A method and apparatus for laser cleaning and performance enhancement of aluminum alloys

By using a combined microsecond pulsed laser and nanosecond pulsed laser cleaning method, the problems of low efficiency and substrate damage in traditional laser cleaning have been solved, achieving efficient cleaning and mechanical property enhancement of aluminum alloy surfaces.

CN119387241BActive Publication Date: 2026-11-24ARMOR ACADEMY OF CHINESE PEOPLES LIBERATION ARMY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411577600.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-11-06
Publication Date
2026-11-24
Estimated Expiration
2044-11-06

AI Technical Summary

Technical Problem

Traditional laser cleaning methods have a narrow range of contaminants on aluminum alloy surfaces, low cleaning efficiency, and complex optimization of laser cleaning and strengthening process parameters, which can easily lead to damage to the substrate.

Method used

A combined cleaning method using microsecond pulsed laser and nanosecond pulsed laser is employed. The microsecond pulsed laser first forms the scanning area, followed by the nanosecond pulsed laser, which partially overlaps with it. By combining laser parameters with different pulse widths and frequencies, the surface cleaning and performance enhancement of aluminum alloys can be achieved.

Benefits of technology

It improves laser cleaning efficiency, simultaneously enhances the mechanical properties of aluminum alloys, avoids damage to the substrate, and achieves efficient cleaning and strengthening effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119387241B_ABST
    Figure CN119387241B_ABST
Patent Text Reader

Abstract

The application provides a processing method and device for laser cleaning and performance strengthening of an aluminum alloy, and the processing method comprises the following steps: fixing an aluminum alloy base body, and determining a surface cleaning area of the aluminum alloy base body; setting cleaning process parameters of a microsecond pulse laser head and a nanosecond pulse laser head control system according to the surface cleaning area of the aluminum alloy base body; and performing composite laser cleaning along a scanning path according to a laser scanning area formed by the microsecond pulse laser head and a laser scanning area formed by the nanosecond pulse laser head according to the cleaning process parameters; wherein, during the composite laser cleaning, the microsecond pulse laser is in front and forms a microsecond pulse laser scanning area A1, the nanosecond pulse laser is in back and forms a nanosecond pulse laser scanning area A2, and the microsecond pulse laser scanning area A1 and the nanosecond pulse laser scanning area A2 partially overlap. One technical effect of the application is to improve the laser cleaning efficiency and strengthen the mechanical properties of the aluminum alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of laser processing technology, specifically relating to a processing method and apparatus for laser cleaning and performance enhancement of aluminum alloys. Background Technology

[0002] Traditional laser cleaning methods utilize a single laser source, primarily relying on the thermal effect of light to heat and remove contaminants. However, due to varying working environments and the complex composition of contaminants on aluminum alloy surfaces, which often contain multiple pollutants, using a single laser to optimize parameters for specific contaminants is only suitable for cleaning those specific contaminants. Overall, using a single laser source suffers from limitations in terms of the narrow range of contaminant types that can be cleaned and low cleaning efficiency.

[0003] Furthermore, laser cleaning and the subsequent enhancement of the mechanical properties of the material surface are two separate processes. Conventional surface enhancement methods first require cleaning the metal substrate surface, followed by a strengthening process. If laser cleaning and laser shock peening are used separately to improve surface mechanical properties, the process parameters for laser cleaning and laser shock peening need to be pre-optimized. The two processes cannot be performed simultaneously, increasing the overall complexity of the process.

[0004] In existing technologies, conventional laser cleaning methods enhance the cleaning effect by increasing the laser energy density to avoid incomplete cleaning. However, increasing the laser energy density can also cause damage to the substrate during cleaning and increases the difficulty of optimizing laser parameters. Therefore, it is necessary to find a way to rationally allocate laser energy to avoid substrate damage during the laser cleaning process. Summary of the Invention

[0005] The present invention aims to solve at least one of the technical problems existing in the prior art, and to provide a new technical solution for a processing method and apparatus for laser cleaning and performance enhancement of aluminum alloys.

