Super-hydrophobic electromagnetic shielding paper and preparation method and application thereof
By using superhydrophobic electromagnetic shielding paper with gradient distribution of carbon fibers, metal-plated glass fibers, and glass fiber structures, the problems of low shielding strength, easy failure, and insufficient mechanical properties of existing shielding papers are solved, achieving highly efficient electromagnetic shielding and long-life superhydrophobic effect.
Patent Information
- Application Number
- CN202411772251.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-12-04
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-12-04
AI Technical Summary
Existing electromagnetic shielding paper has low shielding strength, is prone to failure, has insufficient mechanical properties, short service life, and poor hydrophobicity.
A superhydrophobic electromagnetic shielding paper with a gradually changing density gradient is formed by using carbon fiber, metal-plated glass fiber and glass fiber in a gradient distribution structure and bonding them with resin adhesive. This is combined with a non-woven fabric layer to enhance mechanical strength.
It achieves high-efficiency electromagnetic shielding performance (average shielding effectiveness ≥25dB from 8 to 12.4GHz), long-term stability, tensile strength ≥9N/15mm, hydrophobic angle ≥147°, and is suitable for harsh environments.
Smart Images

Figure CN119465695B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electromagnetic shielding materials technology, and in particular to a superhydrophobic electromagnetic shielding paper, its preparation method, and its application. Background Technology
[0002] With the rapid development of communication technology and the widespread use of electronic devices, electromagnetic waves have brought convenience to people, but at the same time, they have also had certain impacts on human health and precision electronic devices. Therefore, electromagnetic shielding materials have become one of the indispensable materials in production and daily life.
[0003] In existing technologies, electromagnetic shielding paper is mainly constructed from metal-based fibers, metal particles, carbon-based fibers, carbon particles, or a mixture of several materials with plant fibers. For example, some literature reports using plant fibers as the skeleton fibers, filled with nickel powder, silicon carbide, and ferrite / glass fibers; others report using a mixture of chopped carbon fibers and plant fibers; still others report using a mixture of lignocellulose nanofibers and plant fiber surface-modified MXene. However, the shielding strength of these electromagnetic shielding papers is relatively low, and their shielding performance is prone to failure. Furthermore, the shielding paper may be subjected to tensile stress during use, and the current shielding paper has relatively low mechanical properties, making it prone to breakage. These defects result in a short service life and unsatisfactory performance of existing electromagnetic shielding paper. Summary of the Invention
[0004] The main objective of this invention is to provide a superhydrophobic electromagnetic shielding paper, its preparation method, and its application. The technical problem to be solved is how to prepare a superhydrophobic electromagnetic shielding paper that has high shielding performance (average shielding effectiveness ≥25dB at 8-12.4GHz) and can maintain its shielding performance for a long time with a long service life; at the same time, it also has high mechanical strength (tensile strength ≥9N / 15mm) and good hydrophobicity (hydrophobic angle ≥147°), thus making it more suitable for practical use.
[0005] The objective of this invention and the technical problem it solves are achieved through the following technical solution. A method for preparing superhydrophobic electromagnetic shielding paper according to this invention includes the following steps:
[0006] S11. Carbon fiber, metal-plated glass fiber, and glass fiber are dispersed in water and stirred evenly to obtain a fiber slurry; wherein the mass ratio of carbon fiber, metal-plated glass fiber, and glass fiber is 0.1-0.4:0.1-0.4:1.
[0007] S12 allows the fiber pulp to settle naturally, then presses and dries to obtain a first shielding paper with a gradient density distribution.
[0008] S13 Apply resin adhesive to the surface of the first shielding paper and dry it to obtain superhydrophobic electromagnetic shielding paper.
[0009] The objectives of this invention and the technical problems it addresses can be further achieved by the following technical measures.
