Method for preparing spherical composite agglomerate abrasive for silicon carbide wafer thinning grinding wheel
By preparing spherical composite deposited abrasives and utilizing the chemical bonding of diamond, white corundum, and ceramic binders, the performance deficiencies of existing silicon carbide wafer thinning abrasives have been solved, achieving high-efficiency processing and long-life silicon carbide wafer thinning abrasives.
Patent Information
- Application Number
- CN202411766030.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-12-03
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-12-03
AI Technical Summary
Existing abrasives used for silicon carbide wafer thinning grinding wheels cannot achieve characteristics such as good sphericity, large cutting force, and good self-sharpening properties, resulting in low processing efficiency and short lifespan.
A mixture of diamond abrasive, white fused alumina abrasive, and ceramic binder is used. After uniform mixing, centrifugal spray granulation, and sintering, spherical composite abrasive is formed. The white fused alumina abrasive and the ceramic binder form chemical bonds through Al2O3 melting and infiltration, which enhances the bonding strength.
It improves the sphericity and compressive strength of the abrasive, extends the service life of the grinding wheel, improves the processing efficiency and surface quality of silicon carbide wafers, and the process is simple and easy to automate.
Smart Images

Figure CN119458169B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of ultra-precision thinning technology for silicon carbide wafers, and more particularly to a method for preparing spherical composite deposited abrasive for silicon carbide wafer thinning grinding wheels. Background Technology
[0002] With the rapid development of the information industry, semiconductor materials have also been upgraded. Third-generation semiconductor materials, represented by silicon carbide, have become the mainstream choice for high-temperature, high-frequency, radiation-resistant, and high-power devices due to their wider bandgap, higher breakdown electric field, thermal conductivity, electron saturation velocity, and radiation resistance.
[0003] In the manufacturing process of silicon carbide-based semiconductor chips, wafer spin-jet thinning is one of the key steps. Rapid wafer thinning reduces package mounting height, chip package size, improves thermal diffusion efficiency, electrical performance, and mechanical properties, and reduces dicing workload. Ceramic-bonded diamond grinding wheels, used for silicon carbide wafer thinning, are manufactured through mixing, molding, and sintering of abrasives, binders, and auxiliary materials. However, these wheels have low processing efficiency and short lifespan. Considering the material properties of silicon carbide, to achieve high wafer surface quality, improve grinding efficiency, and extend wheel life during silicon carbide wafer thinning, the abrasive used in the grinding wheel needs to possess characteristics such as good sphericity, high cutting force, and good self-sharpening properties. However, existing abrasives used in silicon carbide wafer thinning wheels cannot achieve these characteristics.
[0004] Therefore, there is a need to provide a method for preparing spherical composite deposited abrasive for silicon carbide wafer thinning grinding wheels to solve the above-mentioned technical problems. Summary of the Invention
[0005] This invention provides a method for preparing spherical composite deposited abrasive for silicon carbide wafer thinning grinding wheels, in order to solve or at least alleviate the problems mentioned above.
[0006] According to one aspect of the present invention, a method for preparing spherical composite abrasive for silicon carbide wafer thinning grinding wheels is provided, comprising: obtaining a variety of dry raw materials according to a first ratio, and uniformly mixing the variety of dry raw materials to obtain a mixed dry material, wherein the variety of dry raw materials includes diamond abrasive, white corundum abrasive, and ceramic binder; uniformly mixing the mixed dry material with a dispersant, a thickener, and purified water according to a second ratio to obtain a slurry; centrifugally spray-granulating the slurry and drying it to obtain a composite abrasive green; and sintering the composite abrasive green to obtain spherical composite abrasive.
[0007] Optionally, in the preparation method of the spherical composite deposited abrasive for silicon carbide wafer thinning grinding wheel according to the present invention, the first ratio includes the mass percentage of each dry raw material, wherein the mass percentage of diamond abrasive is 50-70%, the mass percentage of white corundum abrasive is 15-25%, and the mass percentage of ceramic binder is 15-25%.
[0008] Optionally, in the preparation method of the spherical composite deposited abrasive for silicon carbide wafer thinning grinding wheel according to the present invention, the second ratio includes the mass percentages of mixed dry materials, dispersant, thickener, and purified water, wherein the mass percentage of the mixed dry materials is 20-40%, the mass percentage of the dispersant is 1-3%, the mass percentage of the thickener is 1-5%, and the mass percentage of the purified water is 56-74%.