[0006] According to a first aspect of the present invention, a processing method for laser cleaning and performance enhancement of aluminum alloys is provided, comprising the following steps:

[0007] Fix the aluminum alloy substrate and determine the area on its surface to be cleaned;

[0008] Based on the area to be cleaned on the surface of the aluminum alloy substrate, the cleaning process parameters of the microsecond pulse laser head and nanosecond pulse laser head control system are set.

[0009] Based on the laser scanning areas formed by the microsecond pulse laser head and the nanosecond pulse laser head, composite laser cleaning is performed along the scanning path according to the cleaning process parameters. During composite laser cleaning, the microsecond pulse laser is in front, forming a microsecond pulse laser scanning area A1, and the nanosecond pulse laser is behind, forming a nanosecond pulse laser scanning area A2. The microsecond pulse laser scanning area A1 and the nanosecond pulse laser scanning area A2 partially overlap.

[0010] Optionally, the overlapping area of ​​the nanosecond pulse laser scanning area A2 and the microsecond pulse laser scanning area A1 is 25%-50% of the area of ​​the microsecond pulse laser scanning area A1.

[0011] Optionally, the width D2 of the nanosecond pulse laser scanning area A2 is equal to the width D1 of the microsecond pulse laser scanning area A1.

[0012] Optionally, the cleaning process parameters include: pulse width, pulse frequency, spot diameter, output power, and scanning speed.

[0013] Optionally, the scanning beams emitted by the nanosecond pulse laser head and the microsecond pulse laser head form an angle of 50° to 75° with the area to be cleaned.

[0014] Optionally, the scanning beam emitted by the nanosecond pulse laser forms a first angle with the aluminum alloy substrate, and the scanning beam emitted by the microsecond pulse laser forms a second angle with the aluminum alloy substrate, wherein the first angle and the second angle are equal, and the spot diameter d2 formed by the nanosecond pulse laser focusing on the area to be cleaned and the spot diameter d1 formed by the microsecond pulse laser focusing on the surface to be cleaned satisfy d2≤d1.

[0015] Optionally, the wavelength of the nanosecond pulse laser generated by the nanosecond pulse laser head is 1064 nm, and the wavelength of the microsecond pulse laser generated by the microsecond pulse laser head is 1064 nm.

[0016] Optionally, the cleaning process parameters of the nanosecond pulse laser head are: pulse width of 100ns-150ns, pulse frequency of 200KHz-400KHz, output power of 80W-100W, and scanning speed of 3000mm / s-7000mm / s.

[0017] The cleaning process parameters of the microsecond pulse laser head are as follows: pulse width of 1μs, pulse frequency of 20KHz~50KHz, output power of 150W-350W, and scanning speed of 800mm / s~2000mm / s.

[0018] According to a second aspect of the present invention, a processing apparatus for laser cleaning and performance enhancement of aluminum alloys is provided, employing the processing method as described in the first aspect, comprising a nanosecond pulse laser head, a microsecond pulse laser head, a first fixed plate, a second fixed plate, a first rotary motor, a second rotary motor, and a temperature sensor;

[0019] An installation area is formed between the first fixing plate and the second fixing plate. The nanosecond pulse laser head, the microsecond pulse laser head, and the temperature sensor are all disposed in the installation area, and the temperature sensor is located between the nanosecond pulse laser head and the microsecond pulse laser head. The nanosecond pulse laser head and the microsecond pulse laser head are rotatably connected to the first fixing plate and the second fixing plate, respectively.

[0020] The first rotary motor is connected to the nanosecond pulse laser head and is used to drive the nanosecond pulse laser head to rotate; the second rotary motor is connected to the microsecond pulse laser head and is used to drive the microsecond pulse laser head to rotate.

[0021] The temperature sensor is used to measure the temperature of the overlapping portion of the microsecond pulse laser scanning area A1 formed by the microsecond pulse laser and the nanosecond pulse laser scanning area A2 formed by the nanosecond pulse laser; wherein the temperature is less than 85% of the melting point of the aluminum alloy matrix.

