A method of flanging a burner tube base
By performing steps such as notching the bend, removing excess material, rounding the sharp edge, pre-bending the edge, and straightening, the problem of cracking at the bend of the flame tube seat was solved, ensuring molding quality and reducing production costs.
Patent Information
- Application Number
- CN202411704523.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-26
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-11-26
AI Technical Summary
The bent edge of the flame tube seat is prone to cracking during the molding process, leading to product scrap and high production costs.
By creating notches on both sides of the bent edge, removing excess material, rounding the sharp edge, pre-bending the edge, thermoforming, and straightening, the risk of bending is reduced, and the forming quality is ensured through multiple bending and straightening processes.
This effectively prevents cracking at the bend, ensures the molding quality of the flame tube seat, and reduces production costs.
Smart Images

Figure CN119501490B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of parts processing technology, and in particular to a method for forming the bending edge of a flame-connecting tube seat. Background Technology
[0002] like Figure 2 The flame tube housing shown is an indispensable component of the engine's combustion system, ensuring coordinated combustion of each flame tube within the combustion chamber and stable operation of the combustion chamber. Its molding quality has a significant impact on engine performance. This flame tube housing is manufactured from sheet metal, is small in size, and has a complex structure. During the molding process, cracks can easily occur at the bent edges, resulting in product scrap. Summary of the Invention
[0003] In view of the above-mentioned defects or deficiencies in the prior art, it is desirable to provide a bending forming method for the flame tube seat, which effectively avoids the problem of cracking at the bending edge, ensures the forming quality of the flame tube seat, and effectively reduces production costs.
[0004] The present invention provides a method for forming the bending edge of a flame-connecting tube seat, comprising the following steps:
[0005] 1) Pre-processing: Mill the cylindrical blank and make a notch on both sides of the bent edge; then wire cut the bottom of the bent edge to remove excess material; then trim the bent edge with clamps to round off its sharp edges.
[0006] 2) Pre-bending: The cylindrical blank is pre-bent at the bending edge using a pre-forming mold, bending it outward by 30°-60° to form a pre-formed blank. The pre-formed blank is then subjected to stress-relieving heat treatment.
[0007] 3) Bending edge: The preformed blank is clamped by the bending edge mold, and the bending edge is manually bent to 90° by thermoforming process to form the bending edge blank.
[0008] 4) Shaping: The bent blank is shaped using a shaping mold to meet the design dimensions of the flame tube seat;
[0009] 5) Machining: The structural features of the bent blank are machined to obtain the flame tube seat.
[0010] Furthermore, in step 2), the bent edge is bent outward at 45° to form the preform blank.
[0011] Furthermore, the preforming mold includes:
[0012] First template;
[0013] The first die is fixedly disposed on the top surface of the first lower template. The top surface of the first die has a first cavity. A clearance groove is provided on one side of the top of the first cavity corresponding to the bent edge. The top surface of the first die is provided with first guide posts on both sides of the first cavity.
[0014] The first upper template is positioned above the first concave mold;
[0015] The first punch is fixedly disposed on the bottom surface of the first upper template. The bottom surface of the first punch is fixedly disposed on the first mold cavity. A bending block is fixedly disposed on the top side of one side of the first module corresponding to the bending edge, which is used to squeeze the bending edge of the cylindrical blank to bend it outward by 30°-60°. The bottom surface of the first punch is provided with a first guide hole corresponding to the first guide post.
[0016] Furthermore, the bending die includes:
[0017] Second template;
[0018] The second die is fixedly disposed on the top surface of the second lower template. The top surface of the second die has a second mold cavity. A recessed step is provided on one side of the top surface of the second die located in the second mold cavity. A groove communicating with the second mold cavity is provided on the top surface of the recessed step corresponding to the bent edge.
[0019] The second punch is fixed in the second mold cavity by screws. A pressure edge is provided on the outer periphery of its top end, and an avoidance step is provided on one side of its top end corresponding to the groove.
[0020] Furthermore, the calibration mold includes:
[0021] The third template has through holes from its bottom to its top surface;
[0022] The third die is fixedly set on the top surface of the third lower template, located above the through hole. The top surface of the third die has a third mold cavity that communicates with the through hole. A shaping groove is set on one side of the top of the third mold cavity corresponding to the bent edge. The top surface of the third die has third guide posts set on both sides of the third mold cavity.