[0010] Preferably, in the aforementioned preparation method, the preparation steps of the fiber pulp are as follows:
[0011] S21. Carbon fiber and first glass fiber are dispersed in water and stirred evenly to obtain pre-entangled fiber slurry; wherein the mass ratio of carbon fiber to first glass fiber is 0.2 to 0.9:1;
[0012] S22 Disperse the metallized glass fiber, the second glass fiber, and the pre-entangled fiber slurry in water and stir evenly to obtain a fiber slurry; wherein the mass ratio of the metallized glass fiber and the second glass fiber is 0.2 to 0.9:1; the ratio of the sum of the mass of the carbon fiber and the first glass fiber to the sum of the mass of the metallized glass fiber and the second glass fiber is 0.2 to 1:1.
[0013] Preferably, in the aforementioned preparation method, the mass ratio of carbon fiber to metal-plated glass fiber is 0.6 to 1.7:1; and the mass ratio of the sum of carbon fiber and metal-plated glass fiber to the glass fiber is 0.35 to 0.70:1.
[0014] Preferably, in the aforementioned preparation method, the diameter of the first glass fiber is ≤0.5μm; the diameter of the second glass fiber is ≤1.5μm; and the diameter of the metal-plated glass fiber is ≤5μm.
[0015] Preferably, in the aforementioned preparation method, the step of applying a resin adhesive to the surface of the first shielding paper is as follows:
[0016] S51 The first shielding paper is immersed in a deionized aqueous solution of acrylic resin for ≤1 min to obtain the second shielding paper;
[0017] S52 then sprays an ethanol solution of fluoroalkylsilane onto the second shielding paper.
[0018] The objective of this invention and the technical problem it solves are achieved through the following technical solution. A superhydrophobic electromagnetic shielding paper according to this invention comprises:
[0019] Metal-plated glass fiber layer;
[0020] A glass fiber layer is disposed adjacent to the metal-plated glass fiber layer;
[0021] A carbon fiber layer is disposed adjacent to the glass fiber layer; glass fibers on one side of the glass fiber layer are inserted into and wound around the carbon fiber in the carbon fiber layer, and glass fibers on the opposite side are inserted into and wound around the metal-plated glass fiber in the metal-plated glass fiber layer; along the thickness direction of the superhydrophobic electromagnetic shielding paper, the metal-plated glass fiber layer, the glass fiber layer, and the carbon fiber layer have a density gradient structure; the metal-plated glass fiber layer, the glass fiber layer, and the carbon fiber layer are bonded together by a resin adhesive.
[0022] The objectives of this invention and the technical problems it addresses can be further achieved by the following technical measures.
[0023] Preferably, the aforementioned superhydrophobic electromagnetic shielding paper has a tensile strength ≥9N / 15mm, an average shielding effectiveness ≥25dB from 8 to 12.4GHz, and a hydrophobic angle ≥147°.
[0024] Preferably, the aforementioned superhydrophobic electromagnetic shielding paper further includes:
[0025] The non-woven fabric layer is disposed on both sides of the superhydrophobic electromagnetic shielding paper and is bonded to the metal-plated glass fiber layer and the carbon fiber layer respectively by the resin adhesive.
[0026] Preferably, the aforementioned superhydrophobic electromagnetic shielding paper is prepared according to the aforementioned preparation method.
[0027] The objective of this invention and the technical problem it solves are achieved by the following technical solution: An application of the aforementioned superhydrophobic electromagnetic shielding paper in the field of electromagnetic shielding materials, according to this invention.