[0022] Optionally, the processing apparatus for laser cleaning and performance enhancement of aluminum alloys further includes a sensor fixture, a first fixed fixture, a second fixed fixture, and a motor storage box; the temperature sensor is fixed to the sensor fixture, the nanosecond pulse laser head is fixed to the first fixed fixture, and the microsecond pulse laser head is fixed to the second fixed fixture; the first fixed fixture and the second fixed fixture are rotatably connected to the first fixed plate and the second fixed plate, respectively;

[0023] The motor storage box is fixed to the side of the second fixing plate away from the first fixing plate. The first rotary motor and the second rotary motor are both disposed in the motor storage box. The output shaft of the first rotary motor passes through the motor storage box and the second fixing plate in sequence and is fixedly connected to the first fixing clamp. The output shaft of the second rotary motor passes through the motor storage box and the second fixing plate in sequence and is fixedly connected to the second fixing clamp.

[0024] One technical advantage of this invention is that:

[0025] In the embodiments of this application, the processing method and apparatus for laser cleaning and performance enhancement of aluminum alloy utilize two light sources, nanosecond pulse laser and microsecond pulse laser with different pulse widths, to perform precise laser cleaning operation after combining them one after the other. This not only improves the efficiency of laser cleaning operation, but also enhances the mechanical properties of aluminum alloy.

[0026] Specifically, the high power of microsecond pulsed lasers is used to perform large-area cleaning and damage on the object to be cleaned, removing 85%-95% of the thickness. Simultaneously, some of the laser energy is transferred to the aluminum alloy substrate during the cleaning process, resulting in energy accumulation and a micro-melting state on the aluminum alloy surface. Then, the high repetition rate and impact of nanosecond pulsed lasers are used to remove the remaining contaminants. Under the repeated impact of multiple pulses, a grain refinement layer forms on the cleaned aluminum alloy surface, improving its mechanical properties. Therefore, this processing method and apparatus for laser cleaning and performance enhancement of aluminum alloys combines the high energy input of microsecond pulsed lasers with the high repetition rate of nanosecond pulsed lasers, improving both laser cleaning efficiency and enhancing the mechanical properties of aluminum alloys. Attached Figure Description

[0027] Figure 1 This is a schematic flowchart of a processing method for laser cleaning and performance enhancement of aluminum alloy according to an embodiment of the present invention.

[0028] Figure 2 This is a schematic flowchart of a processing method for laser cleaning and performance enhancement of aluminum alloy according to another embodiment of the present invention.

[0029] Figure 3 This is a schematic diagram of a processing apparatus for laser cleaning and performance enhancement of aluminum alloys according to an embodiment of the present invention.

[0030] Figure 4 This is a schematic diagram of the working state of a processing device for laser cleaning and performance enhancement of aluminum alloy according to an embodiment of the present invention.

[0031] Figure 5 This is a schematic diagram illustrating the requirements for the laser spot formed by a processing apparatus for laser cleaning and performance enhancement of aluminum alloys according to an embodiment of the present invention.

[0032] Figure 6 This is a schematic diagram of another working state of a processing apparatus for laser cleaning and performance enhancement of aluminum alloys according to an embodiment of the present invention.

[0033] In the diagram: 1-1, Nanosecond pulse laser head; 1-2, Microsecond pulse laser head; 2-1, First fixing plate; 2-2, Second fixing plate; 3, Sensor fixture; 4, Temperature sensor; 5-1, First fixing fixture; 5-2, Second fixing fixture; 6, Motor storage box; 7-1, First rotary motor; 7-2, Second rotary motor. Detailed Implementation

[0034] Various exemplary embodiments of the present application will now be described in detail with reference to the accompanying drawings. It should be noted that, unless otherwise specifically stated, the relative arrangement, numerical expressions, and values ​​of the components and steps set forth in these embodiments do not limit the scope of the present application.

[0035] The embodiments of this application will now be described in detail. Examples of these embodiments are illustrated in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain this application, and should not be construed as limiting this application. All other embodiments obtained by those skilled in the art based on the embodiments of this application without inventive effort are within the scope of protection of this application.

[0036] The terms "first" and "second" in the specification and claims of this application may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise stated, "multiple" means two or more. Furthermore, "and / or" in the specification and claims indicates at least one of the connected objects, and the character " / " generally indicates that the preceding and following objects are in an "or" relationship.

[0037] In the description of this application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc., indicating the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this application.

