A method for repairing lithium iron phosphate

By calcining, granulating, and high-temperature sintering the recovered lithium iron phosphate powder, a stable secondary structure is formed, which solves the problems of incomplete removal of organic matter and insufficient mixing reaction in existing lithium iron phosphate recycling methods. This improves material performance and lithium replenishment efficiency, and promotes the sustainable development of the new energy industry.

CN119349533BActive Publication Date: 2026-11-24SHAANXI CHUANGPU NEW ENERGY TECH CO LTD +3
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411470995.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-10-21
Publication Date
2026-11-24
Estimated Expiration
2044-10-21

AI Technical Summary

Technical Problem

Existing lithium iron phosphate recycling methods suffer from problems such as incomplete removal of organic matter, poor material performance, and insufficient mixing reaction, resulting in poor remediation effects.

Method used

The recovered lithium iron phosphate powder is calcined to remove impurities, mixed with iron source, carbon source and additives, granulated, and then mixed with lithium source and sintered at high temperature to form a stable secondary structure.

Benefits of technology

It improves the performance of lithium iron phosphate materials, increases the utilization rate of valuable metals, reduces environmental pollution, promotes the sustainable development of the new energy industry, and improves lithium replenishment efficiency through unique additives and structural design.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005094684590000071
    Figure BDA0005094684590000071
  • Figure BDA0005094684590000072
    Figure BDA0005094684590000072
Patent Text Reader

Abstract

This invention provides a method for repairing lithium iron phosphate (LFP) materials. The method includes the following steps: S1: calcining the recovered LFP powder to remove impurities; S2: mixing the calcined LFP powder with a mixture containing an iron source, a carbon source, and additives to obtain mixture I; S3: granulating mixture I to obtain granulated particles; S4: mixing the granulated particles with a mixture containing a lithium source and drying to obtain a repair precursor; S5: sintering the repair precursor at high temperature to complete the repair of LFP. By performing calcination to remove impurities, re-granulation, and high-temperature sintering on the recovered LFP material, this invention improves the material's performance, increases the utilization rate of valuable metals, reduces environmental pollution caused by the disposal of waste batteries, and contributes to the sustainable development of the new energy industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of recycling of waste lithium-ion batteries and the recycling of electrode materials, specifically to a method for repairing lithium iron phosphate. Background Technology

[0002] Lithium iron phosphate (LFP) is a relatively mature lithium-ion battery cathode material developed over many years, and it has become the cathode material with the largest production and usage volume. Lithium-ion batteries made from LFP have high specific capacity, good cycle stability, and high-temperature resistance, and are widely used in medical devices, electronic equipment, mining machinery, aerospace, marine exploration, and new energy vehicles. Since China began large-scale research and development of LFP cathode materials, especially with the development and commercialization of new energy vehicles, LFP's production capacity and application scope have surpassed other cathode materials such as lithium cobalt oxide, nickel-cobalt-manganese ternary materials, and lithium manganese oxide, becoming one of the most important lithium-ion cathode materials. In this process, a large number of waste lithium-ion batteries and substandard LFP cathode materials are generated annually. Furthermore, due to the increasing demand for lithium resources in the past two years, the prices of raw materials for manufacturing lithium battery cathode materials, such as lithium carbonate and lithium hydroxide, have risen sharply. How to efficiently recycle lithium battery cathode materials has become a hot research topic in the lithium battery industry and will also become one of the important core competencies for lithium battery companies in the future.

[0003] Chinese patent application (publication number: CN113764765A) provides a method for recycling positive electrode active materials in batteries. The method involves immersing the recovered positive electrode powder from lithium-ion batteries in an NMP solution to remove the PVDF binder, drying the material, adding a eutectic lithium salt of LiNO3 and LiOH to the dried powder, and then sintering it at high temperature to obtain a repaired product. The advantage of this method is that the entire recycling process is relatively simple and the process is highly feasible. The disadvantage is that it does not completely remove some residual organic matter from the electrode, resulting in a significant difference in the performance of the repaired material compared to the original.

[0004] A Chinese patent application (publication number: CN113991101A) proposes to directly mix the lithium iron phosphate material to be repaired, a conductive agent, a lithium replenishing agent, and a binder to make a repaired battery electrode. The advantage is that the operation is simple, but the disadvantage is that the lithium replenishing agent and the lithium iron phosphate material to be repaired are not fully mixed and reacted, resulting in poor repair effect.

