Preparation method and application of biol embedded bismuth-based surface molecular imprinting photocatalyst
By preparing BiOI-embedded bismuth-based surface molecularly imprinted photocatalysts, the problem of poor selective degradation effect of photocatalysts in complex water bodies was solved, achieving efficient selective adsorption and improved photocatalytic performance, reducing environmental pollution and energy consumption.
Patent Information
- Application Number
- CN202411618124.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-13
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-11-13
AI Technical Summary
In existing technologies, photocatalysts are not effective in selectively degrading target pollutants in complex water bodies. Furthermore, the preparation process of traditional molecularly imprinted polymers is environmentally unfriendly, energy-intensive, and the spatial structure of the imprinted cavity and the template pollutant is poorly matched, resulting in low selective degradation efficiency.
A method for preparing BiOI-embedded bismuth-based surface molecularly imprinted photocatalysts was adopted. By simultaneously synthesizing BiOI on the surface of the imprinted catalyst, using ethanol as a solvent, and combining BiOIO₃ nanosheets as a support, BiOI-embedded bismuth-based surface molecularly imprinted photocatalysts were prepared, thereby enhancing the selectivity and photocatalytic performance of the catalyst.
It improves the selective adsorption capacity and photocatalytic performance of the catalyst for target pollutants, reduces the mass transfer distance, enhances light absorption capacity, reduces environmental pollution, and improves the utilization rate of photoactive species.
Smart Images

Figure CN119500283B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of functional polymer preparation technology, specifically relating to a method for preparing a BiOI-embedded bismuth-based surface molecularly imprinted photocatalyst and its application. Background Technology
[0002] Multiphase photocatalysis is a completely green advanced oxidation technology that can rapidly oxidize and decompose various pollutants in water without selectivity. However, the active species produced by photocatalysis have a short lifespan and lack selectivity. In actual water bodies, pollutants are complex in composition, and high concentrations of non-toxic soluble organic matter and various inorganic ions often coexist with low concentrations of target pollutants. Coexisting pollutants will form competitive adsorption on the catalyst surface and be preferentially degraded, resulting in the ineffective consumption of a large number of active species. The number of active species allocated to the target pollutant is limited, leading to poor removal efficiency.
[0003] Molecularly imprinted polymers (MIPs) are adsorbent materials with selective recognition capabilities. Under the guidance of template molecules, these materials copolymerize with functional monomers to form imprinted cavities containing "specific recognition sites." The combined effect of the functional monomer binding sites and the structurally complementary cavities enables the selective adsorption of target pollutants in complex aquatic environments, thereby achieving the purpose of separating and enriching low-concentration target pollutants.
[0004] Existing research has shown that combining molecularly imprinted polymers with photocatalytic materials to construct molecular recognition cavities near the catalytic active sites on the photocatalyst surface can enable the photocatalyst to accurately identify target pollutants under complex matrix conditions and enrich the target pollutants near the catalytic active sites. Under light irradiation, various active species generated by the catalyst can concentrate on attacking the target pollutants, enabling toxic chemicals to be efficiently degraded into non-toxic products, thus achieving the complete removal of target pollutants in a preferential manner.
[0005] Patent document CN111234295B discloses a method for preparing a molecularly imprinted photocatalytic material. The method involves mixing template molecules, functional monomers, and porogens for a prepolymerization reaction to obtain a prepolymer; mixing the prepolymer, crosslinking agent, initiator, and BiOBr and performing a polymerization reaction under a protective atmosphere to obtain a polymer; and eluting the polymer to obtain the molecularly imprinted photocatalytic material by calcination at a temperature of 400-500℃ for 2-4 hours. This patent document has the following three shortcomings: First, the solvents used in the preparation process are non-polar solvents such as acetonitrile or methanol. Although these solvents are commonly used in molecular imprinting preparation, they are environmentally unfriendly and prone to secondary pollution. Using polar solvents such as ethanol is relatively greener, but polar solvents such as ethanol usually affect the binding of functional monomers and template molecules, making it difficult to prepare molecularly imprinted polymers. Second, the removal of template molecules uses a calcination elution method, which requires relatively high temperatures and consumes a lot of energy. Elution with methanol is not effective. Third, from the perspective of selectivity, the selectivity of the prepared molecularly imprinted polymer is not obvious enough. This may be because the molecular structure of the imprinted site is destroyed during calcination, making the imprinted cavity unable to match the structure of the target pollutant. Alternatively, traditional chain functional monomers may form more non-imprinted regions during polymerization due to steric hindrance, resulting in the adsorption of non-target pollutants.