[0038] In the description of this application, it should be noted that, unless otherwise expressly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection between two components. Those skilled in the art can understand the specific meaning of the above terms in this application based on the specific circumstances.

[0039] According to a first aspect of the invention, see Figure 1This invention provides a processing method for laser cleaning and performance enhancement of aluminum alloys. It utilizes nanosecond pulsed lasers and microsecond pulsed lasers to achieve surface cleaning and mechanical property enhancement of aluminum alloys. It makes full use of laser energy, which not only effectively improves the efficiency of laser cleaning, but also simultaneously enhances the mechanical properties of aluminum alloys.

[0040] Specifically, the processing method for laser cleaning and performance enhancement of aluminum alloys includes the following steps:

[0041] Step S11: Fix the aluminum alloy substrate and determine the area on its surface to be cleaned;

[0042] Step S21: Based on the area to be cleaned on the surface of the aluminum alloy substrate, set the cleaning process parameters of the microsecond pulse laser head and nanosecond pulse laser head control system.

[0043] Step S31: Based on the laser scanning area formed by the microsecond pulse laser head and the laser scanning area formed by the nanosecond pulse laser head, perform composite laser cleaning along the scanning path according to the cleaning process parameters; wherein, during composite laser cleaning, the microsecond pulse laser is in front and forms the microsecond pulse laser scanning area A1, and the nanosecond pulse laser is behind and forms the nanosecond pulse laser scanning area A2, and the microsecond pulse laser scanning area A1 and the nanosecond pulse laser scanning area A2 partially overlap.

[0044] In the embodiments of this application, the processing method and apparatus for laser cleaning and performance enhancement of aluminum alloy utilize two light sources, nanosecond pulse laser and microsecond pulse laser with different pulse widths, to perform precise laser cleaning operation after combining them one after the other. This not only improves the efficiency of laser cleaning operation, but also enhances the mechanical properties of aluminum alloy.

[0045] Specifically, the high power of microsecond pulsed lasers is used to perform large-area cleaning and damage on the object to be cleaned, removing 85%-95% of the thickness. Simultaneously, some of the laser energy is transferred to the aluminum alloy substrate during the cleaning process, resulting in energy accumulation and a micro-melting state on the aluminum alloy surface. Then, the high repetition rate and impact of nanosecond pulsed lasers are used to remove the remaining contaminants. Under the repeated impact of multiple pulses, a grain refinement layer forms on the cleaned aluminum alloy surface, improving its mechanical properties. Therefore, this processing method and apparatus for laser cleaning and performance enhancement of aluminum alloys combines the high energy input of microsecond pulsed lasers with the high repetition rate of nanosecond pulsed lasers, improving both laser cleaning efficiency and enhancing the mechanical properties of aluminum alloys.

[0046] For example, nanosecond pulsed laser comes first, that is Figure 5 In (a), the positive y-axis direction corresponds to the microsecond pulse laser being positioned behind. Figure 5 In the negative y-axis direction, the microsecond pulse spot and the nanosecond pulse spot at least partially overlap.

[0047] like Figure 5 As shown in (b), the total scanning length L of the microsecond pulse spot and the nanosecond pulse spot in the y-axis direction is... D1 =L D2 .

[0048] Furthermore, such as Figure 5 As shown in (c) and (d), the motion trajectories of the microsecond pulse spot and the nanosecond pulse spot are both S-shaped. The microsecond pulse spot and the nanosecond pulse spot are required to overlap in the x and y directions, so as to achieve complete cleaning and surface performance enhancement of the aluminum alloy surface.

[0049] In this embodiment, as Figure 5 As shown, the center distance D between the microsecond pulse laser spot and the nanosecond pulse laser spot is adjustable, achieved by changing the angle between the nanosecond pulse laser head and the microsecond pulse laser head and the vertical height of the device. Furthermore, a temperature sensor is located at the center between the nanosecond pulse laser head and the microsecond pulse laser head, used to detect the temperature at the overlapping area of ​​the microsecond pulse laser spot and the nanosecond pulse laser spot. The sensor fixture employs a non-adjustable design to ensure that the temperature sensor's position is fixed in both the vertical and horizontal directions, ensuring accurate temperature measurements.

