Preparation method and application of two-dimensional bismuth-based surface molecular imprinting photocatalyst

A two-dimensional bismuth-based surface molecularly imprinted photocatalyst, prepared by using two-dimensional BiOCl nanosheets as a carrier and ethanol solvent, solves the problem of poor selective degradation effect of molecularly imprinted photocatalysts in complex water bodies in the prior art. It achieves rapid adsorption and efficient degradation of target pollutants, and the degradation process is environmentally friendly and low-cost.

CN119500282BActive Publication Date: 2026-11-24HENAN NORMAL UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411618027.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-11-13
Publication Date
2026-11-24
Estimated Expiration
2044-11-13

AI Technical Summary

Technical Problem

In existing technologies, molecularly imprinted photocatalysts have poor selective degradation effects on target pollutants in complex water bodies, and the solvents and elution methods used in the preparation process are not environmentally friendly, resulting in secondary pollution and high energy consumption.

Method used

Two-dimensional BiOCl nanosheets were used as a carrier, ethanol as a solvent and methanol as an eluent. Two-dimensional bismuth-based surface molecularly imprinted photocatalysts were prepared by prepolymerization and thermal polymerization. By combining the layered structure and surface defects of BiOCl, selective adsorption and rapid degradation of target pollutants were achieved.

Benefits of technology

The prepared two-dimensional bismuth-based surface molecularly imprinted photocatalyst exhibits strong selective adsorption capacity for the target compound venlafaxine in aqueous solution and rapidly degrades it under light conditions, achieving selective photocatalytic removal of venlafaxine from actual water samples. The adsorption equilibrium time is 5 minutes, and the complete degradation time is 20 minutes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119500282B_ABST
    Figure CN119500282B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a two-dimensional bismuth-based surface molecularly imprinted photocatalyst and its application. The method involves dissolving the template molecule venlafaxine and the functional monomer 2-acrylamide-2-methylpropanesulfonic acid in an ethanol solvent containing the support BiOCl, prepolymerizing at 20-40°C for 2-8 h, then adding the crosslinking agent ethylene glycol dimethacrylate and the initiator azobisisobutyronitrile. After ultrasonication and nitrogen protection, the mixture is thermally polymerized at 50-70°C for 20-30 h. The resulting product is then eluted and dried to obtain the two-dimensional bismuth-based surface molecularly imprinted photocatalyst. The imprinted photocatalyst prepared by this invention exhibits strong selective adsorption of the target venlafaxine in aqueous solution and preferential and rapid degradation of venlafaxine under light irradiation, making it suitable for the selective photocatalytic removal of venlafaxine from actual water samples.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of functional polymer preparation technology, specifically relating to a method for preparing a two-dimensional bismuth-based surface molecularly imprinted photocatalyst and its application. Background Technology

[0002] Multiphase photocatalysis is a completely green advanced oxidation technology that can rapidly oxidize and decompose various pollutants in water without selectivity. However, the active species produced by photocatalysis have a short lifespan and lack selectivity. In actual water bodies, pollutants are complex in composition, and high concentrations of non-toxic soluble organic matter and various inorganic ions often coexist with low concentrations of target pollutants. Coexisting pollutants will form competitive adsorption on the catalyst surface and be preferentially degraded, resulting in the ineffective consumption of a large number of active species. The number of active species allocated to the target pollutant is limited, leading to relatively poor removal efficiency.

[0003] Molecularly imprinted polymers (MIPs) are adsorbent materials with selective recognition capabilities. Under the guidance of template molecules, these materials copolymerize with functional monomers to form imprinted cavities containing "specific recognition sites." The synergistic effect of the functional monomer binding sites and the structurally complementary cavities enables the selective adsorption of target pollutants in complex aquatic environments, achieving the separation and enrichment of low-concentration target pollutants. However, as an adsorbent material, the removal of pollutants by MIPs is merely a physical transfer; it cannot decompose pollutants into non-toxic substances. Furthermore, eluting the adsorbed MIPs consumes large amounts of toxic organic solvents, resulting in high costs and a potential for secondary pollution.