[0009] Optionally, in the method for preparing spherical composite deposited abrasive for silicon carbide wafer thinning grinding wheels according to the present invention, the multiple dry raw materials are uniformly mixed to obtain a mixed dry material, including: using a mechanical ball milling method to continuously mix the multiple dry raw materials for a first predetermined time, and then sieving to obtain the mixed dry material.
[0010] Optionally, in the preparation method of the spherical composite deposited abrasive for silicon carbide wafer thinning grinding wheel according to the present invention, the mixed dry material is uniformly mixed with dispersant, thickener and pure water to obtain a slurry, including: using an ultrasonic mechanical composite dispersion method to continuously wet mix the mixed dry material, dispersant, thickener and pure water for a second predetermined time to obtain the slurry.
[0011] Optionally, in the method for preparing spherical composite abrasive for silicon carbide wafer thinning grinding wheels according to the present invention, the slurry is centrifugally spray-granulated and dried to obtain a composite abrasive green blank, comprising: using a centrifugal spray dryer to centrifugally spray-granulate the slurry based on a predetermined centrifugal speed and a predetermined feed rate, and drying based on a drying temperature to obtain a composite abrasive green blank.
[0012] Optionally, in the method for preparing spherical composite deposited abrasive for silicon carbide wafer thinning grinding wheels according to the present invention, the predetermined centrifugal speed is 10000-30000 rpm, the predetermined feed rate is 30-50 ml / min, and the drying temperature is 160-200℃.
[0013] Optionally, in the method for preparing spherical composite abrasive for silicon carbide wafer thinning grinding wheels according to the present invention, sintering the composite abrasive green blank to obtain spherical composite abrasive includes: heating to a sintering temperature based on a predetermined heating rate to sinter the composite abrasive green blank, and holding at the sintering temperature for a third predetermined time to obtain spherical composite abrasive.
[0014] Optionally, in the method for preparing spherical composite deposited abrasive for silicon carbide wafer thinning grinding wheels according to the present invention, the predetermined heating rate is 4°C / min, the sintering temperature is 650-750°C, and the third predetermined duration is 30-60min.
[0015] Optionally, in the method for preparing spherical composite abrasive for silicon carbide wafer thinning grinding wheels according to the present invention, the particle size of the spherical composite abrasive is 30-60 μm.
[0016] Optionally, in the preparation method of the spherical composite deposited abrasive for silicon carbide wafer thinning grinding wheel according to the present invention, the particle size of the diamond abrasive is W0.5-W7.5, the particle size of the white corundum abrasive is W0.5-W3, and the particle size of the ceramic binder is W1-W5.
[0017] Optionally, in the method for preparing spherical composite deposited abrasive for silicon carbide wafer thinning grinding wheels according to the present invention, the ceramic binder is a SiO2-B2O3-Al2O3 glass.
[0018] Optionally, in the method for preparing spherical composite deposited abrasive for silicon carbide wafer thinning grinding wheels according to the present invention, the dispersant is an ammonium salt or an organic polymer.
[0019] Optionally, in the method for preparing spherical composite deposited abrasive for silicon carbide wafer thinning grinding wheels according to the present invention, the thickener is alginic acid, hydroxypropyl starch or alum.
[0020] Optionally, in the method for preparing spherical composite deposited abrasive for silicon carbide wafer thinning grinding wheels according to the present invention, the interface between the white fused alumina abrasive and the ceramic binder in the spherical composite deposited abrasive is adapted to produce Al2O3 melting and infiltration phenomenon, so that the mechanical bond between the white fused alumina abrasive and the ceramic binder is transformed into a chemical bond.
[0021] According to the technical solution of the present invention, a method for preparing spherical composite abrasive for thinning silicon carbide wafers is provided. Diamond abrasive, white fused alumina abrasive, and a ceramic binder are obtained according to a first ratio and uniformly mixed to obtain a mixed dry material. Subsequently, the mixed dry material is uniformly mixed with a dispersant, a thickener, and purified water according to a second ratio to obtain a slurry. The slurry is then centrifugally spray-granulated, dried, and sintered to obtain a composite abrasive green. Thus, the spherical composite abrasive prepared according to the method of the present invention has better sphericity. Moreover, due to the Al2O3 melting phenomenon at the interface between the white fused alumina abrasive and the ceramic binder, the simple mechanical bond between the white fused alumina abrasive and the ceramic binder is transformed into a stronger chemical bond. This enhances the binder's holding force on the diamond, resulting in higher compressive strength and impact resistance of the final prepared spherical composite abrasive, thereby improving the abrasive's self-sharpening property and its grinding force on silicon carbide wafers. Secondly, the silicon carbide wafer thinning grinding wheel prepared based on this spherical composite abrasive can extend the wheel's service life, improve the wheel's processing efficiency on silicon carbide wafers, and simultaneously improve the wafer surface quality. Furthermore, the present invention uses a centrifugal spray granulation process to ensure that the final prepared spherical composite abrasive is spherical with uniform particle size, good flowability, and is not prone to agglomeration. The process for preparing grinding wheels based on this spherical composite abrasive is simple to operate, improves mixing uniformity, and ensures stable slurry flowability, which is beneficial for automated production.
