Glazed ceramic tile and method for its production

By using base glaze and top glaze layers with different viscosities and surface tensions on ceramic tiles, a unique three-dimensional texture is formed, solving the problems of unclear patterns and complicated processes in dry granule decoration, improving the decorative effect and reducing costs.

CN119462107BActive Publication Date: 2026-11-24CHONGQING WONDERFUL CERAMICS CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411615815.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-11-13
Publication Date
2026-11-24
Estimated Expiration
2044-11-13

AI Technical Summary

Technical Problem

In existing technologies, when using dry granules to decorate ceramic tiles, the edges of the dry granule patterns are unclear and the process is cumbersome, resulting in poor three-dimensional decorative effects.

Method used

By employing different viscosities and surface tensions in the base glaze and top glaze layers, with the base glaze having a higher viscosity than the top glaze, and the top glaze exhibiting greater fluidity at high temperatures, a unique three-dimensional texture with macroscopic order and microscopic disorder is formed, simplifying the process.

Benefits of technology

It enhances the decorative effect, avoids the problem of unclear pattern edges, reduces production costs, and improves the durability and service life of ceramic tiles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119462107B_ABST
    Figure CN119462107B_ABST
Patent Text Reader

Abstract

This invention provides a glazed ceramic tile and its preparation method. The glazed ceramic tile includes: a ceramic body, a base glaze layer disposed on the ceramic body, and a top glaze layer disposed on the base glaze layer. The viscosity of the base glaze layer is greater than that of the top glaze layer, and the surface tension of the base glaze layer is greater than that of the top glaze layer. The top glaze layer of this invention has lower viscosity and surface tension, making it easier to form glaze flow. After cooling, it forms an uneven glaze surface, i.e., the top glaze layer produces a glaze flow effect on the base glaze layer, forming a unique macroscopically ordered and microscopically disordered three-dimensional texture, enhancing the decorative effect. Furthermore, it eliminates the need for printing glue patterns, avoiding the problem of unclear pattern edges, and the process is simple.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of ceramic production technology, and in particular to a glazed ceramic tile and its preparation method. Background Technology

[0002] With the upgrading of ceramic tile quality, its value extends beyond surface decoration to include more functions. Ceramic tiles with three-dimensional decorative effects are highly sought after. To enrich the surface effects of ceramic tiles, the ceramic industry has begun using dry granules for decoration. This method typically involves applying a base glaze to the surface of a plain ceramic tile, then printing a pattern using adhesive, applying dry granules over the pattern, and finally applying a protective glaze to create the tile with the dry granule decorative pattern. While this method improves the three-dimensional effect compared to conventional ceramic tiles, the edges of the dry granule pattern are prone to becoming unclear due to the direct application of dry granules onto the adhesive pattern, and the process is cumbersome, resulting in a less than ideal three-dimensional decorative effect.

[0003] Therefore, existing technologies have shortcomings and need to be improved and developed. Summary of the Invention

[0004] The technical problem to be solved by the present invention is to provide a glazed ceramic tile and its preparation method in view of the above-mentioned defects of the prior art. The aim is to solve the problems of unclear edges of dry granule patterns, complicated process and poor three-dimensional decorative effect of the tile surface in the prior art method of decorating ceramic tiles with dry granules.

[0005] The technical solution adopted by this invention to solve the technical problem is as follows:

[0006] The first aspect of this application provides a glazed ceramic tile, wherein the glazed ceramic tile includes: a ceramic body, a base glaze layer disposed on the ceramic body, and a top glaze layer disposed on the base glaze layer; the viscosity of the base glaze layer is greater than the viscosity of the top glaze layer, and the surface tension of the base glaze layer is greater than the surface tension of the top glaze layer.

[0007] Based on the aforementioned technical means, the viscosity of the glaze layer in this embodiment is relatively low. Glazes with low viscosity and high surface tension have high fluidity at high temperatures, easily causing glaze flow. When the surface tension of the glaze is also very low, glaze flow is even more likely to occur, resulting in an uneven glaze surface after cooling. In this way, the glaze layer in this embodiment produces a glaze flow effect on the base glaze layer, forming a unique macroscopically ordered and microscopically disordered three-dimensional texture, enhancing the decorative effect. Furthermore, it eliminates the need for printing glue patterns, avoiding the problem of unclear pattern edges, and simplifying the process.

[0008] In one embodiment of this application, the base glaze layer is a titanium opaque glaze layer, and the top glaze layer is a glossy glaze layer.

[0009] Based on the aforementioned technical means, the base glaze of this application uses titanium opaque glaze, which has a high silica content and low potassium oxide and sodium oxide content, resulting in high viscosity and surface tension at high temperatures; the top glaze is a glossy glaze, with a bright and smooth surface and low viscosity and surface tension. Thus, the titanium opaque glaze layer has high viscosity and surface tension, while the glossy glaze layer has low viscosity and surface tension. The glossy glaze layer produces a flowing glaze effect on the titanium opaque glaze layer, thereby forming a unique three-dimensional texture that is macroscopically ordered and microscopically disordered, resulting in excellent decorative effects.

[0010] In one embodiment of this application, the raw material formulation of the base glaze layer, by mass percentage, includes:

[0011] Kaolin 8-12%, high-temperature potassium sand 22-30%, quartz 20-26%, calcined talc 1-5%, first frit 34-42%.