[0050] Optionally, the overlapping area of ​​the nanosecond pulse laser scanning area A2 and the microsecond pulse laser scanning area A1 is 25%-50% of the area of ​​the microsecond pulse laser scanning area A1. This helps to improve the efficiency of laser cleaning operations and also enhances the mechanical properties of aluminum alloys.

[0051] Optionally, the width D2 of the nanosecond pulsed laser scanning area A2 is equal to the width D1 of the microsecond pulsed laser scanning area A1. This fully utilizes laser energy, effectively improving laser cleaning efficiency and simultaneously enhancing the mechanical properties of the aluminum alloy.

[0052] Optionally, the cleaning process parameters include: pulse width, pulse frequency, spot diameter, output power, and scanning speed. This helps to ensure the effectiveness of laser cleaning.

[0053] Optionally, the scanning beams emitted by the nanosecond pulse laser head and the microsecond pulse laser head form an angle of 50° to 75° with the area to be cleaned.

[0054] In the above embodiments, it is possible to effectively prevent the positions of the nanosecond pulse laser head and the microsecond pulse laser head from interfering with each other and causing damage.

[0055] For example, both microsecond pulsed lasers and nanosecond pulsed lasers control the movement of the laser beam in the x and y directions of the area to be cleaned by rotating a galvanometer in those directions. Since the range of laser beam movement achieved by rotating the galvanometer is limited, it can be combined with the movement of a fixed platform under the aluminum alloy substrate to achieve large-area cleaning and performance enhancement of the aluminum alloy surface.

[0056] Optionally, the scanning beam emitted by the nanosecond pulse laser forms a first angle with the aluminum alloy substrate, and the scanning beam emitted by the microsecond pulse laser forms a second angle with the aluminum alloy substrate, wherein the first angle and the second angle are equal, and the spot diameter d2 formed by the nanosecond pulse laser focusing on the area to be cleaned and the spot diameter d1 formed by the microsecond pulse laser focusing on the surface to be cleaned satisfy d2≤d1.

[0057] In the above embodiments, nanosecond pulse lasers and microsecond pulse lasers can be fully utilized to achieve aluminum alloy surface cleaning and mechanical property enhancement.

[0058] Optionally, the nanosecond pulse laser head generates a nanosecond pulse laser with a wavelength of 1064 nm, and the microsecond pulse laser head generates a microsecond pulse laser with a wavelength of 1064 nm. This enables the nanosecond pulse laser head and the microsecond pulse laser head to achieve surface cleaning and mechanical property enhancement of aluminum alloys.

[0059] Optionally, the cleaning process parameters of the nanosecond pulse laser head are: pulse width of 100ns-150ns, pulse frequency of 200KHz-400KHz, output power of 80W-100W, and scanning speed of 3000mm / s-7000mm / s.

[0060] The cleaning process parameters of the microsecond pulse laser head are as follows: pulse width of 1μs, pulse frequency of 20KHz~50KHz, output power of 150W-350W, and scanning speed of 800mm / s~2000mm / s.

[0061] In the above embodiments, the efficiency of laser cleaning can be improved significantly, and the mechanical properties of aluminum alloys can be strengthened simultaneously.

[0062] For example, before determining the area to be cleaned, the surface of the aluminum alloy substrate is pretreated to remove dust and other foreign matter from the surface of the area to be cleaned.

[0063] According to a second aspect of the invention, see Figure 3 , Figure 4 and Figure 6A processing apparatus for laser cleaning and performance enhancement of aluminum alloys is provided, employing the processing method described in the first aspect. The apparatus includes a nanosecond pulse laser head 1-1, a microsecond pulse laser head 1-2, a first fixed plate 2-1, a second fixed plate 2-2, a first rotary motor 7-1, a second rotary motor 7-2, and a temperature sensor 4. The nanosecond pulse laser head 1-1 is used for enhancing the surface performance of the aluminum alloy substrate, and the microsecond pulse laser head 1-2 is used for cleaning the surface of the aluminum alloy substrate. The temperature sensor 4 is used to monitor temperature changes during laser cleaning and laser cleaning enhancement of the area to be cleaned.