[0022] The above description is merely an overview of the technical solution of the present invention. In order to better understand the technical means of the present invention and to implement it in accordance with the contents of the specification, and in order to make the above and other objects, features and advantages of the present invention more apparent and understandable, specific embodiments of the present invention are described below. Attached Figure Description
[0023] To achieve the foregoing and related objectives, certain illustrative aspects are described herein in conjunction with the following description and accompanying drawings. These aspects indicate various ways in which the principles disclosed herein may be practiced, and all aspects and their equivalents are intended to fall within the scope of the claimed subject matter. The foregoing and other objectives, features, and advantages of this disclosure will become more apparent from the following detailed description, taken in conjunction with the accompanying drawings. Throughout this disclosure, the same reference numerals generally refer to the same parts or elements.
[0024] Figure 1 A schematic flowchart of a method 100 for preparing a spherical composite deposited abrasive for a silicon carbide wafer thinning grinding wheel according to an embodiment of the present invention is shown. Detailed Implementation
[0025] Exemplary embodiments of the present disclosure will now be described in more detail with reference to the accompanying drawings. While exemplary embodiments of the present disclosure are shown in the drawings, it should be understood that the present disclosure may be implemented in various forms and should not be limited to the embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the disclosure to those skilled in the art.
[0026] To address the shortcomings of existing grinding wheels and abrasives in silicon carbide wafer thinning, this invention provides a method 100 for preparing a spherical composite abrasive for silicon carbide wafer thinning grinding wheels. The spherical composite abrasive prepared by the method 100 of this invention exhibits better sphericity, higher compressive strength, and higher impact strength, thereby improving the abrasive's self-sharpening properties and its grinding force on silicon carbide wafers. The silicon carbide wafer thinning grinding wheel prepared based on this spherical composite abrasive can extend the grinding wheel's service life, improve the grinding wheel's processing efficiency on silicon carbide wafers, and simultaneously improve the wafer surface quality.
[0027] Figure 1 A schematic flowchart of a method 100 for preparing a spherical composite deposited abrasive for a silicon carbide wafer thinning grinding wheel according to an embodiment of the present invention is shown.
[0028] The following will combine Figure 1 The following describes in detail the preparation method 100 of the spherical composite deposited abrasive for silicon carbide wafer thinning grinding wheel of the present invention.
[0029] It should be noted that the spherical composite abrasive prepared by the method 100 for preparing spherical composite abrasive for silicon carbide wafer thinning grinding wheels according to the present invention can be used to prepare silicon carbide wafer thinning grinding wheels. Specifically, the silicon carbide wafer thinning grinding wheel in the embodiments of the present invention is a ceramic-bonded diamond grinding wheel used for thinning silicon carbide wafers.
[0030] like Figure 1 As shown, the preparation method 100 of the spherical composite deposited abrasive for silicon carbide wafer thinning grinding wheel includes the following steps 110 to 140.
[0031] First, in step 110, various dry material raw materials are obtained according to the first ratio, and the various dry material raw materials are uniformly mixed to obtain a mixed dry material. Among them, the various dry material raw materials include diamond abrasive, white corundum abrasive, and ceramic binder.
[0032] It should be noted that the first ratio (i.e., the dry material ratio) includes the mass percentage of each dry material. In other words, in step 110, the corresponding mass of diamond abrasive, white fused alumina abrasive, and ceramic binder can be weighed according to the mass percentage of each dry material. In some embodiments, the mass percentage of diamond abrasive can be 50-70%, the mass percentage of white fused alumina abrasive can be 15-25%, and the mass percentage of ceramic binder can be 15-25%.
[0033] In some embodiments, the diamond abrasive in step 110 has a particle size of W0.5-W7.5, the white corundum abrasive has a particle size of W0.5-W3, and the ceramic binder has a particle size of W1-W5. Optionally, the ceramic binder can be a SiO2-B2O3-Al2O3 glass.
