Phosphate nonlinear optical crystal, preparation method and application thereof
By preparing easily grown phosphate nonlinear optical crystals, the problems of frequency doubling effect and insufficient birefringence of existing materials in the ultraviolet and deep ultraviolet bands were solved, enabling their application in all-solid-state lasers.
Patent Information
- Application Number
- CN202411603788.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-12
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-11-12
AI Technical Summary
Existing phosphate nonlinear optical crystal materials have insufficient frequency doubling effect and birefringence in the ultraviolet and deep ultraviolet bands, and are difficult to grow, making it difficult to meet the needs of the optoelectronic industry.
A mixed melt containing an A-containing compound, a P-containing compound, and a flux is prepared. Phosphate nonlinear optical crystals are grown by a high-temperature melt method. The specific steps include calcination, melting, cooling, and single crystal growth to form yttrium phosphate or lutetium phosphate nonlinear optical crystals that are easy to cut and polish.
A nonlinear optical crystal with excellent performance in the ultraviolet-visible range was obtained. It is easy to process and store, does not deliquesce, and is suitable for nonlinear optical devices in all-solid-state lasers.
Smart Images

Figure CN119465402B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of rare earth phosphate compound technology, specifically relating to a phosphate nonlinear optical crystal, its preparation method, and its application. Background Technology
[0002] Functional materials form the material foundation for human survival and development, playing a crucial role in all aspects of our production and life. With rapid socio-economic progress, the demand for materials is increasing daily, and the requirements for their functionality and quality are becoming more stringent. Nonlinear optical (NLO) crystal materials are a branch of optoelectronic functional crystal materials. NLO crystal materials are further divided into naturally grown and artificially grown materials. Ruby and quartz are natural NLO crystal materials. Regarding artificial nonlinear optical crystal materials, a number of commercially available crystal materials have been obtained through experimental growth over the past few decades, including β-BaB₂O₄ (β-BBO), LiB₃O₅ (LBO), KBa₂BO₃F₂ (KBBF), KH₂PO₄ (KDP), KTiOPO₄ (KTP), and AgGaS₂ (AGS). These crystals are widely used in fields such as defense laser communication, medical testing instruments, and solid-state lasers. The demand for linear / nonlinear optical crystals in the visible light region has been largely met, but the demand for linear / nonlinear optical crystals in the ultraviolet (wavelengths below 400 nm) and deep ultraviolet (below 200 nm) bands is still far from sufficient. The need for ultraviolet / deep ultraviolet coherent light in emerging optoelectronic industries, such as semiconductor lithography, laser micromachining, and modern scientific instruments, is increasingly urgent. Therefore, exploring novel NLO crystals with short cutoff edges, wide phase-matching ranges, large octave response coefficients, moderate birefringence, good chemical and thermal stability, non-hygroscopicity, and ease of fabrication remains a challenge in this field.
[0003] In recent years, many high-performance phosphate compounds have been synthesized, such as AM2(PO3)5 (A=K,Rb,Cs; M=Ba) and Ba3P3O. 10 Despite the presence of various phosphate nonlinear optical crystal materials such as X (X = Cl, Br), RbNaMgP2O7, Na3Sc2(PO4)2F3, KLa(PO3)3, and La(PO3)3, they still have their own shortcomings. For example, the frequency doubling effect and low birefringence are the most significant problems facing phosphates. To obtain ultraviolet phosphate nonlinear optical crystal materials with suitable frequency doubling and birefringence, cations or π-conjugated anionic groups with stereochemically active lone pairs of electrons can be introduced. However, d... 0 The introduction of cations, and cations containing lone pairs of electrons, usually results in a significant redshift in the wavelength range.
[0004] In recent years, the introduction of rare earth elements into anionic systems and the design and synthesis of rare earth crystals with novel structures and specific optical properties have attracted widespread attention. Rare earth elements have the following advantages: (1) The valence electron shell structure of rare earth atoms is complex, and their chemical reactivity is second only to alkali metals and alkaline earth metals; (2) They exist stably as +3 cations, and the radii of rare earth elements are similar, so new compounds can often be formed through cation regulation; (3) Rare earth cations can form large coordination polyhedra, which has a certain effect on optimizing optical anisotropy; (4) There are eight ions with closed-shell or near-closed-shell electronic configurations, namely Sc 3+ Y 3+ La 3+ Gd 3+ Ce 3+ (Ce 4+ Eu 3+ and Yb 3+ Lu 3+ This structure is beneficial for the transmission of ultraviolet and deep ultraviolet light through the crystal; (5) Rare earth elements also have strong electronegativity, and when coordinated with oxygen atoms, they can enhance the ionic properties of the target compound, thereby increasing the band gap. Therefore, the synthesis of rare earth phosphates is an effective means of designing excellent nonlinear optical materials.
[0005] However, current research on nonlinear optical crystals made from rare-earth phosphates is relatively limited, and single-crystal growth is difficult. With the increasing demand for optoelectronic devices, there is a need for novel multifunctional crystal materials with comprehensive performance, necessitating the design and synthesis of new nonlinear optical materials. Summary of the Invention
[0006] The purpose of this invention is to provide a phosphate nonlinear optical crystal, its preparation method, and its application. The two types of phosphate nonlinear optical crystals provided by this invention are easy to grow, cut, grind, polish, and store as single crystals. They are stable in air, not easily deliquescent, and insoluble in water. At the same time, they have excellent optical properties and can be used as ultraviolet-visible nonlinear optical crystals in all-solid-state lasers.
[0007] To achieve the above objectives, the present invention provides the following technical solution:
[0008] This invention provides a phosphate nonlinear optical crystal, the chemical formula of which is shown in Formula 1:
[0009] A(PO3)3 Equation 1;
[0010] In Equation 1: A is Y or Lu;
[0011] The phosphate nonlinear optical crystal belongs to the monoclinic crystal system and has a space group of Cc.
[0012] The molecular weight of the yttrium phosphate nonlinear optical crystal is 325.82, and its unit cell parameters are... β=127.581(2)°, Z=4, unit cell volume is
[0013] The molecular weight of the lutetium phosphate nonlinear optical crystal is 411.88, and its unit cell parameters are... β=127.3590(10)°, Z=12, unit cell volume is
[0014]
[0015] This invention provides a method for preparing the phosphate nonlinear optical crystal described above, comprising the following steps:
[0016] A mixed melt was prepared using an A-containing compound, a P-containing compound, and a flux.
[0017] The mixed melt was first cooled to room temperature to obtain phosphate seed crystals;
[0018] The phosphate seed crystal is fixed on the seed crystal rod, and then the preheated seed crystal is lowered into the mixed melt for single crystal growth, and an initial phosphate single crystal is obtained on the seed crystal rod.
[0019] The initial phosphate single crystal was cooled to room temperature to obtain a phosphate nonlinear optical crystal with the chemical formula shown in Formula 1.
[0020] Preferably, the A-containing compound is a Y-containing compound or a Lu-containing compound; the purity of the Y-containing compound is ≥99.9%, and the Y-containing compound includes one or more of Y2O3, YF3, YCl3, YBr3, YI3, and Y2(CO3)3·3H2O; the purity of the Lu-containing compound is ≥99.9%, and the Lu-containing compound includes one or more of Lu2O3, LuF3, LuCl3, LuBr3, and Lu2(CO3)3·xH2O; the purity of the P-containing compound is ≥99.9%, and the P-containing compound includes one or more of NH4H2PO4, H3PO4, and P2O5; the purity of the flux is ≥99.9%, and the flux includes one or more of PbO, PbCl2, PbO-P2O5, PbCl2-P2O5, and PbO-PbCl2.
[0021] Preferably, the method for preparing the mixed melt includes the following steps: mixing a compound containing A and a compound containing P according to the molar ratio of A and P elements in the chemical formula shown in Formula 1, followed by calcination to obtain a polycrystalline phosphate product; the calcination temperature is 600-800℃, and the holding time is 36-48h.
[0022] The polycrystalline phosphate product and the flux are mixed and then melted to obtain a mixed melt; the molar ratio of the polycrystalline phosphate product and the flux is 1:1 to 5; the melting temperature is 650 to 920°C, the holding time is 20 to 48 hours, and the heating rate from room temperature to the melting temperature is 1 to 50°C / hour.
[0023] Preferably, the method for preparing the mixed melt includes the following steps: mixing a compound containing A, a compound containing P, and a flux, and then melting the mixture to obtain a mixed melt; the molar ratio of the compound containing A, the compound containing P, and the flux is 1:3 to 6:1 to 5; the melting temperature is 650 to 920°C, the holding time is 20 to 48 hours, and the heating rate from room temperature to the melting temperature is 1 to 50°C / hour.
[0024] Preferably, the cooling rate of the first cooling is 0.5–10 °C / h;
[0025] The conditions for single crystal growth include: the mixed melt is held at a certain temperature and then cooled, and the seed crystal rod rotates; the holding temperature of the mixed melt is 650-920℃, and the holding time is 15-80 min; the cooling rate is 0.1-3℃ / day; and the rotation speed of the seed crystal rod is 1-60 rpm / min.
[0026] After fixing the phosphate seed crystal on the seed crystal rod, before lowering the preheated seed crystal into the mixed melt, the process further includes: preheating the phosphate seed crystal fixed on the seed crystal rod, wherein the preheating ambient temperature is 650-920°C and the time is 15-80 min;
[0027] The cooling rate of the second cooling is 1 to 100°C / h.
[0028] This invention provides the application of the phosphate nonlinear optical crystal described in the above technical solution or the phosphate nonlinear optical crystal prepared by the preparation method described in the above technical solution as a nonlinear optical crystal.
[0029] Preferably, the phosphate nonlinear optical crystal is used as a deep ultraviolet nonlinear optical crystal.
[0030] Preferably, the phosphate nonlinear optical crystal is used in all-solid-state lasers.
[0031] This invention provides the application of the phosphate nonlinear optical crystal described in the above technical solution or the phosphate nonlinear optical crystal prepared by the preparation method described in the above technical solution in nonlinear optical devices, wherein the nonlinear optical devices include frequency multiplier generators, up or down frequency converters, optical parametric oscillators or laser frequency converters.
[0032] This invention provides a phosphate nonlinear optical crystal, the chemical formula of which is shown in Formula 1. The two crystals provided by this invention have the chemical formulas Y(PO3)3 and Lu(PO3)3, with molecular weights of 325.82 and 411.88, respectively. Both crystals crystallize in the monoclinic crystal system, space group Cc. The unit cell parameters are as follows: β=127.581(2)°,Z=4; β=127.3590(10)°, Z=12, unit cell volume is respectively and Both crystals have a cutoff edge of less than 200 nm and a birefringence between 0.018 (3000 nm) and 0.023 (1064 nm).