[0023] The ejector block is slidably embedded in the through hole in the vertical direction;
[0024] The third upper template is positioned above the third concave mold;
[0025] The third punch is fixedly disposed on the bottom surface of the third upper template. The bottom surface of the third punch is fixedly disposed on the third mold cavity. A bending edge straightening block is fixedly disposed on the top side of one side of the third module corresponding to the bending edge. The bottom surface of the third punch is provided with a third guide hole corresponding to the third guide post.
[0026] Furthermore, the inner diameter of the through hole is larger than the inner diameter of the third mold cavity, the outer diameter of the ejector block is clearance-fitted with the inner diameter of the third mold cavity, and a limiting step is provided on the outer periphery of the bottom end of the ejector block. The outer diameter of the limiting step is larger than the inner diameter of the third mold cavity and is clearance-fitted with the inner diameter of the through hole.
[0027] Compared with the prior art, the beneficial effects of the present invention are:
[0028] The forming method of this invention first creates notches on both sides of the bent edge to separate it, so that only the bent edge is bent subsequently, without fully bending the bottom of the cylindrical blank; then, the excess material at the bottom of the bent edge is removed to reduce the bending height; then, the sharp edge of the bent edge is rounded; this series of pre-processing greatly reduces the risk of cracking when bending the bent edge; then, the bent edge is shaped by two bending processes, further reducing the risk of bending cracking; then, the dimensions of the flame-connecting tube seat are ensured through shaping; finally, the remaining structural features are machined to obtain the flame-connecting tube seat. The forming method of this application effectively avoids the problem of cracking at the bent edge, ensures the forming quality of the flame-connecting tube seat, and effectively reduces production costs.
[0029] It should be understood that the description in the Summary of the Invention is not intended to limit the key or essential features of the embodiments of the present invention, nor is it intended to restrict the scope of the invention. Other features of the invention will become readily apparent from the following description. Attached Figure Description
[0030] Other features, objects, and advantages of the invention will become more apparent from the following detailed description of non-limiting embodiments with reference to the accompanying drawings:
[0031] Figure 1 This is a schematic diagram of the bending forming method for the flame tube seat;
[0032] Figure 2 This is a schematic diagram of the structure of the flame tube socket;
[0033] Figure 3 This is a schematic diagram of the cylindrical blank structure;
[0034] Figure 4 This is a schematic diagram of the cross-sectional structure of the preformed blank;
[0035] Figure 5 This is a schematic diagram of the preforming mold structure;
[0036] Figure 6 This is an exploded structural diagram of a preform mold.
[0037] Figure 7 This is a schematic diagram of the cross-sectional structure of a preforming mold;
[0038] Figure 8 This is a schematic diagram of the bending die structure;
[0039] Figure 9 This is an exploded structural diagram of a bending die;
[0040] Figure 10 This is a schematic diagram of the cross-sectional structure of the bending die;
[0041] Figure 11 This is a schematic diagram of the calibration mold.
[0042] Figure 12 This is a cross-sectional structural diagram of the calibration mold;
[0043] Figure 13 This is an exploded structural diagram of the calibration mold.
[0044] The labels in the diagram are: 1. Flame tube base; 2. Pre-forming mold; 3. Bending mold; 4. Shaping mold; 11. Bending section; 12. Cylindrical blank; 13. Notch; 14. Pre-forming blank.
[0045] 21. First lower mold plate; 22. First cavity mold; 23. First upper mold plate; 24. First punch mold; 25. First mold cavity; 26. Clearance groove; 27. First guide post; 28. First module; 29. Bent edge block; 210. First guide hole;
[0046] 31. Second lower mold plate; 32. Second cavity mold; 33. Second punch mold; 34. Second mold cavity; 35. Recessed step; 36. Profile groove; 37. Screw; 38. Pressing edge; 39. Clearance step;
[0047] 41. Third lower mold plate; 42. Third cavity mold; 43. Unloading block; 44. Third upper mold plate; 45. Third punch mold; 46. Through hole; 47. Third mold cavity; 48. Shaping groove; 49. Third guide post; 410. Third module; 411. Bending edge shaping block; 412. Third guide hole; 413. Limiting step. Detailed Implementation
[0048] The present invention will now be described in further detail with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the invention and not intended to limit it. Furthermore, it should be noted that, for ease of description, only the parts relevant to the invention are shown in the accompanying drawings.
[0049] It should be noted that, unless otherwise specified, the embodiments and features described in the present invention can be combined with each other. The present invention will now be described in detail with reference to the accompanying drawings and embodiments.