[0006] In the preparation of molecularly imprinted polymers (MIPs), the elution effect of template molecules directly affects the adsorption and selectivity of the MIP catalytic material. The high-temperature calcination method used in the aforementioned patent literature for eluting template molecules not only consumes a large amount of energy, but the excessively high temperature can also lead to the degradation of the MIP, thereby destroying the imprinted cavity structure and causing a mismatch between the imprinted cavity and the spatial structure of the template contaminants, resulting in reduced selectivity. Choosing a suitable solvent is also crucial in the preparation of MIPs, as it affects not only the polymerization reaction but also the performance of the final MIP product. Considering environmental protection and production safety, the chosen solvent should ideally be low in toxicity to minimize environmental impact. During the preparation of MIPs, the functional monomers and template molecules are mainly bonded through hydrogen bonds. The stronger the polarity of the solvent, the less conducive it is to hydrogen bond formation. Therefore, non-polar solvents such as acetonitrile or methanol are commonly used, but their disadvantages include high toxicity and environmental unfriendliness. Ethanol, a polar solvent, is relatively environmentally friendly, but it is detrimental to many molecular imprinting methods (especially non-covalent imprinting) because it inhibits the formation of hydrogen bonds between monomers and templates. This is one of the challenges faced by molecular imprinting technology.
[0007] While surface-imprinted photocatalysts have achieved some success in laboratory settings, they have inherent limitations in selectively degrading pollutants in practical applications. First, traditional surface-imprinted photocatalysts rely on adsorption-assisted selective degradation. The coating of the imprinted polymer typically creates additional adsorption sites to selectively adsorb the target pollutant. However, the target pollutant is usually separated from the catalytic site, and the long distance between these sites hinders selective oxidation. Furthermore, the short lifespan of photoactive species leads to their ineffective consumption over long distances, significantly reducing their utilization rate. Second, the imprinted layer covering the catalytically active sites causes light scattering, reducing light absorption and photocatalytic activity. Finally, traditional imprinted polymers generate numerous non-imprinted regions during the polymerization of chain functional monomers. The spatial structure of the imprinted cavity and the template pollutant is poorly matched, making them susceptible to interference from small molecules or structural analogs. This non-specific adsorption and competition between the imprinted polymer and the active material further reduce the degradation efficiency of the target pollutant. Simultaneous synthesis of BiOI with imprinted polymers on the surface of imprinted catalysts holds promise for achieving effective fusion of imprinted and catalytic sites, mitigating the reduction in photocatalytic performance caused by the covering of the imprinted layer. Furthermore, the embedding of BiOI into the imprinted polymer may improve the spatial structure of the imprinted cavity, thereby enhancing selectivity for target analytes. Currently, there are no relevant studies addressing this aspect. Summary of the Invention
[0008] The technical problem solved by this invention is to provide a method for preparing a BiOI-embedded bismuth-based surface molecularly imprinted photocatalyst. The BiOI-embedded bismuth-based surface molecularly imprinted photocatalyst prepared by this method has a strong ability to selectively adsorb the target analyte citalopram in aqueous solution and is preferentially and rapidly degraded under light conditions. It can be used for the selective photocatalytic removal of citalopram from actual water samples.