[0034] In some embodiments, in step 110, a ball mill can be used to continuously mix multiple dry raw materials for a first predetermined time using a mechanical ball milling method. Afterward, the mixed multiple dry raw materials are sieved to obtain a mixed dry material. In some specific embodiments, the first predetermined time can be, for example, 1 hour. That is, a mechanical ball milling method can be used to continuously mix multiple dry raw materials for 1 hour, and then the mixed multiple dry raw materials can be sieved through a 40# sieve to obtain the mixed dry material.
[0035] Subsequently, in step 120, the above-mentioned mixed dry materials can be uniformly mixed with dispersant, thickener and purified water according to the second ratio to obtain slurry.
[0036] It should be understood that the above-mentioned mixed dry materials, dispersant, thickener, and purified water are all slurry components. The second ratio is also the slurry component distribution ratio.
[0037] It should be noted that the second ratio includes the mass percentages of the mixed dry materials, dispersant, thickener, and purified water. In some embodiments, the mass percentage of the mixed dry materials can be 20-40%, the mass percentage of the dispersant can be 1-3%, the mass percentage of the thickener can be 1-5%, and the mass percentage of the purified water can be 56-74%. That is, in step 120, 20-40% of the mixed dry materials, 1-3% of the dispersant, 1-5% of the thickener, and 56-74% of the purified water can be uniformly mixed to obtain a slurry.
[0038] In some embodiments, the dispersant in step 120 may be an ammonium salt or an organic polymer. The thickener may be alginic acid, hydroxypropyl starch, or alum.
[0039] In some embodiments, in step 120, an ultrasonic dispersion device can be used to employ an ultrasonic-mechanical composite dispersion method to continuously wet mix the second proportion of mixed dry materials, dispersant, thickener, and purified water (20-40% mixed dry materials, 1-3% dispersant, 1-5% thickener, and 56-74% purified water) for a second predetermined time to obtain a slurry. In some specific embodiments, the second predetermined time may be, for example, 30 minutes, that is, an ultrasonic-mechanical composite dispersion method can be used to continuously wet mix the second proportion of mixed dry materials, dispersant, thickener, and purified water for 30 minutes to obtain a slurry.
[0040] It should be noted that the ultrasonic mechanical composite dispersion method can prevent sedimentation and agglomeration during the preparation of slurry.
[0041] Next, in step 130, the slurry prepared in step 120 can be centrifugally spray-granulated and dried to obtain a composite abrasive green.
[0042] In some embodiments, in step 130, the slurry can be fed into a centrifugal spray dryer, where it is centrifugally spray-granulated based on a predetermined centrifugal speed and a predetermined feed rate, and then dried based on a drying temperature to obtain a composite abrasive green body. In some specific embodiments, the predetermined centrifugal speed can be 10,000-30,000 rpm, the predetermined feed rate can be 30-50 ml / min, and the drying temperature can be 160-200°C.
[0043] Finally, in step 140, spherical composite abrasive is obtained by sintering the composite abrasive green prepared in step 130.
[0044] In some embodiments, in step 140, during the sintering process, the temperature can be increased to a sintering temperature based on a predetermined heating rate to sinter the composite abrasive green blank, and the sintering temperature is held for a third predetermined time to finally obtain spherical composite abrasive. In some specific embodiments, the predetermined heating rate can be 4℃ / min, the sintering temperature can be 650-750℃, and the third predetermined time can be 30-60min. That is, the sintering process of the composite abrasive green blank is as follows: the temperature is increased to a sintering temperature of 650-750℃ based on a heating rate of 4℃ / min, and the sintering temperature is held for 30-60min to obtain spherical composite abrasive.
[0045] In some embodiments, the particle size of the spherical composite abrasive prepared according to the present invention can be 30-60 μm.
[0046] It should be noted that, in the spherical composite abrasive prepared according to the embodiments of the present invention, Al2O3 infiltration occurs at the interface between the white fused alumina abrasive and the ceramic binder, transforming the simple mechanical bond between the white fused alumina abrasive and the ceramic binder into a stronger chemical bond. This enhances the binder's holding force on the diamond, resulting in higher compressive strength and impact resistance of the final spherical composite abrasive, thereby improving the abrasive's self-sharpening property and its grinding force on silicon carbide wafers. Furthermore, the silicon carbide wafer thinning grinding wheel prepared based on the spherical composite abrasive of the present invention can extend its service life, improve the processing efficiency of silicon carbide wafers, and obtain wafers with high surface quality.
