disclosure. The humidifying laminate 1 includes: a porous reinforcing material 11; and a non-porous membrane 12 disposed on one surface 11a of the porous reinforcing material 11.
[0045] <Porous membrane>
[0046] The aforementioned non-porous membrane functions as a moisture-permeable membrane. The aforementioned humidifying laminate, having the aforementioned non-porous membrane on at least one surface of the aforementioned porous reinforcing material, exhibits moisture permeability exceeding that of a single porous reinforcing material unit. This is presumably because the aforementioned non-porous membrane possesses high water retention. Such a non-porous membrane eliminates the need for uneven shapes to increase surface area, allowing for miniaturization of the humidifying laminate's structure. It should be noted that the aforementioned moisture permeability is based on the moisture permeability test method (cup method) of JIS Z0208-1976. Under conditions of 20°C, 30% relative humidity, and 2.4 m / s, and 20°C, 65% relative humidity, and 0.1 m / s, a moisture permeation cup containing 40 g of water is placed in a constant temperature and humidity bath. The reduction in the combined mass of the water and the moisture permeation cup after 1 hour is converted into a permeation rate per 1 m² of test piece. 2 • The mass over 24 hours is calculated as permeability.
[0047] Furthermore, the aforementioned non-porous membrane preferably exhibits the property that the thicker the membrane, the higher its moisture permeability. In conventional moisture-permeable membranes, moisture permeability decreases due to increased membrane thickness, while in contrast, it is presumed that the aforementioned non-porous membrane has high water retention capacity, thus not causing moisture permeability resistance, and can maintain high moisture permeability even when the membrane thickness increases.
[0048] The thickness of the aforementioned non-porous membrane is preferably 0.5 μm to 5 μm, more preferably 1 μm to 4 μm. If the thickness is 0.5 μm or more, the membrane formation properties become good, improving gas barrier properties and further enhancing moisture permeability. If the thickness is 5 μm or less, a thin film is easily formed, maintaining sufficient moisture permeability, and allowing for miniaturization of the humidifier, resulting in excellent economic efficiency.
[0049] The adsorption isotherm of the aforementioned non-porous membrane is preferably any one of types I to VI shown in IUPAC, and more preferably type III. By making the adsorption isotherm of the non-porous membrane any one of types I to VI shown in IUPAC, the water retention capacity of the non-porous membrane tends to increase, and therefore the aforementioned humidification laminate easily exhibits moisture permeability.
[0050] The moisture content of the non-porous membrane at a relative humidity of 100% is preferably 2% or more, more preferably 2.5% or more, and particularly preferably 3% or more. By ensuring that the moisture content of the non-porous membrane at a relative humidity of 100% is 2% or more, the humidification laminate readily exhibits moisture permeability.
[0051] Furthermore, compared to the aforementioned porous reinforcing material, the moisture content of the aforementioned non-porous membrane at a relative humidity of 100% is preferably 10 times or more, more preferably 15 times or more. By ensuring that the moisture content of the non-porous membrane at a relative humidity of 100% is 10 times or more than that of the porous reinforcing material, the aforementioned humidifying laminate readily exhibits moisture permeability.
[0052] Furthermore, the aforementioned non-porous membrane preferably comprises a thermoplastic resin, and the thermoplastic resin preferably has a cationic portion. Therefore, the aforementioned non-porous membrane preferably has the aforementioned cationic portion. By having the cationic portion, the aforementioned non-porous membrane can exert a repulsive force on scale components that are generally composed mainly of metal ions and have a positive charge, thereby inhibiting the adhesion / accumulation of scale components onto the non-porous membrane.
[0053] To enable the non-porous membrane to absorb moisture, it is preferable that the thermoplastic resin has a hydrophilic portion. Furthermore, to form water-conducting channels within the non-porous membrane, it is preferable that the thermoplastic resin has a hydrophobic portion. Therefore, the thermoplastic resin preferably has both a hydrophilic and a hydrophobic portion. It is presumed that by forming a structure in the non-porous membrane where the hydrophilic and hydrophobic portions are separated, the hydrophilic portion functions as a water-conducting channel, allowing more water vapor to pass through, thus resulting in superior moisture permeability.
[0054] Examples of the aforementioned thermoplastic resins include: acrylic resins, cellulose resins, polyester resins such as polybutylene terephthalate, polyether resins, polyurethane resins, polyvinyl chloride resins, polyethylene, polystyrene resins, polyamide resins, polyacetal resins, polycarbonate resins, polyphenylene sulfide resins, polyether ether ketone, polyimide resins, polytetrafluoroethylene resins, polycaprolactone, and polylactic acid.
[0055] The thermoplastic resins described above preferably have hydrophilic, hydrophobic and cationic portions, and are therefore preferably thermoplastic copolymers containing different monomer components.
[0056] The hydrophilic portion is preferably composed of monomer (a) units (hereinafter referred to as monomer (a)) containing hydrophilic functional groups in the side chains of the copolymer. Furthermore, the hydrophobic portion is preferably composed of monomer (b) units (hereinafter referred to as monomer (b)) containing hydrophobic functional groups in the side chains. Moreover, the hydrophilic and hydrophobic portions are preferably formed within the copolymer. In the non-porous membrane, the copolymer can maintain a core-shell structure with a hydrophobic portion formed on the inner side and a hydrophilic portion formed on the outer side. In this case, the hydrophilic and hydrophobic portions can be formed from the core and shell portions of two or more adjacent copolymers. Alternatively, the copolymer may have a core-shell structure before the formation of the non-porous membrane, but may not maintain this core-shell structure during the formation of the non-porous membrane.