[0012] Based on the above technical means, the base glaze of this application embodiment does not require the use of zirconium silicate, thereby solving the problem of high cost due to the use of zirconium silicate base glaze.

[0013] In one embodiment of this application, the chemical composition of the first melt, by mass percentage, includes:

[0014] SiO2 54.97%, Al2O3 11.21%, Fe2O3 0.12%, CaO 13.75%, MgO 0.45%, K2O2.44%, Na2O 1.37%, ZnO 2.17%, TiO2 13.52% 。

[0015] Based on the above technical means, the chemical composition of the first melting block in the embodiments of this application has significant benefits in optimizing glaze performance, promoting glaze melting and reaction, and improving the quality of ceramic tiles. It can ensure that glazed ceramic tiles form a uniform, smooth and decorative glaze during the firing process, while improving the durability and service life of the product.

[0016] In one embodiment of this application, the chemical composition of the base glaze layer, by mass percentage, includes:

[0017] SiO2 70~74%, Al2O3 10~12%, Fe2O3 0.1~0.2%, CaO 5~6%, MgO 0.5~2%, K2O 1.5~2.5%, Na2O 1~2%, TiO2 5~6%, ZnO 0.5~1%.

[0018] According to the above-mentioned technical means, the base glaze layer of this application embodiment contains titanium dioxide. Titanium dioxide undergoes photocatalysis under light, which accelerates the decomposition of dirt and bacteria, degrades pollutants, and inhibits bacterial reproduction.

[0019] In one embodiment of this application, the raw material formula of the glaze layer, by weight percentage, includes:

[0020] Sodium feldspar 20-30%, calcite 8-12%, second frit 32-42%, quartz 8-12%, dolomite 6-10%, barium carbonate 8-12%, copper oxide 0.1-1%, cobalt oxide 0-0.1%.

[0021] Based on the above-mentioned technical means, the proportion of the surface glaze raw materials in the embodiments of this application makes the surface glaze layer have suitable viscosity and surface tension, thereby producing an ideal glaze flow effect.

[0022] In one embodiment of this application, the chemical composition of the second melt, by mass percentage, includes:

[0023] SiO2 52.37%, Al2O3 17.12%, Fe2O3 0.09%, CaO 11.42%, MgO 1.34%, K2O4.08%, Na2O 11.25%, BaO 1.96%, ZnO 0.37%.

[0024] Based on the above-mentioned technical means, the chemical composition of the second frit in the embodiments of this application has significant benefits in optimizing glaze performance, promoting glaze melting and reaction, and improving the quality of ceramic tiles. It can ensure that glazed ceramic tiles form a uniform, smooth and decorative glaze during the firing process, while improving the durability and service life of the product.

[0025] In one embodiment of this application, the chemical composition of the surface glaze layer, by mass percentage, includes:

[0026] SiO2 50~56%, Al2O3 10~12%, Fe2O3 0.05~0.1%, CaO 12~16%, MgO2~3%, K2O 1~2%, Na2O 6~8%, BaO 9~11%, ZnO 0.1~0.2%, CuO 0.1~1%, CoO 0~0.1%.

[0027] Based on the above-mentioned technical means, the chemical composition of the glaze layer in the embodiments of this application has significant benefits in optimizing physical properties, improving chemical stability, improving the decorative effect of the glaze surface, and promoting the melting and reaction of the glaze. It can ensure that the ceramic tiles form a high-quality and highly decorative glaze surface during the firing process, while improving the durability and service life of the product.

[0028] In one embodiment of this application, the chemical composition of the ceramic green body, by mass percentage, includes:

[0029] SiO2 70-72%, Al2O3 18-20%, Fe2O3 1.5-2.5%, CaO 1-1.5%, MgO 1.0-2.0%, K2O 2-3%, Na2O 1-2%, TiO2 0.5-1.0%, others 0.5-1.0%.

[0030] Based on the above technical means, the chemical composition of the ceramic body in the embodiments of this application optimizes the physical properties of ceramic bricks, improves chemical stability, and enhances color and gloss.

[0031] A second aspect of this application provides a method for preparing the glazed ceramic tile as described above, wherein the method includes:

[0032] The raw materials are prepared according to the predetermined formula and ball-milled to obtain slurry;

[0033] The slurry is spray-dried to obtain ceramic powder, and the ceramic powder is pressed into ceramic blanks.

[0034] After drying the ceramic body, a pre-prepared base glaze is applied to the dried ceramic body to obtain a base glaze layer. The amount of base glaze applied is 400-600 g / m³. 2 ;

[0035] A pre-prepared top glaze is applied onto the base glaze layer to obtain a top glaze layer, wherein the amount of top glaze applied is 700–1000 g / m². 2 ;

[0036] Ceramic blanks with base glaze and top glaze are dried and then fired to obtain glazed ceramic tiles.

[0037] According to the above-mentioned technical means, in this embodiment, the amount of base glaze applied is less than that of top glaze. Because the top glaze layer has lower viscosity and surface tension, it exhibits greater fluidity at high temperatures, easily forming glaze runs. A larger amount of top glaze allows for more complex and richer glaze run textures, enabling the top glaze to freely cover the base glaze, forming unique macroscopically ordered and microscopically disordered three-dimensional textures. The amount of base glaze applied is smaller. Since the main function of the base glaze layer is to adhere to the ceramic body and provide a smooth and uniform base for the top glaze layer, a thinner base glaze layer reduces the amount of glaze used, lowering costs, while not affecting its function as a base.

