A high recovery rate and high grade sulfur concentrate production process

By optimizing the sulfur concentrate production process and adopting a combination of multiple fine and scavenging processes with tailings re-selection technology, the problems of high sulfur concentrate production costs and tailings grade fluctuations have been solved, achieving high-grade, high-recovery, and low-pollution-risk production results.

CN119456210BActive Publication Date: 2026-11-24GUANGDONG GUANGYE YUNLIU MINING CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411192041.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2026-11-24
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

Existing sulfur concentrate production processes suffer from high production costs, large fluctuations in tailings grade, and low recovery rates. In particular, the tailings content is difficult to control, and the risk of pollution discharge is high.

Method used

By employing efficient flotation processes, complex associated mineral separation technologies, and tailings re-selection technologies, combined with non-metallic slurry concentration detection and intelligent control systems, the flotation process is optimized by improving the dosage and type of flotation reagents, adjusting the slurry pH, and using sodium hexametaphosphate and concentrated sulfuric acid as inhibitors and modifiers. Multiple fine and scavenging processes are carried out to optimize the flotation process, increase the tailings re-selection steps, and reduce the tailings content.

Benefits of technology

This achieved a sulfur concentrate grade of over 48%, a recovery rate of over 90%, and a tailings content of less than 3%, thereby reducing production costs and pollution risks, and improving production efficiency and environmental benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119456210B_ABST
    Figure CN119456210B_ABST
Patent Text Reader

Abstract

This invention discloses a high-recovery, high-grade sulfur concentrate production process. The process includes the following steps: S1, crushing the raw ore to below 200 mesh; S2, adding water to the crushed ore to adjust the pH value of the slurry, and soaking and stirring; S3, adding inhibitors and modifiers to the stirred slurry and stirring evenly, then adding concentrated sulfuric acid, xanthate, and No. 2 oil for the first roughing process, obtaining rough concentrate I and rough medium ore I. Rough concentrate I is then subjected to a second roughing process with xanthate to obtain rough concentrate ⅠⅠ and rough tailings. Rough concentrate I and rough concentrate ⅠⅠ are combined and subjected to several cleaning processes to obtain sulfur concentrate. The rough tailings are then subjected to a first scavenging process with concentrated sulfuric acid, xanthate, and No. 2 oil to obtain scavenged tailings I and scavenged medium ore I. Scavenged medium ore I is then subjected to a second scavenging process to obtain scavenged tailings ⅠⅠ, which is the tailings slurry. The sulfur concentrate production process proposed in this invention yields high-quality sulfur concentrate with a grade of over 48%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of mineral processing technology, and in particular to a process for producing high-recovery, high-grade sulfur concentrate. Background Technology

[0002] Sulfur concentrate is an important chemical mineral raw material, mainly used in the manufacture of sulfuric acid. It is also used as a chemical raw material to produce sulfur and various sulfur-containing products. It has important applications in industries such as rubber, papermaking, textiles, food, and matches, and is particularly important in the defense industry for manufacturing various explosives and smoke agents. The slag from sulfur concentrate used in sulfuric acid production can be used in iron and steel smelting. If the slag has a high sulfur content and a low iron content, it can be used as a by-product in cement production—a mixture. Currently, sulfur concentrate production processes still face challenges such as high production costs and fluctuating tailings grade control, sometimes exceeding 5%. Summary of the Invention

[0003] The purpose of this invention is to provide a high-recovery, high-grade sulfur concentrate production process. The sulfur concentrate production process proposed in this invention obtains high-quality sulfur concentrate with a grade of over 48%, reduces tailings content to below 3%, achieves a recovery rate of over 90%, and reduces pollution risks.

[0004] This invention is achieved through the following technical solutions:

[0005] A high-recovery, high-grade sulfur concentrate production process includes the following steps:

[0006] S1. Crush the raw ore to below 200 mesh;

[0007] S2. Add water to the crushed ore to make a slurry with an ore mass concentration of 30% to 45%, adjust the pH of the slurry to 5 to 6, and soak and stir thoroughly.