[0005] To improve the utilization rate of valuable metals, reduce environmental pollution caused by the disposal of waste batteries, and help promote the sustainable development of the new energy industry, this invention studies and designs a method for the remediation of lithium iron phosphate. Summary of the Invention

[0006] Therefore, the technical problem to be solved by the present invention is to overcome the defects mentioned above, thereby providing a method for repairing lithium iron phosphate.

[0007] To address the above problems, this invention provides a method for repairing lithium iron phosphate, comprising the following steps:

[0008] S1: Calcine the recovered lithium iron phosphate powder to remove impurities;

[0009] S2: The calcined lithium iron phosphate powder is mixed with a mixture containing an iron source, a carbon source and additives to obtain mixture I;

[0010] S3: Granulate the mixture I to obtain granulated particles;

[0011] S4: Mix the granulated particles with a mixture containing a lithium source, and dry to obtain a repair precursor;

[0012] S5: The repair precursor is sintered at high temperature to complete the repair of lithium iron phosphate.

[0013] Further, in step S1, the calcination conditions are as follows:

[0014] The sintering environment requires an oxygen content of ≤30PPM, a calcination temperature of 200℃-650℃, and a calcination time of 2-10h.

[0015] Further, in step S2, the molar ratio of the calcined lithium iron phosphate powder to the iron source, the carbon source, and the additive is 1:0.05-0.20:0.02-0.1:0.001-0.05, based on the molar number of lithium, iron, and carbon elements.

[0016] Furthermore, the iron source is selected from one or more soluble or insoluble iron compounds such as ferric phosphate, ferrous oxalate, ferric oxide, and ferric acetate;

[0017] The carbon source is selected from one or more of sucrose, citric acid, and glucose;

[0018] The additive is selected from at least one of azo compounds and alkane compounds.

[0019] Furthermore, the azo compound is selected from at least one of methyl orange, Congo red, and Sudan red;

[0020] The alkane compound is selected from at least one of n-butane, n-hexane, n-heptane, and cyclohexane.

[0021] Furthermore, both the mixture containing an iron source, a carbon source, and additives, and the mixture containing a lithium source, also include a solvent;

[0022] The solvent is selected from water, ethanol, and isopropanol, but at least one of them;

[0023] The amount of solvent used is 5-10 times the content of the mixture containing iron source, carbon source and additives and the mixture containing lithium source, respectively.

[0024] Furthermore, the mixing method described in step S2 is sand milling;

[0025] The grinding conditions are as follows:

[0026] The particle size D50 in the sand mill is 100nm-500nm, and the sand milling time is 1-5 hours.

[0027] Furthermore, in step S3, spray granulation is employed;

[0028] The spray granulation conditions are as follows:

[0029] Small particles are agglomerated into spherical secondary particles through spraying;

[0030] The granulated particles have a relatively uniform size and a porous secondary particle structure.

[0031] Further, in step S4, the molar ratio of the granulated particles to the lithium source is 1:0.02-0.1, based on the molar number of lithium elements.

[0032] The lithium source is selected from one or more of lithium carbonate, lithium hydroxide, lithium acetate, and lithium phosphate;

[0033] The drying conditions are as follows:

[0034] The drying process uses a belt dryer with a drying temperature range of 80℃-200℃. The moisture content of the dried material is ≤10PPM.

[0035] Furthermore, the high-temperature sintering conditions are as follows:

[0036] The high-temperature sintering temperature is 600℃-900℃, and the high-temperature sintering time is 5-20h.

[0037] The method for repairing lithium iron phosphate provided by this invention has the following beneficial effects:

[0038] 1. This invention improves the performance of recycled lithium iron phosphate materials by subjecting them to calcination for impurity removal, re-granulation, and high-temperature sintering. Compared to other recycling methods, this method uses additives and special processes to form a more stable secondary structure, maximizing the recovery of material performance; it also increases the utilization rate of valuable metals, reduces environmental pollution caused by the disposal of waste batteries, and contributes to the sustainable development of the new energy industry.