[0038] The beneficial effects of this application are:

[0039] (1) The titanium opaque glaze layer in this application has high viscosity and surface tension, while the glossy glaze layer has low viscosity and surface tension. The glossy glaze layer produces a glaze flow effect on the titanium opaque glaze layer, thereby forming a unique macroscopically ordered and microscopically disordered three-dimensional texture, which has a very good decorative effect.

[0040] (2) The base glaze layer of this application contains titanium dioxide. Titanium dioxide undergoes photocatalysis under light, which accelerates the decomposition of dirt and bacteria, degrades pollutants, and inhibits bacterial reproduction.

[0041] (3) In the embodiments of this application, the amount of base glaze is less than that of top glaze. Since the viscosity of the top glaze layer is low and the surface tension is also low, it has greater fluidity at high temperature and is prone to forming glaze flow. The amount of base glaze is smaller, which can reduce the amount of glaze used and reduce costs. Attached Figure Description

[0042] Figure 1 This is a schematic diagram of the structure of a glazed ceramic tile according to the present invention.

[0043] Figure 2 This is a rendering of the surface of a glazed ceramic tile according to the present invention.

[0044] Figure 3 This is another brick surface effect image of a glazed ceramic tile in this invention. Detailed Implementation

[0045] To make the objectives, technical solutions, and advantages of this invention clearer and more explicit, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention.

[0046] like Figure 1 As shown in the embodiment of this application, a glazed ceramic tile is provided. The glazed ceramic tile includes: a ceramic body 100, a base glaze layer 200 disposed on the ceramic body 100, and a top glaze layer 300 disposed on the base glaze layer 200; the viscosity of the base glaze layer 200 is greater than the viscosity of the top glaze layer 300, and the surface tension of the base glaze layer 200 is greater than the surface tension of the top glaze layer 300.

[0047] Specifically, the thickness of the base glaze layer 200 is less than the thickness of the top glaze layer 300; that is, the base glaze layer 200 is thinner, and the top glaze layer 300 is thicker. Because the top glaze layer 300 has lower viscosity and surface tension, it exhibits greater fluidity at high temperatures, easily forming flowing glaze. The greater thickness of the top glaze layer 300 allows for the formation of more complex and richer flowing glaze textures, enabling the top glaze to freely cover the base glaze, creating a unique three-dimensional texture that is macroscopically ordered and microscopically disordered. The thinner base glaze layer 200, whose main function is to adhere to the ceramic body 100 and provide a smooth and uniform base for the top glaze layer 300, reduces the amount of glaze used, lowering costs without compromising its function as a base. A thicker glaze layer 300 provides better wear resistance, corrosion resistance, and stain resistance, protecting the ceramic body 100 from external environmental erosion; at the same time, a thicker glaze layer 300 can also better showcase the glaze flow effect and enhance the decorative properties of the ceramic tile.

[0048] The surface glaze layer 300 of this embodiment has a low viscosity. Low viscosity glazes and low surface tension result in high fluidity at high temperatures, easily causing glaze flow. When the surface tension of the glaze is also very low, glaze flow is even more likely to occur, forming an uneven glaze surface after cooling. Thus, the surface glaze layer 300 of this embodiment produces a glaze flow effect on the base glaze layer 200, forming a unique macroscopically ordered and microscopically disordered three-dimensional texture, enhancing the decorative effect. Furthermore, it eliminates the need for printing glue patterns, avoiding the problem of unclear pattern edges, and simplifying the process.

[0049] In one embodiment of this application, the base glaze layer 200 is a titanium opaque glaze layer, and the top glaze layer 300 is a glossy glaze layer.

[0050] Specifically, the base glaze in this embodiment uses a titanium opaque glaze, which has a high silica content and low potassium oxide and sodium oxide content, resulting in high viscosity and surface tension at high temperatures. The top glaze in this embodiment is a glossy glaze with a bright and smooth surface. The silica-alumina molar ratio is controlled at 8-10, while increasing the sodium oxide and barium oxide content to reduce high-temperature viscosity and surface tension. Thus, the titanium opaque glaze layer has high viscosity and surface tension, while the glossy glaze layer has low viscosity and surface tension. The glossy glaze layer produces a flowing glaze effect on the titanium opaque glaze layer, thereby forming a unique macroscopically ordered and microscopically disordered three-dimensional texture with excellent decorative effect.

[0051] Furthermore, the present application's embodiments combine a titanium opaque glaze layer and a glossy glaze layer, achieving the following effects:

[0052] First, titanium opaque glaze typically has an opaque effect, which scatters light and reduces direct light transmission, thus giving ceramic tiles a soft and warm texture. The glossy glaze, on the other hand, has high reflectivity, enhancing the surface gloss of the ceramic tile. The combination of titanium opaque glaze and glossy glaze creates a unique three-dimensional texture that is both macroscopically ordered (such as the overall gloss and color distribution) and microscopically disordered (such as the distribution of tiny particles in the opaque glaze and the flowing texture of the glossy glaze). This texture is both regular and varied, enhancing the decorative effect of the ceramic tile.