[0057] The copolymer preferably contains structural units derived from the monomer (a) as the portion constituting the hydrophilic portion. Examples of the monomer (a) include: monomers containing glycidyl groups, monomers containing hydrolyzable silyl groups, monomers containing acetoacetyl groups, monomers containing hydroxyl groups, monomers containing carboxyl groups, methyl methacrylate, and monomers with cationic functional groups described later. Among these, monomers containing carboxyl groups, methyl methacrylate, and monomers with cationic functional groups described later are preferred. The monomer (a) can be used alone or in combination of two or more. It should be noted that in this specification, "(meth)acrylic acid" refers to at least one of "acrylic acid" and "methacrylic acid".
[0058] Examples of monomers containing glycidyl groups include glycidyl (meth)acrylate and (meth)allyl glycidyl ether.
[0059] Examples of the aforementioned monomers containing hydrolyzable silyl groups include: vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(β-methoxyethoxy)silane, and vinylmethyldimethoxysilane, which are vinyl-based monomers containing silyl groups; and γ-(meth)acryloyloxypropyltrimethoxysilane, γ-(meth)acryloyloxypropylmethyldimethoxysilane, γ-(meth)acryloyloxypropyltriethoxysilane, and γ-(meth)acryloyloxypropylmethyldiethoxysilane, which are (meth)acryloyloxy-based monomers containing silyl groups.
[0060] Examples of monomers containing the acetyl group include: allyl diacetate, acetyl acetoxyethyl (meth)acrylate, acetyl acetoxyethyl crotonate, acetyl acetoxypropyl (meth)acrylate, acetyl acetoxypropyl crotonate, and 2-cyanoacetyl acetoxyethyl (meth)acrylate.
[0061] Examples of hydroxyl-containing monomers include 2-hydroxyethyl methacrylate, hydroxypropyl methacrylate, and 4-hydroxybutyl methacrylate.
[0062] Examples of the aforementioned carboxyl-containing monomers include: crotonic acid, maleic acid, maleic anhydride and other acid anhydride monomers, fumaric acid, citraconic acid, penteneric acid, itaconic acid, acrylamide N-glycolic acid, cinnamic acid and (meth)acrylic acid, etc.
[0063] Furthermore, methyl methacrylate and / or methacrylic acid are particularly preferred as the monomer (a) mentioned above, that is, the hydrophilic part preferably contains the structural unit shown in the following formula (1).
[0064] [Chemical Formula 1]
[0065]
[0066] (R1 and R2 each independently represent a hydrogen atom or a methyl group.)
[0067] The content of the monomer (a) is preferably 20 to 70 mol% relative to all monomer components constituting the copolymer, more preferably 30 to 70 mol%, and even more preferably 40 to 60 mol%. By adjusting the content of the monomer (a) to this range, a hydrophilic portion can be formed in the non-porous membrane, thus easily forming a water-conducting channel and achieving better moisture permeability.
[0068] The copolymer described above preferably contains structural units derived from the monomer (b) as the portion constituting the hydrophobic portion. The monomer (b) is not particularly limited, but preferably contains a hydrocarbon group having two or more carbon atoms; more preferably, (meth)acrylates having two or more carbon atoms are examples. The monomer (b) can be used alone or in combination of two or more.
[0069] Examples of hydrocarbon groups having two or more carbon atoms include aliphatic hydrocarbon groups, alicyclic hydrocarbon groups, aromatic hydrocarbon groups, and groups formed by the bonding of two or more of them.
[0070] Examples of aliphatic hydrocarbon groups include alkyl, alkenyl, and alkynyl groups. Examples of alkyl groups include straight-chain or branched alkyl groups such as ethyl, propyl, isopropyl, butyl, isobutyl, hexyl, octyl, isooctyl, decyl, dodecyl, and stearyl. Examples of alkenyl groups include straight-chain or branched alkenyl groups such as vinyl, allyl, methanallyl, 1-propenyl, isopropenyl, 1-butenyl, 2-butenyl, 3-butenyl, 1-pentenyl, 2-pentenyl, 3-pentenyl, 4-pentenyl, and 5-hexenyl. Examples of alkynyl groups include straight-chain or branched alkynyl groups such as ethynyl and propynyl.
[0071] Examples of alicyclic hydrocarbon groups mentioned above include: cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cyclododecyl, and other cycloalkyl groups with 3 to 12 carbon atoms; cycloalkenyl groups with 3 to 12 carbon atoms such as cyclohexenyl; and bridged cyclic hydrocarbon groups with 4 to 15 carbon atoms such as bicycloheptyl and bicycloheptenyl.
[0072] Examples of aromatic hydrocarbon groups mentioned above include aryl groups with 6 to 14 carbon atoms, such as phenyl and naphthyl (especially aryl groups with 6 to 10 carbon atoms).
[0073] The hydrocarbon group having 2 or more carbon atoms is preferably an aliphatic hydrocarbon group or an aromatic hydrocarbon group, and more preferably a straight-chain or branched alkyl group or an aromatic hydrocarbon group.
[0074] Specifically, the monomer (b) described above is preferably a monomer capable of forming the structural unit described in formula (2) and / or formula (3) below. That is, the hydrophobic portion preferably includes the structural unit shown in formula (2) and / or formula (3) below.
[0075] [Chemical Formula 2]
[0076]
[0077] (R1 represents a hydrogen atom or a methyl group, and R3 represents a hydrogen atom or an alkyl group having 1 to 2 carbon atoms.)
[0078] [Chemical Formula 3]
[0079]
[0080] (R1 represents a hydrogen atom or a methyl group, and R4 represents a branched alkyl group with 3 or more carbon atoms.)
[0081] In the above formula (2), the bonding position of R3 is preferably any one of the hydrocarbons constituting the benzene ring. Examples of monomers that can form the structural unit shown in the above formula (2) include styrene, α-methylstyrene, p-methylstyrene, p-ethylstyrene, etc.
[0082] In the above formula (3), the number of carbon atoms in R4 is preferably 3 to 10. Examples of monomers that can form the structural unit shown in the above formula (3) include: isopropyl methacrylate, isobutyl methacrylate, tert-butyl methacrylate, 2-ethylhexyl methacrylate, etc.