[0004] Combining molecularly imprinted polymers with photocatalytic materials allows for the construction of molecular recognition cavities at or near the catalytically active sites of the photocatalyst. This enables the photocatalyst to accurately identify target pollutants under complex matrix conditions and enrich these pollutants at or near the catalytically active sites. Under illumination, the various active species generated by the catalyst can concentrate on attacking the target pollutants, efficiently degrading toxic chemicals into non-toxic products, thus achieving the complete removal of target pollutants in a preferential manner. During the preparation process, the photocatalyst acts as a carrier, and its morphology and structure directly affect the adsorption performance of the imprinted polymer. The thickness of the imprinted polymer coating layer determines the catalytic performance of the imprinted photocatalyst.

[0005] Patent document CN111234295B discloses a method for preparing a molecularly imprinted photocatalytic material. The method involves mixing template molecules, functional monomers, and porogens for a prepolymerization reaction to obtain a prepolymer; mixing the prepolymer, crosslinking agent, initiator, and BiOBr and performing a polymerization reaction under a protective atmosphere to obtain a polymer; and eluting the polymer to obtain the molecularly imprinted photocatalytic material by calcination at a temperature of 400-500℃ for 2-4 hours. This patent document has the following three shortcomings: First, the solvents used in the preparation process are non-polar solvents such as acetonitrile or methanol. Although these solvents are commonly used in molecular imprinting preparation, they are environmentally unfriendly and prone to secondary pollution. Using polar solvents such as ethanol is relatively greener, but polar solvents such as ethanol usually affect the binding of functional monomers and template molecules, making it difficult to prepare molecularly imprinted polymers. Second, the calcination elution method is used in the removal of template molecules, which requires relatively high temperatures and consumes a lot of energy. Elution with methanol is not effective. Third, from the perspective of selectivity, the selectivity of the prepared molecularly imprinted polymer is not obvious enough. This may be because the molecular structure of the imprinting site is destroyed during the calcination process, so that the imprinted cavity cannot match the structure of the target pollutant, resulting in non-target pollutants being able to enter the imprinted cavity.

[0006] In the preparation of molecularly imprinted polymers (MIPs), the elution effect of template molecules directly affects the adsorption and selectivity of the MIP catalytic material. The high-temperature calcination method used in the aforementioned patent literature for eluting template molecules not only consumes a large amount of energy, but the excessively high temperature can also lead to the degradation of the MIP, thereby destroying the imprinted cavity structure and causing a mismatch between the imprinted cavity and the spatial structure of the template contaminants, resulting in reduced selectivity. Choosing a suitable solvent is also crucial in the preparation of MIPs, as it affects not only the polymerization reaction but also the performance of the final MIP product. Considering environmental protection and production safety, the chosen solvent should ideally be low in toxicity to minimize environmental impact. During the preparation of MIPs, the functional monomers and template molecules are mainly bonded through hydrogen bonds. The stronger the polarity of the solvent, the less conducive it is to hydrogen bond formation. Therefore, non-polar solvents such as acetonitrile or methanol are commonly used, but their disadvantages include high toxicity and environmental unfriendliness. Ethanol, a polar solvent, is relatively environmentally friendly, but it is detrimental to many molecular imprinting methods (especially non-covalent imprinting) because it inhibits the formation of hydrogen bonds between monomers and templates. This is one of the challenges faced by molecular imprinting technology.

[0007] Currently, the preparation of imprinted photocatalysts mostly utilizes three-dimensional metal oxides as supports, with relatively few reports on two-dimensional molecularly imprinted photocatalysts. Compared to traditional 3D nanoparticle photocatalysts, the ultrathin structure of two-dimensional materials reduces the charge surface diffusion distance, enabling the e-... − -h +Minimizing the possibility of recombination. Furthermore, the greater number of "catalytically useful" defects and abundant coordinated unsaturated surface atoms in two-dimensional materials can provide more surface active sites, facilitating charge transfer from the semiconductor to the adsorbate and the construction of imprinted sites on or near the surface active sites, accelerating interfacial photocatalytic reactions. BiOCl is a two-dimensional photocatalytic material with a special layered structure, possessing excellent photogenerated carrier separation efficiency, high chemical stability, tunable physicochemical properties, low cost, abundant resources, and environmental friendliness, making it widely applicable in environmental remediation and energy conversion. However, current research on BiOCl mainly focuses on the degradation of single pollutants, lacking studies on the selective degradation of target pollutants under complex matrix conditions. Summary of the Invention