[0064] An installation area is formed between the first fixing plate 2-1 and the second fixing plate 2-1. The nanosecond pulse laser head 1-1, the microsecond pulse laser head 1-2, and the temperature sensor 4 are all disposed in the installation area, and the temperature sensor 4 is located between the nanosecond pulse laser head 1-1 and the microsecond pulse laser head 1-2. The nanosecond pulse laser head 1-1 and the microsecond pulse laser head 1-2 are rotatably connected to the first fixing plate 2-1 and the second fixing plate 2-2, respectively.

[0065] The first rotary motor 7-1 is connected to the nanosecond pulse laser head 1-1 and is used to drive the nanosecond pulse laser head 1-1 to rotate; the second rotary motor 7-2 is connected to the microsecond pulse laser head 1-2 and is used to drive the microsecond pulse laser head 1-2 to rotate; the first rotary motor 7-1 and the second rotary motor 7-2 enable the nanosecond pulse laser head 1-1 and the microsecond pulse laser head 1-2 to adjust the distance and angle between the two lasers after rotating at a specific angle;

[0066] The temperature sensor 4 is used to measure the temperature of the overlapping portion of the microsecond pulse laser scanning area A1 formed by the microsecond pulse laser and the nanosecond pulse laser scanning area A2 formed by the nanosecond pulse laser; wherein the temperature is less than 85% of the melting point of the aluminum alloy matrix.

[0067] In one example, the temperature sensor needs to be combined with post-processing software to monitor temperature changes in real time during the laser cleaning and performance enhancement process, ensuring that the surface temperature of the aluminum alloy substrate does not exceed 85% of the melting point of the aluminum alloy during the cleaning process.

[0068] In the above embodiment, the microsecond pulsed laser first removes 85%-95% of the cleaning material, while simultaneously inducing the surface metal into a micro-molten state through high-energy input. Furthermore, the high-frequency impact of the nanosecond pulsed laser refines the grains of the micro-molten material, thereby improving surface mechanical properties. In addition, a temperature sensor effectively prevents melting damage to the aluminum alloy substrate, ensuring the safety and stability of the laser cleaning process.

[0069] It should be noted that, compared with existing laser cleaning and laser shock strengthening technologies, this application utilizes the low energy density of microsecond pulsed lasers to achieve cleaning, obtaining a contamination-free aluminum alloy substrate surface with strengthening conditions; and uses high energy density nanosecond pulsed lasers to achieve high-frequency impact on the micro-melted layer of the microsecond pulsed laser-cleaned surface. Under the impact and rapid cooling, the micro-melted layer can achieve grain refinement, thereby improving the mechanical properties of the aluminum alloy surface.

[0070] Optionally, the processing device for laser cleaning and performance enhancement of aluminum alloys further includes a sensor fixture 3, a first fixing fixture 5-1, a second fixing fixture 5-2, and a motor storage box 6; the temperature sensor 4 is fixed to the sensor fixture 3, the nanosecond pulse laser head 1-1 is fixed to the first fixing fixture 5-1, and the microsecond pulse laser head 1-2 is fixed to the second fixing fixture 5-2; the first fixing fixture 5-1 and the second fixing fixture 5-2 are rotatably connected to the first fixing plate 2-1 and the second fixing plate 2-2, respectively;

[0071] The motor storage box 6 is fixed to the side of the second fixing plate 2-2 away from the first fixing plate 2-1. The first rotary motor 7-1 and the second rotary motor 7-2 are both disposed in the motor storage box 6. The output shaft of the first rotary motor 7-1 passes through the motor storage box 6 and the second fixing plate 1-2 in sequence and is fixedly connected to the first fixing clamp 5-1. The output shaft of the second rotary motor 7-2 passes through the motor storage box 6 and the second fixing plate 1-2 in sequence and is fixedly connected to the second fixing clamp 5-2.

[0072] In the above embodiments, the stability of the processing apparatus for laser cleaning and performance enhancement of aluminum alloys can be guaranteed.