[0083] The content of the monomer (b) is preferably 20 mol% to 70 mol% relative to the total monomer components constituting the copolymer, more preferably 30 mol% to 70 mol%, and even more preferably 40 mol% to 60 mol%. By adjusting the content of the monomer (b) to this range, water-conducting channels can be easily formed by forming hydrophobic portions in the non-porous membrane, resulting in better moisture permeability.
[0084] The aforementioned thermoplastic resin may have cationic portions in the hydrophilic portion and / or the hydrophobic portion, or it may have cationic portions elsewhere. Furthermore, the aforementioned thermoplastic resin preferably has cationic portions in the hydrophilic portion. The aforementioned cationic portions are preferably cationic functional groups or groups capable of generating cationic functional groups. The aforementioned groups capable of generating cationic functional groups refer to groups that do not have cationic functional groups in the thermoplastic resin stage, but generate cationic functional groups during the formation of the aforementioned non-porous membrane and during use. Furthermore, the aforementioned cationic functional groups may also be zwitterionic functional groups that contain both cations and anions. Therefore, the aforementioned thermoplastic resin may have anionic portions. Furthermore, the aforementioned thermoplastic resin preferably does not have anionic portions.
[0085] Examples of cationic functional groups include nitrogen-containing groups. Examples of nitrogen-containing groups include groups containing ammonium ions or groups capable of forming ammonium ions. Here, groups capable of forming ammonium ions refer to groups that do not ionize during the thermoplastic resin stage but form ionized bodies during the formation of the non-porous membrane and in use. Examples of groups containing ammonium ions and groups capable of generating ammonium ions include, for example, cyclic groups containing nitrogen atoms such as primary amino, secondary amino, tertiary amino, quaternary ammonium groups, imino (-NH- and =NH-), amidine, imine, hydrazine, amide, imide, and pyridyl groups. Furthermore, examples of zwitterionic functional groups include quaternary ammonium groups. Examples of quaternary ammonium groups include betaine groups and phosphocholine groups. Among the aforementioned thermoplastic resins, from the viewpoint of exerting antibacterial properties and preventing the spread of bacteria from the non-porous membrane, groups that can generate ammonium ions after the non-porous membrane is formed are preferred, and groups that can generate quaternary ammonium groups (quaternary ammonium groups, imide groups) are more preferred.
[0086] When the thermoplastic resin is the copolymer, the copolymer preferably contains structural units derived from monomers having cationic functional groups in their side chains. Examples of monomers having cationic functional groups include monomers having nitrogen-containing groups as functional groups. Examples of monomers having nitrogen-containing groups as functional groups include monomers containing amide groups, monomers containing amino groups, and monomers containing imide groups. Examples of monomers containing amide groups include: N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, N,N-dipropyl (meth)acrylamide, N,N-diisopropyl (meth)acrylamide, N,N-di(n-butyl)(meth)acrylamide, N,N-di(tert-butyl)(meth)acrylamide, and other N,N-dialkyl (meth)acrylamides; N-ethyl (meth)acrylamide, N-isopropyl (meth)acrylamide, N-butyl (meth)acrylamide, N-n-butyl (meth)acrylamide, and other N-alkyl (meth)acrylamides; N-vinylacetamide, N-(2-hydroxyethyl)(meth)acrylamide, etc. N-hydroxyalkyl (meth)acrylamides, such as amines, N-(2-hydroxypropyl)(meth)acrylamide, N-(1-hydroxypropyl)(meth)acrylamide, N-(3-hydroxypropyl)(meth)acrylamide, N-(2-hydroxybutyl)(meth)acrylamide, N-(3-hydroxybutyl)(meth)acrylamide, and N-(4-hydroxybutyl)(meth)acrylamide; N-alkoxyalkyl (meth)acrylamides, such as N-methoxymethyl (meth)acrylamide, N-methoxyethyl (meth)acrylamide, and N-butoxymethyl (meth)acrylamide; and N-alkoxyalkyl (meth)acrylamides, such as N,N-dimethylaminopropyl (meth)acrylamide and N-(meth)acryloylmorpholine. Furthermore, amino-containing monomers include substituted or unsubstituted amino-containing (meth)acrylates such as aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, and tert-butylaminoethyl (meth)acrylate. In addition, examples of monomers containing an imide group include: N-(meth)acryloyloxymethylenesuccinimide, N-(meth)acryloyl-6-oxyhexamethylenesuccinimide, N-(meth)acryloyl-8-oxyhexamethylenesuccinimide, N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, N-phenylmaleimide, N-methylitconimide, N-ethylitconimide, N-butylitconimide, N-octylitconimide, N-2-ethylhexylitconimide, N-cyclohexylitconimide, and N-laurylitconimide. These monomers with cationic functional groups can be used alone or in combination of two or more.
[0087] The content of the monomers having cationic functional groups is preferably 0.5 mol% to 10 mol% relative to the total monomer components constituting the copolymer, more preferably 1 mol% to 7 mol%, and even more preferably 2 mol% to 5 mol%. By adjusting the content of the monomers having cationic functional groups to this range, a repulsive force with scale components can be exerted, and the adhesion / accumulation of scale components to the non-porous membrane can be inhibited.
[0088] Furthermore, the copolymers described above may also contain structural portions derived from the crosslinking agent. As the crosslinking agent, there are no particular limitations as long as it is a compound capable of crosslinking with the side chains of the monomers constituting the copolymer. For example, difunctional compounds having two reactive functional groups are preferred. From the viewpoint of increasing the density of crosslinking within the polymer and adjusting mechanical properties, trifunctional or higher crosslinking agents can be used. Examples of such crosslinking agents include difunctional or higher epoxy-containing compounds and difunctional or higher isocyanate-containing compounds. In the copolymers described above, compounds containing difunctional or higher epoxy groups are particularly preferred from the viewpoint that they can generate quaternary ammonium ions after crosslinking reaction with the functional groups formed on the side chains.