[0039] 2. The present invention also involves recycled materials that are not limited to pure lithium iron phosphate, but can also be used to recycle and repair lithium iron phosphate materials recovered after battery disassembly;

[0040] 3. The present invention also improves the lithium replenishment efficiency and the performance of the finished lithium iron phosphate product by adding special additives and surfactants to the spraying process. Specifically, the secondary particles prepared by the invention have a special structure, namely, micropores on the surface of the spherical secondary particles. Detailed Implementation

[0041] This application discloses a method for repairing lithium iron phosphate, comprising the following steps:

[0042] S1: Calcine the recovered lithium iron phosphate powder to remove impurities;

[0043] S2: The calcined lithium iron phosphate powder is mixed with a mixture containing an iron source, a carbon source and additives to obtain mixture I;

[0044] S3: Granulate the mixture I to obtain granulated particles;

[0045] S4: Mix the granulated particles with a mixture containing a lithium source, and dry to obtain a repair precursor;

[0046] S5: The repair precursor is sintered at high temperature to complete the repair of lithium iron phosphate.

[0047] The method described in this application improves the performance of recycled lithium iron phosphate materials by calcining to remove impurities, re-granulating, and high-temperature sintering. Compared with other recycling processes, this method uses additives and special processes to form a secondary structure with better stability, thereby maximizing the recovery of material performance.

[0048] The method described in this application is not limited to pure lithium iron phosphate material; it can also be used to recycle and repair lithium iron phosphate materials recovered after battery disassembly.

[0049] The spraying process involved in this application, through the addition of special additives and surfactants, gives the prepared secondary particles a special structure, thereby improving the lithium replenishment efficiency and the performance of the finished lithium iron phosphate product.

[0050] The method described in this application uses simple manufacturing equipment and the process is easy to engineer.

[0051] The recycling of lithium iron phosphate material in this application method is achieved through the following steps: discharging and separating the positive electrode sheet from the waste lithium iron phosphate battery, then crushing and separating the positive electrode sheet to obtain the positive electrode material and aluminum foil, which are further subjected to gravity screening to remove impurities to obtain the waste lithium iron phosphate material for the next step of repair.

[0052] This application also discloses some embodiments, in which the calcination conditions in step S1 are:

[0053] The sintering environment requires an oxygen content of ≤30PPM, a calcination temperature of 200℃-650℃, and a calcination time of 2-10h.

[0054] This application also discloses some embodiments. In step S2, the molar ratio of the calcined lithium iron phosphate powder to the iron source, the carbon source, and the additive is 1:0.05-0.20:0.02-0.1:0.001-0.05, based on the molar number of elements, iron element, and carbon element.

[0055] This application also discloses some embodiments, wherein the iron source is selected from one or more of soluble or insoluble iron compounds such as ferric phosphate, ferrous oxalate, ferric oxide, and ferric acetate;

[0056] The carbon source is selected from one or more of sucrose, citric acid, and glucose;

[0057] The additive is selected from at least one of azo compounds and alkane compounds.

[0058] This application also discloses some embodiments, wherein the azo compound is selected from at least one of methyl orange, Congo red, and Sudan red;

[0059] The alkane compound is selected from at least one of n-butane, n-hexane, n-heptane, and cyclohexane.

[0060] This application also discloses some embodiments in which the mixture containing an iron source, a carbon source and additives and the mixture containing a lithium source both further include a solvent;

[0061] The solvent is selected from water, ethanol, and isopropanol, but at least one of them;

[0062] The amount of solvent used is 5-10 times the content of the mixture containing iron source, carbon source and additives and the mixture containing lithium source, respectively.

[0063] This application also discloses some embodiments, in which the mixing method described in step S2 is sand milling;

[0064] The grinding conditions are as follows:

[0065] The particle size D50 in the sand mill is 100nm-500nm, and the sand milling time is 1-5 hours.

[0066] This application also discloses some embodiments in which spray granulation is used in step S3;

[0067] The spray granulation conditions are as follows:

[0068] Small particles are agglomerated into spherical secondary particles through spraying;

[0069] It uses a spray dryer granulator, model PGL-B, to manufacture small particles into agglomerated spherical secondary particles.

[0070] The granulated particles have a relatively uniform size and a porous secondary particle structure.

[0071] This application also discloses some embodiments in which, in step S4, the molar ratio of the granulated particles to the lithium source is 1:0.02-0.1, based on the molar number of lithium elements.

[0072] The lithium source is selected from one or more of lithium carbonate, lithium hydroxide, lithium acetate, and lithium phosphate;

[0073] The drying conditions are as follows:

[0074] The drying process uses a belt dryer with a drying temperature range of 80℃-200℃. The moisture content of the dried material is ≤10PPM.