[0008] The technical problem solved by this invention is to provide a simple and high-performance method for preparing a two-dimensional bismuth-based surface molecularly imprinted photocatalyst. The two-dimensional bismuth-based surface molecularly imprinted photocatalyst prepared by this method has a strong ability to selectively adsorb the target venlafaxine in aqueous solution and is preferentially and rapidly degraded under light conditions. It can be used for the selective photocatalytic removal of venlafaxine from actual water samples.

[0009] To solve the above-mentioned technical problems, the present invention adopts the following technical solution: a method for preparing a two-dimensional bismuth-based surface molecularly imprinted photocatalyst, characterized in that: the template molecule venlafaxine and the functional monomer 2-acrylamide-2-methylpropanesulfonic acid are dissolved in an ethanol solvent containing BiOCl nanosheets as a support, prepolymerized at 20~40℃ for 2~8 h, then the crosslinking agent ethylene glycol dimethacrylate and the initiator azobisisobutyronitrile are added, and after ultrasonication and nitrogen protection, the mixture is thermally polymerized at 50~70℃ for 20~30 h, and after elution and drying, the two-dimensional bismuth-based surface molecularly imprinted photocatalyst is obtained; The BiOCl nanosheets were synthesized by a hydrothermal method. The specific synthesis process was as follows: Bismuth nitrate pentahydrate was dissolved in a mixed solvent of pure water and ethylene glycol with a volume ratio of 0.5~2:1, and then saturated sodium chloride solution was added dropwise. After stirring and mixing for 1~2 h, the mixture was placed in a high-pressure reactor with a polytetrafluoroethylene liner and hydrothermally reacted at 130~180℃ for 3~6 h. After washing several times with water and ethanol and drying, BiOCl nanosheets were obtained.

[0010] Further specified, the molar ratio of the template molecule, functional monomer, crosslinking agent and initiator is 1:2~6:1~16:1.

[0011] Further specifying, the elution process specifically involves Soxhlet extraction for 48 h using a mixture of methanol and acetic acid at a volume ratio of 9:1.

[0012] The two-dimensional bismuth-based surface molecularly imprinted photocatalyst described in this invention is used for the selective photocatalytic removal of linfaxin from actual water samples.

[0013] Compared with the prior art, the present invention has the following advantages and beneficial effects: 1. This invention uses a two-dimensional bismuth-based photocatalyst as a support to prepare a venlafaxine surface-imprinted photocatalyst. By controlling the thickness of the imprinted layer, the catalyst can exhibit properties such as fast adsorption rate, large adsorption capacity, strong anti-interference ability, and fast degradation rate.

[0014] 2. This invention successfully prepared a two-dimensional bismuth-based surface molecularly imprinted photocatalyst using ethanol as the preparation solvent, reducing the secondary pollution to the environment caused by non-polar solvents such as acetonitrile and methanol.

[0015] 3. The present invention uses methanol elution to completely elute the template molecules. The operation is simple and the cost is low. The elution does not affect the structure of the imprint cavity. The material selectivity is good and the imprint factor reaches 4.7. This is because the two-dimensional sheet structure has a flat surface with a large exposure area, and the three-dimensional structure has many pores inside, making it difficult for the template molecules to be removed.