[0089] Examples of the aforementioned epoxy-containing compounds include: bisphenol A and epichlorohydrin type epoxy compounds, polyethylene glycol diglycidyl ether, glycerol diglycidyl ether, glycerol triglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, diglycidyl aniline, N,N,N',N'-tetraglycidyl-m-xylenediamine (e.g., trade name "TETRAD-X", manufactured by Mitsubishi Gas Chemical), 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane (e.g., trade name "TETRAD-C", manufactured by Mitsubishi Gas Chemical), etc.
[0090] The amount of the crosslinking agent used is preferably 1 to 60 moles relative to the total amount of reactive side chains of the copolymer (100 moles), more preferably 2 to 30 moles, and even more preferably 4 to 15 moles. By adjusting the amount of the crosslinking agent used to this range, water-conducting channels can be easily formed in the non-porous membrane, resulting in excellent moisture permeability.
[0091] The weight-average molecular weight of the aforementioned thermoplastic resin is not particularly limited, but is preferably 20,000 to 2,000,000, more preferably 30,000 to 1,500,000, further preferably 50,000 to 1,000,000, and particularly preferably 70,000 to 500,000. The aforementioned weight-average molecular weight is a value calculated based on polystyrene, determined by gel permeation chromatography (GPC).
[0092] The aforementioned non-porous membrane may also contain other components besides the aforementioned thermoplastic resin, to a extent that it does not impair the effect of the humidifying laminate of this disclosure. Examples of such other components include, for instance, preservatives, anti-blocking agents, release agents, and leveling agents. The content of these other components relative to the total amount (100 parts by weight) of the copolymer is preferably 0.1 to 10 parts by weight, more preferably 0.15 to 3 parts by weight, and particularly preferably 0.2 to 2 parts by weight.
[0093] The non-porous membrane, due to the presence of hydrophilic and hydrophobic portions in the copolymer, preferably has a structure in which the hydrophilic and hydrophobic portions are separated on its surface. The maximum diameter of the hydrophilic portion on the surface of the non-porous membrane is preferably 50 nm or less, more preferably 20 nm or less. If the maximum diameter of the hydrophilic portion is 50 nm or less, substances larger than 50 nm are less likely to permeate through the non-porous membrane, and the non-porous membrane can be used as a barrier film to prevent substances larger than 50 nm (e.g., viruses) from permeating. The diameter of the hydrophilic portion is evaluated by the following method: using the adhesion measurement mode of a scanning probe microscope (SPM), the regions with high adsorption (hydrophilic portion) and low adsorption (hydrophobic portion) are numerically represented by adhesion. Image analysis software is used for processing, and the diameter of the hydrophilic portion can be calculated in the form of an equivalent circle diameter. Furthermore, the maximum diameter is the largest diameter among the diameters of the hydrophilic portion (equivalent circle diameter) calculated as described above.
[0094] It should be noted that, in this disclosure, structures with a maximum diameter of 50 nm or less in the hydrophilic portion do not allow components larger than 50 nm to pass through, and therefore only water vapor passes through. Therefore, the pores in the non-porous membrane described in this disclosure do not include pores smaller than 50 nm formed in the hydrophilic portion. Furthermore, when the maximum diameter of the hydrophilic portion exceeds 50 nm, there is a possibility that components other than water vapor can pass through. Therefore, a membrane having multiple structures with a maximum diameter of more than 50 nm in the hydrophilic portion is defined as a porous membrane.
[0095] The aforementioned non-porous membrane is preferably formed by coating. Because it is formed by coating, a non-porous membrane can be easily manufactured, which easily inhibits the spread of scale components, bacteria, etc.
[0096] <Porous Reinforcing Materials>
[0097] Preferably, the porous reinforcing material described above serves as a support for the non-porous membrane and exhibits excellent moisture permeability.
[0098] The material used to form the porous reinforcing material can be either a hydrophilic or a hydrophobic material, but a hydrophobic material is preferred. If the hydrophobic material is used, when the composition for forming a non-porous membrane is coated, the composition does not permeate into the porous reinforcing material. Therefore, in the porous reinforcing material, there is no need for a guiding substrate to prevent the composition from flowing down from the side opposite to the coating surface.
[0099] Materials used to form the porous reinforcing material include, for example, organic materials such as polyolefin resins, cellulose resins, polycarbonate resins, polyamide resins, polyimide resins, polyamide-imide resins, and fluorine resins, as well as inorganic materials such as metals, glass, and ceramics. Among these, since the non-porous membrane can be formed on the porous reinforcing material at a relatively low temperature, and from the viewpoint of excellent moisture permeability and water resistance, organic materials are preferred, and polyolefin resins are particularly preferred. The materials may also be fibrous, such as metal fibers or inorganic fibers. The materials used to form the porous reinforcing material may be only one type or two or more types.
[0100] Examples of porous reinforcing materials include: resin porous membranes, inorganic porous membranes, metal porous membranes, and fibrous substrates.
[0101] The aforementioned polyolefin resins are polymers (including olefin-based elastomers) that are composed of olefins as essential monomer components; that is, they are polymers whose molecules (in one molecule) contain at least structural units derived from olefins. There are no particular limitations on the olefins mentioned above; examples include α-olefins such as ethylene, propylene, 1-butene, and 4-methyl-1-pentene.
[0102] Examples of the aforementioned polyolefin resins include polymers that use ethylene as an essential monomer component (polyethylene resins), polymers that use propylene as an essential monomer component (polypropylene resins), ionomers, and amorphous cyclic olefin polymers.
[0103] The porosity of the aforementioned porous reinforcing material is not particularly limited, but is preferably 30% to 90% by volume, more preferably 40% to 70% by volume. If the porosity is 30% by volume or more, the moisture permeability becomes better. If the porosity is 90% by volume or less, the support performance of the non-porous membrane becomes better.