[0008] S3. After stirring, first add inhibitors and modifiers to the slurry and stir evenly. Then add concentrated sulfuric acid, xanthate, and No. 2 oil for the first roughing to obtain rough concentrate I and rough medium ore I. Add xanthate to rough medium ore I for the second roughing to obtain rough concentrate ⅠⅠ and rough tailings. Combine rough concentrate I and rough concentrate ⅠⅠ for several cleaning processes to obtain sulfur concentrate. Add concentrated sulfuric acid, xanthate, and No. 2 oil to the rough tailings for the first scavenging to obtain scavenged tailings I and scavenged medium ore I. Scavenged medium ore I is then scavenged a second time to obtain scavenged tailings ⅠⅠ, which is the tailings slurry.

[0009] The sulfur concentrate production process proposed in this invention includes efficient flotation technology in the mineral processing stage, separation technology for complex associated minerals, tailings reprocessing technology, flotation technology for refractory ores, heavy metal pollution control technology, and xanthate degradation technology for mineral processing wastewater. This enables the sulfur concentrate to achieve a grade of over 48% and a recovery rate of over 90%, while reducing tailings content to below 3%, thus minimizing pollution risks. The non-metallic slurry concentration detection device, the high-recovery intelligent grinding and classification control system, the fluorescent sulfur element rapid analyzer, and the online slurry pH detection device improve the automation level of the mineral processing equipment and increase production efficiency. Furthermore, by controlling the dosage and type of flotation reagents during the flotation stage, the cost of mine wastewater treatment can be reduced and the treatment effect improved, resulting in better environmental and social benefits than similar products.

[0010] Preferably, the inhibitor mentioned in step S3 is sodium hexametaphosphate, and the modifier is H2SO4 (concentrated sulfuric acid).

[0011] Further preferably, the dosages of the inhibitor and modifier in step S3 are 6.0-7.0 kg / t and 0.01-0.03 kg / t, respectively. Even more preferably, the dosages of the inhibitor and modifier are 6.5 kg / t and 0.02 kg / t, respectively. In this invention, kg / t refers to the mass (kg) of the inhibitor, modifier, concentrated sulfuric acid, xanthate, or No. 2 oil added to each ton of ore to be treated. Xanthate refers to a sulfide ore collector.

[0012] Preferably, when the grade of the raw ore is ≤27%±3% (low grade ore), the refining process described in step S3 is four-stage refining; when the grade of the raw ore is >27%±3% (high grade ore), the refining process described in step S3 is three-stage refining.

[0013] Further optimization, the specific steps of the four-stage refining process in step S3 are as follows: after merging rough concentrate I and rough concentrate ⅠⅠ, xanthate and No. 2 oil are added for the first refining to obtain refined concentrate I and refined middlings I. Refined concentrate I is then subjected to a second refining to obtain refined concentrate ⅠⅠ and refined middlings ⅠⅠ. Refined concentrate ⅠⅠ is added to xanthate for the third refining to obtain refined concentrate ⅠⅠⅠ and refined middlings ⅠⅠⅠ. Refined middlings ⅠⅠ are combined with rough concentrate I and rough concentrate ⅠⅠ for the first refining. Refined concentrate ⅠⅠⅠ is then subjected to a fourth refining to obtain sulfur concentrate and refined tailings, wherein the grade of the sulfur concentrate is ≥48%. Refined middlings ⅠⅠⅠ are mixed with refined concentrate I for the second refining. Refined tailings are mixed with refined concentrate ⅠⅠ for the third refining.

[0014] Further optimization involves combining middlings I and scavenged tailings I with rough middlings I for a second roughing process.

[0015] Further optimization, the specific steps of the three-stage refining process in step S3 are as follows: after merging rough concentrate I and rough concentrate ⅠⅠ, xanthate and No. 2 oil are added for the first refining to obtain refined concentrate I and refined middlings I. Refined concentrate I is then subjected to a second refining to obtain refined concentrate ⅠⅠ and refined middlings ⅠⅠ. Refined concentrate ⅠⅠ is added to xanthate for the third refining to obtain sulfur concentrate and refined tailings. The grade of the sulfur concentrate is ≥48%. Refined middlings ⅠⅠ is combined with rough concentrate I and rough concentrate ⅠⅠ for the first refining. Refined tailings are mixed with refined concentrate I for the second refining.