[0033] This invention provides a method for preparing the phosphate nonlinear optical crystal described in the above-mentioned technical solution. The invention employs a high-temperature melt method (spontaneous crystallization, melt pulling, and melt top seed crystal method) and a flux method to grow the crystal; it has the advantages of fast growth rate, low cost, and easy acquisition of large-size crystals. The crystals obtained by the preparation method of this invention are easy to grow, easy to cut, easy to grind, easy to polish, and easy to store. They are stable in air, not easily deliquescent, and insoluble in water; they can be used as ultraviolet-visible nonlinear optical crystals in all-solid-state lasers.
[0034] The results of the embodiments show that the single crystal size of the two phosphate nonlinear optical crystals provided by the present invention is on the order of centimeters, and they are transparent and unencapsulated. Based on the crystallographic data of the crystals, the crystal blanks are oriented, cut to the required angle, thickness, and cross-sectional dimensions, and the light-transmitting surfaces of the crystals are polished, thus enabling their use as nonlinear optical devices. Both Y(PO3)3 and Lu(PO3)3 nonlinear optical crystals have advantages such as ultraviolet light transmission, stable physicochemical properties, low hygroscopicity, and ease of processing and storage. Attached Figure Description
[0035] Figure 1 The powder X-ray diffraction pattern of the single-phase polycrystalline powder prepared in the embodiments of the present invention is shown. Figure 1 In Figure (a), the XRD pattern of the single-phase polycrystalline powder of Y(PO3)3 compound prepared in Example 1 is shown, and in Figure (b), the XRD pattern of the single-phase polycrystalline powder of Lu(PO3)3 compound prepared in Example 16 is shown.
[0036] Figure 2 A schematic diagram illustrating the working principle of the nonlinear optical device provided by this invention;
[0037] Figure 2In the middle: 1 is a laser, 2 is a full-focus lens, 3 is a Y(PO3)3 or Lu(PO3)3 nonlinear optical crystal, 4 is a beam splitter, and 5 is a filter.
[0038] Figure 3 The crystal structures of Y(PO3)3 and Lu(PO3)3 prepared in the embodiments of the present invention are shown below. Figure 3 (a) in the diagram is the crystal diagram of Y(PO3)3. Figure 3 (b) in the diagram is the crystal diagram of Lu(PO3)3;
[0039] Figure 4 Thermogravimetric-differential thermal curves of single-phase polycrystalline powder prepared in embodiments of the present invention are shown. Figure 4 In Figure (a), the thermogravimetric-differential thermal curve of the single-phase polycrystalline powder of Y(PO3)3 compound prepared in Example 1 is shown. Figure 4 (b) in the figure is the thermogravimetric-differential thermal curve of the single-phase polycrystalline powder of Lu(PO3)3 compound prepared in Example 16;
[0040] Figure 5 The infrared spectrum of the single-phase polycrystalline powder prepared in an embodiment of the present invention is shown below. Figure 5 Image (a) in the image is the infrared spectrum of the single-phase polycrystalline powder of Y(PO3)3 compound prepared in Example 1. Figure 5 (b) is the infrared spectrum of the Lu(PO3)3 compound single-phase polycrystalline powder prepared in Example 16;
[0041] Figure 6 The image shows the UV-Vis diffuse reflectance spectrum of the single-phase polycrystalline powder prepared in an embodiment of the present invention. Figure 6 (a) in the image is the UV-Vis diffuse reflectance spectrum of the single-phase polycrystalline powder of Y(PO3)3 compound prepared in Example 1. Figure 6 (b) is the UV-Vis diffuse reflectance spectrum of the Lu(PO3)3 compound single-phase polycrystalline powder prepared in Example 16. Detailed Implementation
[0042] This invention provides a phosphate nonlinear optical crystal, the chemical formula of which is shown in Formula 1:
[0043] A(PO3)3 Equation 1;
[0044] In Equation 1: A is Y or Lu;
[0045] The phosphate nonlinear optical crystal belongs to the monoclinic crystal system and has a space group of Cc.
[0046] The molecular weight of the yttrium phosphate nonlinear optical crystal is 325.82, and its unit cell parameters are... β=127.581(2)°, Z=4, unit cell volume is
[0047] The molecular weight of the lutetium phosphate nonlinear optical crystal is 411.88, and its unit cell parameters are... β=127.3590(10)°, Z=12, unit cell volume is
[0048]
[0049] This invention provides a method for preparing the phosphate nonlinear optical crystal described above, comprising the following steps:
[0050] A mixed melt was prepared using an A-containing compound, a P-containing compound, and a flux.
[0051] The mixed melt was first cooled to room temperature to obtain phosphate seed crystals;
[0052] The phosphate seed crystal is fixed on the seed crystal rod, and then the preheated seed crystal is lowered into the mixed melt for single crystal growth, and an initial phosphate single crystal is obtained on the seed crystal rod.
[0053] The initial phosphate single crystal was cooled to room temperature to obtain a phosphate nonlinear optical crystal with the chemical formula shown in Formula 1.
[0054] In this invention, unless otherwise specified, all raw materials / components used in the preparation are commercially available products well known to those skilled in the art.
[0055] This invention uses an A-containing compound, a P-containing compound, and a flux to prepare a mixed melt. In this invention, the A-containing compound is a Y-containing compound or a Lu-containing compound. The purity of the Y-containing compound is preferably ≥99.9%, and the Y-containing compound preferably includes one or more of Y₂O₃, YF₃, YCl₃, YBr₃, YI₃, and Y₂(CO₃)₃·3H₂O. The purity of the Lu-containing compound is preferably ≥99.9%, and the Lu-containing compound preferably includes one or more of Lu₂O₃, LuF₃, LuCl₃, LuBr₃, and Lu₂(CO₃)₃·xH₂O. The purity of the P-containing compound is preferably ≥99.9%, and the P-containing compound preferably includes one or more of NH₄H₂PO₄, H₃PO₄, and P₂O₅. The purity of the flux is preferably ≥99.9%, and the flux preferably includes one or more of PbO, PbCl₂, PbO-P₂O₅ systems, PbCl₂-P₂O₅ systems, and PbO-PbCl₂ systems. The PbO-P2O5 system comprises PbO and P2O5. The preferred molar ratio of PbO to P2O5 in the PbO-P2O5 system is 1 to 5:1. The PbCl2-P2O5 system comprises PbCl2 and P2O5. The preferred molar ratio of PbCl2 to P2O5 in the PbCl2-P2O5 system is 1 to 5:1. The PbO-PbCl2 system comprises PbO and PbCl2. The preferred molar ratio of PbO to PbCl2 in the PbO-PbCl2 system is 1 to 5:1.
[0056] In this invention, the method for preparing the mixed melt preferably includes the following steps: mixing an A-containing compound and a P-containing compound according to the molar ratio of A to P elements in the chemical formula shown in Formula 1, followed by calcination to obtain a polycrystalline phosphate product. In this invention, the Y-containing compound and the P-containing compound are preferably mixed at a molar ratio of Y to P elements of 1:3. The Lu-containing compound and the P-containing compound are preferably mixed at a molar ratio of Lu to P elements of 1:3. In this invention, before calcination, the mixture preferably further includes: first grinding the mixed raw material to obtain a first ground powder; pre-calcining the first ground powder to obtain a pre-calcined material; and cooling the pre-calcined material to room temperature followed by a second grinding to obtain a second ground powder. Preferably, the second ground powder is then calcined. This invention does not have special requirements for the specific implementation of the first and second grinding processes. The pre-calcination temperature is preferably 300–350°C, and the pre-calcination holding time is preferably 24–36 hours. In this invention, the mixed raw materials or the second ground powder are preferably placed in a crucible and calcined in a muffle furnace. The crucible is preferably an open-faced corundum crucible or an open-faced platinum crucible. The crucible's dimensions are preferably Φ60mm × 60mm. The calcination temperature is preferably 600–800℃, and the holding time is preferably 36–48 hours. In a specific embodiment of this invention, when the A-containing compound is a Y-containing compound, the calcination temperature is specifically 750℃. When the A-containing compound is a Lu-containing compound, the calcination temperature is specifically 650℃. Preferably, the product obtained from the calcination is slowly cooled to room temperature to obtain a polycrystalline phosphate product. The polycrystalline phosphate product is a Y(PO3)3 polycrystalline product or a Lu(PO3)3 polycrystalline product.
[0057] After obtaining the polycrystalline phosphate product, the present invention mixes the polycrystalline phosphate product and a flux and then melts them to obtain a mixed melt. In the present invention, the molar ratio of the polycrystalline phosphate product to the flux is preferably 1:1 to 5, and specifically 1:5 or 1:1 in the embodiments. Preferably, the mixture obtained by mixing the polycrystalline phosphate product and the flux is placed in a platinum crucible and then placed in a single crystal growth furnace for melting. The melting temperature is preferably 650 to 920°C, and specifically 650°C, 920°C, 750°C, 870°C, 770°C, 800°C, 780°C, 700°C, 790°C, 680°C, 830°C, 840°C, 880°C, 850°C, or 900°C in the embodiments. The holding time for the melting process is preferably 20–48 hours, and specifically in the embodiments, it is 20 hours, 24 hours, 30 hours, 48 hours, 22 hours, 46 hours, 34 hours, 36 hours, 48 hours, 25 hours, 29 hours, 44 hours, 26 hours, 43 hours, 42 hours, 32 hours, or 28 hours. The heating rate from room temperature to the melting temperature is preferably 1–50 °C / hour, and specifically in the embodiments, it is 2 °C / hour, 50 °C / hour, 3 °C / hour, 10 °C / hour, 8 °C / hour, 25 °C / hour, 0.5 °C / hour, 5 °C / hour, 20 °C / hour, 1 °C / hour, 15 °C / hour, 33 °C / hour, 28 °C / hour, 34 °C / hour, 43 °C / hour, 45 °C / hour, 23 °C / hour, 38 °C / hour, 44 °C / hour, 17 °C / hour, 29 °C / hour, or 12 °C / hour.
[0058] Alternatively, the method for preparing the mixed melt preferably includes the following steps: mixing a compound containing A, a compound containing P, and a flux, and then melting the mixture to obtain a mixed melt. In this invention, the molar ratio of the compound containing A, the compound containing P, and the flux is preferably 1:3 to 6:1 to 5, and specifically 1:5:1, 1:1:1, 1:2:1, 1:3:1, or 1:4:1 in the embodiments. Preferably, the mixture obtained by mixing the compound containing A, the compound containing P, and the flux is placed in a platinum crucible and then melted in a single crystal growth furnace. The melting temperature is preferably 650 to 920°C, and specifically 650°C, 920°C, 750°C, 870°C, 770°C, 800°C, 780°C, 700°C, 790°C, 680°C, 830°C, 840°C, 880°C, 850°C, or 900°C in the embodiments. The holding time for the melting process is preferably 20–48 hours, and specifically in the embodiments, it is 20 hours, 24 hours, 30 hours, 48 hours, 22 hours, 46 hours, 34 hours, 36 hours, 48 hours, 25 hours, 29 hours, 44 hours, 26 hours, 43 hours, 42 hours, 32 hours, or 28 hours. The heating rate from room temperature to the melting temperature is preferably 1–50 °C / hour, and specifically in the embodiments, it is 2 °C / hour, 50 °C / hour, 3 °C / hour, 10 °C / hour, 8 °C / hour, 25 °C / hour, 0.5 °C / hour, 5 °C / hour, 20 °C / hour, 1 °C / hour, 15 °C / hour, 33 °C / hour, 28 °C / hour, 34 °C / hour, 43 °C / hour, 45 °C / hour, 23 °C / hour, 38 °C / hour, 44 °C / hour, 17 °C / hour, 29 °C / hour, or 12 °C / hour.