[0104] The thickness of the porous reinforcing material is not particularly limited, but from the viewpoint of adequately supporting the non-porous membrane, it is preferably 5 μm or more, and more preferably 10 μm or more. Furthermore, considering excellent moisture permeability and economy, the thickness of the porous reinforcing material is preferably 50 μm or less, and more preferably 30 μm or less.
[0105] From the viewpoint that the aforementioned non-porous membrane can be easily formed, the surface of the aforementioned porous reinforcing material possessing the aforementioned non-porous membrane side (e.g., Figure 1 Surface 11a) shown in the diagram preferably undergoes a hydrophilic treatment. In particular, when a hydrophobic material is used as the material forming the porous reinforcing material, this hydrophilic treatment is preferred. Examples of such hydrophilic treatments include corona discharge treatment and plasma treatment. Through these hydrophilic treatments, carboxyl, hydroxyl, or carbonyl groups can be generated on the surface of the porous reinforcing material, making it easier for the composition used to form the non-porous membrane to wet and spread on the surface of the porous reinforcing material, thus easily forming the non-porous membrane. Furthermore, this improves the adhesion between the porous reinforcing material and the non-porous membrane. Moreover, when the porous reinforcing material formed from the hydrophobic substrate is stored as a wound, the wound has one side in contact with the other side; however, since the hydrophilic side is in contact with the hydrophobic side, adhesion can be prevented.
[0106] The surface tension of the side of the porous reinforcing material on which the non-porous membrane is formed is preferably 35 dyn / cm to 55 dyn / cm, more preferably 37 dyn / cm to 50 dyn / cm. If the surface tension is 35 dyn / cm or higher, the composition for forming the non-porous membrane is easily applied, and the non-porous membrane is easily formed. If the surface tension is 55 dyn / cm or lower, the composition for forming the non-porous membrane does not excessively wet and spread, and the non-porous membrane is easily formed on the surface of the porous reinforcing material. It should be noted that when the surface of the porous reinforcing material has undergone hydrophilication treatment, the side on which the non-porous membrane is formed is the side that has undergone the hydrophilication treatment.
[0107] The surface tension of the interior of the porous reinforcing material (i.e., the interior of the region where the non-porous membrane is not formed) is preferably less than 35 dyn / cm, more preferably less than 33 dyn / cm. If the surface tension is less than 35 dyn / cm, the composition used to form the non-porous membrane can be suppressed from penetrating into the interior of the porous reinforcing material, and the non-porous membrane can be easily formed on the surface of the porous reinforcing material. It should be noted that when the surface of the porous reinforcing material has undergone hydrophilic treatment, the interior of the porous reinforcing material refers to the interior of the region where the hydrophilic treatment has not been performed. Furthermore, the surface tension of the interior can be obtained by measuring a cross-section obtained by cutting the porous reinforcing material.
[0108] The moisture content of the porous reinforcing material at 100% relative humidity is preferably 0.01% to 0.5%, more preferably 0.05% to 0.4%, and particularly preferably 0.1% to 0.3%. From the viewpoint that the moisture content of the non-porous membrane is more than 10 times that of the porous reinforcing material, the moisture content of the porous reinforcing material at 100% relative humidity is preferably within the above range.
[0109] The adsorption isotherm of the aforementioned porous reinforcing material is preferably any one of types I to VI shown in IUPAC, and more preferably type III. By making the adsorption isotherm of the porous reinforcing material any one of types I to VI shown in IUPAC, the water retention capacity of the non-porous membrane tends to increase, thus making it easier to achieve moisture permeability.
[0110] The aforementioned porous reinforcing material, based on the JIS Z0208-1976 moisture permeability test method (cup method), preferably has a moisture permeability of 1350 g / (m³) under the conditions of 20°C, 65% relative humidity, and 0.1 m / s wind speed. 2 ·24h or less, more preferably 1000g / (m 2 ·24h and below.
[0111] Furthermore, the moisture permeability of the aforementioned porous reinforcing material, based on the moisture permeability test method (cup method) of JIS Z0208-1976, under the conditions of temperature 20℃, relative humidity 30%, and wind speed 2.4m / s, is preferably 18000 g / (m³). 2 ·24h or less, more preferably 15000g / (m 2 ·24h or less, further preferably 10000g / (m 2 ·24h and below.
[0112] The aforementioned humidification laminate, based on the JIS Z0208-1976 test method (cup method) for humidity permeability, preferably exhibits a humidity permeability exceeding 1350 g / (m³) under the conditions of 20°C, 65% relative humidity, and 0.1 m / s wind speed. 2 ·24h), more preferably 1370g / (m 2 • 24h or more. The above-mentioned humidification laminate has excellent moisture permeability, therefore, a moisture permeability exceeding 1350 g / (m³) can be used. 2 The structure of ·24h).
[0113] Furthermore, the aforementioned humidification laminate, based on the JIS Z0208-1976 test method (cup method) for humidity permeability, preferably exhibits a humidity permeability exceeding 18000 g / (m³) under conditions of 20°C, 30% relative humidity, and 2.4 m / s wind speed. 2 ·24h), more preferably 19000g / (m 2• 24h or more, more preferably 20000g / (m 2 • 24h or more. The above-mentioned humidification laminate has excellent moisture permeability, therefore, a moisture permeability exceeding 18000 g / (m³) can be used. 2 The structure of ·24h).
[0114] Furthermore, compared to the aforementioned porous reinforcing material monomer, the difference in humidity permeability between the aforementioned humidifying laminate and the aforementioned porous reinforcing material monomer, based on the humidity permeability test method (cup method) of JIS Z0208-1976, under the conditions of temperature 20°C, relative humidity 65%, and wind speed 0.1 m / s, is preferably 0 g / (m³). 2 • 24h or more, more preferably 10g / (m 2 • 24h or more, especially preferably 30g / (m 2 ·24h) or more.