[0053] Secondly, due to its opaque properties, the titanium opaque glaze layer can increase the thickness and uniformity of the glaze surface, thereby improving the glaze surface's wear resistance, corrosion resistance, and other properties.

[0054] Third, the combination of titanium opaque glaze and glossy glaze eliminates the need for additional printing glue patterns, simplifying the production process. This application relies on the natural flow of the glaze and the cooling and curing process to form the texture, reducing the need for manual intervention and complex pattern design.

[0055] In one embodiment of this application, the raw material formula of the base glaze layer 200, by mass percentage, includes:

[0056] Kaolin 8-12%, high-temperature potassium sand 22-30%, quartz 20-26%, calcined talc 1-5%, first frit 34-42%.

[0057] Specifically, in preparing the base glaze, the raw materials are mixed according to the above formula, and 0.1% sodium carboxymethyl cellulose (CMC), 0.05% sodium tripolyphosphate, 0.2% sodium hexapolymetaphosphate, and 0.05% preservative (such as JS-3036, LF-15, JS-459, etc.) by weight of the base glaze are added. The mixture is then ball-milled in a ball mill at a weight ratio of material:ball:water = 1:2:0.4. The fineness is controlled to be 0.7-1.0% residue on a 10,000-mesh sieve to obtain the base glaze slurry.

[0058] Kaolin possesses excellent plasticity, which helps the base glaze layer 200 to form a good adhesion and uniform coating on the ceramic body 100. Furthermore, the whiteness of kaolin helps improve the aesthetics of ceramic products. It also enhances the suspension and stability of the glaze, allowing it to distribute evenly during firing and forming a smooth, uniform glaze surface. High-temperature potassium sand is a major component in the formation of the glassy phase, possessing a wide melting range and high-temperature viscosity. This broadens the melting and maturation temperature range of the glaze, facilitating porcelain formation and lowering the firing temperature, improving the gloss, transparency, and smoothness of the glaze layer, and enhancing its chemical stability. Quartz can combine with other oxides at high temperatures to form a stable glassy phase structure, enhancing the hardness and wear resistance of the glaze surface. The addition of quartz also improves the gloss and transparency of the glaze surface. Calcined talc can increase the wear resistance of glazes, fill minor defects, and improve the smoothness of the glaze surface. It can also adjust the melting temperature of the glaze, making it easier for the glaze to melt at the appropriate temperature and form a uniform glaze layer, preventing cracking and peeling, and improving the stability and durability of the glaze surface. The first frit can melt rapidly at high temperatures, promoting the melting and mixing of various components in the glaze, forming a uniform glassy phase structure, and enhancing the glaze's resistance to chemical corrosion, thus extending its service life.

[0059] The base glaze of this invention does not require the use of zirconium silicate, thus solving the problem of high cost caused by using zirconium silicate base glaze.

[0060] In one embodiment of this application, the chemical composition of the first melt, by mass percentage, includes:

[0061] SiO2 54.97%, Al2O3 11.21%, Fe2O3 0.12%, CaO 13.75%, MgO 0.45%, K2O2.44%, Na2O 1.37%, ZnO 2.17%, TiO2 13.52% 。

[0062] In this application, SiO2, as the main chemical component, can react with other oxides at high temperatures to form a stable glassy phase structure, enhancing the hardness and wear resistance of the glaze, and helping to improve the suspension and stability of the glaze, ensuring uniform distribution of the glaze during firing. Al2O3 combines with SiO2 to form mullite crystals, enhancing the strength and stability of the glaze. Simultaneously, Al2O3 can affect the viscosity of the liquid phase, helping to resist high-temperature deformation and ensuring the stability of the glaze during high-temperature firing. CaO and MgO, as alkaline earth metal oxides, can lower the firing temperature of the glaze, improving its mechanical strength and transparency; they can also promote the melting and reaction of the glaze, making the glaze more uniform and smooth. K2O and Na2O, as alkali metal oxides, are important flux components in the glaze, promoting its melting and reaction. They can lower the melting point of the glaze, allowing it to form a uniform glassy phase structure at lower temperatures. ZnO can improve the gloss and whiteness of the glaze. TiO2 can improve the whiteness of the glaze, giving ceramic tiles a purer and brighter color. It can also act as a flux to promote the melting and reaction of the glaze. By controlling the content of Fe2O3, the color and tone of the glaze can be fine-tuned.

[0063] The chemical composition of the first frit in this embodiment has significant benefits in optimizing glaze performance, promoting glaze melting and reaction, and improving the quality of ceramic tiles. It can ensure that glazed ceramic tiles form a uniform, smooth and decorative glaze during the firing process, while improving the durability and service life of the product.

[0064] In one embodiment of this application, the chemical composition of the base glaze layer 200, by mass percentage, includes:

[0065] SiO2 70~74%, Al2O3 10~12%, Fe2O3 0.1~0.2%, CaO 5~6%, MgO 0.5~2%, K2O 1.5~2.5%, Na2O 1~2%, TiO2 5~6%, ZnO 0.5~1%.