[0016] 4. In this invention, bismuth chloride (BiOCl) is a two-dimensional photocatalyst with a unique layered structure and internal electric field effect, which is beneficial for the effective separation and rapid transport of photogenerated carriers. Compared with commonly used three-dimensional molecularly imprinted photocatalytic matrices, BiOCl has a more positive valence band potential, which can more continuously and effectively activate molecular oxygen under light excitation, thereby achieving better degradation and removal of organic pollutants. In addition, the more "catalytically useful" defects and abundant coordinated unsaturated surface atoms in the layered structure can provide more surface active sites, thereby promoting the transfer of charge from the semiconductor to the adsorbate and accelerating the interfacial photocatalytic reaction. This is beneficial for the rapid recognition, adsorption, and efficient degradation of target pollutants by the imprinted catalyst. The adsorption equilibrium time of the molecularly imprinted polymer prepared in this invention for the target pollutant is 5 min, and the complete degradation time is 20 min, both of which are much lower than 1 h and 2 h in the literature (CN111234295B). Attached Figure Description

[0017] Figure 1 This is a schematic diagram of the synthesis route of the support BiOCl and the imprinted photocatalyst MI-BiOCl in this invention.

[0018] Figure 2 These are electron microscope images of the support, imprinted photocatalyst, and non-imprinted photocatalyst in this invention.

[0019] Figure 3 This is an adsorption kinetic diagram of the imprinted photocatalyst and the non-imprinted photocatalyst of this invention.

[0020] Figure 4 These are the adsorption isotherms of the imprinted and non-imprinted photocatalysts of this invention.

[0021] Figure 5 This is a graph showing the change in the removal rate of venlafaxine by the imprinted photocatalyst and photocatalyst support of the present invention over time in the presence of the interfering substance humic acid. Detailed Implementation

[0022] The following examples further illustrate the above-described content of the present invention, but it should not be construed as limiting the scope of the subject matter of the present invention to the following examples. All technologies implemented based on the above-described content of the present invention fall within the scope of the present invention. Example 1

[0023] Preparation of BiOCl nanosheets: 0.5 g of bismuth nitrate pentahydrate was dissolved in 55 mL of a mixed solvent of pure water and ethylene glycol with a volume ratio of 1:1. Then, 8 mL of saturated sodium chloride solution was added dropwise. After stirring and mixing for 1 h, the mixture was placed in a high-pressure reactor with a polytetrafluoroethylene liner and hydrothermally reacted at 130 °C for 3 h. After washing several times with water and ethanol and drying, BiOCl nanosheets were obtained.

[0024] Preparation of imprinted photocatalyst: Using 30 mL of ethanol as solvent, 0.10 g of the self-made BiOCl nanosheets (support), 0.1 mmol of venlafaxine (template molecule), and 0.4 mmol of 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 30 °C for 4 h. Then, 0.1 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After sonication and N2 purging, the mixture was thermally polymerized at 60 °C for 24 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture at a volume ratio of 9:1 using a Soxhlet extractor for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 2

[0025] Preparation of BiOCl nanosheets: 0.5 g of bismuth nitrate pentahydrate was dissolved in 55 mL of a mixed solvent of pure water and ethylene glycol with a volume ratio of 1:1. Then, 8 mL of saturated sodium chloride solution was added dropwise. After stirring and mixing for 1 h, the mixture was placed in a high-pressure reactor with a polytetrafluoroethylene liner and hydrothermally reacted at 130 °C for 3 h. After washing several times with water and ethanol and drying, BiOCl nanosheets were obtained.

[0026] Preparation of imprinted photocatalyst: Using 30 mL ethanol as solvent, 0.10 g of the self-made BiOCl nanosheets (support), 0.1 mmol of venlafaxine (template molecule), and 0.4 mmol of 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 30 °C for 4 h. Then, 0.3 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After sonication and N2 purging, the mixture was thermally polymerized at 60 °C for 24 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture with a volume ratio of 9:1 using a Soxhlet extractor for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 3

[0027] Preparation of BiOCl nanosheets: 0.5 g of bismuth nitrate pentahydrate was dissolved in 55 mL of a mixed solvent of pure water and ethylene glycol with a volume ratio of 1:1. Then, 8 mL of saturated sodium chloride solution was added dropwise. After stirring and mixing for 1 h, the mixture was placed in a high-pressure reactor with a polytetrafluoroethylene liner and hydrothermally reacted at 130 °C for 3 h. After washing several times with water and ethanol and drying, BiOCl nanosheets were obtained.