[0050] Please refer to Figures 1 to 13 The present invention provides a method for forming the bending edge of a flame-connecting tube seat, comprising the following steps:
[0051] 1) Pre-processing: Mill the cylindrical blank 12 and make a notch 13 on both sides of the bent edge 11; then wire cut the bottom of the bent edge 11 to remove excess material; then trim the bent edge 11 with clamps to round its sharp edge.
[0052] 2) Pre-bending: The bending part 11 of the cylindrical blank 12 is pre-bent by the pre-forming mold 2, so that it is bent outward by 30°-60° to form a pre-formed blank 14, and the pre-formed blank 14 is subjected to stress relief heat treatment.
[0053] 3) Bending the edge: The preformed blank 14 is clamped by the bending edge mold 3, and the bending edge part 11 is manually bent to 90° to form a bending edge blank by thermoforming process.
[0054] 4) Shaping: The bent blank is shaped using the shaping mold 4 to meet the design dimensions of the flame tube seat 1;
[0055] 5) Machining: The structural features of the bent blank are machined to obtain the flame tube seat 1.
[0056] In this embodiment, when processing and forming the flame tube seat 1, notches 13 are first made on both sides of the bent edge portion 11 to separate the bent edge portion 11 from the rest of the bottom end of the cylindrical blank 12, so that only the bent edge portion 11 needs to be bent in the future, without having to bend the bottom end of the cylindrical blank 12 completely, reducing the bending range and effectively reducing the risk of bending cracks.
[0057] Then, the excess material at the bottom of the bent edge 11 is removed to reduce the height of the bent edge; then the sharp edge of the bent edge 11 is rounded to effectively reduce the risk of bending and cracking.
[0058] Then, the curved edge 11 of the cylindrical blank 12 is pre-bent using the pre-forming mold 2, and then stress relief heat treatment is performed to eliminate the stress in the curved edge 11.
[0059] The preformed blank 14 is then clamped using the bending mold 3, and then heated to the process temperature. After heating, a pad is placed on the bending part 11, and the bending part 11 is manually bent to 90° by hammering the pad to form the bending blank. The bending part 11 is formed by bending twice, which reduces the risk of bending cracking due to excessive bending in one bending.
[0060] Then, the dimensions of the flame-connecting tube seat 1 are ensured through calibration; the remaining structural features are then machined to obtain the flame-connecting tube seat. The forming method of this application effectively avoids the problem of cracking at the bent edge, ensures the forming quality of the flame-connecting tube seat, and effectively reduces production costs.
[0061] In a preferred embodiment, in step 2), the bent edge is bent outward at 45° to form a preform blank 14, and the bending angle is equally divided into two bends, reducing the risk of bending cracks caused by excessive bending angle in a single bend.
[0062] In a preferred embodiment, such as Figures 5-7 As shown, the preforming mold 2 includes:
[0063] First template 21;
[0064] The first die 22 is fixedly set on the top surface of the first lower template 21. The top surface of the first die 22 has a first mold cavity 25. A relief groove 26 is set on one side of the top of the first mold cavity 25 corresponding to the bent edge 11. The top surface of the first die 22 is provided with first guide posts 27 on both sides of the first mold cavity 25.
[0065] The first upper template 23 is positioned above the first concave mold 22;
[0066] The first punch 24 is fixedly set on the bottom surface of the first upper template 23. The bottom surface of the first punch 24 is fixedly set with the first module 28 corresponding to the first mold cavity 25. The top of one side of the first module 28 is fixedly set with the bending edge block 29 corresponding to the bending edge 11, which is used to press the bending edge 11 of the cylindrical blank 12 to bend it outward by 30°-60°. The bottom surface of the first punch 24 is provided with the first guide hole 210 corresponding to the first guide post 27.
[0067] In this embodiment, when pre-bending the cylindrical blank 12 after pre-processing, the cylindrical blank 12 is inverted so that the bent edge 11 faces upward, and it is embedded into the first mold cavity 25; then the cylindrical blank 12 is rotated so that the bent edge 11 is aligned with the relief groove 26. At this time, the first upper template 23 is slowly pressed down by the hydraulic equipment, and the first punch 24 is pressed down together. The first guide post 27 is first inserted into the corresponding first guide hole 210; under the guidance, the first module 28 is inserted into the cylindrical blank 12, and then the bending block 29 slowly squeezes the bent edge 11 of the cylindrical blank 12, making it bend outward. After the mold is closed, the pre-bending is completed. The pre-bending forming effect is good, ensuring the forming quality of the flame tube seat 1.