[0115] Furthermore, compared to the aforementioned porous reinforcing material monomer, the difference in humidity permeability between the aforementioned humidifying laminate and the aforementioned porous reinforcing material monomer, based on the humidity permeability test method (cup method) of JIS Z0208-1976, under the conditions of temperature 20°C, relative humidity 30%, and wind speed 02.4 m / s, is preferably 0 g / (m³). 2 • 24h or more, more preferably 1000g / (m 2 • 24h or more, especially preferably 2000g / (m 2 ·24h) or more.
[0116] The thickness of the humidifying laminate is not particularly limited, but is preferably 5.5 μm to 55 μm, more preferably 7 μm to 30 μm. By making the thickness of the humidifying laminate 5.5 μm or more, it is easy to achieve moisture permeability, and by making the thickness of the humidifying laminate 55 μm or less, it is economical and easy to miniaturize when used in a humidifier.
[0117] [Manufacturing method of laminated body for humidification]
[0118] The humidifying laminate of this disclosure can be manufactured by forming the non-porous membrane on at least one surface of the porous reinforcing material using known or conventional methods. For example, the non-porous membrane can be formed directly on one surface of the porous reinforcing material, or the non-porous membrane can be temporarily formed on another support and then transferred (adhered) to one surface of the porous reinforcing material, thereby forming the non-porous membrane on the porous reinforcing material. From the viewpoint of excellent adhesion between the non-porous membrane and the porous reinforcing material, the former method is preferred.
[0119] Alternatively, a hydrophilic treatment can be applied to the surface of the non-porous membrane on the side where the porous reinforcing material is disposed. Examples of such hydrophilic treatments include those described above.
[0120] The aforementioned non-porous membrane can be formed by coating (applying) a composition for forming the aforementioned non-porous membrane onto the aforementioned porous reinforcing material or other support, and then desolventizing the resulting coating by heating or the like.
[0121] The aforementioned porous reinforcing material suppresses adhesion by performing the aforementioned hydrophilic treatment, and therefore can be manufactured by a roll-to-roll method in which a non-porous film is formed on the aforementioned porous reinforcing material that has been pre-made into a wound body, and then the wound body is made again.
[0122] The above composition can be prepared using known or conventional methods. For example, it can be prepared by dissolving or dispersing the copolymer in a solvent and adding additives such as preservatives as needed. Water and / or water-soluble solvents are preferred as the solvent. It is conceivable that when water or a water-soluble solvent is used, the copolymer is dispersed in the composition in a core-shell shape with a hydrophobic inner portion and a hydrophilic outer portion. By using such a composition, the hydrophilic and hydrophobic portions separate when the coating film dries, forming a non-porous film with water-conducting channels. Furthermore, it is conceivable that the hydrophobic portions become firmly bonded to each other, resulting in better water resistance.
[0123] Examples of water-soluble solvents mentioned above include: aliphatic water-soluble alcohols such as methanol, ethanol, n-propanol, and isopropanol; and glycol ethers such as ethylene glycol monomethyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, and propylene glycol monoethyl ether. Only one of these water-soluble solvents may be used, or two or more may be used.
[0124] The proportion (concentration) of the copolymer in the above composition in which the copolymer is dissolved or dispersed is not particularly limited, but is preferably 0.5 to 5% by mass, more preferably 1 to 4% by mass, and even more preferably 1.5 to 3% by mass. If the concentration is 5% by mass or less, the coating thickness becomes thicker, and thus the thickness of the dried non-porous membrane becomes more uniform. As a result, a non-porous membrane with excellent gas barrier properties and further thinning can be formed, and as a result, the moisture permeability is further improved. In addition, if the concentration is within the above range, the coatability is excellent, and a non-porous membrane with excellent moisture permeability and gas barrier properties is easily formed.
[0125] It should be noted that the coating of the above composition can also be performed using known coating methods. For example, gravure roller coaters, reverse roller coaters, kiss roll coaters, dip roller coaters, doctor blade coaters, spray coaters, comma coaters, direct coaters, and other coating machines can be used. Through such coating, a non-porous film can be easily formed.
[0126] The heating temperature for desolventizing the above-mentioned coating is preferably 35°C to 90°C, more preferably 40°C to 85°C, and even more preferably 45°C to 80°C. The heating time can be appropriately set, for example, 5 seconds to 20 minutes, preferably 5 seconds to 10 minutes, and more preferably 10 seconds to 5 minutes. The above-mentioned composition can be used to form a non-porous membrane at low temperatures below 90°C (especially below 80°C), thus facilitating membrane formation. Furthermore, a polyolefin resin with excellent moisture permeability can be used as a porous reinforcing material.
[0127] The humidifying laminate formed on at least one surface of the porous reinforcing material using the above method exhibits excellent moisture permeability and allows for miniaturization of the humidifier's shape. It should be noted that the humidifying laminate refers to a laminate that allows water vapor to move through it. Furthermore, the humidifying laminate has a structure where the hydrophilic and hydrophobic portions are separated, thus it can also be used as a moisture-permeable barrier membrane. When the diameter of the hydrophilic portion is small, as a moisture-permeable barrier membrane, small hydrophilic substances (e.g., water vapor) are allowed to pass through the hydrophilic portion, while larger substances (e.g., viruses) are prevented from passing through, thereby separating the two.
[0128] Moreover, the above-mentioned humidification laminate can be made into a thin film compared with the conventional moisture-permeable membrane, so when used in humidifiers, the shape itself can be miniaturized, and the economy is also excellent.
[0129] [Bag-shaped water-retaining container]
[0130] By covering the outside of the frame with the aforementioned humidifying laminate, a bag-shaped water-retaining container can be made.