[0073] In one specific implementation, see Figure 2 The processing method for laser cleaning and performance enhancement of aluminum alloys includes the following steps:

[0074] Step S21: Fix the aluminum alloy substrate and determine the area on its surface to be cleaned;

[0075] Step S22: Based on the area to be cleaned on the surface of the aluminum alloy substrate, set the angle between the nanosecond pulse laser head and the microsecond pulse laser head, the distance between the center of the laser spot, and the laser cleaning process parameters;

[0076] Step S23: The individual light spots generated by the microsecond pulse laser head and the nanosecond pulse laser head are scanned and overlapped into a pulse spot cleaning area under the action of the scanning galvanometer; at the same time, it is ensured that the nanosecond pulse laser scanning area is within the area of ​​the microsecond pulse laser scanning area.

[0077] Step S24: In the process of laser cleaning and strengthening of aluminum alloy substrate, the microsecond pulse laser is applied first, followed by the nanosecond pulse laser, and the generated microsecond pulse spot and nanosecond pulse spot at least partially overlap.

[0078] In the above embodiments, laser energy is fully utilized, which not only effectively improves the efficiency of laser cleaning, but also simultaneously enhances the mechanical properties of aluminum alloys.

[0079] For example, when fixing the aluminum alloy substrate, the range of cleaning and performance enhancement is selected; the height and position of the device are adjusted, and the height and initial position of the device are adjusted according to the thickness and size of the cleaning material.

[0080] In this application, the first and second fixing plates are made of aluminum alloy. The rotating shafts of the first and second fixing clamps are fixed at four holes in the first and second fixing plates, supported by bearings, ensuring smooth rotation of the first fixing clamp and the nanosecond pulse laser head, as well as the second fixing clamp and the microsecond pulse laser head. The first and second fixing plates are also used to fix the sensor clamp and the motor storage box, ensuring that the above components are tightly fixed without relative displacement.

[0081] For example, the rotation angles of the nanosecond pulse laser head and the microsecond pulse laser head are limited to a certain range, and the included angles between the nanosecond pulse laser head and the microsecond pulse laser head and the first fixed plate or the second fixed plate are equal, thereby ensuring that the overlapping area of ​​the cleaning spot and the performance enhancement spot is directly below the temperature sensor.

[0082] For example, both the first and second rotary motors are servo motors, and the laser angle is adjusted by controlling the rotation angle.

[0083] It is understood that the above embodiments are merely exemplary implementations used to illustrate the principles of the present invention, and the present invention is not limited thereto. For those skilled in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.

Claims

1. A processing method for laser cleaning and performance strengthening of aluminum alloys, characterized by, Includes the following steps: Fix the aluminum alloy substrate and determine the area on its surface to be cleaned; Based on the area to be cleaned on the surface of the aluminum alloy substrate, cleaning process parameters for the microsecond pulse laser head and nanosecond pulse laser head control system are set; wherein, the cleaning process parameters for the nanosecond pulse laser head are: pulse width of 100 ns - 150 ns, pulse frequency of 200 kHz - 400 kHz, output power of 80 W - 100 W, and scanning speed of 3000 mm / s - 7000 mm / s; the cleaning process parameters for the microsecond pulse laser head are: pulse width of 1 μs, pulse frequency of 20 kHz - 50 kHz, output power of 150 W - 350 W, and scanning speed of 800 mm / s - 2000 mm / s; Based on the laser scanning areas formed by the microsecond pulse laser head and the nanosecond pulse laser head, composite laser cleaning is performed along the scanning path according to the cleaning process parameters. During composite laser cleaning, the microsecond pulse laser precedes and forms the microsecond pulse laser scanning area A1, while the nanosecond pulse laser follows and forms the nanosecond pulse laser scanning area A2. The microsecond pulse laser scanning area A1 and the nanosecond pulse laser scanning area A2 partially overlap. The overlap area between the nanosecond pulse laser scanning area A2 and the microsecond pulse laser scanning area A1 is 25%-50% of the area of ​​the microsecond pulse laser scanning area A1. The process involves using the high power of the microsecond pulsed laser to clean and destroy contaminants over a large area, removing 85%-95% of the contaminant thickness. Simultaneously, some of the laser energy during the cleaning process is transferred to the aluminum alloy substrate, causing energy accumulation and creating a micro-melting state on the surface of the aluminum alloy substrate. The high repetition rate and impact of the nanosecond pulsed laser are then used to remove the remaining contaminant thickness. Under the repeated impact of multiple pulses, a grain refinement layer is formed on the cleaned surface of the aluminum alloy substrate, thereby enhancing the mechanical properties of the aluminum alloy substrate while performing composite laser cleaning.