[0016] For further optimization, the dosage of xanthate and No. 2 oil added in the first selection is 0.3-0.5 kg / t, and the dosage of xanthate added in the third selection is 0.5-0.7 kg / t. No reagents are added in the second and fourth selections. For an even further optimization, the dosage of xanthate and No. 2 oil added in the first selection is 0.4 kg / t, and the dosage of xanthate added in the third selection is 0.6 kg / t.

[0017] Further optimization involves the following steps: in step S3, the amounts of concentrated sulfuric acid, xanthate, and No. 2 oil added in the first roughing stage are 0.5-0.7 kg / t, 0.3-0.5 kg / t, and 0.06-0.08 kg / t, respectively; in the second roughing stage, the amount of xanthate added is 0.5-0.7 kg / t; in the first scavenging stage, the amounts of concentrated sulfuric acid, xanthate, and No. 2 oil added are 0.5-0.7 kg / t, 0.3-0.5 kg / t, and 0.04-0.06 kg / t, respectively; and no reagents are added in the second scavenging stage. In a further optimization step, the amounts of concentrated sulfuric acid, xanthate, and No. 2 oil added in the first roughing stage in step S3 are 0.6 kg / t, 0.4 kg / t, and 0.07 kg / t, respectively. The amount of xanthate added in the second roughing stage is 0.6 kg / t. The amounts of concentrated sulfuric acid, xanthate, and No. 2 oil added in the first scavenging stage are 0.6 kg / t, 0.4 kg / t, and 0.05 kg / t, respectively. No reagents are added in the second scavenging stage.

[0018] Preferably, after the tailings slurry in step S3 is separated by sedimentation, the solid material undergoes a first roughing process to obtain rough concentrate I and rough medium concentrate I. Rough medium concentrate I then undergoes a second roughing process to obtain rough concentrate ⅠⅠ and tailings. The grade of the tailings is ≤3%. Rough concentrate I and rough concentrate ⅠⅠ are combined for further refining to obtain refined concentrate and refined tailings. The refined concentrate enters the slurry pool for flotation treatment in step S3. The refined tailings are combined with the solid material for the first roughing process.

[0019] Compared with the prior art, the beneficial effects of the present invention are:

[0020] 1. This invention explores the influence of different pH values ​​on mineral processing technical indicators and determines a reasonable reagent system; under existing grinding conditions, pH is adjusted by H2SO4 to activate the properties of the pulp and improve the flotation effect.

[0021] 2. Based on existing process parameters, reagent system, experience, and methods, the existing process of the flotation system will be technically upgraded. The flotation production process of the lean ore line will be upgraded from "two roughers, two cleaners, and two scavengers" to "two roughers, four cleaners, and two scavengers"; the flotation production process of the rich ore line will be upgraded from "two roughers, one cleaner, and one scavenger" to "two roughers, three cleaners, and two scavengers"; and the high-quality sulfur concentrate with a grade of ≥48% will be stably produced with a theoretical recovery rate of ≥90%.

[0022] 3. The present invention adds a tailings desulfurization system, which reduces the tailings content to below 3% through tailings re-selection desulfurization technology, significantly reducing the tailings grade and improving the mineral processing recovery rate on the original basis.

[0023] 4. This invention explores the formulation of flotation reagents, conducts reagent type experiments, uses a new reagent, ethyl thiocyanate, reduces the amount of flotation reagents used, and changes the flotation reagent system. Attached Figure Description

[0024] Figure 1 The above are process flow diagrams for embodiments 1-3 of the present invention.

[0025] Figure 2 This is a process flow diagram of embodiments 4-8 of the present invention.

[0026] Figure 3 The above is a flotation flow chart of the tailings desulfurization system in Examples 1-8. Detailed Implementation

[0027] The present invention will be further described in detail below with reference to the embodiments. These embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Experimental methods in the following embodiments that do not specify specific conditions are generally performed under conventional conditions in the art or as recommended by the manufacturer; the raw materials and reagents used, unless otherwise specified, are considered to be commercially available materials and reagents that can be obtained through conventional markets and other commercial channels.

[0028] Example 1

[0029] Reference Figure 1 and Figure 3 A high-recovery, high-grade sulfur concentrate production process includes the following steps:

[0030] S1. Crush the raw ore (grade 27% ± 3%) to below 200 mesh;

[0031] S2. Add water to the crushed ore to make a slurry with an ore mass concentration of 40%, and use concentrated sulfuric acid to adjust the pH of the slurry to 5-6, and soak and stir thoroughly.