[0028] By employing the above technical solution, the superhydrophobic electromagnetic shielding paper, its preparation method, and its application proposed in this invention have at least the following advantages:
[0029] This invention proposes a superhydrophobic electromagnetic shielding paper, its preparation method, and its application. The method involves preparing a fiber slurry by rationally proportioning carbon fiber, metallized glass fiber, and glass fiber. This slurry is then allowed to settle naturally, forming a shielding paper with a gradient density distribution. Finally, a resin adhesive is used to bond the various fibers together, resulting in the superhydrophobic electromagnetic shielding paper of this invention. The superhydrophobic electromagnetic shielding paper obtained by this invention exhibits good overall performance, possessing high shielding performance with an average shielding efficiency ≥25dB in the 8–12.4 GHz range. Further optimization using aluminized glass fiber as the metallized glass fiber further improves the average shielding efficiency in the 8–12.4 GHz range to ≥29dB. Further optimization of the fiber ratio further increases the average shielding efficiency in the 8–12.4 GHz range to over 40dB. Furthermore, the electromagnetic shielding efficiency in this invention comes from the combination of carbon fiber and metallized fiber, eliminating the risk of easily detached metal fibers. The material consists of granules, and each fiber surface is coated with a resin binder, preventing it from oxidizing and peeling off when exposed to water or air, thus maintaining good electromagnetic shielding performance over a long period. Furthermore, the optimal ratio of carbon fiber, metallized glass fiber, and glass fiber in this invention results in high mechanical strength, preventing damage from tensile stress; its tensile strength is ≥9N / 15mm, and through optimized fiber ratios and parameter design, its tensile strength can reach as high as 16.5N / 15mm. Its excellent electromagnetic shielding performance retention and high mechanical strength ensure a long service life. Furthermore, the resin binder coating on the fiber surface gives the shielding paper good hydrophobicity, further ensuring a long service life. Finally, the electromagnetic shielding paper of this invention can maintain stable performance even in harsh operating environments.
[0030] The above description is merely an overview of the technical solution of the present invention. In order to better understand the technical means of the present invention and to implement it in accordance with the contents of the specification, the preferred embodiments of the present invention are described in detail below with reference to the accompanying drawings. Attached Figure Description
[0031] Figure 1 This is a schematic diagram of the superhydrophobic electromagnetic shielding structure of the present invention;
[0032] Figure 2 Cross-sectional view of the superhydrophobic electromagnetic shielding paper in Embodiment 1 of the present invention;
[0033] Figure 3 This is a diagram showing the Al element distribution of the superhydrophobic electromagnetic shielding paper in Embodiment 1 of the present invention;
[0034] Figure 4 This is a C element distribution diagram of the superhydrophobic electromagnetic shielding paper in Embodiment 1 of the present invention;
[0035] Figure 5 This is a diagram illustrating the electromagnetic shielding effectiveness of the superhydrophobic electromagnetic shielding paper in Embodiment 1 of the present invention.
[0036] Figure 6 This is a microscope photograph of the hydrophobic angle measured by the superhydrophobic electromagnetic shielding paper in Embodiment 1 of the present invention. Detailed Implementation
[0037] To further illustrate the technical means and effects adopted by the present invention to achieve its intended purpose, the following, in conjunction with the accompanying drawings and preferred embodiments, provides a detailed description of the specific implementation methods, structures, features, and effects of a superhydrophobic electromagnetic shielding paper, its preparation method, and its application according to the present invention. In the following description, different "embodiments" or "embodiments" do not necessarily refer to the same embodiment. Furthermore, specific features, structures, or characteristics in one or more embodiments can be combined in any suitable manner.
[0038] This invention proposes a superhydrophobic electromagnetic shielding paper, as shown in the attached figure. Figure 1 As shown, it includes:
[0039] Metal-plated glass fiber layer 1;
[0040] A glass fiber layer 2 is disposed adjacent to the metal-plated glass fiber layer;
[0041] A carbon fiber layer 3 is disposed adjacent to the glass fiber layer; glass fibers on one side of the glass fiber layer penetrate and wrap around the carbon fibers in the carbon fiber layer, and glass fibers on the opposite side penetrate and wrap around the metal-plated glass fiber layer; along the thickness direction of the superhydrophobic electromagnetic shielding paper, the metal-plated glass fiber layer, the glass fiber layer, and the carbon fiber layer have a density gradient structure; the metal-plated glass fiber layer, the glass fiber layer, and the carbon fiber layer are bonded together by a resin adhesive.