[0059] After obtaining the mixed melt, the present invention first cools the mixed melt to room temperature to obtain phosphate seed crystals. In the present invention, the temperature of the mixed melt during the first cooling is preferably 650-920℃, specifically 650℃, 920℃, 750℃, 870℃, 770℃, 800℃, 780℃, 700℃, 790℃, 680℃, 830℃, 840℃, 880℃, 850℃, or 900℃. The preferred cooling rate for the first cooling step is 0.5-10℃ / h, specifically 1℃ / h, 0.5℃ / h, 2℃ / h, 5℃ / h, 1.8℃ / h, 10℃ / h, 7℃ / h, 6℃ / h, 1.6℃ / h, 7.8℃ / h, 6.8℃ / h, 7.5℃ / h, 0.8℃ / h, 0.5℃ / h, 3.5℃ / h, 3.2℃ / h, 9℃ / h, 4.7℃ / h, 1.5℃ / h, 2.8℃ / h, 4.5℃ / h, or 6.5℃ / h in the embodiments. The phosphate seed crystals are obtained by spontaneous crystallization of the mixed melt.
[0060] After obtaining the phosphate seed crystal, the present invention fixes the phosphate seed crystal onto a seed crystal rod, and then lowers the preheated seed crystal into the mixed melt for single crystal growth, obtaining an initial phosphate single crystal on the seed crystal rod. In the present invention, the phosphate seed crystal is fixed on the seed crystal rod in any orientation. In the present invention, the mixed melt is located in a platinum crucible in the single crystal growth furnace, and the present invention preferably lowers the phosphate seed crystal fixed on the seed crystal rod from the top of the single crystal growth furnace. After fixing the phosphate seed crystal onto the seed crystal rod and before lowering the preheated seed crystal into the mixed melt, the present invention preferably further includes: preheating the phosphate seed crystal fixed on the seed crystal rod. The preheating is carried out in a single crystal growth furnace. The preferred preheating temperature is 650–920°C, and the preferred preheating time is 15–80 min, specifically 60 min, 55 min, 48 min, 80 min, 30 min, 15 min, 34 min, 25 min, 75 min, 24 min, 20 min, 42 min, 54 min, 36 min, or 72 min in the embodiments. After preheating, a preheated seed crystal is obtained. Preferably, the preheated seed crystal is placed in the mixed melt for single crystal growth. The preferred conditions for single crystal growth include: the mixed melt is held at a certain temperature and then cooled, and the seed crystal rod rotates. The preferred holding temperature of the mixed melt is 650–920°C, and the preferred holding time is 15–80 min. In the embodiments, the specific holding times are 60 min, 80 min, 30 min, 50 min, 30 min, 18 min, 15 min, 76 min, 55 min, 19 min, 21 min, 45 min, 25 min, 50 min, 65 min, 75 min, 60 min, 48 min, or 72 min. During the holding process, the phosphate seed crystals remelt in the mixed melt.The cooling rate is preferably 0.1–3℃ / day, specifically 0.1℃ / day, 1℃ / day, 0.2℃ / day, 0.8℃ / day, 3℃ / day, 0.7℃ / day, 2.2℃ / day, 1.8℃ / day, 1.9℃ / day, 2.3℃ / day, 0.3℃ / day, 0.9℃ / day, 0.5℃ / day, 2.5℃ / day, 2.2℃ / day, 2.8℃ / day, or 1.2℃ / day in the embodiments; the rotation speed of the seed crystal rod is preferably 1–60 rpm / min, specifically 1 rpm / min or 12 rpm / min in the embodiments. n, 25rpm / min, 54rpm / min, 55rpm / min, 47rpm / min, 37rpm / min, 57rpm / min, 18rpm / min, 12rpm / min, 37rpm / min, 22r pm / min, 34rpm / min, 60rpm / min, 32rpm / min, 17rpm / min, 15rpm / min, 8rpm / min, 45rpm / min, 55rpm / min or 48rpm / min.
[0061] In this invention, once the initial phosphate single crystal has grown to the required size, the initial phosphate single crystal is removed from the surface of the mixed melt.
[0062] After obtaining the initial phosphate single crystal, the present invention further cools the initial phosphate single crystal to room temperature to obtain a phosphate nonlinear optical crystal with the chemical formula shown in Formula 1. In the present invention, the cooling rate of the second cooling is preferably 1–100 °C / h, specifically 1 °C / h, 20 °C / h, 30 °C / h, 10 °C / h, 50 °C / h, 70 °C / h, 100 °C / h, 87 °C / h, 67 °C / h, 4 °C / h, 44 °C / h, 15 °C / h, 40 °C / h, 60 °C / h, 100 °C / h, or 75 °C / h in the embodiments. The second cooling is preferably performed in a single crystal growth furnace. After obtaining the phosphate nonlinear optical crystal with the chemical formula shown in Formula 1, the present invention removes the obtained phosphate nonlinear optical crystal with the chemical formula shown in Formula 1 from the furnace chamber of the single crystal growth furnace, thus obtaining a yttrium phosphate nonlinear optical crystal or a lutetium phosphate nonlinear optical crystal.
[0063] This invention provides the application of the phosphate nonlinear optical crystal described in the above technical solution or the phosphate nonlinear optical crystal prepared by the preparation method described in the above technical solution as a nonlinear optical crystal.
[0064] In this invention, the phosphate nonlinear optical crystal is used as a deep ultraviolet nonlinear optical crystal.
[0065] In this invention, the phosphate nonlinear optical crystal is used in an all-solid-state laser.
[0066] This invention provides the application of the phosphate nonlinear optical crystal described in the above-described technical solution, or the phosphate nonlinear optical crystal prepared by the preparation method described in the above-described technical solution, in nonlinear optical devices. In this invention, the nonlinear optical device includes a frequency multiplier, an up- or down-frequency converter, an optical parametric oscillator, or a laser frequency converter.
[0067] In a specific embodiment of the present invention, the yttrium phosphate nonlinear optical crystal, with the molecular formula Y(PO3)3, is prepared by a solid-state reaction method according to the following chemical reaction formula:
[0068] (1)Y2O3+6NH4H2PO4→2Y(PO3)3+6NH3↑+9H2O↑
[0069] (2)Y2(CO3)3·3H2O+6NH4H2PO4→2Y(PO3)3+3CO2↑+6NH3↑+12H2O↑
[0070] (3)YF3+3NH4H2PO4→Y(PO3)3+3NH3↑+3H2O↑+3HF↑
[0071] (4)YCl3+3NH4H2PO4→Y(PO3)3+3NH3↑+3H2O↑+3HCl↑
[0072] (5)YBr3+3NH4H2PO4→Y(PO3)3+3NH3↑+3H2O↑+3HBr↑
[0073] (6)YI3+3NH4H2PO4→Y(PO3)3+3NH3↑+3H2O↑+3HI↑
[0074] (7) Y₂O₃ + 3P₂O₅ → 2Y(PO₃)₃
[0075] (8)Y2(CO3)3·3H2O+3P2O5→2Y(PO3)3+3CO2↑+3H2O↑
[0076] (9)Y2O3+6H3PO4→2Y(PO3)3+9H2O↑
[0077] (10)Y2(CO3)3·3H2O+6H3PO4→2Y(PO3)3+3CO2↑+12H2O↑
[0078] (11)YF3+3H3PO4→Y(PO3)3+3HF↑+3H2O↑
[0079] (12)YCl3+3H3PO4→Y(PO3)3+3H2O↑+3HCl↑
[0080] (13)YBr3+3H3PO4→Y(PO3)3+3H2O↑+3HBr↑
[0081] (14)YI3+3H3PO4→Y(PO3)3+3H2O↑+3HI↑
[0082] In a specific embodiment of the present invention, the lutetium phosphate nonlinear optical crystal, with the molecular formula Lu(PO3)3, is prepared by a solid-state reaction method according to the following chemical reaction formula:
[0083] (1)Lu2O3+6NH4H2PO4→2Lu(PO3)3+6NH3↑+9H2O↑
[0084] (2)Lu2(CO3)3·xH2O+6NH4H2PO4→2Lu(PO3)3+3CO2↑+6NH3↑+(9+x)H2O↑
[0085] (3)LuF3+3NH4H2PO4→Lu(PO3)3+3NH3↑+3H2O↑+3HF↑
[0086] (4)LuCl3+3NH4H2PO4→Lu(PO3)3+3NH3↑+3H2O↑+3HCl↑
[0087] (5)LuBr3+3NH4H2PO4→Lu(PO3)3+3NH3↑+3H2O↑+3HBr↑
[0088] (6) Lu₂O₃ + 3P₂O₅ → 2Lu(PO₃)₃
[0089] (7)Lu2(CO3)3·xH2O+3P2O5→2Lu(PO3)3+3CO2↑+(3+x)H2O↑
[0090] (8)Lu2O3+6H3PO4→2Lu(PO3)3+9H2O↑
[0091] (9)Lu2(CO3)3·xH2O+6H3PO4→2Lu(PO3)3+3CO2↑+(9+x)H2O↑
[0092] (10)LuF3+3H3PO4→Lu(PO3)3+3HF↑+3H2O↑
[0093] (11)LuCl3+3H3PO4→Lu(PO3)3+3H2O↑+3HCl↑
[0094] (12)LuBr3+3H3PO4→Lu(PO3)3+3H2O↑+3HBr↑
[0095] To further illustrate the present invention, the technical solutions provided by the present invention will be described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0096] The following Examples 1-14 show the preparation of yttrium phosphate single crystals with the chemical formula Y(PO3)3 by solid-state reaction method.
[0097] In Examples 16-27 below, lutetium phosphate single crystals with the chemical formula Lu(PO3)3 were prepared by solid-state reaction method.
[0098] Example 1
[0099] According to the chemical reaction formula Y₂O₃ + 6NH₄H₂PO₄ → 2Y(PO₃)₃ + 6NH₃↑ + 9H₂O↑, Y(PO₃)₃ nonlinear optical crystals were prepared.