[0066] The base glaze layer 200 in this embodiment contains titanium dioxide. Titanium dioxide undergoes photocatalysis under light, accelerating the decomposition of dirt and bacteria, degrading pollutants, and inhibiting bacterial growth. The photocatalytic effect of titanium dioxide is used for disinfection and deodorization in many aspects of daily life, such as in paints used in toilet renovations and house walls, which often contain titanium dioxide.

[0067] In one embodiment of this application, the raw material formula of the glaze layer 300, by mass percentage, includes:

[0068] Sodium feldspar 20-30%, calcite 8-12%, second frit 32-42%, quartz 8-12%, dolomite 6-10%, barium carbonate 8-12%, copper oxide 0.1-1%, cobalt oxide 0-0.1%.

[0069] Specifically, in preparing the glaze, the raw materials are mixed according to the above formula, and 0.15% sodium carboxymethyl cellulose (CMC), 0.3% sodium tripolyphosphate, and 0.05% preservative are added according to the total mass of the glaze. The mixture is then added to a ball mill for ball milling at a weight ratio of material:ball:water = 1:2:0.4. The fineness is controlled so that the residue on a 10,000-mesh sieve is 0.1-0.3%, thus obtaining the glaze slurry.

[0070] The formulation of the glaze raw materials in this embodiment of the application results in the glaze layer 300 having suitable viscosity and surface tension, thereby producing an ideal glaze flow effect.

[0071] In one embodiment of this application, the chemical composition of the second melt, by mass percentage, includes:

[0072] SiO2 52.37%, Al2O3 17.12%, Fe2O3 0.09%, CaO 11.42%, MgO 1.34%, K2O4.08%, Na2O 11.25%, BaO 1.96%, ZnO 0.37%.

[0073] Specifically, components such as SiO2, Al2O3, CaO, and MgO in the frit can melt rapidly at high temperatures to form a stable glassy phase structure; the presence of alkali metal oxides such as K2O and Na2O can further lower the melting point and accelerate the melting process of the glaze.

[0074] The chemical composition of the second frit in this embodiment has significant benefits in optimizing glaze performance, promoting glaze melting and reaction, and improving the quality of ceramic tiles. It can ensure that glazed ceramic tiles form a uniform, smooth and decorative glaze during the firing process, while improving the durability and service life of the product.

[0075] In one embodiment of this application, the chemical composition of the surface glaze layer 300, by mass percentage, includes:

[0076] SiO2 50~56%, Al2O3 10~12%, Fe2O3 0.05~0.1%, CaO 12~16%, MgO2~3%, K2O 1~2%, Na2O 6~8%, BaO 9~11%, ZnO 0.1~0.2%, CuO 0.1~1%, CoO 0~0.1%.

[0077] Specifically, SiO2, as the main component, contributes to the formation of a hard glaze, improving the wear resistance and scratch resistance of ceramic tiles. The addition of Al2O3 also enhances the hardness of the glaze, making it more durable. Appropriate CaO and MgO content helps improve the toughness of the glaze, preventing it from easily cracking under external forces. The high content of SiO2 and Al2O3 gives the glaze excellent corrosion resistance, enabling it to resist the erosion of various chemicals. The chemical composition of the glaze makes the surface smooth and less prone to dirt accumulation, making it easy to clean and maintain. The addition of CuO can inhibit bacterial growth to some extent. The addition of CuO and CoO provides a rich variety of colors for the glaze, making the decorative effect of ceramic tiles more diverse. At the same time, these oxides can also affect the gloss of the glaze. K2O and Na2O, as fluxing agents, can lower the melting point of the glaze, promoting its melting and reaction.

[0078] The chemical composition of the glaze layer 300 of the present invention has significant benefits in optimizing physical properties, improving chemical stability, enhancing the decorative effect of the glaze, and promoting glaze melting and reaction. It can ensure that ceramic tiles form a high-quality, highly decorative glaze during the firing process, while improving the durability and service life of the product.

[0079] In one embodiment of this application, the chemical composition of the ceramic green body 100, by mass percentage, includes:

[0080] SiO2 70-72%, Al2O3 18-20%, Fe2O3 1.5-2.5%, CaO 1-1.5%, MgO 1.0-2.0%, K2O 2-3%, Na2O 1-2%, TiO2 0.5-1.0%, others 0.5-1.0%.

[0081] Specifically, SiO2 and Al2O3 are the main components of the ceramic body 100. Their high content helps to form a hard crystal structure, thereby improving the strength and hardness of the ceramic body 100. This makes the ceramic products more durable and able to withstand greater pressure and wear. By adjusting the ratio of SiO2, Al2O3 and other oxides (such as CaO and MgO), the coefficient of thermal expansion of the ceramic body 100 can be optimized, thereby improving its thermal shock resistance and enabling the ceramic products to maintain stable performance in environments with large temperature variations. Appropriate K2O and Na2O content helps to lower the melting point of the ceramic body 100, making it easier to melt and form during firing, which helps to improve the production efficiency and processing performance of the ceramic products. TiO2 and other oxides in the ceramic body 100 help to improve its oxidation resistance, preventing oxidation reactions at high temperatures that would lead to performance degradation. The presence of oxides such as Fe2O3 and TiO2 provides the ceramic body 100 with a rich variety of colors. By adjusting the content and ratio of these oxides, ceramic products with unique colors can be customized.

[0082] The chemical composition of the ceramic body 100 in this embodiment optimizes the physical properties of the ceramic brick, improves its chemical stability, and enhances its color and gloss.