[0042] In the above technical solution, although it is described as a three-layer structure according to the different fiber materials, in reality, glass fiber not only exists as the middle layer, but also a portion of glass fiber extends downward into the metal-plated glass fiber layer to form an entangled structure with the metal-plated glass fiber layer, forming a transition layer from the metal-plated glass fiber layer to the glass fiber layer; a portion of glass fiber extends upward into the carbon fiber layer to form an entangled structure with the carbon fiber layer, forming a transition layer from the carbon fiber layer to the glass fiber layer. As described above, the superhydrophobic electromagnetic shielding paper of the present invention actually consists of, from bottom to top, a metal-plated glass fiber layer / a transition layer formed by the entanglement of metal-plated glass fiber and glass fiber / a glass fiber layer / a transition layer formed by the entanglement of carbon fiber and glass fiber / a carbon fiber layer. Because carbon fiber has a lower density and metal-plated glass fiber has a higher density, the two are difficult to bond together; the present invention cleverly utilizes glass fiber with a medium density as a medium, and effectively combines the difficult-to-bond carbon fiber and metal-plated glass fiber through the technical solution of the present invention, forming an overall structure with good bonding strength; the superhydrophobic electromagnetic shielding paper of the present invention has a density gradient structure from the metal-plated glass fiber layer to the carbon fiber layer. The layered material with a gradually changing density gradient is beneficial for enhancing the process of electromagnetic wave absorption and reflection, thereby enhancing the shielding effectiveness of the shielding paper.
[0043] Furthermore, in order to ensure that the layered material with the gradually changing density gradient can maintain its structure stably over a long period of time, the present invention uses a resin adhesive to bond the fiber layers together. On the one hand, this stabilizes the structure, and on the other hand, the resin adhesive can also form a coating structure on the fibers, thereby improving the hydrophobicity of the shielding paper.
[0044] In the above technical solutions, both carbon fiber and metal-plated glass fiber have good electromagnetic shielding effects. Carbon fiber has a thinner diameter, which is beneficial to the strength of the shielding paper, but it is expensive. Metal-plated glass fiber, on the other hand, has a thicker diameter and lower strength, but its cost is also lower. This invention organically combines carbon fiber and metal-plated glass fiber into a whole through the above technical solutions, ensuring both the mechanical strength of the shielding paper and its electromagnetic shielding effectiveness, while also effectively controlling its cost. In some specific embodiments of this invention, the superhydrophobic electromagnetic shielding paper has a tensile strength ≥9N / 15mm and an average shielding effectiveness ≥25dB from 8 to 12.4GHz.
[0045] This invention also proposes a method for preparing superhydrophobic electromagnetic shielding paper, which includes the following steps:
[0046] The first step is to prepare the fiber slurry. Specifically, carbon fiber, metallized glass fiber, and glass fiber are dispersed in water and stirred evenly to obtain the fiber slurry. To ensure good synergy among the three fibers and achieve optimal overall performance, the preferred mass ratio of carbon fiber, metallized glass fiber, and glass fiber is 0.1–0.4:0.1–0.4:1. Since excessively coarse fibers may affect the formation of the shielding paper, to ensure successful film formation of the shielding paper prepared by this invention, the preferred diameter of all fibers is ≤15 μm. The stirring process parameters can be selected according to conventional methods in the art, and this invention does not impose specific limitations on them. The proportion of water added during slurry preparation is not specifically limited, as long as it allows for smooth fiber dispersion and sufficient fiber dispersion and entanglement.
[0047] Furthermore, in order to ensure high shielding strength and good mechanical properties of the shielding paper, the present invention further preferably has a fiber diameter of ≤0.5μm for the first glass fiber, a fiber diameter of ≤1.5μm for the second glass fiber, and a diameter of ≤5μm for the metal-plated glass fiber.
[0048] The second step is to allow the fiber pulp to settle naturally, press, and dry it to obtain a first shielding paper with a density gradient distribution.
[0049] In the above steps, after the fiber pulp is prepared, it is first allowed to stand, and then allowed to settle naturally. Natural settling can be performed using conventional methods in the art; in one specific embodiment of the invention, the drain valve of the fiber pulp container is opened, and it is allowed to settle naturally on the forming wire of the paper machine through suction filtration to form a gradient structure. The invention does not specifically limit this method. Pressing and drying can also be performed using conventional methods in the art, as long as the moisture content is reduced to a set level. The invention does not specifically limit this method. For example, drying can be carried out at a temperature of 80℃ to 160℃ depending on the fiber properties.