[0009] To solve the above-mentioned technical problems, the present invention adopts the following technical solution: a method for preparing a BiOI-embedded bismuth-based surface molecularly imprinted photocatalyst, characterized in that the specific process is as follows: the template molecule citalopram and the functional monomer 2-acrylamide-2-methylpropanesulfonic acid are dissolved in ethanol solvent and prepolymerized at 20~40℃ for 2~8 h; then the carrier BiOIO3 nanosheets and bismuth nitrate pentahydrate are added and ultrasonically dispersed and dissolved; then KI solution is added dropwise and stirred for 1~3 h; then the crosslinking agent ethylene glycol dimethacrylate and the initiator azobisisobutyronitrile are added; after ultrasonication and nitrogen protection, the mixture is thermally polymerized at 50~70℃ for 20~30 h; after elution and drying, the BiOI-embedded bismuth-based surface molecularly imprinted photocatalyst is obtained. The BiOIO3 nanosheets were synthesized by a hydrothermal method. The specific synthesis process was as follows: Bismuth nitrate pentahydrate and potassium iodate were dissolved in pure water, stirred for 1-2 h, and then placed in a high-pressure reactor with a polytetrafluoroethylene liner. The mixture was hydrothermally reacted at 130-180℃ for 3-8 h. After washing with water and ethanol several times and drying, BiOIO3 nanosheets were obtained.
[0010] Further specified, the molar ratio of the template molecule, functional monomer, crosslinking agent and initiator is 1:2~6:1~16:1; the molar ratio of the template molecule, bismuth nitrate pentahydrate and KI is 1:2~3:2~64.
[0011] Further specifying, the elution process specifically involves Soxhlet extraction for 48 h using a mixture of methanol and acetic acid at a volume ratio of 9:1.
[0012] The BiOI-embedded bismuth-based surface molecularly imprinted photocatalyst described in this invention is used for the selective photocatalytic removal of linfaxin from actual water samples.
[0013] Compared with the prior art, the present invention has the following advantages and beneficial effects: 1. This invention uses a method of simultaneous synthesis of BiOI and surface-imprinted polymers to prepare citalopram surface-imprinted photocatalysts. By controlling the BiOI content, the catalyst can be made to have properties such as high selectivity, good photocatalytic performance, large adsorption capacity and strong anti-interference ability.
[0014] 2. This invention uses ethanol as the preparation solvent, which reduces the secondary pollution to the environment caused by non-polar solvents such as acetonitrile and methanol.
[0015] 3. This invention employs a method of simultaneous synthesis of BiOI and imprinted polymers, and simultaneous coating of BiOIO3, to embed the photocatalyst BiOI into the imprinted polymer. Simultaneously, it forms a heterojunction with the support BiOIO3. This not only allows the photocatalyst to bind tightly to the adsorption sites, reducing mass transfer distance and improving the utilization rate of photoactive species, but also enhances the catalyst's light absorption capacity, extending it from ultraviolet light to visible light. Furthermore, during the simultaneous synthesis of BiOI and the imprinted polymer, BiOI also participates in the formation of imprinted sites and fills non-imprinted regions, making the imprinted cavity more compatible with the spatial structure of the target molecule, thus significantly improving selectivity. Attached Figure Description
[0016] Figure 1 This is a schematic diagram of the synthesis route of the carrier BiOIO3 and the imprinted photocatalyst EMI-Bi / Bi in this invention.
[0017] Figure 2 These are scanning electron microscope (SEM) images of the support, imprinted photocatalyst, and non-imprinted photocatalyst in this invention.
[0018] Figure 3 This is an adsorption kinetic diagram of the imprinted photocatalyst and the non-imprinted photocatalyst of this invention.
[0019] Figure 4 These are the adsorption isotherms of the imprinted and non-imprinted photocatalysts of this invention.