[0100] a. Mix Y₂O₃ and NH₄H₂PO₄ in an agate mortar at a molar ratio of 1:6 and grind thoroughly until fully homogeneous. Then, place the mixture into a Φ60mm×60mm open-face corundum crucible, put it in a muffle furnace, slowly heat to 350℃, hold at that temperature for 24 hours, cool to room temperature, remove, grind a second time, transfer to another open-face corundum crucible, put it in a muffle furnace, heat to 750℃ again, hold at that temperature for 48 hours, slowly cool to room temperature, remove, grind to obtain a single-phase polycrystalline powder of yttrium phosphate compound, and then perform X-ray analysis on the product, such as... Figure 1 As shown in (a), the obtained X-ray spectrum is consistent with the X-ray spectrum obtained from the yttrium phosphate single crystal structure.
[0101] b. With a molar ratio of 1:5, the polycrystalline powder obtained in step a is mixed evenly with flux PbO, heated to 920℃ at a heating rate of 50℃ / h, and kept at the temperature for 20h to obtain a mixed melt.
[0102] c. Preparation of seed crystals: After cooling the mixed melt obtained in step b, transfer it to a single crystal growth furnace, heat it to 920℃ until the melt is uniform and transparent, and slowly cool it to room temperature at a rate of 1℃ / h to obtain Y(PO3)3 seed crystals through spontaneous crystallization.
[0103] d. Crystal growth: Fix the seed crystal obtained in step c onto the seed crystal rod. The seed crystal can be fixed on the seed crystal rod in any direction. Lower the seed crystal from the top of the crystal growth furnace and preheat the seed crystal for 60 minutes. Then, lower the seed crystal into a mixed melt of Y(PO3)3 and flux heated to 920°C for remelting. Maintain the temperature for 60 minutes and slowly cool it down at a rate of 0.1°C / day. Rotate the seed crystal rod at a speed of 1 rpm / min to grow the crystal. After the single crystal grows to the required size, lift the crystal off the liquid surface and cool it down to room temperature at a rate of 1°C / h. Then, take the crystal out of the furnace to obtain the Y(PO3)3 nonlinear optical crystal.
[0104] Example 2
[0105] According to the chemical reaction formula Y2(CO3)3·3H2O+6NH4H2PO4→2Y(PO3)3+3CO2↑+6NH3↑+12H2O↑, Y(PO3)3 nonlinear optical crystal was prepared.
[0106] The preparation of Y(PO3)3 compound single-phase polycrystalline powder was carried out according to step a in Example 1:
[0107] Y(PO3)3 polycrystalline powder and flux PbO were mixed evenly at a molar ratio of 1:1 and placed into a platinum crucible. The mixture was heated to 750°C at a heating rate of 2°C / h and held at that temperature for 24h to obtain a mixed melt.
[0108] Preparation of seed crystals: After cooling the obtained mixed melt, transfer it to a single crystal growth furnace, heat it to 750℃ until the melt is uniform and transparent, and then cool it to room temperature at 0.5℃ / h to obtain Y(PO3)3 seed crystals through spontaneous crystallization.
[0109] Crystal growth: The obtained seed crystal is fixed on the seed crystal rod. The seed crystal is fixed on the seed crystal rod in any direction. The seed crystal is lowered from the top of the crystal growth furnace and preheated for 55 minutes. The seed crystal is then lowered into a mixed melt of Y(PO3)3 and flux heated to 750°C for remelting. The temperature is kept constant for 80 minutes and then slowly cooled at a rate of 1°C / day. The seed crystal rod is rotated at a speed of 12 rpm / min to grow the crystal. After the single crystal grows to the required size, the crystal is lifted off the liquid surface and cooled to room temperature at a rate of 20°C / h. Then the crystal is taken out of the furnace to obtain the Y(PO3)3 nonlinear optical crystal.
[0110] Example 3
[0111] According to the chemical reaction formula YF3 + 3NH4H2PO4 → Y(PO3)3 + 3NH3↑ + 3H2O↑ + 3HF↑, Y(PO3)3 nonlinear optical crystal was prepared.
[0112] The preparation of Y(PO3)3 compound single-phase polycrystalline powder was carried out according to step a in Example 1:
[0113] Y(PO3)3 polycrystalline powder and flux PbCl2 were mixed evenly at a molar ratio of 1:1 and placed into a platinum crucible. The mixture was heated to 870°C in a muffle furnace at a heating rate of 3°C / h and held at that temperature for 30h to obtain a mixed melt.
[0114] Preparation of seed crystals: After cooling the obtained mixed melt, transfer it to a single crystal growth furnace, heat it to 870℃ until the melt is uniform and transparent, and then slowly cool it to room temperature at a rate of 1℃ / h to obtain Y(PO3)3 seed crystals through spontaneous crystallization.
[0115] Crystal growth: The obtained seed crystal is fixed on the seed crystal rod. The seed crystal is fixed on the seed crystal rod in any direction. The seed crystal is lowered from the top of the crystal growth furnace and preheated for 60 minutes. The seed crystal is then lowered into a mixed melt of Y(PO3)3 and flux heated to 870℃ for remelting. The temperature is kept constant for 30 minutes and then slowly cooled at a rate of 0.2℃ / day. The seed crystal rod is rotated at a speed of 25 rpm / min to grow the crystal. After the single crystal grows to the required size, the crystal is lifted off the liquid surface and cooled to room temperature at a rate of 30℃ / h. Then the crystal is taken out of the furnace to obtain the Y(PO3)3 nonlinear optical crystal.
[0116] Example 4
[0117] According to the chemical reaction formula YCl3 + 3NH4H2PO4 → Y(PO3)3 + 3NH3↑ + 3H2O↑ + 3HCl↑, Y(PO3)3 nonlinear optical crystal was prepared.
[0118] The preparation of Y(PO3)3 compound single-phase polycrystalline powder was carried out according to step a in Example 1:
[0119] Y(PO3)3 polycrystalline powder and flux PbO-PbCl2 were mixed evenly in a molar ratio of 1:5:1 and placed into a platinum crucible. The mixture was heated to 650°C in a muffle furnace at a heating rate of 5°C / h and held at that temperature for 36h to obtain a mixed melt.
[0120] Preparation of seed crystals: After cooling the obtained mixed melt, transfer it to a single crystal growth furnace, heat it to 650℃ until the melt is uniform and transparent, and then cool it to room temperature at a rate of 2℃ / h to obtain Y(PO3)3 seed crystals through spontaneous crystallization.
[0121] Crystal growth: The obtained seed crystal is fixed on the seed crystal rod. The seed crystal is fixed on the seed crystal rod in any direction. The seed crystal is lowered from the top of the crystal growth furnace and preheated for 48 minutes. The seed crystal is then lowered into a mixed melt of Y(PO3)3 and flux heated to 650°C for remelting. The temperature is kept constant for 50 minutes and then slowly cooled at a rate of 0.8°C / day. The seed crystal rod is rotated at a speed of 25 rpm / min to grow the crystal. After the single crystal grows to the required size, the crystal is lifted off the liquid surface and cooled to room temperature at a rate of 10°C / h. Then the crystal is taken out of the furnace to obtain the Y(PO3)3 nonlinear optical crystal.
[0122] Example 5
[0123] According to the chemical reaction formula YBr3 + 3NH4H2PO4 → Y(PO3)3 + 3NH3↑ + 3H2O↑ + 3HBr↑, a Y(PO3)3 nonlinear optical crystal was prepared.
[0124] The preparation of Y(PO3)3 compound single-phase polycrystalline powder was carried out according to step a in Example 1:
[0125] Y(PO3)3 polycrystalline powder and flux PbCl2 were mixed evenly at a molar ratio of 1:5 and placed into a platinum crucible. The mixture was heated to 770°C in a muffle furnace at a heating rate of 10°C / h and held at that temperature for 48h to obtain a mixed melt.
[0126] Preparation of seed crystals: After cooling the obtained mixed melt, transfer it to a single crystal growth furnace, heat it to 770℃ until the melt is uniform and transparent, and then cool it to room temperature at a rate of 5℃ / h to obtain Y(PO3)3 seed crystals through spontaneous crystallization.
[0127] Crystal growth: The obtained seed crystal is fixed on the seed crystal rod. The seed crystal is fixed on the seed crystal rod in any direction. The seed crystal is lowered from the top of the crystal growth furnace and preheated for 80 minutes. The seed crystal is then lowered into a mixed melt of Y(PO3)3 and flux heated to 770°C for remelting. The temperature is kept constant for 30 minutes and then slowly cooled at a rate of 3°C / day. The seed crystal rod is rotated at a speed of 54 rpm / min to grow the crystal. After the single crystal grows to the required size, the crystal is lifted off the liquid surface and cooled to room temperature at a rate of 50°C / h. Then the crystal is taken out of the furnace to obtain the Y(PO3)3 nonlinear optical crystal.
[0128] Example 6
[0129] According to the chemical reaction formula YI3 + 3NH4H2PO4 → Y(PO3)3 + 3NH3↑ + 3H2O↑ + 3HI↑, Y(PO3)3 nonlinear optical crystal was prepared.
[0130] The preparation of Y(PO3)3 compound single-phase polycrystalline powder was carried out according to step a in Example 1:
[0131] Y(PO3)3 polycrystalline powder and flux PbO-PbCl2 were mixed evenly in a molar ratio of 1:1:1 and placed into a platinum crucible. The mixture was heated to 880℃ in a muffle furnace at a rate of 20℃ / h and held at that temperature for 48h to obtain a mixed melt.
[0132] Preparation of seed crystals: After cooling the obtained mixed melt, transfer it to a single crystal growth furnace, heat it to 880℃ until the melt is uniform and transparent, and then slowly cool it to room temperature at a rate of 1.8℃ / h to obtain Y(PO3)3 seed crystals through spontaneous crystallization.
[0133] Crystal growth: The obtained seed crystal is fixed on the seed crystal rod. The seed crystal is fixed on the seed crystal rod in any direction. The seed crystal is lowered from the top of the crystal growth furnace and preheated for 30 minutes. The seed crystal is then lowered into a mixed melt of Y(PO3)3 and flux at 880°C for remelting. The temperature is kept constant for 30 minutes and then slowly cooled at a rate of 0.7°C / day. The seed crystal rod is rotated at a speed of 55 rpm / min to grow the crystal. After the single crystal grows to the required size, the crystal is lifted off the liquid surface and cooled to room temperature at a rate of 70°C / h. Then the crystal is taken out of the furnace to obtain the Y(PO3)3 nonlinear optical crystal.
[0134] Example 7
[0135] According to the chemical reaction formula Y₂O₃ + 3P₂O₅ → 2Y(PO₃)₃, a Y(PO₃)₃ nonlinear optical crystal was prepared.