[0050] Because carbon fiber has an extremely fine diameter and a very light specific gravity, while metal-coated glass fiber has a relatively high specific gravity, it is difficult to organically fuse the two together. In order to form a complete material, this invention preferably uses glass fiber to link the two. The specific gravity of glass fiber is between that of carbon fiber and metal-coated glass fiber. Through natural settling, the glass fiber can be mainly positioned between the carbon fiber and the metal-coated glass fiber. To strengthen the link between the three, one side of the glass fiber extends into the interior of the carbon fiber, forming an intertwined link with the carbon fiber; the other side of the glass fiber extends into the interior of the metal-coated glass fiber, forming an intertwined link with the metal-coated glass fiber; thus, the carbon fiber and the metal-coated glass fiber are linked into a whole by the glass fiber.
[0051] To enhance the fusion effect between carbon fiber and glass fiber, the present invention preferably follows these steps when preparing the fiber slurry:
[0052] Carbon fibers and first glass fibers are dispersed in water and stirred evenly to obtain a pre-entangled fiber slurry. In this step, the first glass fiber is not limited by its material or specifications, but by the timing of its addition, indicating that it is first mixed separately with the carbon fibers to pre-bring them into contact, thereby forming a pre-entangled linking structure. To better control the proportion of the pre-entangled structure between the carbon fibers and the glass fibers, the present invention preferably uses a mass ratio of carbon fibers to first glass fibers of 0.2 to 0.9:1.
[0053] Next, the metallized glass fiber, the second glass fiber, and the pre-entangled fiber slurry are dispersed in water and stirred evenly to obtain a fiber slurry. In this step, the second glass fiber is not limited by its material or specifications, but by the timing of its addition. This indicates that it is mixed with the pre-entangled carbon fiber and glass fiber mixture and the metallized glass fiber at a later stage, allowing the three fibers to come into contact and undergo secondary entanglement, forming a fiber slurry with a specific entanglement structure. This ensures that it will not delaminate in subsequent process steps, thus guaranteeing the strength of the electromagnetic shielding paper of this invention. To ensure that the second glass fiber can form an intermediate dielectric layer in subsequent processes while also extending into the carbon fiber layer and the metallized glass fiber layer on both sides, the mass ratio of the metallized glass fiber to the second glass fiber is preferably 0.2 to 0.9:1. That is, by adding a larger amount of glass fiber to the fiber slurry system, the carbon fiber and the metallized glass fiber are organically fused into a strong overall structure.
[0054] Extensive experimental analysis revealed that when the mass ratio of carbon fiber to metal-plated glass fiber is controlled at 0.6–1.7:1, the two fibers achieve a better balance. Sufficient carbon fiber imparts high shielding strength to the shielding paper, while sufficient metal-plated glass fiber reduces the cost of the shielding paper. Furthermore, under this ratio, the two fibers can form a well-bonded structure with a density gradient through entanglement with glass fiber and bonding with resin adhesive. As a result, the shielding paper of this invention has high shielding strength, good mechanical properties, and is cost-effective.
[0055] Extensive experimental analysis revealed that when the mass ratio of carbon fiber and metallized glass fiber to glass fiber is controlled at 0.35–0.70:1, the three fibers achieve a better balance. Sufficient glass fiber not only maintains the high-temperature resistance of conventional shielding paper but also ensures a certain thickness of glass fiber interlayer to form a better density gradient structure. Furthermore, enough glass fiber extends into the carbon fiber layer and metallized glass fiber layer on both sides to ensure stable bonding among the three, preventing delamination of the carbon fiber layer and metallized glass fiber layer, thus providing sufficient mechanical properties for the shielding paper.