[0131] The frame is preferably made of a rigid material, such as resin, metal / alloy materials, etc. Furthermore, the frame can be a plate-shaped or bag-shaped frame manufactured by extrusion molding, a plate-shaped frame manufactured by injection molding, or a bag-shaped structure created by bonding two or more plate-shaped frames together. Additionally, holes can be provided after the bag-shaped frame is manufactured, or frames with pre-formed holes can be manufactured.
[0132] Preferably, a portion or all of the contact area between the laminated body and the frame is glued. The method of gluing to the frame is not particularly limited; it can be done using known or conventional adhesives, or by welding methods such as ultrasonic welding, high-frequency welding, or thermal welding.
[0133] The above method can be used to make a bag-shaped water-retaining container. The bag-shaped water-retaining container has a laminated body arranged on the outside of the frame structure. The water in the liquid that is introduced into the bag-shaped water-retaining container is absorbed by the laminated body as water vapor, diffuses within the laminated body, and can be released from the entire laminated body.
[0134] Furthermore, multiple of the aforementioned bag-shaped water-retaining containers can be incorporated to create a humidifier. Such a humidifier offers improved humidification performance compared to previous models, thus achieving the same performance while miniaturizing the humidifier, and is also cost-effective.
[0135] Therefore, the humidifier described above improves moisture permeability by having the aforementioned humidification laminate, thereby enabling miniaturization and making it suitable for use in air conditioners, ventilation devices, air purifiers, and other applications.
[0136] The various solutions disclosed in this specification can also be combined with any other features disclosed in this specification. The various configurations and combinations of configurations in each embodiment are merely examples, and appropriate additions, omissions, substitutions, and other modifications can be made to the configuration without departing from the spirit of this disclosure. Furthermore, the inventions of this disclosure are not limited to the embodiments or the following examples, but only to the patent claims.
[0137] Example
[0138] The following describes one embodiment of the present disclosure in more detail based on an example.
[0139] Example 1
[0140] A coating solution with a resin concentration of 10% by mass was prepared by diluting 100 parts by mass of a thermoplastic resin solution with 22 parts by mass of ethanol and 143 parts by mass of distilled water. The thermoplastic resin solution contained: 47 moles of isobutyl acrylate and 1 mole of styrene as structural units forming the hydrophobic portion of the polymer; 21 moles of acrylic acid and 28 moles of methyl acrylate as structural units forming the hydrophilic portion; 3 moles of imide as structural units forming the cationic portion; and 2 moles of epoxy compound as a crosslinking agent. On the other hand, a surface of a porous polypropylene resin substrate (thickness: 20 μm, porosity: 48 vol%) was corona treated to form a hydrophilic surface with a surface tension of 39 dyn. Then, using a wire rod, the above composition was coated onto the hydrophilic surface of the porous reinforcing material and heated at 70°C for 1 minute to form a non-porous film (thickness: 1 μm). Thus, the humidifying laminate of Example 1 was produced.
[0141] Examples 2-3
[0142] By varying the thickness of the non-porous membrane, the humidifying laminates of Examples 2 and 3 were prepared in the same manner as in Example 1.
[0143] [evaluate]
[0144] The humidifying laminates obtained in the Examples and Comparative Examples were evaluated as described below. The evaluation results are recorded in the table. In addition, a porous substrate made of polypropylene resin without a non-porous membrane was evaluated as Comparative Example 1.
[0145] (1) Moisture permeability
[0146] For the humidifying laminates obtained in the examples and comparative examples, the permeability was determined based on the permeability test method (cup method) of JIS Z0208-1976. Specifically, after the humidifying laminates obtained in the examples and comparative examples were placed in the test environment for more than 2 hours, they were used as permeable sheets to cover the permeable cups and tested for airtightness. Then, a permeable cup containing 40g of water was placed in a constant temperature and humidity chamber at a temperature of 20°C, a relative humidity of 30%, and a wind speed of 2.4m / s. The reduction in the total mass of the water and the permeable cup after 1 hour was converted into a permeability of 1m² of test sheet. 2 • The mass over 24 hours was calculated as the permeability. In addition, permeability was also measured under the same conditions: temperature 20°C, relative humidity 65%, and virtually no wind (wind speed 0.1 m / s).
[0147] (2) Moisture content
[0148] For each humidification laminate obtained in the examples and comparative examples, the moisture content was determined by water vapor adsorption method.
[0149] [Table 1]
[0150] (Table 1)
[0151]
[0152] As shown in the results of Examples 1-3, it can be confirmed that the humidification laminate of this disclosure, having a non-porous membrane, has a moisture permeability exceeding that of the porous reinforcing material monomer shown in Comparative Example 1. Furthermore, it was confirmed that the thicker the non-porous membrane, the higher the moisture permeability.
[0153] The following describes variations of the invention disclosed herein.
[0154] [Postscript 1]
[0155] A humidifying laminate comprises: a porous reinforcing material; and a non-porous membrane laminated on at least one side of the porous reinforcing material to function as a moisture-permeable membrane, wherein the moisture permeability of the laminate is greater than or equal to the moisture permeability of a single porous reinforcing material.
[0156] [Postscript 2]
[0157] According to the humidification laminate described in Appendix 1, the non-porous membrane has the property that the thicker the membrane, the higher the humidity permeability.
[0158] [Postscript 3]
[0159] According to Appendix 1 or 2, the humidification laminate wherein the adsorption isotherm of the porous reinforcing material is any one of type I to VI shown in IUPAC.
[0160] [Postscript 4]
[0161] The humidifying laminate according to any one of Appendices 1 to 3, wherein the adsorption isotherm of the porous reinforcing material is of type III as shown in IUPAC.
[0162] [Postscript 5]
[0163] The humidification laminate according to any one of Appendices 1 to 4, wherein the adsorption isotherm of the non-porous membrane is any one of types I to VI shown in IUPAC.