[0047] The following three specific embodiments (the first embodiment, the second embodiment, and the third embodiment) will be used to describe in detail the material composition and process parameters involved in the preparation of spherical composite abrasive.
[0048] In the first embodiment, the various dry raw materials used may include: diamond abrasive with a particle size of W0.5-W7.5, white corundum abrasive with a particle size of W0.5-W3, and ceramic binder with a particle size of W1-W5. The various dry raw materials and the first proportions in the first embodiment are shown in Table 1 below.
[0049] Table 1. Various dry raw materials and their first proportions in the first embodiment.
[0050] Dry raw materials Diamond abrasive White fused alumina abrasive Ceramic binder First proportion / wt% 50% 25% 25%
[0051] In the first embodiment, diamond abrasive, white corundum abrasive, and ceramic binder of the corresponding mass can be weighed according to the first ratio in Table 1 and added to the ball mill jar. 5mm hard alloy balls can be added to the ball mill jar. The ball-to-material ratio can be 2:1. Then, the various dry raw materials of the first ratio can be continuously mixed for 1 hour using a ball mill mechanical ball milling method. After that, the mixture can be passed through a 40# sieve to obtain the mixed dry material.
[0052] In the first embodiment, the dispersant in the slurry components can be an organic polymer, and the thickener can be alginic acid. That is, the mixed dry materials, organic polymer, alginic acid, and purified water can be uniformly mixed according to the second ratio to obtain the slurry. The slurry components and the second ratio in the first embodiment are specifically shown in Table 2 below.
[0053] Table 2. Slurry components and second proportions in the first embodiment.
[0054] Slurry components Mixed dry materials Organic polymers alginic acid purified water Second ratio / wt% 40% 3% 1% 56%
[0055] In the first embodiment, after obtaining the mixed dry material, the mixed dry material, organic polymer, alginic acid, and purified water can be placed into an ultrasonic dispersion device according to the second ratio in Table 2. Then, the mixture is continuously wet-mixed for 30 minutes using an ultrasonic mechanical composite dispersion method to obtain a slurry. During the wet mixing process, the rotation speed of the ultrasonic dispersion device can be controlled at 500 rpm and the ultrasonic power at 600 W.
[0056] Next, the slurry can be fed into a centrifugal spray dryer to centrifuge and dry the slurry. During this process, the centrifugal speed of the centrifugal spray dryer can be controlled at 20,000 rpm, the feed rate at 40 ml / min, the drying temperature at 200℃, and the outlet temperature at 150℃. After this process is completed, a composite abrasive green body can be obtained.
[0057] Finally, during the sintering process of the composite abrasive green, the temperature can be raised to 750℃ at a heating rate of 4℃ / min, and held at 750℃ for 60min to obtain spherical composite abrasive.
[0058] The spherical composite abrasive prepared according to the first embodiment has an average particle size of 55 μm and an average compressive strength of 4.86 MPa.
[0059] In the second embodiment, the various dry raw materials used may include: diamond abrasive with a particle size of W0.5-W7.5, white corundum abrasive with a particle size of W0.5-W3, and ceramic binder with a particle size of W1-W5. The various dry raw materials and the first proportions in the second embodiment are shown in Table 3 below.
[0060] Table 3 shows the various dry raw materials and their first proportions in the second embodiment.
[0061] Dry raw materials Diamond abrasive White fused alumina abrasive Ceramic binder First proportion / wt% 70% 15% 15%
[0062] In the second embodiment, diamond abrasive, white corundum abrasive, and ceramic binder of the corresponding mass can be weighed according to the first ratio in Table 3 and added to the ball mill jar. 5mm hard alloy balls can be added to the ball mill jar, and the ball-to-material ratio can be 2:1. Then, the various dry raw materials of the first ratio can be continuously mixed for 1 hour using a ball mill mechanical ball milling method, and then passed through a 40# sieve to obtain mixed dry material.
[0063] In the second embodiment, the dispersant in the slurry components can be an organic polymer, and the thickener can be alginic acid. That is, the mixed dry materials, organic polymer, alginic acid, and purified water can be uniformly mixed according to the second ratio to obtain the slurry. The slurry components and the second ratio in the second embodiment are specifically shown in Table 4 below.
[0064] Table 4. Slurry components and second proportions in the second embodiment.