[0056] Furthermore, by controlling the ratio of the sum of the masses of carbon fiber and first glass fiber (denoted as A) to the sum of the masses of metal-plated glass fiber and second glass fiber (denoted as B) (i.e., A to B) within an appropriate range, preferably a ratio of 0.2 to 1:1, the present invention can control the thickness ratio of the carbon fiber layer to the metal-plated glass fiber layer in the layered structure of the electromagnetic shielding paper to be appropriate. This avoids the carbon fiber layer being too thin relative to the metal-plated glass fiber layer, or vice versa, thereby ensuring good bonding and high strength of the overall structure formed during the subsequent settling process.
[0057] Finally, a resin adhesive is applied to the surface of the first shielding paper and dried to obtain a superhydrophobic electromagnetic shielding paper. The step of applying the resin adhesive to the surface of the first shielding paper is as follows: the first shielding paper is immersed in a deionized aqueous solution of acrylic resin for ≤1 minute to obtain a second shielding paper; wherein, the acrylic resin can be a modified acrylic resin, which coats the fiber surface to form a protective layer for the fiber structure and also bonds the fibers together, ensuring a stable density gradient structure in the shielding paper. The modified acrylic resin can be any conventional adhesive used for shielding paper in the art, and this invention does not specifically limit its use. Then, an ethanol solution of fluoroalkylsilane is sprayed onto the second shielding paper to form a highly hydrophobic structure on the surface of the acrylic resin. This invention, by sequentially setting acrylic resin and fluoroalkylsilane on the fiber surface, together form a superhydrophobic structure on the paper surface, giving the shielding paper superhydrophobic properties. The superhydrophobic electromagnetic shielding paper prepared by the method of this invention has a tensile strength ≥9N / 15mm, an average shielding effectiveness ≥25dB from 8 to 12.4GHz, and a hydrophobic angle ≥147°, exhibiting excellent comprehensive performance.
[0058] To further improve the mechanical strength of the superhydrophobic electromagnetic shielding paper, the superhydrophobic electromagnetic shielding paper of the present invention also includes a nonwoven fabric layer; the nonwoven fabric layer is disposed on both sides of the superhydrophobic electromagnetic shielding paper and is bonded to the metal-plated glass fiber layer and the carbon fiber layer respectively by resin adhesive. By providing nonwoven fabric layers on both sides of the shielding paper, the mechanical strength of the shielding paper can be greatly improved. As shown in Example 9, its tensile strength is increased from 15 N / 15 mm in Example 1 to 32.5 N / 15 mm in Example 9, an increase of up to 116.7%.
[0059] The superhydrophobic electromagnetic shielding paper described above is preferably prepared according to the preparation method described above in this invention.
[0060] This invention also proposes an application of the aforementioned superhydrophobic electromagnetic shielding paper in the field of electromagnetic shielding materials. The applicant has found that although the electromagnetic shielding effect is generally good when shielding paper is applied with one side of the carbon fiber layer as the surface through which electromagnetic waves are incident, it is preferable to use the side of the metal-plated glass fiber layer as the surface through which electromagnetic waves are incident, as shown in the test results of Example 5.
[0061] The present invention will be further described below with reference to specific embodiments, but this should not be construed as a limitation on the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above description of the present invention still fall within the scope of protection of the present invention.
[0062] Example 1
[0063] This embodiment prepares the shielding paper using a natural settling method, and the specific steps are as follows:
[0064] 1) Place 1g of glass fiber with a diameter of 0.1μm and 0.5g of carbon fiber into 2L of deionized water, and stir in a mixer at 3000 rpm for 5 minutes to make the carbon fiber and glass fiber intertwine.
[0065] 2) Take 0.5g of aluminized glass fiber with a diameter of 5μm, 1.5g of the mixed fiber in step 1), 1g of glass fiber with a diameter of 1.5μm and mix it with 4L of deionized water, and prepare a mixed slurry using the same stirring conditions as in step 1).