[0020] Figure 5 This is a graph showing the change over time in the removal rate of citalopram from municipal wastewater using the imprinted photocatalyst and photocatalyst carrier of this invention. Detailed Implementation
[0021] The following examples further illustrate the above-described content of the present invention, but it should not be construed as limiting the scope of the subject matter of the present invention to the following examples. All technologies implemented based on the above-described content of the present invention fall within the scope of the present invention. Example 1
[0022] Preparation of BiOIO3 nanosheets: 0.5 g of bismuth nitrate pentahydrate and 0.2 g of potassium iodate were dissolved in pure water and stirred for 1 h. The mixture was then placed in a high-pressure reactor lined with polytetrafluoroethylene and hydrothermally reacted at 130 °C for 3 h. After washing with water and ethanol several times and drying, BiOIO3 nanosheets were obtained.
[0023] Preparation of imprinted photocatalyst: Using 20 mL of ethanol as solvent, 0.1 mmol citalopram (template molecule) and 0.2 mmol 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 20 °C for 2 h. Then, 0.10 g of the self-made BiOIO3 nanosheets (support) and 0.2 mmol bismuth nitrate pentahydrate were added. After thorough dispersion and dissolution by ultrasonication, 10 mL of an aqueous solution containing 0.2 mmol KI was added dropwise and stirred for 1 h. Then, 0.2 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After ultrasonication and N2 purging, thermal polymerization was initiated at 50 °C for 20 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture with a volume ratio of 9:1 by Soxhlet extraction for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 2
[0024] Preparation of BiOIO3 nanosheets: 0.5 g of bismuth nitrate pentahydrate and 0.2 g of potassium iodate were dissolved in pure water and stirred for 2 h. The mixture was then placed in a high-pressure reactor lined with polytetrafluoroethylene and hydrothermally reacted at 130 °C for 3 h. After washing with water and ethanol several times and drying, BiOIO3 nanosheets were obtained.
[0025] Preparation of imprinted photocatalyst: Using 20 mL of ethanol as solvent, 0.1 mmol citalopram (template molecule) and 0.2 mmol 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 20 °C for 2 h. Then, 0.10 g of the self-made BiOIO3 nanosheets (support) and 0.2 mmol bismuth nitrate pentahydrate were added. After thorough dispersion and dissolution by ultrasonication, 10 mL of an aqueous solution containing 0.2 mmol KI was added dropwise and stirred for 1 h. Then, 0.2 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After ultrasonication and N2 purging, thermal polymerization was initiated at 50 °C for 20 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture with a volume ratio of 9:1 by Soxhlet extraction for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 3
[0026] Preparation of BiOIO3 nanosheets: 0.5 g of bismuth nitrate pentahydrate and 0.2 g of potassium iodate were dissolved in pure water and stirred for 1 h. The mixture was then placed in a high-pressure reactor lined with polytetrafluoroethylene and hydrothermally reacted at 180 °C for 3 h. After washing with water and ethanol several times and drying, BiOIO3 nanosheets were obtained.
[0027] Preparation of imprinted photocatalyst: Using 20 mL of ethanol as solvent, 0.1 mmol citalopram (template molecule) and 0.2 mmol 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 20 °C for 2 h. Then, 0.10 g of the self-made BiOIO3 nanosheets (support) and 0.2 mmol bismuth nitrate pentahydrate were added. After thorough dispersion and dissolution by ultrasonication, 10 mL of an aqueous solution containing 0.2 mmol KI was added dropwise and stirred for 1 h. Then, 0.2 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After ultrasonication and N2 purging, thermal polymerization was initiated at 50 °C for 20 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture with a volume ratio of 9:1 by Soxhlet extraction for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 4
[0028] Preparation of BiOIO3 nanosheets: 0.5 g of bismuth nitrate pentahydrate and 0.2 g of potassium iodate were dissolved in pure water and stirred for 1 h. The mixture was then placed in a high-pressure reactor lined with polytetrafluoroethylene and subjected to hydrothermal reaction at 180 °C for 8 h. After washing with water and ethanol several times and drying, BiOIO3 nanosheets were obtained.