[0065] Slurry components Mixed dry materials Organic polymers alginic acid purified water Second ratio / wt% 40% 3% 1% 56%
[0066] In the second embodiment, after obtaining the mixed dry material, the mixed dry material, organic polymer, alginic acid, and purified water can be placed into an ultrasonic dispersion device according to the second ratio in Table 4. Then, the mixture is continuously wet-mixed for 30 minutes using an ultrasonic mechanical composite dispersion method to obtain a slurry. During the wet mixing process, the rotation speed of the ultrasonic dispersion device can be controlled at 500 rpm and the ultrasonic power at 600 W.
[0067] Next, the slurry can be fed into a centrifugal spray dryer to centrifuge and dry the slurry. During this process, the centrifugal speed of the centrifugal spray dryer can be controlled at 20,000 rpm, the feed rate at 40 ml / min, the drying temperature at 200℃, and the outlet temperature at 150℃. After this process is completed, a composite abrasive green body can be obtained.
[0068] Finally, during the sintering process of the composite abrasive green, the temperature can be raised to 750℃ at a heating rate of 4℃ / min, and held at 750℃ for 60min to obtain spherical composite abrasive.
[0069] The spherical composite abrasive prepared according to the second embodiment has an average particle size of 55 μm and an average compressive strength of 4.41 MPa.
[0070] In the third embodiment, the various dry raw materials used may include: diamond abrasive with a particle size of W0.5-W7.5, white corundum abrasive with a particle size of W0.5-W3, and ceramic binder with a particle size of W1-W5. The various dry raw materials and the first proportions in the third embodiment are shown in Table 5 below.
[0071] Table 5 shows the various dry raw materials and their first proportions in the third embodiment.
[0072] Dry raw materials Diamond abrasive White fused alumina abrasive Ceramic binder First proportion / wt% 75% 0% 25%
[0073] In the third embodiment, diamond abrasive, white corundum abrasive, and ceramic binder of the corresponding mass can be weighed according to the first ratio in Table 5 and added to the ball mill jar. 5mm hard alloy balls can be added to the ball mill jar, and the ball-to-material ratio can be 2:1. Then, the various dry raw materials of the first ratio can be continuously mixed for 1 hour using a ball mill mechanical ball milling method, and then passed through a 40# sieve to obtain mixed dry material.
[0074] In the third embodiment, the dispersant in the slurry components can be an organic polymer, and the thickener can be alginic acid. That is, the mixed dry materials, organic polymer, alginic acid, and purified water can be uniformly mixed according to the second ratio to obtain the slurry. The slurry components and the second ratio in the third embodiment are specifically shown in Table 6 below.
[0075] Table 6. Slurry components and second proportions in the third embodiment.
[0076] Slurry components Mixed dry materials Organic polymers alginic acid purified water Second ratio / wt% 40% 3% 1% 56%
[0077] In the third embodiment, after obtaining the mixed dry material, the mixed dry material, organic polymer, alginic acid, and purified water can be placed into an ultrasonic dispersion device according to the second ratio in Table 6. Then, the mixture is continuously wet-mixed for 30 minutes using an ultrasonic mechanical composite dispersion method to obtain a slurry. During the wet mixing process, the rotation speed of the ultrasonic dispersion device can be controlled at 500 rpm and the ultrasonic power at 600 W.
[0078] Next, the slurry can be fed into a centrifugal spray dryer to centrifuge and dry the slurry. During this process, the centrifugal speed of the centrifugal spray dryer can be controlled at 20,000 rpm, the feed rate at 40 ml / min, the drying temperature at 200℃, and the outlet temperature at 150℃. After this process is completed, a composite abrasive green body can be obtained.
[0079] Finally, during the sintering process of the composite abrasive green, the temperature can be raised to 750℃ at a heating rate of 4℃ / min, and held at 750℃ for 60min to obtain spherical composite abrasive.
[0080] The spherical composite abrasive prepared according to the third embodiment has an average particle size of 55 μm and an average compressive strength of 3.58 MPa.
[0081] The above is merely a description of specific implementation examples of the present invention. It should be noted that the specific material composition and process involved in the preparation method 100 of the spherical composite deposited abrasive for silicon carbide wafer thinning grinding wheel of the present invention are not limited to the specific parameters described in the above embodiments.
[0082] It is worth noting that the main difference between the first, second, and third embodiments mentioned above lies in the different first proportions of the dry raw materials. Based on these different first proportions, the compressive strength of the final prepared spherical composite abrasive varies. Specifically, because the third embodiment did not use white corundum abrasive (0% by mass) when preparing the mixed dry materials, the compressive strength of the spherical composite abrasive prepared in the third embodiment is significantly lower than that prepared in the first and second embodiments.