[0028] Preparation of imprinted photocatalyst: Using 30 mL ethanol as solvent, 0.10 g of the self-made BiOCl nanosheets (support), 0.1 mmol venlafaxine (template molecule) and 0.4 mmol 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 30 °C for 4 h. Then, 0.5 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After sonication and N2 purging, the mixture was thermally polymerized at 60 °C for 24 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture with a volume ratio of 9:1 using a Soxhlet extractor for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 4

[0029] Preparation of BiOCl nanosheets: 0.5 g of bismuth nitrate pentahydrate was dissolved in 55 mL of a mixed solvent of pure water and ethylene glycol with a volume ratio of 1:1. Then, 8 mL of saturated sodium chloride solution was added dropwise. After stirring and mixing for 1 h, the mixture was placed in a high-pressure reactor with a polytetrafluoroethylene liner and hydrothermally reacted at 130 °C for 3 h. After washing several times with water and ethanol and drying, BiOCl nanosheets were obtained.

[0030] Preparation of imprinted photocatalyst: Using 30 mL of ethanol as solvent, 0.10 g of the self-made BiOCl nanosheets (support), 0.1 mmol of venlafaxine (template molecule), and 0.4 mmol of 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 30 °C for 4 h. Then, 0.8 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After sonication and N2 purging, the mixture was thermally polymerized at 60 °C for 24 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture with a volume ratio of 9:1 using a Soxhlet extractor for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 5

[0031] Preparation of BiOCl nanosheets: 0.5 g of bismuth nitrate pentahydrate was dissolved in 55 mL of a mixed solvent of pure water and ethylene glycol with a volume ratio of 1:1. Then, 8 mL of saturated sodium chloride solution was added dropwise. After stirring and mixing for 1 h, the mixture was placed in a high-pressure reactor with a polytetrafluoroethylene liner and hydrothermally reacted at 130 °C for 3 h. After washing several times with water and ethanol and drying, BiOCl nanosheets were obtained.

[0032] Preparation of imprinted photocatalyst: Using 30 mL of ethanol as solvent, 0.10 g of the self-made BiOCl nanosheets (support), 0.1 mmol of venlafaxine (template molecule), and 0.4 mmol of 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 30 °C for 4 h. Then, 0.8 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After sonication and N2 purging, the mixture was thermally polymerized at 60 °C for 24 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture with a volume ratio of 9:1 using a Soxhlet extractor for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 6

[0033] Preparation of BiOCl nanosheets: 0.5 g of bismuth nitrate pentahydrate was dissolved in 55 mL of a mixed solvent of pure water and ethylene glycol with a volume ratio of 1:1. Then, 8 mL of saturated sodium chloride solution was added dropwise. After stirring and mixing for 1 h, the mixture was placed in a high-pressure reactor with a polytetrafluoroethylene liner and hydrothermally reacted at 130 °C for 3 h. After washing several times with water and ethanol and drying, BiOCl nanosheets were obtained.

[0034] Preparation of imprinted photocatalyst: Using 30 mL ethanol as solvent, 0.10 g of the self-made BiOCl nanosheets (support), 0.1 mmol venlafaxine (template molecule), and 0.4 mmol 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 30 °C for 4 h. Then, 1.2 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After sonication and N2 purging, the mixture was thermally polymerized at 60 °C for 24 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture with a volume ratio of 9:1 using a Soxhlet extractor for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 7

[0035] Preparation of BiOCl nanosheets: 0.5 g of bismuth nitrate pentahydrate was dissolved in 55 mL of a mixed solvent of pure water and ethylene glycol with a volume ratio of 1:1. Then, 8 mL of saturated sodium chloride solution was added dropwise. After stirring and mixing for 1 h, the mixture was placed in a high-pressure reactor with a polytetrafluoroethylene liner and hydrothermally reacted at 130 °C for 3 h. After washing several times with water and ethanol and drying, BiOCl nanosheets were obtained.