[0032] S3. First, add 6.5 kg / t of sodium hexametaphosphate and 0.02 kg / t of concentrated sulfuric acid (the amount of sodium hexametaphosphate or concentrated sulfuric acid added depends on the mass of the slurry) to the stirred slurry. After stirring evenly, add concentrated sulfuric acid, xanthate, and No. 2 oil for the first roughing. The dosages of concentrated sulfuric acid, xanthate, and No. 2 oil are 0.6 kg / t, 0.4 kg / t, and 0.07 kg / t, respectively (the dosages of concentrated sulfuric acid, xanthate, and No. 2 oil added depend on the mass of the slurry). This yields roughing concentrate I and roughing middlings I. Add 0.6 kg / t of xanthate to roughing middlings I for the second roughing to obtain roughing concentrate ⅠⅠ and roughing tailings. Combine roughing concentrate I and roughing concentrate ⅠⅠ, then add 0.4 kg / t of xanthate and 0.4 kg / t of No. 2 oil for the first cleaning to obtain cleaned concentrate I and cleaned middlings I. Cleaned concentrate I then undergoes a second cleaning to obtain... The process involves selecting concentrate ⅠⅠ and middlings ⅠⅠ. The concentrate ⅠⅠ is then treated with 0.6 kg / t xanthate for a third cleaning process to obtain selected concentrate ⅠⅠⅠ and selected middlings ⅠⅠⅠ. The middlings ⅠⅠ is then combined with the rougher concentrate Ⅰ and rougher concentrate ⅠⅠ for a first cleaning process. The selected concentrate ⅠⅠⅠ undergoes a fourth cleaning process to obtain sulfur concentrate and selected tailings. The sulfur concentrate has a grade of 40% and a recovery rate of 85%. The middlings ⅠⅠⅠ is mixed with the selected concentrate Ⅰ for a second cleaning process. The selected tailings are then mixed with the selected concentrate ⅠⅠ for a third cleaning process. The rougher tailings are treated with concentrated sulfuric acid, xanthate, and No. 2 oil for a first scavenging process to obtain scavenged tailings Ⅰ and scavenged middlings Ⅰ. The amounts of concentrated sulfuric acid, xanthate, and No. 2 oil used are 0.6 kg / t, 0.4 kg / t, and 0.05 kg / t, respectively. The scavenged middlings Ⅰ undergoes a second scavenging process to obtain scavenged tailings ⅠⅠ, which is the tailings slurry. The middlings I and scavenged tailings I are then combined with the roughing middlings I for a second roughing process.

[0033] The solid material undergoes a first roughing process to obtain rough concentrate I and rough medium ore I. Rough medium ore I then undergoes a second roughing process to obtain rough concentrate 1I and tailings. The grade of the tailings is ≤3%. Rough concentrate I and rough concentrate 1I are combined for further refining to obtain refined concentrate and refined tailings. The refined concentrate enters the slurry pool for flotation treatment in step S3. The refined tailings are combined with the solid material for the first roughing process.

[0034] Example 2

[0035] Similar to Example 1, except that the dosages of inhibitor and modifier were 6.0 kg / t and 0.01 kg / t, respectively; the dosages of xanthate and No. 2 oil added in the first fine-grained stage were both 0.3 kg / t; and the dosage of xanthate added in the third fine-grained stage was 0.5 kg / t. In the first roughing stage, the dosages of concentrated sulfuric acid, xanthate, and No. 2 oil were 0.5 kg / t, 0.3 kg / t, and 0.06 kg / t, respectively; in the second roughing stage, the dosage of xanthate was 0.5 kg / t; and in the first scavenging stage, the dosages of concentrated sulfuric acid, xanthate, and No. 2 oil were 0.5 kg / t, 0.3 kg / t, and 0.04 kg / t, respectively. The recovery rate was 85%, and the sulfur concentrate grade was 46.73%.