[0083] Furthermore, this invention also prepared corresponding silicon carbide wafer thinning grinding wheels based on the spherical composite abrasive prepared in the first, second, and third embodiments, respectively, and conducted grinding performance tests on the silicon carbide wafer thinning grinding wheels corresponding to the first, second, and third embodiments. The specific testing method is as follows: the grinding wheel was installed on a single-station thinning machine. Taking a 6-inch conductive silicon carbide wafer as an example, the spindle speed was set to 2200 rpm, the feed rate to 141 rpm, and the feed amount to 40 μm, so that the silicon carbide wafer could be ground by the grinding wheel. Then, the roughness of the ground silicon carbide wafer was detected under a white light interferometer, and the wear of the grinding wheel after grinding was detected using a contact measuring instrument, thereby achieving the grinding performance test of the grinding wheel. The performance test results of the grinding wheels corresponding to the three embodiments are shown in Table 7 below.
[0084] Table 7. Grinding wheel performance test results
[0085]
[0086] It is evident that, because the third embodiment did not use white corundum abrasive (0% by mass) when preparing the mixed dry material, the compressive strength of the spherical composite abrasive prepared in the third embodiment is significantly lower than that of the spherical composite abrasive prepared in the first and second embodiments. Under these circumstances, the silicon carbide wafer thinning grinding wheel prepared based on the spherical composite abrasive of the third embodiment has a higher surface roughness and poorer wafer surface quality after grinding, and the grinding wheel wear is relatively high and the grinding wheel service life is low.
[0087] In summary, according to the preparation method of the spherical composite abrasive for silicon carbide wafer thinning grinding wheels of the present invention, diamond abrasive, white fused alumina abrasive, and ceramic binder are obtained according to a first ratio and uniformly mixed to obtain a mixed dry material. Subsequently, the mixed dry material is uniformly mixed with a dispersant, a thickener, and purified water according to a second ratio to obtain a slurry. The slurry is then centrifugally spray-granulated, dried, and sintered to obtain a composite abrasive green. Thus, the spherical composite abrasive prepared according to the method of the present invention has better sphericity. Moreover, due to the Al2O3 melting phenomenon at the interface between the white fused alumina abrasive and the ceramic binder, the simple mechanical bond between the white fused alumina abrasive and the ceramic binder is transformed into a stronger chemical bond. This enhances the binder's holding force on the diamond, resulting in higher compressive strength and impact strength of the final prepared spherical composite abrasive, thereby improving the abrasive's self-sharpening property and its grinding force on silicon carbide wafers. Secondly, the silicon carbide wafer thinning grinding wheel prepared based on this spherical composite abrasive can extend the wheel's service life, improve the wheel's processing efficiency on silicon carbide wafers, and simultaneously improve the wafer surface quality. Furthermore, the present invention uses a centrifugal spray granulation process to ensure that the final prepared spherical composite abrasive is spherical with uniform particle size, good flowability, and is not prone to agglomeration. The process for preparing grinding wheels based on this spherical composite abrasive is simple to operate, improves mixing uniformity, and ensures stable slurry flowability, which is beneficial for automated production.
[0088] Furthermore, embodiments of the present invention also disclose: A11, the method as described in any one of A1-A10, wherein the particle size of the diamond abrasive is W0.5-W7.5, the particle size of the white fused abrasive is W0.5-W3, and the particle size of the ceramic binder is W1-W5. A12, the method as described in any one of A1-A11, wherein the ceramic binder is a SiO2-B2O3-Al2O3 glass. A13, the method as described in any one of A1-A12, wherein the dispersant is an ammonium salt or an organic polymer. A14, the method as described in any one of A1-A13, wherein the thickener is alginic acid, hydroxypropyl starch, or alum. A15, the method as described in any one of A1-A14, wherein the interface between the white fused abrasive and the ceramic binder in the spherical composite abrasive is suitable for Al2O3 melting and infiltration, so that the mechanical bond between the white fused abrasive and the ceramic binder is transformed into a chemical bond.
[0089] Numerous specific details are set forth in the specification provided herein. However, it will be understood that embodiments of the invention may be practiced without these specific details. In some instances, well-known methods, structures, and techniques have not been shown in detail so as not to obscure the understanding of this specification.
[0090] Similarly, it should be understood that, in order to streamline this disclosure and aid in understanding one or more of the various aspects of the invention, in the above description of exemplary embodiments of the invention, various features of the invention are sometimes grouped together in a single embodiment, figure, or description thereof.