[0136] The preparation of Y(PO3)3 compound single-phase polycrystalline powder was carried out according to step a in Example 1:
[0137] Y(PO3)3 polycrystalline powder and flux PbO-P2O5 were mixed evenly in a molar ratio of 1:5:1 and placed into a platinum crucible. The mixture was heated to 880°C in a muffle furnace at a heating rate of 30°C / h and held at that temperature for 30h to obtain a mixed melt.
[0138] Preparation of seed crystals: After cooling the obtained mixed melt, transfer it to a single crystal growth furnace, heat it to 770℃ until the melt is uniform and transparent, and then slowly cool it to room temperature at a rate of 10℃ / h to obtain Y(PO3)3 seed crystals through spontaneous crystallization.
[0139] Crystal growth: The obtained seed crystal is fixed on the seed crystal rod. The seed crystal is fixed on the seed crystal rod in any direction. The seed crystal is lowered from the top of the crystal growth furnace and preheated for 80 minutes. The seed crystal is then lowered into a mixed melt of Y(PO3)3 and flux at 880°C for remelting. The temperature is kept constant for 50 minutes and then slowly cooled at a rate of 2.2°C / day. The seed crystal rod is rotated at a speed of 47 rpm / min to grow the crystal. After the single crystal grows to the required size, the crystal is lifted off the liquid surface and cooled to room temperature at a rate of 100°C / h. Then the crystal is taken out of the furnace to obtain the Y(PO3)3 nonlinear optical crystal.
[0140] Example 8
[0141] According to the chemical reaction formula Y2(CO3)3·3H2O+3P2O5→2Y(PO3)3+3CO2↑+3H2O↑, Y(PO3)3 nonlinear optical crystal was prepared.
[0142] The preparation of Y(PO3)3 compound single-phase polycrystalline powder was carried out according to step a in Example 1:
[0143] Y(PO3)3 polycrystalline powder and flux PbCl2-P2O5 were mixed evenly in a molar ratio of 1:1:1 and placed into a platinum crucible. The mixture was heated to 780°C in a muffle furnace at a heating rate of 1°C / h and held at that temperature for 25h to obtain a mixed melt.
[0144] Preparation of seed crystals: After cooling the obtained mixed melt, transfer it to a single crystal growth furnace, heat it to 780℃ until the melt is uniform and transparent, and then slowly cool it to room temperature at a rate of 7℃ / h to obtain Y(PO3)3 seed crystals through spontaneous crystallization.
[0145] Crystal growth: The obtained seed crystal is fixed on the seed crystal rod. The seed crystal is fixed on the seed crystal rod in any direction. The seed crystal is lowered from the top of the crystal growth furnace and preheated for 15 minutes. The seed crystal is then lowered into a mixed melt of Y(PO3)3 and flux heated to 780°C for remelting. The temperature is held constant for 18 minutes and then slowly cooled at a rate of 1.8°C / day. The seed crystal rod is rotated at a speed of 37 rpm / min to grow the crystal. After the single crystal grows to the required size, the crystal is lifted off the liquid surface and cooled to room temperature at a rate of 100°C / h. Then the crystal is taken out of the furnace to obtain the Y(PO3)3 nonlinear optical crystal.
[0146] Example 9
[0147] According to the chemical reaction Y₂O₃ + 6H₃PO₄ → 2Y(PO₃)₃ + 9H₂O↑, Y(PO₃)₃ nonlinear optical crystals were prepared.
[0148] The preparation of Y(PO3)3 compound single-phase polycrystalline powder was carried out according to step a in Example 1:
[0149] Y(PO3)3 polycrystalline powder and flux PbCl2-P2O5 were mixed evenly in a molar ratio of 1:5:1 and placed into a platinum crucible. The mixture was heated to 800℃ in a muffle furnace at a heating rate of 15℃ / h and held at that temperature for 29h to obtain a mixed melt.
[0150] Preparation of seed crystals: After cooling the obtained mixed melt, transfer it to a single crystal growth furnace, heat it to 800℃ until the melt is uniform and transparent, and then slowly cool it to room temperature at a rate of 6℃ / h to obtain Y(PO3)3 seed crystals through spontaneous crystallization.
[0151] Crystal growth: The obtained seed crystal is fixed on the seed crystal rod. The seed crystal is fixed on the seed crystal rod in any direction. The seed crystal is lowered from the top of the crystal growth furnace and preheated for 15 minutes. The seed crystal is then lowered into a mixed melt of Y(PO3)3 and flux heated to 800℃ for remelting. The temperature is held constant for 15 minutes and then slowly cooled at a rate of 1.8℃ / day. The seed crystal rod is rotated at a speed of 57 rpm / min to grow the crystal. After the single crystal grows to the required size, the crystal is lifted off the liquid surface and cooled to room temperature at a rate of 87℃ / h. Then the crystal is taken out of the furnace to obtain the Y(PO3)3 nonlinear optical crystal.
[0152] Example 10
[0153] According to the chemical reaction formula Y2(CO3)3·3H2O+6H3PO4→2Y(PO3)3+3CO2↑+12H2O↑, Y(PO3)3 nonlinear optical crystal was prepared.
[0154] The preparation of Y(PO3)3 compound single-phase polycrystalline powder was carried out according to step a in Example 1:
[0155] Y(PO3)3 polycrystalline powder and flux PbO-P2O5 were mixed evenly in a molar ratio of 1:1:1 and placed into a platinum crucible. The mixture was heated to 700°C in a muffle furnace at a heating rate of 33°C / h and held at that temperature for 44h to obtain a mixed melt.
[0156] Preparation of seed crystals: After cooling the obtained mixed melt, transfer it to a single crystal growth furnace, heat it to 700℃ until the melt is uniform and transparent, and then slowly cool it to room temperature at a rate of 1.6℃ / h to obtain Y(PO3)3 seed crystals through spontaneous crystallization.
[0157] Crystal growth: The obtained seed crystal is fixed on the seed crystal rod. The seed crystal is fixed on the seed crystal rod in any direction. The seed crystal is lowered from the top of the crystal growth furnace and preheated for 34 minutes. The seed crystal is then lowered into a mixed melt of Y(PO3)3 and flux heated to 700℃ for remelting. The temperature is held constant for 15 minutes and then slowly cooled at a rate of 1.9℃ / day. The seed crystal rod is rotated at a speed of 54 rpm / min to grow the crystal. After the single crystal grows to the required size, the crystal is lifted off the liquid surface and cooled to room temperature at a rate of 1℃ / h. Then the crystal is taken out of the furnace to obtain the Y(PO3)3 nonlinear optical crystal.
[0158] Example 11
[0159] According to the chemical reaction formula YF3 + 3H3PO4 → Y(PO3)3 + 3HF↑ + 3H2O↑, Y(PO3)3 nonlinear optical crystal was prepared.
[0160] The preparation of Y(PO3)3 compound single-phase polycrystalline powder was carried out according to step a in Example 1:
[0161] Y(PO3)3 polycrystalline powder and flux PbO-PbCl2 were mixed evenly in a molar ratio of 1:2:1 and placed into a platinum crucible. The mixture was heated to 790°C in a muffle furnace at a heating rate of 28°C / h and held at that temperature for 26h to obtain a mixed melt.
[0162] Preparation of seed crystals: After cooling the obtained mixed melt, transfer it to a single crystal growth furnace, heat it to 790℃ until the melt is uniform and transparent, and then slowly cool it to room temperature at a rate of 7.8℃ / h to obtain Y(PO3)3 seed crystals through spontaneous crystallization.
[0163] Crystal growth: The seed crystal is fixed on the seed crystal rod in any orientation. The seed crystal is lowered from the top of the crystal growth furnace and preheated for 25 minutes. The seed crystal is then lowered into a mixed melt of Y(PO3)3 and flux heated to 790°C for remelting. The temperature is held constant for 76 minutes and then slowly cooled at a rate of 2.3°C / day. The seed crystal rod is rotated at a speed of 18 rpm / min to grow the crystal. Once the single crystal has grown to the required size, it is lifted off the liquid surface and cooled to room temperature at a rate of 67°C / h. The crystal is then removed from the furnace to obtain the Y(PO3)3 nonlinear optical crystal.
[0164] Example 12
[0165] According to the chemical reaction formula YCl3 + 3H3PO4 → Y(PO3)3 + 3H2O↑ + 3HCl↑, Y(PO3)3 nonlinear optical crystal was prepared.
[0166] The preparation of Y(PO3)3 compound single-phase polycrystalline powder was carried out according to step a in Example 1:
[0167] Y(PO3)3 polycrystalline powder and flux PbO-P2O5 were mixed evenly in a molar ratio of 1:3:1 and placed into a platinum crucible. The mixture was heated to 680°C in a muffle furnace at a heating rate of 34°C / h and held at that temperature for 43h to obtain a mixed melt.
[0168] Preparation of seed crystals: After cooling the obtained mixed melt, transfer it to a single crystal growth furnace, heat it to 680℃ until the melt is uniform and transparent, and then slowly cool it to room temperature at a rate of 6.8℃ / h to obtain Y(PO3)3 seed crystals through spontaneous crystallization.
[0169] Crystal growth: The obtained seed crystal is fixed on the seed crystal rod. The seed crystal is fixed on the seed crystal rod in any direction. The seed crystal is lowered from the top of the crystal growth furnace and preheated for 75 minutes. The seed crystal is then lowered into a mixed melt of Y(PO3)3 and flux heated to 680°C for remelting. The temperature is kept constant for 55 minutes and then slowly cooled at a rate of 3°C / day. The seed crystal rod is rotated at a speed of 12 rpm / min to grow the crystal. After the single crystal grows to the required size, the crystal is lifted off the liquid surface and cooled to room temperature at a rate of 4°C / h. Then the crystal is taken out of the furnace to obtain the Y(PO3)3 nonlinear optical crystal.
[0170] Example 13
[0171] According to the chemical reaction formula YBr3 + 3H3PO4 → Y(PO3)3 + 3H2O↑ + 3HBr↑, Y(PO3)3 nonlinear optical crystals were prepared.
[0172] The preparation of Y(PO3)3 compound single-phase polycrystalline powder was carried out according to step a in Example 1:
[0173] Y(PO3)3 polycrystalline powder and flux PbCl2-P2O5 were mixed evenly in a molar ratio of 1:4:1 and placed into a platinum crucible. The mixture was heated to 830°C in a muffle furnace at a heating rate of 43°C / h and held at that temperature for 36h to obtain a mixed melt.
[0174] Preparation of seed crystals: After cooling the obtained mixed melt, transfer it to a single crystal growth furnace, heat it to 830℃ until the melt is uniform and transparent, and then slowly cool it to room temperature at a rate of 7.5℃ / h to obtain Y(PO3)3 seed crystals through spontaneous crystallization.