[0036] Preparation of imprinted photocatalyst: Using 30 mL ethanol as solvent, 0.10 g of the self-made BiOCl nanosheets (support), 0.1 mmol venlafaxine (template molecule) and 0.4 mmol 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 30 °C for 4 h. Then, 1.6 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After sonication and N2 purging, the mixture was thermally polymerized at 60 °C for 24 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture with a volume ratio of 9:1 using a Soxhlet extractor for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 8

[0037] Preparation of BiOCl nanosheets: 0.5 g of bismuth nitrate pentahydrate was dissolved in 55 mL of a mixed solvent of pure water and ethylene glycol with a volume ratio of 1:1. Then, 8 mL of saturated sodium chloride solution was added dropwise. After stirring and mixing for 1 h, the mixture was placed in a high-pressure reactor with a polytetrafluoroethylene liner and hydrothermally reacted at 130 °C for 3 h. After washing several times with water and ethanol and drying, BiOCl nanosheets were obtained.

[0038] Preparation of imprinted photocatalyst: Using 30 mL of ethanol as solvent, 0.10 g of the self-made BiOCl nanosheets (support), 0.1 mmol of venlafaxine (template molecule), and 0.2 mmol of 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 30 °C for 4 h. Then, 0.4 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After sonication and N2 purging, the mixture was thermally polymerized at 60 °C for 24 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture with a volume ratio of 9:1 using a Soxhlet extractor for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 9

[0039] Preparation of BiOCl nanosheets: 0.5 g of bismuth nitrate pentahydrate was dissolved in 55 mL of a mixed solvent of pure water and ethylene glycol with a volume ratio of 1:1. Then, 8 mL of saturated sodium chloride solution was added dropwise. After stirring and mixing for 1 h, the mixture was placed in a high-pressure reactor with a polytetrafluoroethylene liner and hydrothermally reacted at 130 °C for 3 h. After washing several times with water and ethanol and drying, BiOCl nanosheets were obtained.

[0040] Preparation of imprinted photocatalyst: Using 30 mL ethanol as solvent, 0.10 g of the self-made BiOCl nanosheets (support), 0.1 mmol venlafaxine (template molecule), and 0.6 mmol 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 30 °C for 4 h. Then, 0.4 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After sonication and N2 purging, the mixture was thermally polymerized at 60 °C for 24 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture with a volume ratio of 9:1 using a Soxhlet extractor for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 10

[0041] Preparation of BiOCl nanosheets: 0.5 g of bismuth nitrate pentahydrate was dissolved in 55 mL of a mixed solvent of pure water and ethylene glycol with a volume ratio of 1:1. Then, 8 mL of saturated sodium chloride solution was added dropwise. After stirring and mixing for 1 h, the mixture was placed in a high-pressure reactor with a polytetrafluoroethylene liner and hydrothermally reacted at 130 °C for 3 h. After washing several times with water and ethanol and drying, BiOCl nanosheets were obtained.

[0042] Preparation of imprinted photocatalyst: Using 30 mL of ethanol as solvent, 0.10 g of the self-made BiOCl nanosheets (support), 0.1 mmol of venlafaxine (template molecule), and 0.4 mmol of 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 30 °C for 4 h. Then, 0.8 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After sonication and N2 purging, the mixture was thermally polymerized at 60 °C for 24 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture with a volume ratio of 9:1 using a Soxhlet extractor for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 11

[0043] Preparation of BiOCl nanosheets: 0.5 g of bismuth nitrate pentahydrate was dissolved in 55 mL of a mixed solvent of pure water and ethylene glycol with a volume ratio of 1:1. Then, 8 mL of saturated sodium chloride solution was added dropwise. After stirring and mixing for 1 h, the mixture was placed in a high-pressure reactor with a polytetrafluoroethylene liner and hydrothermally reacted at 130 °C for 3 h. After washing several times with water and ethanol and drying, BiOCl nanosheets were obtained.