[0164] [Postscript 6]
[0165] The humidification laminate according to any one of Appendices 1 to 5, wherein the adsorption isotherm of the non-porous membrane is of type III as shown in IUPAC.
[0166] [Postscript 7]
[0167] According to any one of Appendices 1 to 6, the moisture content of the non-porous membrane at 100% relative humidity is more than 15 times that of the porous reinforcing material at 100% relative humidity.
[0168] [Postscript 8]
[0169] The humidifying laminate according to any one of Appendices 1 to 7, wherein the non-porous membrane is disposed on the water side of the liquid relative to the porous reinforcing material for absorbing water from the liquid and releasing it into the air.
[0170] [Postscript 9]
[0171] The humidifying laminate according to any one of Appendices 1 to 8, wherein the non-porous membrane comprises a thermoplastic resin having a cationic portion, the cationic portion containing a group comprising ammonium ions or a group capable of forming ammonium ions.
[0172] [Postscript 10]
[0173] The humidifying laminate according to any one of Appendices 1 to 9, wherein the thermoplastic resin has a hydrophilic portion containing a structural unit as shown in formula (1).
[0174] [Chemical Formula 1]
[0175]
[0176] R1 and R2 each independently represent a hydrogen atom or a methyl group.
[0177] [Postscript 11]
[0178] The humidifying laminate according to any one of Appendices 1 to 10, wherein the thermoplastic resin has a hydrophobic portion containing structural units represented by formula (2) and / or formula (3).
[0179] [Chemical Formula 2]
[0180]
[0181] R1 represents a hydrogen atom or a methyl group, and R3 represents an alkyl group with 1 to 2 carbon atoms.
[0182] [Chemical Formula 3]
[0183]
[0184] R1 represents a hydrogen atom or a methyl group, and R4 represents a branched alkyl group with 3 or more carbon atoms.
[0185] [Postscript 12]
[0186] The humidifying laminate according to any one of Appendices 1 to 11, wherein the non-porous membrane is coated in such a way that it covers at least one surface of the porous reinforcing material.
[0187] [Postscript 13]
[0188] A humidifier comprising a plurality of bag-shaped water-retaining containers formed by bonding a humidifying laminate according to any one of Appendices 1 to 12 to a frame.
[0189] [Postscript 14]
[0190] An air conditioner equipped with a humidifier as described in Appendix 13.
[0191] [Postscript 15]
[0192] A ventilation device equipped with a humidifier as described in Appendix 13.
[0193] [Postscript 16]
[0194] An air purifier equipped with a humidifier as described in Appendix 13.
[0195] Explanation of reference numerals in the attached figures
[0196] 1: Layered structure;
[0197] 11: Porous reinforcing materials;
[0198] 11a: One facet of a porous reinforcing material;
[0199] 12: Non-porous membrane.
Claims
1. A humidifying laminate comprising: a porous reinforcing material; and a non-porous membrane laminated on at least one side of the porous reinforcing material to function as a moisture-permeable membrane, wherein... The moisture permeability of the laminate is higher than that of the porous reinforcing material monomer. The non-porous membrane comprises a thermoplastic resin. The thickness of the non-porous membrane is 0.5µm to 5µm. The non-porous membrane possesses the property that the thicker the membrane, the higher its moisture permeability. The thermoplastic resin has a hydrophilic portion containing one or more structural units selected from monomers containing glycidyl groups, monomers containing hydrolyzable silyl groups, monomers containing acetyl groups, and structural units represented by the following formula (1). In the formula, R1 and R2 independently represent hydrogen atoms or methyl groups.
2. The humidifying laminate according to claim 1, wherein, The adsorption isotherm of the porous reinforcing material is any one of type I to VI shown in IUPAC.
3. The humidifying laminate according to claim 1 or 2, wherein, The adsorption isotherm of the porous reinforcing material is of type III as shown in IUPAC.
4. The humidifying laminate according to claim 1 or 2, wherein, The adsorption isotherm of the non-porous membrane is any one of type I to VI shown in IUPAC.
5. The humidifying laminate according to claim 1 or 2, wherein, The adsorption isotherm of the non-porous membrane is of type III as shown in IUPAC.
6. The humidifying laminate according to claim 1 or 2, wherein, The moisture content of the non-porous membrane at 100% relative humidity is more than 10 times that of the porous reinforcing material at 100% relative humidity.
7. The humidifying laminate according to claim 1 or 2, wherein, The non-porous membrane is disposed on the water side of the liquid relative to the porous reinforcing material, for absorbing water from the liquid and releasing it into the air.
8. The humidifying laminate according to claim 1 or 2, wherein, The non-porous membrane comprises a thermoplastic resin having a cationic portion, wherein the cationic portion contains a group comprising ammonium ions or a group capable of forming ammonium ions.
9. The humidifying laminate according to claim 1 or 2, wherein, The thermoplastic resin has a hydrophobic portion, which contains structural units shown in formula (2) and / or formula (3) below. In formula (2), R1 represents a hydrogen atom or a methyl group, and R3 represents an alkyl group with 1 to 2 carbon atoms. In formula (3), R1 represents a hydrogen atom or a methyl group, and R4 represents a branched alkyl group with 3 or more carbon atoms.
10. The humidifying laminate according to claim 1 or 2, wherein, The non-porous membrane is coated in such a way that it covers at least one surface of the porous reinforcing material.
11. A humidifier comprising a plurality of bag-shaped water-retaining containers formed by bonding a humidifying laminate according to claim 1 or 2 to a frame.
12. An air conditioner equipped with a humidifier according to claim 11.
13. A ventilation device equipped with a humidifier according to claim 11.
14. An air purifier equipped with a humidifier according to claim 11.
Citation Information
Patent Citations
Humidifying sheet
JP2001174008A
Quick lime manufacturing system
JP2022096876A
Gas-liquid separating element, gas-liquid separator, and gas-liquid separating unit
JP2003097831A
Laminate
WO2022070948A1