[0029] Preparation of imprinted photocatalyst: Using 20 mL of ethanol as solvent, 0.1 mmol citalopram (template molecule) and 0.2 mmol 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 20 °C for 2 h. Then, 0.10 g of the self-made BiOIO3 nanosheets (support) and 0.2 mmol bismuth nitrate pentahydrate were added. After thorough dispersion and dissolution by ultrasonication, 10 mL of an aqueous solution containing 0.2 mmol KI was added dropwise and stirred for 1 h. Then, 0.2 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After ultrasonication and N2 purging, thermal polymerization was initiated at 50 °C for 20 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture with a volume ratio of 9:1 by Soxhlet extraction for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 5
[0030] Preparation of BiOIO3 nanosheets: 0.5 g of bismuth nitrate pentahydrate and 0.2 g of potassium iodate were dissolved in pure water and stirred for 1 h. The mixture was then placed in a high-pressure reactor lined with polytetrafluoroethylene and subjected to hydrothermal reaction at 180 °C for 8 h. After washing with water and ethanol several times and drying, BiOIO3 nanosheets were obtained.
[0031] Preparation of imprinted photocatalyst: Using 20 mL of ethanol as solvent, 0.1 mmol citalopram (template molecule) and 0.6 mmol 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 20 °C for 2 h. Then, 0.10 g of the self-made BiOIO3 nanosheets (support) and 0.2 mmol bismuth nitrate pentahydrate were added. After thorough dispersion and dissolution by ultrasonication, 10 mL of an aqueous solution containing 0.2 mmol KI was added dropwise and stirred for 1 h. Then, 0.2 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After ultrasonication and N2 purging, thermal polymerization was initiated at 50 °C for 20 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture with a volume ratio of 9:1 by Soxhlet extraction for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 6
[0032] Preparation of BiOIO3 nanosheets: 0.5 g of bismuth nitrate pentahydrate and 0.2 g of potassium iodate were dissolved in pure water and stirred for 1 h. The mixture was then placed in a high-pressure reactor lined with polytetrafluoroethylene and subjected to hydrothermal reaction at 180 °C for 8 h. After washing with water and ethanol several times and drying, BiOIO3 nanosheets were obtained.
[0033] Preparation of imprinted photocatalyst: Using 20 mL of ethanol as solvent, 0.1 mmol citalopram (template molecule) and 0.6 mmol 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 40 °C for 2 h. Then, 0.10 g of the self-made BiOIO3 nanosheets (support) and 0.2 mmol bismuth nitrate pentahydrate were added. After thorough dispersion and dissolution by ultrasonication, 10 mL of an aqueous solution containing 0.2 mmol KI was added dropwise and stirred for 1 h. Then, 0.2 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After ultrasonication and N2 purging, thermal polymerization was initiated at 50 °C for 20 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture with a volume ratio of 9:1 by Soxhlet extraction for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 7
[0034] Preparation of BiOIO3 nanosheets: 0.5 g of bismuth nitrate pentahydrate and 0.2 g of potassium iodate were dissolved in pure water and stirred for 1 h. The mixture was then placed in a high-pressure reactor lined with polytetrafluoroethylene and subjected to hydrothermal reaction at 180 °C for 8 h. After washing with water and ethanol several times and drying, BiOIO3 nanosheets were obtained.
[0035] Preparation of imprinted photocatalyst: Using 20 mL of ethanol as solvent, 0.1 mmol citalopram (template molecule) and 0.6 mmol 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 40 °C for 8 h. Then, 0.10 g of the self-made BiOIO3 nanosheets (support) and 0.2 mmol bismuth nitrate pentahydrate were added. After thorough dispersion and dissolution by ultrasonication, 10 mL of an aqueous solution containing 0.2 mmol KI was added dropwise and stirred for 1 h. Then, 0.2 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After ultrasonication and N2 purging, thermal polymerization was initiated at 50 °C for 20 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture with a volume ratio of 9:1 by Soxhlet extraction for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 8
[0036] Preparation of BiOIO3 nanosheets: 0.5 g of bismuth nitrate pentahydrate and 0.2 g of potassium iodate were dissolved in pure water and stirred for 1 h. The mixture was then placed in a high-pressure reactor lined with polytetrafluoroethylene and subjected to hydrothermal reaction at 180 °C for 8 h. After washing with water and ethanol several times and drying, BiOIO3 nanosheets were obtained.