[0066] 3) Pour the mixed slurry from step 2) into the slurry tank of the film-making machine and let it stand for 2 minutes;
[0067] 4) Open the drain valve to allow the slurry from step 3) to fall naturally onto the forming wire to form a paper film;
[0068] 5) Press the paper film from step 4) at 2MPa and dry it at 100℃ for 5 minutes;
[0069] 6) Immerse the paper obtained in step 5) in a solution of deionized water and acrylic resin at a mass ratio of 60:1 for 30 seconds, then remove it;
[0070] 7) Dissolve fluoroalkylsilane (FAS-17) in anhydrous ethanol at a mass ratio of 1:60, spray the mixture onto the surface of the composite paper obtained in step 6), and then dry it at 120°C for 20 minutes to obtain hydrophobic shielding paper.
[0071] The cross-sectional microstructure of the shielding paper prepared in this embodiment is shown in the attached figure. Figure 2 As shown; Appendix Figure 3 The image shows the Al elemental distribution in a cross-section including the metal fiber layer. Figure 4 The figure shows the C element distribution of a cross section containing the carbon fiber layer.
[0072] The shielding paper prepared in this embodiment was tested using conventional testing methods in the art. Its tensile strength was 15 N / 15 mm, and its average shielding effectiveness in the range of 8–12.4 GHz was 34.8 dB (electromagnetic waves incident from the direction of the carbon fiber layer). The test results are attached. Figure 5 As shown; the hydrophobic angle is 153.2°, as... Figure 6 As shown.
[0073] Examples 2-11
[0074] The process steps are the same as in Example 1, and the process parameters and differences are detailed in Table 1; in Example 5, when testing the shielding performance, electromagnetic waves were also incident from the direction of the metal-plated glass fiber layer; in Example 9, 20g / m² of material was laid on both the top and bottom surfaces of the shielding paper film. 2 The nonwoven fabric layer was then pressed, and the performance test results are shown in Table 1.
[0075] Table 1
[0076]
[0077] Note: "Shielding effectiveness 1" in the table is the result obtained by testing with electromagnetic waves incident from the direction of the carbon fiber layer; "Shielding effectiveness 2" is the result obtained by testing with electromagnetic waves incident from the direction of the metal-coated glass fiber layer.
[0078] As can be seen from the test results of the examples and comparative examples, changing the diameter of the glass fiber will affect the degree of mixing between the glass fiber and the carbon fiber; as the diameter of the glass fiber increases, the tensile strength and hydrophobic angle of the shielding paper gradually decrease, while the shielding effectiveness for electromagnetic shielding changes little, as shown in Examples 1 to 3.
[0079] As can be seen from the test results of the examples and comparative examples, changing the carbon fiber content can significantly affect the mechanical strength and shielding effectiveness of the shielding paper; as the carbon fiber content increases, the electromagnetic shielding effectiveness of the shielding paper is significantly improved, and the tensile strength of the shielding paper also gradually increases, but the rate of increase gradually slows down; while the effect on the hydrophobic angle is relatively small, as shown in Examples 1, 4 to 5.
[0080] As can be seen from the test results of the examples and comparative examples, changing the content of aluminized glass fiber will affect the mixing and stacking of the fibers; as the content of aluminized glass fiber increases, the tensile strength of the shielding paper gradually decreases, the electromagnetic shielding effectiveness gradually increases, while the effect on the hydrophobic angle is relatively small, as shown in Examples 2, 6 and 7.
[0081] As can be seen from the test results of the examples and comparative examples, placing non-woven fabric on both sides of the shielding paper can greatly improve the tensile strength of the shielding paper, as shown in Examples 2 and 9.
[0082] As can be seen from the test results of the examples and comparative examples, when electromagnetic waves are incident on the surface of the shielding paper, a better electromagnetic shielding effect can be achieved than when the electromagnetic waves are incident on the surface of the carbon fiber layer, as shown in Example 5.
[0083] The technical features in the claims and / or specification of this invention can be combined, and the combination is not limited to the combinations obtained through reference in the claims. Technical solutions obtained by combining the technical features in the claims and / or specification are also within the scope of protection of this invention.
[0084] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Any simple modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention shall still fall within the scope of the technical solution of the present invention.