[0044] Preparation of imprinted photocatalyst: Using 30 mL of ethanol as solvent, 0.10 g of the self-made BiOCl nanosheets (support), 0.1 mmol of venlafaxine (template molecule), and 0.4 mmol of 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 30 °C for 4 h. Then, 0.8 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After sonication and N2 purging, the mixture was thermally polymerized at 60 °C for 24 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture with a volume ratio of 9:1 using a Soxhlet extractor for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 12

[0045] Preparation of BiOCl nanosheets: 0.5 g of bismuth nitrate pentahydrate was dissolved in 55 mL of a mixed solvent of pure water and ethylene glycol with a volume ratio of 1:1. Then, 8 mL of saturated sodium chloride solution was added dropwise. After stirring and mixing for 1 h, the mixture was placed in a high-pressure reactor with a polytetrafluoroethylene liner and hydrothermally reacted at 180 °C for 3 h. After washing several times with water and ethanol and drying, BiOCl nanosheets were obtained.

[0046] Preparation of imprinted photocatalyst: Using 30 mL of ethanol as solvent, 0.10 g of the self-made BiOCl nanosheets (support), 0.1 mmol of venlafaxine (template molecule), and 0.4 mmol of 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 30 °C for 4 h. Then, 0.8 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After sonication and N2 purging, the mixture was thermally polymerized at 60 °C for 24 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture with a volume ratio of 9:1 using a Soxhlet extractor for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 13

[0047] Preparation of BiOCl nanosheets: 0.5 g of bismuth nitrate pentahydrate was dissolved in 55 mL of a mixed solvent of pure water and ethylene glycol with a volume ratio of 1:1. Then, 1 mL of saturated sodium chloride solution was added dropwise. After stirring and mixing for 1 h, the mixture was placed in a high-pressure reactor with a polytetrafluoroethylene liner and hydrothermally reacted at 130 °C for 3 h. After washing several times with water and ethanol and drying, BiOCl nanosheets were obtained.

[0048] Preparation of imprinted photocatalyst: Using 30 mL of ethanol as solvent, 0.10 g of the self-made BiOCl nanosheets (support), 0.1 mmol of venlafaxine (template molecule), and 0.4 mmol of 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 30 °C for 4 h. Then, 0.8 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After sonication and N2 purging, the mixture was thermally polymerized at 60 °C for 24 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture with a volume ratio of 9:1 using a Soxhlet extractor for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 14

[0049] Preparation of BiOCl nanosheets: 0.5 g of bismuth nitrate pentahydrate was dissolved in 55 mL of a mixed solvent of pure water and ethylene glycol with a volume ratio of 1:1. Then, 1 mL of saturated sodium chloride solution was added dropwise. After stirring and mixing for 1 h, the mixture was placed in a high-pressure reactor with a polytetrafluoroethylene liner and hydrothermally reacted at 130 °C for 6 h. After washing several times with water and ethanol and drying, BiOCl nanosheets were obtained.

[0050] Preparation of imprinted photocatalyst: Using 30 mL of ethanol as solvent, 0.10 g of the self-made BiOCl nanosheets (support), 0.1 mmol of venlafaxine (template molecule), and 0.4 mmol of 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 30 °C for 4 h. Then, 0.8 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After sonication and N2 purging, the mixture was thermally polymerized at 60 °C for 24 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture with a volume ratio of 9:1 using a Soxhlet extractor for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 15

[0051] 20 mg of the imprinted photocatalyst (MI-BiOCl) and the non-imprinted photocatalyst (NI-BiOCl) prepared in Example 1 were respectively mixed with 50 mL of 20 mg L... -1 The venlafaxine aqueous solution was mixed and allowed to adsorb at room temperature with shaking for a certain period of time (0-60 min). The supernatant was then collected and the absorbance at 225 nm was measured using a UV spectrophotometer. The results are as follows: Figure 3 As shown. Example 16