[0175] Crystal growth: The obtained seed crystal is fixed on the seed crystal rod. The seed crystal is fixed on the seed crystal rod in any direction. The seed crystal is lowered from the top of the crystal growth furnace and preheated for 24 minutes. The seed crystal is then lowered into a mixed melt of Y(PO3)3 and flux heated to 830℃ for remelting. The temperature is held constant for 19 minutes and then slowly cooled at a rate of 0.9℃ / day. The seed crystal rod is rotated at a speed of 37 rpm / min to grow the crystal. After the single crystal grows to the required size, the crystal is lifted off the liquid surface and cooled to room temperature at a rate of 44℃ / h. Then the crystal is taken out of the furnace to obtain the Y(PO3)3 nonlinear optical crystal.
[0176] Example 14
[0177] According to the chemical reaction formula YI3 + 3H3PO4 → Y(PO3)3 + 3H2O↑ + 3HI↑, Y(PO3)3 nonlinear optical crystal was prepared.
[0178] The preparation of Y(PO3)3 compound single-phase polycrystalline powder was carried out according to step a in Example 1:
[0179] Y(PO3)3 polycrystalline powder and flux PbO-PbCl2 were mixed evenly in a molar ratio of 1:4:1 and placed into a platinum crucible. The mixture was heated to 840°C in a muffle furnace at a heating rate of 45°C / h and held at that temperature for 42h to obtain a mixed melt.
[0180] Preparation of seed crystals: After cooling the obtained mixed melt, transfer it to a single crystal growth furnace, heat it to 840℃ until the melt is uniform and transparent, and then slowly cool it to room temperature at a rate of 0.8℃ / h to obtain Y(PO3)3 seed crystals through spontaneous crystallization.
[0181] Crystal growth: The obtained seed crystal is fixed on the seed crystal rod. The seed crystal is fixed on the seed crystal rod in any direction. The seed crystal is lowered from the top of the crystal growth furnace and preheated for 34 minutes. The seed crystal is then lowered into a mixed melt of Y(PO3)3 and flux heated to 840℃ for remelting. The temperature is held constant for 21 minutes and then slowly cooled at a rate of 2.3℃ / day. The seed crystal rod is rotated at a speed of 1 rpm / min to grow the crystal. After the single crystal grows to the required size, the crystal is lifted off the liquid surface and cooled to room temperature at a rate of 1℃ / h. Then the crystal is taken out of the furnace to obtain the Y(PO3)3 nonlinear optical crystal.
[0182] Example 15
[0183] The Y(PO3)3 crystals obtained in Examples 1-14 were processed according to matching directions, and then... Figure 2 As shown, when placed at position 3, at room temperature, a weak 532nm frequency-doubled green light output was observed using the 1064nm output of a Q-switched Nd:YAG laser as the light source.
[0184] Example 16
[0185] According to the chemical reaction formula Lu₂O₃ + 6NH₄H₂PO₄ → 2Lu(PO₃)₃ + 6NH₃↑ + 9H₂O↑, Lu(PO₃)₃ nonlinear optical crystal was prepared.
[0186] a. Mix Lu₂O₃ and NH₄H₂PO₄ in an agate mortar at a molar ratio of 1:6 and grind thoroughly until fully homogeneous. Then, place the mixture into a Φ60mm×60mm open-face corundum crucible, put it in a muffle furnace, slowly heat to 350℃, hold at that temperature for 24 hours, cool to room temperature, remove, grind a second time, transfer to another open-face corundum crucible, put it in a muffle furnace, heat to 650℃ again, hold at that temperature for 48 hours, slowly cool to room temperature, remove, grind to obtain lutetium phosphate compound single-phase polycrystalline powder, and then perform X-ray analysis on the product, such as... Figure 1 As shown in (b), the obtained X-ray spectrum is consistent with the X-ray spectrum obtained from the lutetium phosphate single crystal structure.
[0187] b. With a molar ratio of 1:5, the polycrystalline powder obtained in step a is mixed evenly with flux PbO, heated to 920℃ at a heating rate of 23℃ / h, and kept at the temperature for 32h to obtain a mixed melt.
[0188] c. Preparation of seed crystals: After cooling the mixed melt obtained in step b, transfer it to a single crystal growth furnace, heat it to 920℃ until the melt is uniform and transparent, and slowly cool it to room temperature at a rate of 0.5℃ / h to obtain Lu(PO3)3 seed crystals through spontaneous crystallization.
[0189] d. Crystal growth: Fix the seed crystal obtained in step c onto the seed crystal rod. The seed crystal can be fixed on the seed crystal rod in any direction. Lower the seed crystal from the top of the crystal growth furnace and preheat the seed crystal for 20 minutes. Then, lower the seed crystal into a mixed melt of Lu(PO3)3 and flux heated to 920°C for remelting. Maintain the temperature for 15 minutes and slowly cool it down at a rate of 0.5°C / day. Rotate the seed crystal rod at a speed of 12 rpm / min to grow the crystal. After the single crystal grows to the required size, lift the crystal off the liquid surface and cool it down to room temperature at a rate of 15°C / h. Then, take the crystal out of the furnace to obtain the Lu(PO3)3 nonlinear optical crystal.
[0190] Example 17
[0191] According to the chemical reaction formula Lu2(CO3)3·xH2O+6NH4H2PO4→2Lu(PO3)3+3CO2↑+6NH3↑+(9+x)H2O↑, Lu(PO3)3 nonlinear optical crystal was prepared.
[0192] The preparation of Lu(PO3)3 compound single-phase polycrystalline powder was carried out according to step a in Example 16:
[0193] Lu(PO3)3 polycrystalline powder and flux PbCl2 were mixed evenly at a molar ratio of 1:1 and placed into a platinum crucible. The mixture was heated to 800°C at a heating rate of 50°C / h and held at that temperature for 22h to obtain a mixed melt.
[0194] Preparation of seed crystals: After cooling the obtained mixed melt, transfer it to a single crystal growth furnace, heat it to 800℃ until the melt is uniform and transparent, and then cool it to room temperature at 3.5℃ / h to obtain Lu(PO3)3 seed crystals through spontaneous crystallization.
[0195] Crystal growth: The obtained seed crystal is fixed on the seed crystal rod. The seed crystal is fixed on the seed crystal rod in any direction. The seed crystal is lowered from the top of the crystal growth furnace and preheated for 60 minutes. The seed crystal is then lowered into a mixed melt of Lu(PO3)3 and flux heated to 800℃ for remelting. The temperature is kept constant for 45 minutes and then slowly cooled at a rate of 0.1℃ / day. The seed crystal rod is rotated at a speed of 22 rpm / min to grow the crystal. After the single crystal grows to the required size, the crystal is lifted off the liquid surface and cooled to room temperature at a rate of 20℃ / h. Then the crystal is taken out of the furnace to obtain the Lu(PO3)3 nonlinear optical crystal.
[0196] Example 18
[0197] According to the chemical reaction formula LuF3 + 3NH4H2PO4 → Lu(PO3)3 + 3NH3↑ + 3H2O↑ + 3HF↑, Lu(PO3)3 nonlinear optical crystal was prepared.
[0198] The preparation of Lu(PO3)3 compound single-phase polycrystalline powder was carried out according to step a in Example 16:
[0199] Lu(PO3)3 polycrystalline powder and flux PbO-P2O5 were mixed evenly in a molar ratio of 1:5:1 and placed into a platinum crucible. The mixture was heated to 880°C in a muffle furnace at a heating rate of 45°C / h and held at that temperature for 48h to obtain a mixed melt.
[0200] Preparation of seed crystals: After cooling the obtained mixed melt, transfer it to a single crystal growth furnace, heat it to 880℃ until the melt is uniform and transparent, and then slowly cool it to room temperature at a rate of 3.2℃ / h to obtain Lu(PO3)3 seed crystals through spontaneous crystallization.
[0201] Crystal growth: The obtained seed crystal is fixed on the seed crystal rod. The seed crystal is fixed on the seed crystal rod in any direction. The seed crystal is lowered from the top of the crystal growth furnace and preheated for 80 minutes. The seed crystal is then lowered into a mixed melt of Lu(PO3)3 and flux heated to 880°C for remelting. The temperature is kept constant for 80 minutes and then slowly cooled at a rate of 3°C / day. The seed crystal rod is rotated at a speed of 34 rpm / min to grow the crystal. After the single crystal grows to the required size, the crystal is lifted off the liquid surface and cooled to room temperature at a rate of 1°C / h. Then the crystal is taken out of the furnace to obtain the Lu(PO3)3 nonlinear optical crystal.
[0202] Example 19
[0203] According to the chemical reaction formula LuCl3 + 3NH4H2PO4 → Lu(PO3)3 + 3NH3↑ + 3H2O↑ + 3HCl↑, Lu(PO3)3 nonlinear optical crystal was prepared.
[0204] The preparation of Lu(PO3)3 compound single-phase polycrystalline powder was carried out according to step a in Example 16:
[0205] Lu(PO3)3 polycrystalline powder and flux PbO-PbCl2 were mixed evenly in a molar ratio of 1:5:1 and placed into a platinum crucible. The mixture was heated to 650°C in a muffle furnace at a heating rate of 1°C / h and held at that temperature for 20h to obtain a mixed melt.
[0206] Preparation of seed crystals: After cooling the obtained mixed melt, transfer it to a single crystal growth furnace, heat it to 650℃ until the melt is uniform and transparent, and then cool it to room temperature at a rate of 10℃ / h to obtain Lu(PO3)3 seed crystals through spontaneous crystallization.
[0207] Crystal growth: The obtained seed crystal is fixed on the seed crystal rod. The seed crystal is fixed on the seed crystal rod in any direction. The seed crystal is lowered from the top of the crystal growth furnace and preheated for 42 minutes. The seed crystal is then lowered into a mixed melt of Lu(PO3)3 and flux heated to 650°C for remelting. The temperature is kept constant for 30 minutes and then slowly cooled at a rate of 2.5°C / day. The seed crystal rod is rotated at a speed of 60 rpm / min to grow the crystal. After the single crystal grows to the required size, the crystal is lifted off the liquid surface and cooled to room temperature at a rate of 40°C / h. Then the crystal is taken out of the furnace to obtain the Lu(PO3)3 nonlinear optical crystal.
[0208] Example 20
[0209] According to the chemical reaction formula LuBr3 + 3NH4H2PO4 → Lu(PO3)3 + 3NH3↑ + 3H2O↑ + 3HBr↑, Lu(PO3)3 nonlinear optical crystal was prepared.
[0210] The preparation of Lu(PO3)3 compound single-phase polycrystalline powder was carried out according to step a in Example 16:
[0211] Lu(PO3)3 polycrystalline powder and flux PbO were mixed evenly in a molar ratio of 1:1 and placed into a platinum crucible. The mixture was heated to 780°C in a muffle furnace at a heating rate of 8°C / h and held at that temperature for 46h to obtain a mixed melt.
[0212] Preparation of seed crystals: After cooling the obtained mixed melt, transfer it to a single crystal growth furnace, heat it to 780℃ until the melt is uniform and transparent, and then cool it to room temperature at a rate of 0.8℃ / h to obtain Lu(PO3)3 seed crystals through spontaneous crystallization.