[0075] This application also discloses some embodiments, wherein the high-temperature sintering conditions are as follows:

[0076] The high-temperature sintering temperature is 600℃-900℃, and the high-temperature sintering time is 5-20h.

[0077] The specific method is as follows:

[0078] Vacuum furnace calcination: The recovered lithium iron phosphate powder material is placed in a vacuum sintering furnace, ensuring that the oxygen content is less than or equal to 30 PPM, the sintering temperature range is 200℃-650℃, the sintering time is 2-10 hours, and the material is collected after sintering.

[0079] Sand milling and mixing: The vacuum-calcined recycled material is mixed with iron source, carbon source, additives and water according to the repair material. The mixture is then fully mixed by sand milling for 1-5 hours. The particle size D50 during sand milling is 100nm-500nm. The material to be sprayed is obtained after sand milling.

[0080] Spray drying: The material to be sprayed after sand milling is prepared into relatively uniform porous secondary particles through a spray drying system.

[0081] Drying and Lithium Supplementation: The sprayed granules, lithium source, and water are thoroughly mixed and stirred, and then dried using a belt dryer to obtain dried material to be burned. The molar ratio of the granules to the lithium source is 1:0.02-0.1, based on the molar number of lithium elements. The drying temperature range is 80℃-200℃, and the moisture content of the dried material is ≤10PPM.

[0082] High-temperature sintering: The material to be sintered is sintered at a high temperature of 600℃-900℃ under nitrogen protection (oxygen content ≤30PPM) for 5-20 hours to obtain repaired lithium iron phosphate material.

[0083] Comparative Example 1

[0084] The recovered lithium iron phosphate powder was sintered at 500℃ for 2 hours and then collected, and recorded as sample 1.

[0085] Comparative Example 2

[0086] The recovered lithium iron phosphate powder was sintered at 500℃ for 2 hours and then collected. The molar ratio of the material to be repaired, iron source, carbon source, lithium source, and surfactant was 1:0.2:0.003:0.05:0.002, where the iron source was iron phosphate, the carbon source was glucose, the surfactant was n-butane, and the lithium source was lithium carbonate. The material to be repaired, iron source, carbon source, surfactant, and water were mixed to obtain a spray material. After re-granulation, the lithium source and a certain amount of water were added, and then the material was dried to obtain the material to be sintered. The material to be sintered was sintered at 750℃ for 10 hours to obtain the repaired lithium iron phosphate material, which was designated as sample 2.

[0087] Comparative Example 3

[0088] The recovered lithium iron phosphate powder was sintered at 500℃ for 2 hours and then collected. The molar ratio of the material to be repaired, iron source, carbon source, lithium source, and surfactant was 1:0.2:0.003:0.2:0.002, where ferrous oxalate was used as the iron source, glucose as the carbon source, n-butane as the surfactant, and lithium phosphate as the lithium source. The material to be repaired, iron source, carbon source, surfactant, and a certain amount of water were mixed to obtain a spray material. After re-granulation, the lithium source and a certain amount of water were added, and the material was dried to obtain the material to be sintered. The material to be sintered was sintered at 750℃ for 10 hours to obtain the repaired lithium iron phosphate material, which was designated as sample 3.

[0089] Comparative Example 4

[0090] The recovered lithium iron phosphate powder was sintered at 500℃ for 2 hours and then collected. The molar ratio of the material to be repaired, iron source, carbon source, lithium source, and surfactant was 1:0.1:0.004:0.1:0.002, where the iron source was ferric oxide, the carbon source was glucose, the surfactant was an azo compound, and the lithium source was lithium acetate. The material to be repaired, the iron source, the carbon source, the surfactant, and a certain amount of water were mixed to obtain a spray material. After re-granulation, the lithium source and a certain amount of water were added, and then the material was dried to obtain the material to be sintered. The material to be sintered was sintered at 750℃ for 10 hours to obtain the repaired lithium iron phosphate material, which was designated as sample 4.

[0091] Performance tests were performed on the obtained samples 1-4.

[0092] 1. Test its performance, including its pH value and specific surface area.