[0037] Preparation of imprinted photocatalyst: Using 20 mL of ethanol as solvent, 0.1 mmol citalopram (template molecule) and 0.6 mmol 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 40 °C for 8 h. Then, 0.10 g of the self-made BiOIO3 nanosheets (support) and 0.3 mmol bismuth nitrate pentahydrate were added. After thorough dispersion and dissolution by ultrasonication, 10 mL of an aqueous solution containing 0.2 mmol KI was added dropwise and stirred for 1 h. Then, 0.2 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After ultrasonication and N2 purging, thermal polymerization was initiated at 50 °C for 20 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture with a volume ratio of 9:1 by Soxhlet extraction for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 9
[0038] Preparation of BiOIO3 nanosheets: 0.5 g of bismuth nitrate pentahydrate and 0.2 g of potassium iodate were dissolved in pure water and stirred for 1 h. The mixture was then placed in a high-pressure reactor lined with polytetrafluoroethylene and subjected to hydrothermal reaction at 180 °C for 8 h. After washing with water and ethanol several times and drying, BiOIO3 nanosheets were obtained.
[0039] Preparation of imprinted photocatalyst: Using 20 mL of ethanol as solvent, 0.1 mmol citalopram (template molecule) and 0.6 mmol 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 40 °C for 8 h. Then, 0.10 g of the self-made BiOIO3 nanosheets (support) and 0.3 mmol bismuth nitrate pentahydrate were added. After thorough dispersion and dissolution by ultrasonication, 10 mL of an aqueous solution containing 0.001 mmol KI was added dropwise and stirred for 1 h. Then, 0.2 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After ultrasonication and N2 purging, thermal polymerization was initiated at 50 °C for 20 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture with a volume ratio of 9:1 by Soxhlet extraction for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 10
[0040] Preparation of BiOIO3 nanosheets: 0.5 g of bismuth nitrate pentahydrate and 0.2 g of potassium iodate were dissolved in pure water and stirred for 1 h. The mixture was then placed in a high-pressure reactor lined with polytetrafluoroethylene and subjected to hydrothermal reaction at 180 °C for 8 h. After washing with water and ethanol several times and drying, BiOIO3 nanosheets were obtained.
[0041] Preparation of imprinted photocatalyst: Using 20 mL of ethanol as solvent, 0.1 mmol citalopram (template molecule) and 0.6 mmol 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 40 °C for 8 h. Then, 0.10 g of the self-made BiOIO3 nanosheets (support) and 0.3 mmol bismuth nitrate pentahydrate were added. After thorough dispersion and dissolution by ultrasonication, 10 mL of an aqueous solution containing 0.001 mmol KI was added dropwise and stirred for 3 h. Then, 0.2 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After ultrasonication and N2 purging, thermal polymerization was initiated at 50 °C for 20 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture with a volume ratio of 9:1 by Soxhlet extraction for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 11
[0042] Preparation of BiOIO3 nanosheets: 0.5 g of bismuth nitrate pentahydrate and 0.2 g of potassium iodate were dissolved in pure water and stirred for 1 h. The mixture was then placed in a high-pressure reactor lined with polytetrafluoroethylene and subjected to hydrothermal reaction at 180 °C for 8 h. After washing with water and ethanol several times and drying, BiOIO3 nanosheets were obtained.