[0091] Those skilled in the art will understand that the modules, units, or components of the devices in the examples disclosed herein may be arranged in the devices described in this embodiment, or alternatively may be located in one or more devices different from the devices in this example.
[0092] Those skilled in the art will understand that the modules in the device of the embodiment can be adaptively changed and placed in one or more devices different from that embodiment. Modules, units, or components in the embodiment can be combined into a single module, unit, or component, and further, they can be divided into multiple sub-modules, sub-units, or sub-components.
[0093] Furthermore, those skilled in the art will understand that although some embodiments described herein include certain features included in other embodiments but not others, combinations of features from different embodiments are meant to be within the scope of the invention and form different embodiments.
[0094] As used herein, unless otherwise specified, the use of ordinal numbers such as “first,” “second,” “third,” etc., to describe ordinary objects merely indicates different instances of similar objects and is not intended to imply that the objects being described must have a given order in time, space, ordering, or any other manner.
[0095] Although the invention has been described with respect to a limited number of embodiments, those skilled in the art will understand from the foregoing description that other embodiments are conceivable within the scope of the invention described herein. Furthermore, it should be noted that the language used in this specification has been chosen primarily for readability and edibility purposes, and not for the purpose of explaining or limiting the subject matter of the invention.
Claims
1. A method for preparing spherical composite deposited abrasive for silicon carbide wafer thinning grinding wheels, comprising: Multiple dry raw materials are obtained according to a first ratio, and the multiple dry raw materials are uniformly mixed to obtain a mixed dry material. The multiple dry raw materials include diamond abrasive, white fused alumina abrasive, and ceramic binder. The first ratio includes the mass percentage of each dry raw material, wherein the mass percentage of diamond abrasive is 50-70%, the mass percentage of white fused alumina abrasive is 15-25%, and the mass percentage of ceramic binder is 15-25%. According to the second ratio, the mixed dry material is continuously wet-mixed with dispersant, thickener and pure water for a second predetermined time using an ultrasonic mechanical composite dispersion method to obtain a slurry; The slurry is centrifugally sprayed and granulated based on a predetermined centrifugal speed and a predetermined feed rate, and then dried based on a drying temperature to obtain a composite abrasive green body. The predetermined centrifugal speed is 10000-30000 rpm, the predetermined feed rate is 30-50 ml / min, and the drying temperature is 160-200℃. The composite abrasive green is sintered to obtain spherical composite abrasive with a particle size of 30-60 μm. The interface between the white fused alumina abrasive and the ceramic binder in the spherical composite abrasive is suitable for Al2O3 melting and infiltration, so that the mechanical bond between the white fused alumina abrasive and the ceramic binder is transformed into a chemical bond.
2. The method as described in claim 1, wherein, The second ratio includes the mass percentages of the mixed dry materials, dispersant, thickener, and purified water, wherein the mass percentage of the mixed dry materials is 20-40%, the mass percentage of the dispersant is 1-3%, the mass percentage of the thickener is 1-5%, and the mass percentage of the purified water is 56-74%.
3. The method as described in claim 1, wherein, The various dry raw materials are uniformly mixed to obtain a mixed dry material, comprising: The various dry raw materials are continuously mixed for a first predetermined time using a mechanical ball milling method, and then sieved to obtain a mixed dry material.
4. The method according to any one of claims 1-3, wherein, The composite abrasive green is sintered to obtain spherical composite abrasive, comprising: The composite abrasive green is heated to a predetermined heating rate to sinter the green material, and then held at the sintering temperature for a third predetermined duration to obtain spherical composite abrasive.
5. The method of claim 4, wherein, The predetermined heating rate is 4℃ / min, the sintering temperature is 650-750℃, and the third predetermined duration is 30-60min.
6. The method according to any one of claims 1-3, wherein, The diamond abrasive has a particle size of W0.5-W7.5, the white corundum abrasive has a particle size of W0.5-W3, and the ceramic binder has a particle size of W1-W5.
7. The method according to any one of claims 1-3, wherein, The ceramic binder is a SiO2-B2O3-Al2O3 glass.
8. The method according to any one of claims 1-3, wherein, The dispersant is an ammonium salt or an organic polymer.
9. The method according to any one of claims 1-3, wherein, The thickener is alginic acid, hydroxypropyl starch, or alum.
Citation Information
Patent Citations
Method for preparing ceramic bond stacking abrasive material through centrifugal drying granulation technology