[0068] In a preferred embodiment, such as Figures 8-10 As shown, the bending die 3 includes:
[0069] Second template 31;
[0070] The second cavity 32 is fixedly disposed on the top surface of the second lower template 31. The top surface of the second cavity 32 is provided with a second mold cavity 34. A recessed step 35 is provided on one side of the top surface of the second cavity 34. A profile groove 36 communicating with the second mold cavity 34 is provided on the top surface of the recessed step 35 corresponding to the bent edge 11.
[0071] The second punch 33 is fixed in the second mold cavity 34 by screws 37. A pressure edge 38 is provided on the outer periphery of its top end, and an avoidance step 39 is provided on one side of its top end corresponding to the profile groove 36.
[0072] In this embodiment, when bending the bent edge 11 of the preform blank 14, it is embedded into the second mold cavity 34, so that the bent edge 11 is placed above the profile groove 36; then the second punch 33 is inserted into the preform blank 14, with the clearance step 39 facing the bent edge 11; then the screw 37 is passed through the connecting through hole on the second punch 33 and threadedly connected to the threaded hole at the bottom of the second mold cavity 34, the screw 37 is tightened, and the pressing edge 38 presses and fixes the top of the preform blank 14, thus completing the clamping;
[0073] At this time, the preformed blank 14 and the bending mold 3 are placed together in the heating equipment for heating. After heating to the process temperature, a pad is placed on the bending part 11, and the pad is hammered until the bending part 11 fits on the molded groove 36. The bending part 11 is then manually bent to 90°. The bending forming effect is good, ensuring the forming quality of the flame tube seat 1.
[0074] In a preferred embodiment, such as Figures 11-13 As shown, the calibration mold 4 includes:
[0075] The third lower template 41 has through holes 46 from its bottom surface to its top surface;
[0076] The third die 42 is fixedly set on the top surface of the third lower template 41, located above the through hole 46. The top surface of the third die 41 has a third mold cavity 47 that communicates with the through hole 46. A shaping groove 48 is provided on one side of the top of the third mold cavity 47 corresponding to the bent edge 11. The top surface of the third die 42 is provided with third guide posts 49 on both sides of the third mold cavity 47.
[0077] The ejector block 43 is slidably embedded in the through hole 46 in the vertical direction;
[0078] The third upper mold plate 44 is set above the third cavity mold 42;
[0079] The third punch 45 is fixedly set on the bottom surface of the third upper template 44. The bottom surface of the third punch 45 is fixedly set with the third module 410 corresponding to the third mold cavity 47. The top of one side of the third module 410 is fixedly set with the bending edge 11 with the bending edge shaping block 411. The bottom surface of the third punch 45 is provided with the third guide hole 412 corresponding to the third guide post 49.
[0080] In this embodiment, when straightening the bent blank, it is embedded in the third mold cavity 47, and the bent part 11 is embedded in the straightening groove 48; then, the third upper mold plate 44 is slowly pressed down by the hydraulic equipment, and the third punch 45 is pressed down together. The third guide post 49 is first inserted into the corresponding third guide hole 412; under the guidance, the third module 410 is inserted into the bent blank and cooperates with the third mold cavity 47 to straighten the main body of the bent blank; the straightening block 411 is pressed on the bent part 11 and cooperates with the straightening groove 48 to straighten the bent part 11 of the bent blank; after the mold is closed, the straightening is completed, the straightening effect is good, and the forming quality of the flame tube seat 1 is ensured.
[0081] In a preferred embodiment, such as Figure 12 As shown, the inner diameter of the through hole 46 is larger than the inner diameter of the third mold cavity 47. The outer diameter of the ejector block 43 is clearance-fitted with the inner diameter of the third mold cavity 47. A limiting step 413 is provided on the outer periphery of the bottom end of the ejector block 43. The outer diameter of the limiting step 413 is larger than the inner diameter of the third mold cavity 47 and is clearance-fitted with the inner diameter of the through hole 46.
[0082] In this embodiment, after the curved blank is shaped, the hydraulic equipment lifts the third upper mold plate 44, and then the ejector block 43 is pushed up. The ejector block 43 lifts the curved blank, completing the automatic ejection. After the limiting step 413 abuts against the bottom of the third mold cavity 47, the ejector block 43 can no longer move upward, and the ejection is just completed. The structure is reasonably designed and the ejection is convenient.
[0083] In the description of this specification, the terms "connection," "installation," and "fixing," etc., should be interpreted broadly. For example, "connection" can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection or an indirect connection through an intermediate medium. Those skilled in the art can understand the specific meaning of the above terms in this application according to the specific circumstances.