[0213] Crystal growth: The obtained seed crystal is fixed on the seed crystal rod. The seed crystal is fixed on the seed crystal rod in any direction. The seed crystal is lowered from the top of the crystal growth furnace and preheated for 15 minutes. The seed crystal is then lowered into a mixed melt of Lu(PO3)3 and flux heated to 780°C for remelting. The temperature is kept constant for 25 minutes and then slowly cooled at a rate of 3°C / day. The seed crystal rod is rotated at a speed of 32 rpm / min to grow the crystal. After the single crystal grows to the required size, the crystal is lifted off the liquid surface and cooled to room temperature at a rate of 60°C / h. Then the crystal is taken out of the furnace to obtain the Y(PO3)3 nonlinear optical crystal.
[0214] Example 21
[0215] According to the chemical reaction Lu₂O₃ + 3P₂O₅ → 2Lu(PO₃)₃, Lu(PO₃)₃ nonlinear optical crystals were prepared.
[0216] The preparation of Lu(PO3)3 compound single-phase polycrystalline powder was carried out according to step a in Example 16:
[0217] Lu(PO3)3 polycrystalline powder and flux PbO-P2O5 were mixed evenly in a molar ratio of 1:1:1 and placed into a platinum crucible. The mixture was heated to 900℃ in a muffle furnace at a rate of 38℃ / h and held at that temperature for 36h to obtain a mixed melt.
[0218] Preparation of seed crystals: After cooling the obtained mixed melt, transfer it to a single crystal growth furnace, heat it to 900℃ until the melt is uniform and transparent, and then slowly cool it to room temperature at a rate of 9℃ / h to obtain Lu(PO3)3 seed crystals through spontaneous crystallization.
[0219] Crystal growth: The obtained seed crystal is fixed on the seed crystal rod. The seed crystal is fixed on the seed crystal rod in any direction. The seed crystal is lowered from the top of the crystal growth furnace and preheated for 34 minutes. The seed crystal is then lowered into a mixed melt of Lu(PO3)3 and flux heated to 900°C for remelting. The temperature is kept constant for 50 minutes and then slowly cooled at a rate of 1°C / day. The seed crystal rod is rotated at a speed of 17 rpm / min to grow the crystal. After the single crystal grows to the required size, the crystal is lifted off the liquid surface and cooled to room temperature at a rate of 100°C / h. Then the crystal is taken out of the furnace to obtain the Lu(PO3)3 nonlinear optical crystal.
[0220] Example 22
[0221] According to the chemical reaction formula Lu2(CO3)3·xH2O+3P2O5→2Lu(PO3)3+3CO2↑+(3+x)H2O↑, Lu(PO3)3 nonlinear optical crystal was prepared.
[0222] The preparation of Lu(PO3)3 compound single-phase polycrystalline powder was carried out according to step a in Example 16:
[0223] Lu(PO3)3 polycrystalline powder and flux PbO-PbCl2 were mixed evenly in a molar ratio of 1:1:1 and placed into a platinum crucible. The mixture was heated to 750°C in a muffle furnace at a heating rate of 44°C / h and held at that temperature for 28h to obtain a mixed melt.
[0224] Preparation of seed crystals: After cooling the obtained mixed melt, transfer it to a single crystal growth furnace, heat it to 750℃ until the melt is uniform and transparent, and then slowly cool it to room temperature at a rate of 4.7℃ / h to obtain Lu(PO3)3 seed crystals through spontaneous crystallization.
[0225] Crystal growth: The obtained seed crystal is fixed on the seed crystal rod. The seed crystal is fixed on the seed crystal rod in any direction. The seed crystal is lowered from the top of the crystal growth furnace and preheated for 48 minutes. The seed crystal is then lowered into a mixed melt of Lu(PO3)3 and flux heated to 750°C for remelting. The temperature is held constant for 65 minutes and then slowly cooled at a rate of 0.3°C / day. The seed crystal rod is rotated at a speed of 17 rpm / min to grow the crystal. After the single crystal grows to the required size, the crystal is lifted off the liquid surface and cooled to room temperature at a rate of 80°C / h. Then the crystal is taken out of the furnace to obtain the Lu(PO3)3 nonlinear optical crystal.
[0226] Example 23
[0227] According to the chemical reaction formula Lu₂O₃ + 6H₃PO₄ → 2Lu(PO₃)₃ + 9H₂O↑, Lu(PO₃)₃ nonlinear optical crystal was prepared.
[0228] The preparation of Lu(PO3)3 compound single-phase polycrystalline powder was carried out according to step a in Example 16:
[0229] Lu(PO3)3 polycrystalline powder and flux PbCl2-P2O5 were mixed evenly in a molar ratio of 1:5:1 and placed into a platinum crucible. The mixture was heated to 850°C in a muffle furnace at a heating rate of 17°C / h and held at that temperature for 30h to obtain a mixed melt.
[0230] Preparation of seed crystals: After cooling the obtained mixed melt, transfer it to a single crystal growth furnace, heat it to 850℃ until the melt is uniform and transparent, and then slowly cool it to room temperature at a rate of 1.5℃ / h to obtain Lu(PO3)3 seed crystals through spontaneous crystallization.
[0231] Crystal growth: The obtained seed crystal is fixed on the seed crystal rod. The seed crystal is fixed on the seed crystal rod in any direction. The seed crystal is lowered from the top of the crystal growth furnace and preheated for 54 min. The seed crystal is then lowered into a mixed melt of Lu(PO3)3 and flux heated to 850℃ for remelting. The temperature is held constant for 75 min and then slowly cooled at a rate of 0.8℃ / day. The seed crystal rod is rotated at a speed of 15 rpm / min to grow the crystal. After the single crystal grows to the required size, the crystal is lifted off the liquid surface and cooled to room temperature at a rate of 25℃ / h. Then the crystal is taken out of the furnace to obtain the Lu(PO3)3 nonlinear optical crystal.
[0232] Example 24
[0233] (13) Prepare Lu(PO3)3 nonlinear optical crystals according to the chemical reaction formula Lu2(CO3)3·xH2O+6H3PO4→2Lu(PO3)3+3CO2↑+(9+x)H2O↑:
[0234] The preparation of Lu(PO3)3 compound single-phase polycrystalline powder was carried out according to step a in Example 16:
[0235] Lu(PO3)3 polycrystalline powder and flux PbCl2 were mixed evenly at a molar ratio of 1:5 and placed into a platinum crucible. The mixture was heated to 700°C in a muffle furnace at a heating rate of 25°C / h and held at that temperature for 24h to obtain a mixed melt.
[0236] Preparation of seed crystals: After cooling the obtained mixed melt, transfer it to a single crystal growth furnace, heat it to 700℃ until the melt is uniform and transparent, and then slowly cool it to room temperature at a rate of 2.8℃ / h to obtain Lu(PO3)3 seed crystals through spontaneous crystallization.
[0237] Crystal growth: The obtained seed crystal is fixed on the seed crystal rod. The seed crystal is fixed on the seed crystal rod in any direction. The seed crystal is lowered from the top of the crystal growth furnace and preheated for 36 minutes. The seed crystal is then lowered into a mixed melt of Lu(PO3)3 and flux heated to 700°C for remelting. The temperature is kept constant for 60 minutes and then slowly cooled at a rate of 1.8°C / day. The seed crystal rod is rotated at a speed of 8 rpm / min to grow the crystal. After the single crystal grows to the required size, the crystal is lifted off the liquid surface and cooled to room temperature at a rate of 8°C / h. Then the crystal is taken out of the furnace to obtain the Lu(PO3)3 nonlinear optical crystal.
[0238] Example 25
[0239] According to the chemical reaction formula LuF3 + 3H3PO4 → Lu(PO3)3 + 3HF↑ + 3H2O↑, Lu(PO3)3 nonlinear optical crystal was prepared.
[0240] The preparation of Lu(PO3)3 compound single-phase polycrystalline powder was carried out according to step a in Example 16:
[0241] Lu(PO3)3 polycrystalline powder and flux PbCl2-P2O5 were mixed evenly in a molar ratio of 1:1:1 and placed into a platinum crucible. The mixture was heated to 780°C in a muffle furnace at a heating rate of 29°C / h and held at that temperature for 44h to obtain a mixed melt.
[0242] Preparation of seed crystals: After cooling the obtained mixed melt, transfer it to a single crystal growth furnace, heat it to 780℃ until the melt is uniform and transparent, and then slowly cool it to room temperature at a rate of 4.5℃ / h to obtain Lu(PO3)3 seed crystals through spontaneous crystallization.
[0243] Crystal growth: The obtained seed crystal is fixed on the seed crystal rod. The seed crystal is fixed on the seed crystal rod in any direction. The seed crystal is lowered from the top of the crystal growth furnace and preheated for 55 minutes. The seed crystal is then lowered into a mixed melt of Lu(PO3)3 and flux heated to 780°C for remelting. The temperature is held constant for 48 minutes and then slowly cooled at a rate of 2.2°C / day. The seed crystal rod is rotated at a speed of 45 rpm / min to grow the crystal. After the single crystal grows to the required size, the crystal is lifted off the liquid surface and cooled to room temperature at a rate of 10°C / h. Then the crystal is taken out of the furnace to obtain the Lu(PO3)3 nonlinear optical crystal.
[0244] Example 26
[0245] According to the chemical reaction formula LuCl3 + 3H3PO4 → Lu(PO3)3 + 3H2O↑ + 3HCl↑, Lu(PO3)3 nonlinear optical crystal was prepared.
[0246] The preparation of Lu(PO3)3 compound single-phase polycrystalline powder was carried out according to step a in Example 16:
[0247] Lu(PO3)3 polycrystalline powder and flux PbO-PbCl2 were mixed evenly in a molar ratio of 1:3:1 and placed into a platinum crucible. The mixture was heated to 680°C in a muffle furnace at a heating rate of 12°C / h and held at that temperature for 32h to obtain a mixed melt.
[0248] Preparation of seed crystals: After cooling the obtained mixed melt, transfer it to a single crystal growth furnace, heat it to 680℃ until the melt is uniform and transparent, and then slowly cool it to room temperature at a rate of 6.5℃ / h to obtain Lu(PO3)3 seed crystals through spontaneous crystallization.
[0249] Crystal growth: The seed crystal is fixed on the seed crystal rod in any orientation. The seed crystal is lowered from the top of the crystal growth furnace and preheated for 72 minutes. The seed crystal is then lowered into a mixed melt of Lu(PO3)3 and flux heated to 680°C for remelting. The temperature is held constant for 72 minutes and then slowly cooled at a rate of 2.8°C / day. The seed crystal rod is rotated at 55 rpm / min to grow the crystal. Once the single crystal has grown to the required size, it is lifted off the liquid surface and cooled to room temperature at a rate of 70°C / h. The crystal is then removed from the furnace to obtain the Lu(PO3)3 nonlinear optical crystal.