[0083] This application also provides a method for preparing the glazed ceramic tile as described above, the method comprising:

[0084] Step S100: Prepare the raw materials according to the predetermined raw material formula and ball mill them to obtain slurry;

[0085] Step S200: Spray dry the mud to obtain ceramic powder, and press the ceramic powder into a ceramic blank;

[0086] Step S300: After drying the ceramic body, apply a pre-prepared base glaze to the dried ceramic body to obtain a base glaze layer. The amount of base glaze applied is 400-600 g / m³. 2 ;

[0087] Step S400: Apply a pre-prepared top glaze to the base glaze layer to obtain a top glaze layer. The amount of top glaze applied is 700-1000 g / m². 2 ;

[0088] Step S500: After drying, the ceramic body with base glaze and top glaze is fired to obtain glazed ceramic tiles.

[0089] Specifically, in step S100, the raw materials are wet-milled according to the blank formula, with a weight ratio of material:ball:water = 1:1.2:0.4, to obtain a slurry. The slurry has a moisture content of 30-35% and a fineness of 2-2.5% residue on a 10,000-mesh sieve. In step S200, the slurry is spray-dried in a spray drying tower to obtain ceramic powder. The ceramic powder has a moisture content of 5.5-6.5%, a bulk density ≥0.91, and a 40-mesh sieve residue controlled at 48-58%. The ceramic powder is then pressed into ceramic blanks. In step S300, the ceramic blanks are dried in a drying kiln. A base glaze is applied to the dried blanks with a specific gravity of 1.77-1.79, a flow rate of 27-32 seconds, and a glaze application rate of 400-600 g / m³. 2 In step S400, a pre-prepared top glaze is applied onto the base glaze layer, with a specific gravity of 1.80±0.01, a flow rate of 35–40 seconds, and an application rate of 700–1000 g / m³. 2 In step S500, the green body after applying glaze slurry is dried in an infrared dryer and fired in a roller kiln at a firing temperature of 1180-1220℃ for a firing cycle of 45-55 minutes. Then, after edge grinding, packaging, and warehousing, glazed ceramic tiles are obtained.

[0090] In this embodiment, the amount of base glaze applied is less than that of top glaze. Because the top glaze layer has lower viscosity and surface tension, it exhibits greater fluidity at high temperatures, easily forming glaze runs. A larger amount of top glaze allows for more complex and richer glaze run textures, enabling it to freely cover the base glaze and create unique macroscopically ordered, microscopically disordered three-dimensional textures. The smaller amount of base glaze, whose main function is to adhere to the ceramic body and provide a smooth, uniform base for the top glaze, reduces glaze usage, lowers costs, and does not affect its function as a base. A thicker top glaze layer provides better wear resistance, corrosion resistance, and stain resistance, protecting the ceramic body from environmental erosion. Simultaneously, a thicker top glaze layer better showcases the glaze run effect, enhancing the decorative appeal of the ceramic tile.

[0091] This invention, through adjustments to the glaze formula, can produce ceramic tiles with a three-dimensional textured surface and a smooth, warm glaze. Walking barefoot or wearing socks on these tiles can massage acupoints on the soles of the feet, providing a massage effect. Furthermore, these ceramic tiles can be installed at the bottom of swimming pools and other locations. This solves the problems of insufficient three-dimensional effect and cumbersome manufacturing processes associated with traditional ceramic tiles. Additionally, the base glaze of this invention does not require zirconium silicate, thus addressing the high cost associated with using zirconium silicate base glazes.

[0092] The following are specific examples for illustration.

[0093] Example 1

[0094] By mass percentage, 10% kaolin, 26% high-temperature potassium sand, 24% quartz, 3% talc, and 37% first frit are mixed together. Then, 0.1% CMC, 0.05% sodium tripolyphosphate, 0.2% sodium hexapolyphosphate, and 0.05% preservative are added to the total mass of the glaze. The mixture is then ball-milled in a weight ratio of material:ball:water = 1:2:0.4. The fineness is controlled to be 0.7-1.0% residue on a 10,000-mesh sieve to obtain the base glaze.

[0095] By mass percentage, 25% albite, 10% calcite, 35% second frit, 11% quartz, 8% dolomite, 10% barium carbonate, 0.98% copper oxide, and 0.02% cobalt oxide are mixed. Then, 0.15% CMC, 0.3% sodium tripolyphosphate, and 0.05% preservative are added to the total mass of the glaze. The mixture is then ball-milled in a ball mill at a weight ratio of material:ball:water = 1:2:0.4. The fineness is controlled to be 0.1-0.3% residue on a 10,000-mesh sieve to obtain the surface glaze.

[0096] The preparation steps of ceramic tiles include:

[0097] Step A1: According to the raw material formula, calculate the weight ratio of material:ball:water = 1:1.2:0.4 and perform wet ball milling to obtain a slurry with a moisture content of 30-35% and a fineness of 2-2.5% residue on a 10,000-mesh sieve. The slurry is then passed through a spray drying tower to obtain a green body powder with a moisture content of 5.5-6.5%, a bulk density ≥0.91, and a 40-mesh sieve residue controlled at 48-58%, which is then pressed into green bodies.