[0084] In the description of this specification, the terms "one embodiment," "some embodiments," etc., refer to specific features, structures, materials, or characteristics described in connection with that embodiment or example, which are included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0085] The above are merely preferred embodiments of this application and are not intended to limit this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.
Claims
1. A method for forming the bending edge of a flame-connecting tube seat, characterized in that, Includes the following steps: 1) Pre-processing: Mill the cylindrical blank (12) and make a notch (13) on both sides of the bent edge (11); then wire cut the bottom of the bent edge (11) to remove excess material; then pliers the bent edge (11) to round its sharp edge. 2) Pre-bending: The bending part (11) of the cylindrical blank (12) is pre-bent by using the pre-forming mold (2) to bend it outward by 30°-60° to form a pre-formed blank (14). The pre-formed blank (14) is subjected to stress relief heat treatment. 3) Bending edge: The preformed blank (14) is clamped by the bending edge mold (3), and the bending edge part (11) is manually bent to 90° by thermoforming process to form the bending edge blank. 4) Correction: The bending blank is corrected by the correction mold (4) to meet the design dimensions of the flame tube seat (1); 5) Machining: The structural features of the bent blank are machined to obtain the flame tube seat (1); The preforming mold (2) includes: First template (21); The first die (22) is fixedly disposed on the top surface of the first lower template (21). The top surface of the first die (22) is provided with a first mold cavity (25). A relief groove (26) is provided on one side of the top of the first mold cavity (25) corresponding to the bent edge (11). The top surface of the first die (22) is provided with first guide posts (27) on both sides of the first mold cavity (25). The first upper template (23) is positioned above the first cavity (22); and The first punch (24) is fixedly disposed on the bottom surface of the first upper template (23). The bottom surface of the first punch (24) is fixedly disposed on the first mold cavity (25) with a first module (28). The top of one side of the first module (28) is fixedly disposed on the bent edge part (11) with a bent edge block (29) for pressing the bent edge part (11) of the cylindrical blank (12) to bend it outward by 30°-60°. The bottom surface of the first punch (24) is provided with a first guide hole (210) corresponding to the first guide post (27). The bending die (3) includes: Second template (31); The second die (32) is fixedly disposed on the top surface of the second lower template (31). The top surface of the second die (32) is provided with a second mold cavity (34). A recessed step (35) is provided on one side of the top surface of the second die (32) located in the second mold cavity (34). The top surface of the recessed step (35) is provided with a profile groove (36) corresponding to the bent edge (11) that connects to the second mold cavity (34). The second punch (33) is fixed in the second mold cavity (34) by screws (37). A pressure edge (38) is provided on the outer periphery of its top end, and a clearance step (39) is provided on one side of its top end corresponding to the profile groove (36).
2. The method for forming the bending edge of the flame-connecting tube seat according to claim 1, characterized in that, In step 2), the bent edge (11) is bent outward at 45° to form the preform blank (14).
3. The method for forming the bend of the flame tube seat according to claim 1, characterized in that, The calibration mold (4) includes: The third lower template (41) has through holes (46) from its bottom surface to its top surface; The third die (42) is fixedly set on the top surface of the third lower template (41) and located above the through hole (46). The top surface of the third die (42) is provided with a third mold cavity (47) that communicates with the through hole (46). A shaping groove (48) is provided on one side of the top of the third mold cavity (47) corresponding to the bent edge (11). The top surface of the third die (42) is provided with third guide posts (49) on both sides of the third mold cavity (47). The ejector block (43) is slidably embedded in the through hole (46) in the vertical direction; The third upper template (44) is positioned above the third concave mold (42); The third punch (45) is fixedly disposed on the bottom surface of the third upper template (44). The bottom surface of the third punch (45) is fixedly disposed on the third mold cavity (47) with a third module (410). The top of one side of the third module (410) is fixedly disposed on the bent edge part (11) with a bent edge straightening block (411). The bottom surface of the third punch (45) is provided with a third guide hole (412) corresponding to the third guide post (49).
4. The method for forming the bending edge of the flame tube seat according to claim 3, characterized in that, The inner diameter of the through hole (46) is larger than the inner diameter of the third mold cavity (47). The outer diameter of the ejector block (43) is clearance-fitted with the inner diameter of the third mold cavity (47). A limiting step (413) is provided on the outer periphery of the bottom end of the ejector block (43). The outer diameter of the limiting step (413) is larger than the inner diameter of the third mold cavity (47) and clearance-fitted with the inner diameter of the through hole (46).
Citation Information
Patent Citations
Commercial vehicle mudguard support and manufacturing process
CN113753135A