[0036] Example 3

[0037] Similar to Example 1, except that the dosages of inhibitor and modifier were 7.0 kg / t and 0.03 kg / t, respectively; the dosages of xanthate and No. 2 oil added in the first fine-grained stage were both 0.5 kg / t; and the dosage of xanthate added in the third fine-grained stage was 0.7 kg / t. In the first roughing stage, the dosages of concentrated sulfuric acid, xanthate, and No. 2 oil were 0.7 kg / t, 0.5 kg / t, and 0.08 kg / t, respectively; in the second roughing stage, the dosage of xanthate was 0.7 kg / t; and in the first scavenging stage, the dosages of concentrated sulfuric acid, xanthate, and No. 2 oil were 0.7 kg / t, 0.5 kg / t, and 0.06 kg / t, respectively. The recovery rate was 88%, and the sulfur concentrate grade was 47.73%.

[0038] Example 4

[0039] Reference Figure 2 and Figure 3 A high-recovery, high-grade sulfur concentrate production process includes the following steps:

[0040] S1. Crush the raw ore (grade 31.5% ± 3%) to below 200 mesh;

[0041] S2. Add water to the crushed ore to make a slurry with an ore mass concentration of 32%, and use concentrated sulfuric acid to adjust the pH of the slurry to 5-6, and soak and stir thoroughly.

[0042] S3. First, add 6.5 kg / t of sodium hexametaphosphate and 0.02 kg / t of concentrated sulfuric acid to the stirred slurry (the amount of sodium hexametaphosphate or concentrated sulfuric acid added depends on the mass of the slurry). After stirring evenly, add concentrated sulfuric acid, xanthate, and No. 2 oil for the first roughing process. The amounts of concentrated sulfuric acid, xanthate, and No. 2 oil are 0.6 kg / t, 0.4 kg / t, and 0.07 kg / t, respectively (the amounts of concentrated sulfuric acid, xanthate, and No. 2 oil added depend on the mass of the slurry). This yields roughing concentrate I and roughing medium concentrate I. Add 0.6 kg / t of xanthate to roughing medium concentrate I for the second roughing process to obtain roughing concentrate ⅠⅠ and roughing tailings. Combine roughing concentrate I and roughing concentrate ⅠⅠ and add 0.4 kg / t of xanthate. The first cleaning process involves mixing t of xanthate and 0.4 kg / t of No. 2 oil to obtain refined concentrate I and refined middlings I. Refined concentrate I undergoes a second cleaning process to obtain refined concentrate ⅠⅠ and refined middlings ⅠⅠ. Refined concentrate ⅠⅠ is then mixed with xanthate for a third cleaning process to obtain sulfur concentrate and refined tailings. The sulfur concentrate has a grade of 48.12% and a recovery rate of 90%. Refined middlings ⅠⅠ is combined with rougher concentrate I and rougher concentrate ⅠⅠ for a first cleaning process. Refined tailings are mixed with refined concentrate I for a second cleaning process. Rougher tailings are added with concentrated sulfuric acid, xanthate, and No. 2 oil for a first scavenging process to obtain scavenged tailings I and scavenged middlings I. Scavenged middlings I undergo a second scavenging process to obtain scavenged tailings ⅠⅠ, which is the tailings slurry. Refined middlings I and scavenged tailings I are then combined with rougher middlings I for a second roughing process.

[0043] The solid material undergoes a first roughing process to obtain rough concentrate I and rough medium ore I. Rough medium ore I then undergoes a second roughing process to obtain rough concentrate 1I and tailings. The grade of the tailings is ≤3%. Rough concentrate I and rough concentrate 1I are combined for further refining to obtain refined concentrate and refined tailings. The refined concentrate enters the slurry pool for flotation treatment in step S3. The refined tailings are combined with the solid material for the first roughing process.

[0044] Example 5

[0045] Similar to Example 4, except that the dosages of inhibitor and modifier were 6.0 kg / t and 0.01 kg / t, respectively; the dosages of xanthate and No. 2 oil added in the first fine-grained stage were both 0.3 kg / t; and the dosage of xanthate added in the third fine-grained stage was 0.5 kg / t. In the first roughing stage, the dosages of concentrated sulfuric acid, xanthate, and No. 2 oil were 0.5 kg / t, 0.3 kg / t, and 0.06 kg / t, respectively; in the second roughing stage, the dosage of xanthate was 0.5 kg / t; and in the first scavenging stage, the dosages of concentrated sulfuric acid, xanthate, and No. 2 oil were 0.5 kg / t, 0.3 kg / t, and 0.04 kg / t, respectively. The recovery rate was 76%, and the sulfur concentrate grade was 47.97%.