[0043] Preparation of imprinted photocatalyst: Using 20 mL of ethanol as solvent, 0.1 mmol citalopram (template molecule) and 0.6 mmol 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 40 °C for 8 h. Then, 0.10 g of the self-made BiOIO3 nanosheets (support) and 0.3 mmol bismuth nitrate pentahydrate were added. After thorough dispersion and dissolution by ultrasonication, 10 mL of an aqueous solution containing 0.001 mmol KI was added dropwise and stirred for 3 h. Then, 1.6 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After ultrasonication and N2 purging, thermal polymerization was initiated at 50 °C for 20 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture with a volume ratio of 9:1 by Soxhlet extraction for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 12
[0044] Preparation of BiOIO3 nanosheets: Bismuth nitrate pentahydrate and potassium iodate were dissolved in pure water, stirred for 1 h, and then placed in a high-pressure reactor lined with polytetrafluoroethylene. The mixture was hydrothermally reacted at 180℃ for 8 h. After washing with water and ethanol several times and drying, BiOIO3 nanosheets were obtained.
[0045] Preparation of imprinted photocatalyst: Using 20 mL of ethanol as solvent, 0.1 mmol citalopram (template molecule) and 0.6 mmol 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 40 °C for 8 h. Then, 0.10 g of the self-made BiOIO3 nanosheets (support) and 0.3 mmol bismuth nitrate pentahydrate were added. After thorough dispersion and dissolution by ultrasonication, 10 mL of an aqueous solution containing 0.001 mmol KI was added dropwise and stirred for 3 h. Then, 1.6 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After ultrasonication and N2 purging, thermal polymerization was initiated at 70 °C for 20 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture with a volume ratio of 9:1 by Soxhlet extraction for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 13
[0046] Preparation of BiOIO3 nanosheets: Bismuth nitrate pentahydrate and potassium iodate were dissolved in pure water, stirred for 1 h, and then placed in a high-pressure reactor lined with polytetrafluoroethylene. The mixture was hydrothermally reacted at 180℃ for 8 h. After washing with water and ethanol several times and drying, BiOIO3 nanosheets were obtained.
[0047] Preparation of imprinted photocatalyst: Using 20 mL of ethanol as solvent, 0.1 mmol citalopram (template molecule) and 0.6 mmol 2-acrylamide-2-methylpropanesulfonic acid (functional monomer) were prepolymerized at 40 °C for 8 h. Then, 0.10 g of the self-made BiOIO3 nanosheets (support) and 0.3 mmol bismuth nitrate pentahydrate were added. After thorough dispersion and dissolution by ultrasonication, 10 mL of an aqueous solution containing 0.001 mmol KI was added dropwise and stirred for 3 h. Then, 1.6 mmol of crosslinking agent ethylene glycol dimethacrylate and 0.1 mmol of initiator azobisisobutyronitrile were added. After ultrasonication and N2 purging, thermal polymerization was initiated at 70 °C for 30 h to obtain the product. The product was then extracted with a methanol / acetic acid mixture with a volume ratio of 9:1 by Soxhlet extraction for 48 h and vacuum dried to obtain the imprinted photocatalyst. Example 14
[0048] 20 mg of the imprinted photocatalyst (EMI-Bi / Bi) and the non-imprinted photocatalyst (ENI-Bi / Bi) prepared in Example 1 were respectively mixed with 50 mL of 20 mg L of each. -1 The mixture was stirred at room temperature with citalopram aqueous solution for a certain period of time (0-80 min) before adsorption. The supernatant was then collected and the absorbance at 238 nm was measured using a UV spectrophotometer. The results are as follows: Figure 3 As shown. Example 15
[0049] 20 mg of the imprinted photocatalyst (EMI-Bi / Bi) and the non-imprinted photocatalyst (ENI-Bi / Bi) prepared in Example 1 were respectively mixed with 50 mL of citalopram aqueous solution (0-100 mg / L). -1 After adsorption by shaking at room temperature for 80 min, the supernatant was collected and the absorbance at 238 nm was measured using a UV spectrophotometer. The results are as follows: Figure 4 As shown. Example 16