2. The processing method for laser cleaning and performance enhancement of aluminum alloys according to claim 1, characterized in that, The width D2 of the nanosecond pulse laser scanning area A2 is equal to the width D1 of the microsecond pulse laser scanning area A1.

3. The processing method for laser cleaning and performance enhancement of aluminum alloys according to claim 1, characterized in that, The cleaning process parameters include: pulse width, pulse frequency, spot diameter, output power, and scanning speed.

4. The processing method for laser cleaning and performance enhancement of aluminum alloys according to claim 1, characterized in that, The scanning beams emitted by the nanosecond pulse laser head and the microsecond pulse laser head form an angle of 50° to 75° with the area to be cleaned.

5. The processing method for laser cleaning and performance enhancement of aluminum alloys according to claim 1, characterized in that, The scanning beam emitted by the nanosecond pulse laser forms a first angle with the aluminum alloy substrate, and the scanning beam emitted by the microsecond pulse laser forms a second angle with the aluminum alloy substrate. The first angle and the second angle are equal. The spot diameter d2 formed by the nanosecond pulse laser focusing on the area to be cleaned and the spot diameter d1 formed by the microsecond pulse laser focusing on the surface to be cleaned satisfy d2≤d1.

6. The processing method for laser cleaning and performance enhancement of aluminum alloys according to claim 1, characterized in that, The nanosecond pulse laser generated by the nanosecond pulse laser head has a wavelength of 1064 nm, and the microsecond pulse laser generated by the microsecond pulse laser head has a wavelength of 1064 nm.

7. A processing apparatus for laser cleaning and performance enhancement of aluminum alloys, characterized in that, The processing method described in any one of claims 1 to 6 includes a nanosecond pulse laser head, a microsecond pulse laser head, a first fixed plate, a second fixed plate, a first rotary motor, a second rotary motor, and a temperature sensor. An installation area is formed between the first fixing plate and the second fixing plate. The nanosecond pulse laser head, the microsecond pulse laser head, and the temperature sensor are all disposed in the installation area, and the temperature sensor is located between the nanosecond pulse laser head and the microsecond pulse laser head. The nanosecond pulse laser head and the microsecond pulse laser head are rotatably connected to the first fixing plate and the second fixing plate, respectively. The first rotary motor is connected to the nanosecond pulse laser head and is used to drive the nanosecond pulse laser head to rotate; the second rotary motor is connected to the microsecond pulse laser head and is used to drive the microsecond pulse laser head to rotate. The temperature sensor is used to measure the temperature of the overlapping portion of the microsecond pulse laser scanning area A1 formed by the microsecond pulse laser and the nanosecond pulse laser scanning area A2 formed by the nanosecond pulse laser; wherein the temperature is less than 85% of the melting point of the aluminum alloy matrix.

8. The processing apparatus for laser cleaning and performance enhancement of aluminum alloys according to claim 7, characterized in that, It also includes a sensor clamp, a first fixing clamp, a second fixing clamp, and a motor storage box; the temperature sensor is fixed to the sensor clamp, the nanosecond pulse laser head is fixed to the first fixing clamp, and the microsecond pulse laser head is fixed to the second fixing clamp; the first fixing clamp and the second fixing clamp are rotatably connected to the first fixing plate and the second fixing plate, respectively; The motor storage box is fixed to the side of the second fixing plate away from the first fixing plate. The first rotary motor and the second rotary motor are both disposed in the motor storage box. The output shaft of the first rotary motor passes through the motor storage box and the second fixing plate in sequence and is fixedly connected to the first fixing clamp. The output shaft of the second rotary motor passes through the motor storage box and the second fixing plate in sequence and is fixedly connected to the second fixing clamp.

Citation Information

Patent Citations

  • CO2 laser / nanosecond pulse laser compound cleaning method

    CN109821823A

  • Laser cleaning system and method for protecting base material from being melted

    CN111530853A

  • Double-light-source composite laser cleaning method and device

    CN115958020A