[0250] Example 27
[0251] According to the chemical reaction formula LuBr3 + 3H3PO4 → Lu(PO3)3 + 3H2O↑ + 3HBr↑, Lu(PO3)3 nonlinear optical crystal was prepared.
[0252] The preparation of Lu(PO3)3 compound single-phase polycrystalline powder was carried out according to step a in Example 16:
[0253] Lu(PO3)3 polycrystalline powder and flux PbCl2 were mixed evenly in a molar ratio of 1:2 and placed into a platinum crucible. The mixture was heated to 800°C in a muffle furnace at a heating rate of 5°C / h and held at that temperature for 34h to obtain a mixed melt.
[0254] Preparation of seed crystals: After cooling the obtained mixed melt, transfer it to a single crystal growth furnace, heat it to 800℃ until the melt is uniform and transparent, and then slowly cool it to room temperature at a rate of 0.8℃ / h to obtain Lu(PO3)3 seed crystals through spontaneous crystallization.
[0255] Crystal growth: The obtained seed crystal is fixed on the seed crystal rod. The seed crystal is fixed on the seed crystal rod in any direction. The seed crystal is lowered from the top of the crystal growth furnace and preheated for 45 minutes. The seed crystal is then lowered into a mixed melt of Lu(PO3)3 and flux heated to 800℃ for remelting. The temperature is held constant for 18 minutes and then slowly cooled at a rate of 1.2℃ / day. The seed crystal rod is rotated at a speed of 48 rpm / min to grow the crystal. After the single crystal grows to the required size, the crystal is lifted off the liquid surface and cooled to room temperature at a rate of 75℃ / h. Then the crystal is taken out of the furnace to obtain the Lu(PO3)3 nonlinear optical crystal.
[0256] Example 28
[0257] The arbitrary Lu(PO3)3 crystals obtained in Examples 16-27 were processed according to matching directions, and then... Figure 2 As shown, when placed at position 3, at room temperature, a weak 532nm frequency-doubled green light output was observed using the 1064nm output of a Q-switched Nd:YAG laser as the light source.
[0258] As can be seen from the above embodiments, the preparation method provided by the present invention can obtain Y(PO3)3 and Lu(PO3)3 nonlinear optical crystals with centimeter-sized crystals. By using a large-sized crucible and extending the crystal growth period, correspondingly large-sized nonlinear optical crystals Y(PO3)3 and Lu(PO3)3 can be obtained. Y(PO3)3 and Lu(PO3)3 nonlinear optical crystals are easy to grow, transparent and unencapsulated, and have the advantages of fast growth rate, low cost, and easy acquisition of large-sized crystals.
[0259] Figure 4 Thermogravimetric-differential thermal curves of single-phase polycrystalline powder prepared in embodiments of the present invention are shown. Figure 4 In Figure (a), the thermogravimetric-differential thermal curve of the single-phase polycrystalline powder of Y(PO3)3 compound prepared in Example 1 is shown. Figure 4 (b) in the figure shows the thermogravimetric-differential thermal curve of the single-phase polycrystalline powder of Lu(PO3)3 compound prepared in Example 16. Figure 4 It can be concluded that the Y(PO3)3 compound single-phase polycrystalline powder and Lu(PO3)3 compound single-phase polycrystalline powder prepared in the embodiments of the present invention did not exhibit significant weight loss during the slow temperature rise from room temperature to 1000℃, and no obvious endothermic or exothermic peaks appeared on the DTA curve. This preliminarily confirms that these two nonlinear optical crystals possess good thermal stability.
[0260] Figure 5 The infrared spectrum of the single-phase polycrystalline powder prepared in an embodiment of the present invention is shown below. Figure 5 Image (a) in the image is the infrared spectrum of the single-phase polycrystalline powder of Y(PO3)3 compound prepared in Example 1. Figure 5(b) is the infrared spectrum of the Lu(PO3)3 compound single-phase polycrystalline powder prepared in Example 16. Figure 5 The following conclusions were drawn to confirm the characteristic vibrational modes of the P-atom anionic group: [Vibrational modes are described in the range of 3500 to 1600 cm⁻¹]. -1 No OH- was found within the range - Vibrational bands associated with H₂O. A(PO₃)₃ (A = Y or Lu) at 1257 and 1255 cm⁻¹. -1 And 1097, 1106 and 1030cm -1 The absorption peaks are characteristic peaks of the PO stretching vibration. 772, 749, 711, and 709 cm⁻¹ -1 The absorption peak is a characteristic peak of the symmetric and asymmetric tensile vibration of POP, while the 512 cm⁻¹ peak is a characteristic peak of the symmetric and asymmetric tensile vibration of POP. -1 and 484-546cm -1 The absorption peaks are mainly characteristic peaks of the fundamental vibration of the PO4 group. Infrared spectroscopy further confirms the presence of [PO3] in the crystal. ∞ The presence of functional groups.
[0261] Figure 6 The image shows the UV-Vis diffuse reflectance spectrum of the single-phase polycrystalline powder prepared in an embodiment of the present invention. Figure 6 (a) in the image is the UV-Vis diffuse reflectance spectrum of the single-phase polycrystalline powder of Y(PO3)3 compound prepared in Example 1. Figure 6 (b) is the UV-Vis diffuse reflectance spectrum of the Lu(PO3)3 compound single-phase polycrystalline powder prepared in Example 16. Figure 6 The following conclusions were drawn from the identification of the characteristic vibrational modes of the P atom anionic group:
[0262] Both materials have an ultraviolet absorption cutoff edge of less than 200 nm and a reflectance of 50%-60%. According to the Kubelka-Munk function... (R represents reflectivity). The band gap values of Y(PO3)3 and Lu(PO3)3 are both greater than 6.2 eV, indicating that the two crystals mentioned above belong to deep ultraviolet optical crystals.
[0263] Using the preparation method and applications of yttrium phosphate and lutetium phosphate nonlinear optical crystals described in this invention, large-size Y(PO3)3 and Lu(PO3)3 nonlinear optical crystals are obtained. Based on the crystallographic data of the crystals, the crystal blanks are oriented, and the crystals are cut according to the required angle, thickness, and cross-sectional dimensions. The light-transmitting surfaces of the crystals are polished, and they can then be used as nonlinear optical devices. Both Y(PO3)3 and Lu(PO3)3 nonlinear optical crystals have advantages such as light transmission up to the ultraviolet region, stable physicochemical properties, resistance to deliquescence, and ease of processing and storage.
[0264] Although the above embodiments have provided a detailed description of the present invention, they are only some embodiments of the present invention, and not all embodiments. Other embodiments can be obtained based on these embodiments without creative effort, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preparing a phosphate nonlinear optical crystal, characterized in that, The chemical formula of the phosphate nonlinear optical crystal is shown in Formula 1: A(PO3)3 Equation 1; In Equation 1: A is Y or Lu; The phosphate nonlinear optical crystal belongs to the monoclinic crystal system and has a space group of Cc. The molecular weight of the yttrium phosphate nonlinear optical crystal is 325.82, and its unit cell parameters are a=14.1535(13) Å, b=6.7016(7) Å, c=10.0726(17) Å, β=127.581(2)°, Z=4, and the unit cell volume is 757.14(17) Å. 3 ; The lutetium phosphate nonlinear optical crystal has a molecular weight of 411.88, cell parameters of a = 13.9731(7) Å, b = 20.0291(10) Å, c = 9.9585(4) Å, β = 127.3590(10)°, Z = 12, and a unit cell volume of 2215.30(18) Å. 3 ; The preparation method includes the following steps: A mixed melt is prepared using a compound containing A, a compound containing P, and a flux. The flux includes one or more of PbO, PbCl2, PbO-P2O5, PbCl2-P2O5, and PbO-PbCl2. The compound containing A is a compound containing Y or Lu, wherein the purity of the Y-containing compound is ≥99.9%, and the Y-containing compound includes one or more of Y2O3, YF3, YCl3, YBr3, YI3, and Y2(CO3)3·3H2O. The purity of the Lu-containing compound is ≥99.9%, and the Lu-containing compound includes one or more of Lu2O3, LuF3, LuCl3, LuBr3, and Lu2(CO3)3·xH2O. The purity of the P-containing compound is ≥99.9%, and the P-containing compound includes one or more of NH4H2PO4, H3PO4, and P2O5. The purity of the flux is ≥99.9%. The method for preparing the mixed melt includes the following steps: A compound containing A and a compound containing P are mixed according to the molar ratio of A to P in the chemical formula shown in Formula 1, and then calcined to obtain a polycrystalline phosphate product; the calcination temperature is 600–800℃, and the holding time is 36–48 h; the polycrystalline phosphate product is mixed with a flux and then melted to obtain a mixed melt; the molar ratio of the polycrystalline phosphate product to the flux is 1:1–5; the melting temperature is 650–920℃, and the holding time is 20–48 h, and then cooled to room temperature. The heating rate to the melting temperature is 1–50 °C / h; or the preparation method of the mixed melt includes the following steps: mixing a compound containing A, a compound containing P, and a flux, and then melting the mixture to obtain a mixed melt; the molar ratio of the compound containing A, the compound containing P, and the flux is 1:3–6:1–5; the melting temperature is 650–920 °C, the holding time is 20–48 h, and the heating rate from room temperature to the melting temperature is 1–50 °C / h; The mixed melt is first cooled to room temperature to obtain phosphate seed crystals, and the cooling rate of the first cooling is 0.5 to 10 °C / h; The phosphate seed crystal is fixed on a seed crystal rod, and the phosphate seed crystal fixed on the seed crystal rod is preheated at an ambient temperature of 650–920°C for 15–80 min. Then, the preheated seed crystal is lowered into a mixed melt for single crystal growth, and an initial phosphate single crystal is obtained on the seed crystal rod. The conditions for single crystal growth include: the mixed melt is held at a certain temperature and then cooled, and the seed crystal rod rotates. The holding temperature of the mixed melt is 650–920°C, and the holding time is 15–80 min. The cooling rate is 0.1–3°C / day. The rotation speed of the seed crystal rod is 1–60 rpm. The initial phosphate single crystal is cooled to room temperature to obtain a phosphate nonlinear optical crystal with the chemical formula shown in Formula 1. The cooling rate of the second cooling is 1 to 100 °C / h. The phosphate nonlinear optical crystal is used as a deep ultraviolet nonlinear optical crystal.
2. The application of the phosphate nonlinear optical crystal prepared by the method of claim 1 in all-solid-state lasers.
3. The application of the phosphate nonlinear optical crystal prepared by the method of claim 1 in nonlinear optical devices, characterized in that, The nonlinear optical devices include frequency multipliers, up or down frequency converters, optical parametric oscillators, or laser frequency converters.