[0050] 20 mg of the imprinted photocatalyst (EMI-Bi / Bi), the non-imprinted photocatalyst (ENI-Bi / Bi), and the photocatalyst support (BiOIO3) prepared in Example 1 were dispersed in 50 mL of a solution containing 20 mg of citalopram. -1 ) and humic acid (60 mg / L) -1 In a mixed aqueous solution of citalopram, the mixture was stirred for 40 min in the dark to ensure adsorption-desorption equilibrium. Stirring was then continued for 180 min under a 500 W xenon lamp. The concentration of citalopram in the solution was determined at intervals using high-performance liquid chromatography (HPLC). The results are as follows: Figure 5 As shown. Example 17
[0051] The imprinted photocatalyst prepared in Example 1 was used for the photocatalytic degradation of citalopram in actual wastewater. Spiked experiments showed a removal rate greater than 90%, which, under the same conditions, was more than 17% higher than that of traditional imprinted photocatalysts and more than 28% higher than that of photocatalyst carriers. This indicates that the obtained imprinted photocatalyst has good practicality for the degradation of venlafaxine; after 7 cycles of use, the adsorption capacity of the imprinted photocatalyst for venlafaxine still reached 31 mg / g. -1 The total removal rate still reached over 83%, indicating that the obtained imprinted polymer has excellent regeneration adsorption performance and stability.
[0052] The above embodiments describe the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are only illustrative of the principles of the present invention. Various changes and modifications can be made to the present invention without departing from the scope of the principles of the present invention, and all such changes and modifications fall within the protection scope of the present invention.
Claims
1. A method for preparing a BiOI-embedded bismuth-based surface molecularly imprinted photocatalyst, characterized in that, The specific process is as follows: Citalopram template molecule and functional monomer 2-acrylamide-2-methylpropanesulfonic acid are dissolved in ethanol solvent and prepolymerized at 20~40℃ for 2~8 h. Then, BiOIO3 nanosheets and bismuth nitrate pentahydrate are added and ultrasonically dispersed and dissolved. KI solution is then added dropwise and stirred for 1~3 h. Then, ethylene glycol dimethacrylate crosslinking agent and azobisisobutyronitrile initiator are added. After ultrasonication and nitrogen protection, thermal polymerization is carried out at 50~70℃ for 20~30 h. After elution and drying, BiOI embedded bismuth-based surface molecularly imprinted photocatalyst is obtained. The BiOIO3 nanosheets were synthesized by a hydrothermal method. The specific synthesis process was as follows: Bismuth nitrate pentahydrate and potassium iodate were dissolved in pure water, stirred for 1-2 h, and then placed in a high-pressure reactor with a polytetrafluoroethylene liner. The reaction was carried out at 130-180℃ for 3-8 h. After washing with water and ethanol several times and drying, BiOIO3 nanosheets were obtained. The elution process specifically involves Soxhlet extraction for 48 h using a mixture of methanol and acetic acid at a volume ratio of 9:
1.
2. The method for preparing the BiOI-embedded bismuth-based surface molecularly imprinted photocatalyst according to claim 1, characterized in that: The molar ratio of the template molecule, functional monomer, crosslinking agent and initiator is 1:2~6:1~16:1; the molar ratio of the template molecule, bismuth nitrate pentahydrate and KI is 1:2~3:2~64.
3. The BiOI-embedded bismuth-based surface molecularly imprinted photocatalyst prepared according to claim 1 or 2 is used for the selective photocatalytic removal of citalopram from actual water samples.
Citation Information
Patent Citations
A molecularly imprinted photocatalytic material, its preparation method and application
CN111234295B
Preparation method of carbon-doped BiOI / BiOIO3 heterostructure
CN108786859A
Preparation method and application of molecularly imprinted BiOI / g-carbon nitride catalyst
CN117443426A