Claims
1. A method for preparing a superhydrophobic electromagnetic shielding paper, characterized in that, It includes the following steps: S11. Carbon fiber, metal-plated glass fiber, and glass fiber are dispersed in water and stirred evenly to obtain a fiber slurry; wherein the mass ratio of the carbon fiber, metal-plated glass fiber, and glass fiber is 0.1~0.4:0.1~0.4:1; the preparation steps of the fiber slurry are as follows: carbon fiber and first glass fiber are dispersed in water and stirred evenly to obtain a pre-entangled fiber slurry; metal-plated glass fiber, second glass fiber, and the pre-entangled fiber slurry are dispersed in water and stirred evenly to obtain a fiber slurry; the fiber diameter of the first glass fiber is ≤0.5μm; the mass ratio of the carbon fiber to the first glass fiber is 0.2~0.9:1; the fiber diameter of the second glass fiber is ≤1.5μm; the mass ratio of the metal-plated glass fiber to the second glass fiber is 0.2~0.9:1; S12 allows the fiber pulp to settle naturally, then presses and dries to obtain a first shielding paper with a gradient density distribution. S13 Apply resin adhesive to the first shielding paper, specifically by immersing the first shielding paper in a deionized aqueous solution of acrylic resin for ≤1 min to obtain the second shielding paper; then spray an ethanol solution of fluoroalkylsilane onto the second shielding paper; and dry to obtain superhydrophobic electromagnetic shielding paper.
2. The preparation method according to claim 1, characterized in that, The ratio of the sum of the masses of the carbon fiber and the first glass fiber to the sum of the masses of the metal-plated glass fiber and the second glass fiber is 0.2 to 1:
1.
3. The preparation method according to claim 1 or 2, characterized in that, The mass ratio of the carbon fiber to the metal-plated glass fiber is 0.6~1.7:1; the mass ratio of the sum of the carbon fiber and the metal-plated glass fiber to the glass fiber is 0.35~0.70:
1.
4. The preparation method according to claim 1, characterized in that, The diameter of the metal-coated glass fiber is ≤5μm.
5. A superhydrophobic electromagnetic shielding paper obtained by the preparation method according to any one of claims 1 to 4, characterized in that, It includes: Metal-plated glass fiber layer; A glass fiber layer is disposed adjacent to the metal-plated glass fiber layer; A carbon fiber layer is disposed adjacent to the glass fiber layer; glass fibers on one side of the glass fiber layer are inserted into and wound around the carbon fiber in the carbon fiber layer, and glass fibers on the opposite side are inserted into and wound around the metal-plated glass fiber in the metal-plated glass fiber layer; along the thickness direction of the superhydrophobic electromagnetic shielding paper, the metal-plated glass fiber layer, the glass fiber layer, and the carbon fiber layer have a density gradient structure; the metal-plated glass fiber layer, the glass fiber layer, and the carbon fiber layer are bonded together by a resin adhesive.
6. The superhydrophobic electromagnetic shielding paper according to claim 5, characterized in that, Its tensile strength is ≥9 N / 15mm, its average shielding effectiveness is ≥25dB from 8 to 12.4GHz, and its hydrophobic angle is ≥147°.
7. The superhydrophobic electromagnetic shielding paper according to claim 5, characterized in that, It also includes: The non-woven fabric layer is disposed on both sides of the superhydrophobic electromagnetic shielding paper and is bonded to the metal-plated glass fiber layer and the carbon fiber layer respectively by the resin adhesive.
8. The application of the superhydrophobic electromagnetic shielding paper according to any one of claims 5 to 7 in the field of electromagnetic shielding materials.
Citation Information
Patent Citations
Conductive glass fiber reinforced plastic, conductive glass fiber reinforced plastic plate and preparation method of conductive glass fiber reinforced plastic plate
CN110669324A
Multifunctional flexible electromagnetic shielding film product and preparation method thereof
CN118076077A
Electromagnetic wave shielding sheet and method for producing the same
KR101558748B1