[0052] 20 mg of the imprinted photocatalyst (MI-BiOCl) and the non-imprinted photocatalyst (NI-BiOCl) prepared in Example 1 were respectively mixed with 50 mL of venlafaxine aqueous solution (0-80 mg / L). -1 After adsorption by shaking at room temperature for 1 h, the supernatant was collected and the absorbance at 225 nm was measured using a UV spectrophotometer. The results are as follows: Figure 4 As shown. Example 17

[0053] 20 mg of the imprinted photocatalyst (MI-BiOCl) and photocatalyst support (BiOCl) prepared in Example 1 were dispersed in 50 mL of a solution containing venlafaxine (20 mg / L). -1 ) and humic acid (20 mg L) -1 In a mixed aqueous solution of [unspecified ingredient], the mixture was stirred for 30 min in the dark to ensure adsorption-desorption equilibrium. Stirring was continued under a 500 W xenon lamp, and the concentration of venlafaxine in the solution was determined at intervals using high-performance liquid chromatography (HPLC). Results are as follows: Figure 5 As shown. Example 18

[0054] The imprinted photocatalyst prepared in Example 1 was used for the photocatalytic degradation of venlafaxine in actual wastewater. Spiking experiments showed a removal rate close to 100%, with a residual concentration of venlafaxine of 12.5 ppb after degradation. This indicates that the obtained imprinted photocatalyst has good practicality for the degradation of venlafaxine; after four cycles of use, the adsorption capacity of the imprinted photocatalyst for venlafaxine still reached 15 mg g. -1 The total removal rate still reached over 98%, indicating that the obtained imprinted polymer has excellent regeneration adsorption performance and stability.

[0055] The above embodiments describe the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are only illustrative of the principles of the present invention. Various changes and modifications can be made to the present invention without departing from the scope of the principles of the present invention, and all such changes and modifications fall within the protection scope of the present invention.

Claims

1. A method for preparing a two-dimensional bismuth-based surface molecularly imprinted photocatalyst, characterized in that... The specific process is as follows: the template molecule venlafaxine and the functional monomer 2-acrylamide-2-methylpropanesulfonic acid are dissolved in an ethanol solvent containing BiOCl nanosheets as a support, and prepolymerized at 20~40℃ for 2~8 h. Then, the crosslinking agent ethylene glycol dimethacrylate and the initiator azobisisobutyronitrile are added. After ultrasonication and nitrogen protection, the mixture is thermally polymerized at 50~70℃ for 20~30 h. After elution and drying, a two-dimensional bismuth-based surface molecularly imprinted photocatalyst is obtained. The BiOCl nanosheets were synthesized by a hydrothermal method. The specific synthesis process was as follows: Bismuth nitrate pentahydrate was dissolved in a mixed solvent of pure water and ethylene glycol with a volume ratio of 0.5~2:1, and then saturated sodium chloride solution was added dropwise. After stirring and mixing for 1~2 h, the mixture was placed in a high-pressure reactor with a polytetrafluoroethylene liner and hydrothermally reacted at 130~180℃ for 3~6 h. After washing several times with water and ethanol and drying, BiOCl nanosheets were obtained.

2. The method for preparing two-dimensional bismuth-based surface molecular imprinting photocatalyst according to claim 1, characterized in that: The molar ratio of the template molecule, functional monomer, crosslinking agent, and initiator is 1:2~6:1~16:

1.

3. The method for preparing two-dimensional bismuth-based surface molecular imprinting photocatalyst according to claim 1, characterized in that: The elution process specifically involves Soxhlet extraction for 48 h using a mixture of methanol and acetic acid at a volume ratio of 9:

1.

4. The two-dimensional bismuth-based surface molecularly imprinted photocatalyst prepared by the method according to any one of claims 1 to 3 is used for the selective photocatalytic removal of venlafaxine from actual water samples.

Citation Information

Patent Citations

  • A molecularly imprinted photocatalytic material, its preparation method and application

    CN111234295B

  • Molecularly imprinted photocatalytic material as well as preparation method and application thereof

    CN111234295A

  • Photocatalytic system for enantio-selective enrichment

    US20230390751A1