[0098] Step A2: The billet is dried in a drying kiln;

[0099] Step A3: Apply a base glaze to the dried body with a specific gravity of 1.78, a flow rate of 30 seconds, and a glaze application rate of 575 grams per square meter.

[0100] Step A4: Apply a layer of glaze with a specific gravity of 1.81, a flow rate of 37 seconds, and a glaze application rate of 826 grams per square meter.

[0101] Step A5: The glazed body is dried in an infrared dryer.

[0102] Step A6: Firing in a roller kiln at a temperature of 1201℃ for a period of 48 minutes;

[0103] Step A7: Packaging and warehousing. The pass rate was 95.9%.

[0104] Example 2

[0105] By mass percentage, 8% kaolin, 27% high-temperature potassium sand, 21% quartz, 5% talc, and 39% first frit are mixed together. Then, 0.1% CMC, 0.05% sodium tripolyphosphate, 0.2% sodium hexapolyphosphate, and 0.05% preservative are added to the total mass of the glaze. The mixture is then added to a ball mill and ball-milled at a weight ratio of 1:2:0.4. The fineness is controlled to be 0.7-1.0% residue on a 10,000-mesh sieve to obtain the base glaze.

[0106] By mass percentage, 23% albite, 11% calcite, 41.7% second frit, 7% quartz, 8% dolomite, 9% barium carbonate, 0.2% copper oxide, and 0.1% cobalt oxide are mixed. Then, 0.15% CMC, 0.3% sodium tripolyphosphate, and 0.05% preservative are added to the total mass of the glaze. The mixture is then ball-milled in a ball mill at a weight ratio of material:ball:water = 1:2:0.4. The fineness is controlled to be 0.1-0.3% residue on a 10,000-mesh sieve to obtain the surface glaze.

[0107] The preparation steps of ceramic tiles include:

[0108] Step B1: According to the raw material formula, calculate the weight ratio of material:ball:water = 1:1.2:0.4 and perform wet ball milling to obtain a slurry with a moisture content of 30-35% and a fineness of 2-2.5% residue on a 10,000-mesh sieve. The slurry is then passed through a spray drying tower to obtain a green body powder with a moisture content of 5.5-6.5%, a bulk density ≥0.91, and a 40-mesh sieve residue controlled at 48-58%, which is then pressed into green bodies.

[0109] Step B2: The billet is dried in a drying kiln;

[0110] Step B3: Apply a base glaze to the dried body with a specific gravity of 1.79, a flow rate of 28 seconds, and a glaze application rate of 431 grams per square meter.

[0111] Step B4: Apply a layer of glaze with a specific gravity of 1.80, a flow rate of 35 seconds, and a glaze application rate of 790 grams per square meter.

[0112] Step B5: The glazed body is dried in an infrared dryer.

[0113] Step B6: Firing in a roller kiln at a temperature of 1190℃ for a period of 51 minutes;

[0114] Step B7: Packaging and warehousing. The pass rate was 96.8%.

[0115] Example 3

[0116] By mass percentage, 12% kaolin, 25% high-temperature potassium sand, 26% quartz, 2% talc, and 35% first frit are mixed together. Then, 0.1% CMC, 0.05% sodium tripolyphosphate, 0.2% sodium hexapolyphosphate, and 0.05% preservative are added to the total mass of the glaze. The mixture is then ball-milled in a weight ratio of material:ball:water = 1:2:0.4. The fineness is controlled to be 0.7-1.0% residue on a 10,000-mesh sieve to obtain the base glaze.

[0117] By mass percentage, 29% albite, 8% calcite, 37% second frit, 8% quartz, 6% dolomite, 11.5% barium carbonate, 0.47% copper oxide, and 0.03% cobalt oxide are mixed. Then, 0.15% CMC, 0.3% sodium tripolyphosphate, and 0.05% preservative are added to the total mass of the glaze. The mixture is then ball-milled in a ball mill at a weight ratio of material:ball:water = 1:2:0.4. The fineness is controlled to be 0.1-0.3% residue on a 10,000-mesh sieve to obtain the surface glaze.

[0118] The preparation steps of ceramic tiles include:

[0119] Step C1: According to the raw material formula, calculate the weight ratio of material:ball:water = 1:1.2:0.4 and perform wet ball milling to obtain a slurry with a moisture content of 30-35% and a fineness of 2-2.5% residue on a 10,000-mesh sieve. The slurry is then passed through a spray drying tower to obtain a green body powder with a moisture content of 5.5-6.5%, a bulk density ≥0.91, and a 40-mesh sieve residue controlled at 48-58%, which is then pressed into green bodies.

[0120] Step C2: The billet is dried in a drying kiln;

[0121] Step C3: Apply a base glaze to the dried body with a specific gravity of 1.79, a flow rate of 31 seconds, and a glaze application rate of 540 grams per square meter.

[0122] Step C4: Apply a layer of glaze with a specific gravity of 1.81, a flow rate of 39 seconds, and a glaze application rate of 934 grams per square meter.

[0123] Step C5: The glazed body is dried in an infrared dryer.

[0124] Step C6: Firing in a roller kiln at a temperature of 1209℃ for a period of 45 minutes;

[0125] Step C7: Packaging and warehousing. The pass rate was 95.2%.