[0093] 2. Unrepaired lithium iron phosphate material was directly used to make battery electrodes for electrical performance testing. The electrode ratio was active material: conductive agent: binder = 90:5:5. The active material was lithium iron phosphate, the conductive agent was Super P conductive agent, and the binder was PVDF. The electrolyte concentration was 1.2 mol / L, and the solvent ratio was EC:DMC:EMC = 1:1:1. Button cells were fabricated, and the initial charge / discharge efficiency and rate performance were tested. The data are shown in Tables 1 and 2.

[0094] Table 1

[0095]

[0096] Table 2

[0097]

[0098] As can be seen from Tables 1 and 2, the repair method proposed in this invention effectively improves the overall performance of lithium iron phosphate. Comparative Examples 2 and 4 show better repair effects, while Comparative Example 3 has some negative impacts on performance due to changes in the element ratio. Better results can be achieved by combining it with other compounds and optimizing the formulation.

[0099] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention. The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the technical principles of the present invention, and these improvements and modifications should also be considered within the protection scope of the present invention.

Claims

1. A method of repairing lithium iron phosphate, characterized by, Includes the following steps: S1: Calcine the recovered lithium iron phosphate powder to remove impurities; S2: The calcined lithium iron phosphate powder is mixed with a mixture containing an iron source, a carbon source and additives to obtain mixture I; S3: Granulate the mixture I to obtain granulated particles; S4: Mix the granulated particles with a mixture containing a lithium source, and dry to obtain a repair precursor; S5: The repair precursor is sintered at high temperature to complete the repair of lithium iron phosphate. The additive is selected from at least one of methyl orange, Congo red, Sudan red, n-butane, n-hexane, n-heptane, and cyclohexane.

2. The method for repairing lithium iron phosphate according to claim 1, characterized in that: In step S1, the calcination conditions are as follows: The sintering environment requires an oxygen content of ≤30ppm, a calcination temperature of 200℃-650℃, and a calcination time of 2-10h.

3. The method for repairing lithium iron phosphate according to claim 1, characterized in that: In step S2, the molar ratio of the calcined lithium iron phosphate powder to the iron source, the carbon source, and the additive is 1:0.05-0.20:0.02-0.1:0.001-0.05, based on the molar number of lithium, iron, and carbon elements.

4. The method for repairing lithium iron phosphate according to claim 1, characterized in that: The iron source is selected from one or more compounds of ferric phosphate, ferrous oxalate, ferric oxide, and ferric acetate; The carbon source is selected from one or more of sucrose, citric acid, and glucose.

5. The method for repairing lithium iron phosphate according to claim 1, characterized in that: The mixture containing an iron source, a carbon source, and additives, and the mixture containing a lithium source, both also include a solvent. The solvent is selected from at least one of water, ethanol, and isopropanol; The amount of solvent used is 5-10 times the content of the mixture containing iron source, carbon source and additives and the mixture containing lithium source, respectively.

6. The method for repairing lithium iron phosphate according to claim 1, characterized in that: The mixing method described in step S2 is sand milling; The grinding conditions are as follows: The particle size D50 in the sand mill is 100nm-500nm, and the sand milling time is 1-5 hours.

7. The method for repairing lithium iron phosphate according to claim 1, characterized in that: In step S3, spray granulation is used; The spray granulation conditions are as follows: Small particles are agglomerated into spherical secondary particles through spraying; The granulated particles have a relatively uniform size and a porous secondary particle structure.

8. The method for repairing lithium iron phosphate according to claim 1, characterized in that: In step S4, the molar ratio of the granulated particles to the lithium source is 1:0.02-0.1, based on the molar number of lithium elements. The lithium source is selected from one or more of lithium carbonate, lithium hydroxide, lithium acetate, and lithium phosphate; The drying conditions are as follows: The drying process uses a belt dryer with a drying temperature range of 80℃-200℃. The moisture content of the dried material is ≤10ppm.

9. The method for repairing lithium iron phosphate according to claim 1, characterized in that: The high-temperature sintering conditions are as follows: The high-temperature sintering temperature is 600℃-900℃, and the high-temperature sintering time is 5-20h.

Citation Information

Patent Citations

  • Recycling method and recycling equipment for positive electrode active material of lithium ion battery

    CN113764765A

  • Lithium supplementing method for lithium iron phosphate lithium ion battery and lithium iron phosphate lithium ion battery

    CN113991101A

  • Preparation method of lithium manganese iron phosphate

    CN116443839A

  • Recycling of lithium-based electrochemical cells

    WO2019232574A1