[0046] Example 6

[0047] Similar to Example 4, except that the dosages of inhibitor and modifier were 7.0 kg / t and 0.03 kg / t, respectively; the dosages of xanthate and No. 2 oil added in the first fine-grained stage were both 0.5 kg / t; and the dosage of xanthate added in the third fine-grained stage was 0.7 kg / t. In the first roughing stage, the dosages of concentrated sulfuric acid, xanthate, and No. 2 oil were 0.7 kg / t, 0.5 kg / t, and 0.08 kg / t, respectively; in the second roughing stage, the dosage of xanthate was 0.7 kg / t; and in the first scavenging stage, the dosages of concentrated sulfuric acid, xanthate, and No. 2 oil were 0.7 kg / t, 0.5 kg / t, and 0.06 kg / t, respectively. The recovery rate was 86%, and the sulfur concentrate grade was 47.66%.

[0048] Example 7

[0049] Similar to Example 4, except that: the pulp concentration was 35%; the dosages of inhibitor and modifier were 6.0 kg / t and 0.01 kg / t, respectively; the dosages of xanthate and No. 2 oil added in the first cleaning were both 0.3 kg / t; and the dosage of xanthate added in the third cleaning was 0.5 kg / t. In the first roughing stage, the dosages of concentrated sulfuric acid, xanthate, and No. 2 oil were 0.5 kg / t, 0.3 kg / t, and 0.06 kg / t, respectively; in the second roughing stage, the dosage of xanthate was 0.5 kg / t; and in the first scavenging stage, the dosages of concentrated sulfuric acid, xanthate, and No. 2 oil were 0.5 kg / t, 0.3 kg / t, and 0.04 kg / t, respectively. The recovery rate was 80%, and the sulfur concentrate grade was 47.68%.

[0050] Example 8

[0051] Similar to Example 4, except that: the pulp concentration was 42%; the dosages of inhibitor and modifier were 7.0 kg / t and 0.03 kg / t, respectively; the dosages of xanthate and No. 2 oil added in the first cleaning were both 0.5 kg / t; and the dosage of xanthate added in the third cleaning was 0.7 kg / t. In the first roughing stage, the dosages of concentrated sulfuric acid, xanthate, and No. 2 oil were 0.7 kg / t, 0.5 kg / t, and 0.08 kg / t, respectively; in the second roughing stage, the dosage of xanthate was 0.7 kg / t; and in the first scavenging stage, the dosages of concentrated sulfuric acid, xanthate, and No. 2 oil were 0.7 kg / t, 0.5 kg / t, and 0.06 kg / t, respectively. The recovery rate was 83%, and the sulfur concentrate grade was 47.88%.

[0052] The above description of the embodiments is only for the purpose of helping to understand the technical solution and core idea of ​​the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principle of the present invention, and these improvements and modifications also fall within the protection scope of the claims of the present invention.

Claims

1. A high-recovery, high-grade sulfur concentrate production process, characterized in that, Includes the following steps: S1. Crush the raw ore to below 200 mesh; S2. Add water to the crushed ore to make a slurry with an ore mass concentration of 30% to 45%, adjust the pH of the slurry to 5 to 6, and soak and stir thoroughly. S3. After stirring, first add inhibitors and modifiers to the slurry and stir evenly. Then add concentrated sulfuric acid, xanthate, and No. 2 oil for the first roughing process, obtaining roughing concentrate I and roughing medium ore I. Add xanthate to roughing medium ore I for a second roughing process, obtaining roughing concentrate ⅠⅠ and roughing tailings. Combine roughing concentrate I and roughing concentrate ⅠⅠ for several cleaning processes, obtaining sulfur concentrate. Add concentrated sulfuric acid, xanthate, and No. 2 oil to the roughing tailings for the first scavenging process, obtaining scavenging tailings I and scavenging medium ore I. Ore I undergoes a second scavenging process to obtain scavenged tailings ⅠⅠ, which is tailings slurry. After sedimentation and separation, the solid matter in the tailings slurry undergoes a first roughing process to obtain rough concentrate I and rough medium concentrate I. Rough medium concentrate I undergoes a second roughing process to obtain rough concentrate ⅠⅠ and tailings. The grade of the tailings is ≤3%. Rough concentrate I and rough concentrate ⅠⅠ are combined for further refining to obtain refined concentrate and refined tailings. The refined concentrate enters the slurry pool for flotation treatment in step S3. The refined tailings are combined with the solid matter for the first roughing process.