[0126] The present invention can achieve the following effects:

[0127] First, the ceramic tile of the present invention has a wavy and crisscrossing surface with a strong three-dimensional effect, a smooth and delicate glaze, and a massage function.

[0128] Secondly, the ceramic tile of this invention has a strong sense of layering in its glaze, a rustic color, and a shimmering sheen, achieving the visual effect of a gentle breeze rippling across the sea, creating blue-green waves. Figure 2 and Figure 3 As shown.

[0129] Third, the production process of the glazed ceramic tile with massage function of the present invention is stable, simple, has a high rate of excellence, low cost, and can be mass-produced.

[0130] This invention provides a glazed ceramic tile and its preparation method. The glazed ceramic tile includes: a ceramic body, a base glaze layer disposed on the ceramic body, and a top glaze layer disposed on the base glaze layer. The viscosity of the base glaze layer is greater than that of the top glaze layer, and the surface tension of the base glaze layer is greater than that of the top glaze layer. The top glaze layer of this invention has lower viscosity and surface tension, making it easier to form glaze flow. After cooling, it forms an uneven glaze surface, i.e., the top glaze layer produces a glaze flow effect on the base glaze layer, forming a unique macroscopically ordered and microscopically disordered three-dimensional texture, enhancing the decorative effect. Furthermore, it eliminates the need for printing glue patterns, avoiding the problem of unclear pattern edges, and the process is simple.

[0131] It should be understood that the application of the present invention is not limited to the examples above. Those skilled in the art can make improvements or modifications based on the above description, and all such improvements and modifications should fall within the protection scope of the appended claims.

Claims

1. A glazed ceramic tile, characterized in that, The glazed ceramic tile includes: a ceramic body, a base glaze layer disposed on the ceramic body, and a top glaze layer disposed on the base glaze layer; the viscosity of the base glaze layer is greater than the viscosity of the top glaze layer, and the surface tension of the base glaze layer is greater than the surface tension of the top glaze layer; The raw material formula of the glaze layer, by mass percentage, includes: Albite 20-30%, calcite 8-12%, second frit 32-42%, quartz 8-12%, dolomite 6-10%, barium carbonate 8-12%, copper oxide 0.1-1%, cobalt oxide 0-0.1%; The chemical composition of the second melt, by mass percentage, includes: SiO252.37%, Al2O317.12%, Fe2O30.09%, CaO 11.42%, MgO 1.34%, K2O 4.08%, Na2O11.25%, BaO 1.96%, ZnO 0.37%; The raw material formula of the base glaze layer, by mass percentage, includes: Kaolin 8-12%, high-temperature potassium sand 22-30%, quartz 20-26%, calcined talc 1-5%, first frit 34-42%; The chemical composition of the first melt, by mass percentage, includes: SiO254.97%, Al2O311.21%, Fe2O30.12%, CaO 13.75%, MgO 0.45%, K2O 2.44%, Na2O 1.37%, ZnO 2.17%, TiO213.52%.

2. The glazed ceramic tile according to claim 1, characterized in that, The base glaze layer is a titanium opaque glaze layer, and the top glaze layer is a glossy glaze layer.

3. The glazed ceramic tile according to claim 1, characterized in that, The chemical composition of the base glaze layer, by mass percentage, includes: SiO270~74%, Al2O310~12%, Fe2O30.1~0.2%, CaO 5~6%, MgO 0.5~2%, K2O 1.5~2.5%, Na2O 1~2%, TiO25~6%, ZnO 0.5~1%.

4. The glazed ceramic tile according to claim 1, characterized in that, The chemical composition of the surface glaze layer, by mass percentage, includes: SiO250~56%, Al2O310~12%, Fe2O30.05~0.1%, CaO 12~16%, MgO 2~3%, K2O 1~2%, Na2O 6~8%, BaO 9~11%, ZnO 0.1~0.2%, CuO 0.1~1%, CoO 0~0.1%.

5. The glazed ceramic tile according to claim 1, characterized in that, The chemical composition of the ceramic green body, by mass percentage, includes: SiO2 70~72%, Al2O3 18~20%, Fe2O3 1.5~2.5%, CaO 1~1.5%, MgO 1.0~2.0%, K2O 2~3%, Na2O 1~2%, TiO2 0.5~1.0%, others 0.5~1.0%.

6. A method for preparing glazed ceramic tiles as described in any one of claims 1 to 5, characterized in that, The method includes: The raw materials are prepared according to the predetermined formula and ball-milled to obtain slurry; The slurry is spray-dried to obtain ceramic powder, and the ceramic powder is pressed into ceramic blanks. After drying the ceramic body, a previously prepared underglaze is applied on the dried ceramic body to obtain an underglaze layer, the application amount of the underglaze being 400~600g / m 2 ; A pre-prepared top glaze is applied onto the base glaze layer to obtain a top glaze layer, wherein the amount of top glaze applied is 700~1000g / m². 2 ; Ceramic blanks with base glaze and top glaze are dried and then fired to obtain glazed ceramic tiles.

Citation Information

Patent Citations

  • Furnace transmutation glaze ceramic tile and preparation method thereof

    CN114163245A

  • Glazed tile with bright star effect on surface and preparation method of glazed tile

    CN114292131A

  • Titanium white opaque ground coat and ceramic plate

    CN115304277A

  • Green glaze, ceramic tile and preparation method thereof

    CN115710088A