2. The sulfur concentrate production process according to claim 1, characterized in that, The inhibitor mentioned in step S3 is sodium hexametaphosphate, and the modifier is H2SO4.

3. The sulfur concentrate production process according to claim 1 or 2, characterized in that, In step S3, the dosages of the inhibitor and the modulator are 6.0-7.0 kg / t and 0.01-0.03 kg / t, respectively.

4. The sulfur concentrate production process according to claim 1, characterized in that, When the grade of the raw ore is ≤27%±3%, the refining process described in step S3 is four-stage refining; when the grade of the raw ore is >27%±3%, the refining process described in step S3 is three-stage refining.

5. The sulfur concentrate production process according to claim 4, characterized in that, The specific steps of the four-stage refining process described in step S3 are as follows: after merging rough concentrate I and rough concentrate ⅠⅠ, xanthate and No. 2 oil are added for the first refining to obtain refined concentrate I and refined middlings I. Refined concentrate I is then subjected to a second refining to obtain refined concentrate ⅠⅠ and refined middlings ⅠⅠ. Refined concentrate ⅠⅠ is then added to xanthate for a third refining to obtain refined concentrate ⅠⅠⅠ and refined middlings ⅠⅠⅠ. Refined middlings ⅠⅠ are then combined with rough concentrate I and rough concentrate ⅠⅠ for the first refining. Refined concentrate ⅠⅠⅠ is then subjected to a fourth refining to obtain sulfur concentrate and refined tailings. The grade of the sulfur concentrate is ≥48%. Refined middlings ⅠⅠⅠ are mixed with refined concentrate I for the second refining. Refined tailings are mixed with refined concentrate ⅠⅠ for the third refining.

6. The sulfur concentrate production process according to claim 5, characterized in that, The middlings I and scavenged tailings I are then combined with the roughing middlings I for a second roughing process.

7. The sulfur concentrate production process according to claim 4, characterized in that, The specific steps of the three-stage refining process described in step S3 are as follows: after merging rough concentrate I and rough concentrate ⅠⅠ, xanthate and No. 2 oil are added for the first refining to obtain refined concentrate I and refined middlings I. Refined concentrate I is then subjected to a second refining to obtain refined concentrate ⅠⅠ and refined middlings ⅠⅠ. Refined concentrate ⅠⅠ is added to xanthate for the third refining to obtain sulfur concentrate and refined tailings. The grade of the sulfur concentrate is ≥48%. Refined middlings ⅠⅠ is combined with rough concentrate I and rough concentrate ⅠⅠ for the first refining. Refined tailings are mixed with refined concentrate I for the second refining.

8. The sulfur concentrate production process according to claim 5 or 7, characterized in that, The dosage of xanthate and No. 2 oil added in the first selection was 0.3-0.5 kg / t, the dosage of xanthate added in the third selection was 0.5-0.7 kg / t, and no reagents were added in the second and fourth selections.

9. The sulfur concentrate production process according to claim 1, characterized in that, In step S3, the amounts of concentrated sulfuric acid, xanthate, and No. 2 oil added in the first roughing stage are 0.5-0.7 kg / t, 0.3-0.5 kg / t, and 0.06-0.08 kg / t, respectively. The amount of xanthate added in the second roughing stage is 0.5-0.7 kg / t. The amounts of concentrated sulfuric acid, xanthate, and No. 2 oil added in the first scavenging stage are 0.5-0.7 kg / t, 0.3-0.5 kg / t, and 0.04-0.06 kg / t, respectively. No reagents are added in the second scavenging stage.

Citation Information

Patent Citations

  • Method for producing high-grade sulfur concentrated ore from sulfurous iron ore with stepped flotation method

    CN102357422A

  • Method for separating copper and molybdenum from slime-containing sulfur-containing low-grade copper-molybdenum ore

    CN107971124A