High-strength low-temperature co-fired ceramic material and water-based tape casting method thereof

High-strength, low-temperature co-fired ceramic materials were prepared by water-based casting process, which solved the problem of insufficient mechanical strength and achieved the preparation of high-strength, low-cost, and environmentally friendly ceramic materials, suitable for electronic packaging materials.

CN119504235BActive Publication Date: 2026-11-24HEFEI INSTITUTE OF PHYSICAL SCIENCE CHINESE ACADEMY OF SCIENCES
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411277943.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2026-11-24
Estimated Expiration
2044-09-12

AI Technical Summary

Technical Problem

The insufficient mechanical strength of existing low-temperature co-fired ceramic materials limits the miniaturization and integration of electronic products.

Method used

A water-based casting process is adopted, in which high-strength alumina ceramic powder, silicon nitride ceramic powder, alumina fiber and glass powder are mixed, and water, dispersant, binder, plasticizer and defoamer are added. The mixture is ball-milled into a uniform slurry, which is then cast and sintered under vacuum hot pressing to obtain a high-strength low-temperature co-fired ceramic material.

Benefits of technology

A high-strength, low-temperature co-fired ceramic material was obtained, which has excellent mechanical properties, is suitable for industrial production, has low cost, is environmentally friendly, and has a thermal expansion coefficient that matches that of silicon semiconductor material, making it suitable for electronic packaging materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention belongs to the field of low-temperature co-fired ceramic materials, specifically relating to a high-strength low-temperature co-fired ceramic material and its water-based casting preparation method. This preparation method uses water as the sole solvent in the casting process. High-strength alumina ceramic powder, silicon nitride ceramic powder, alumina fiber, and glass powder are mixed, water and dispersant are added, and then ball-milled. Plasticizer, binder, and defoamer are added, and ball-milling continues to produce a uniform slurry suitable for casting. After defoaming, casting, and drying, a uniform and smooth cast film is obtained. High-strength low-temperature co-fired ceramic material can be obtained after vacuum hot-pressing solid-state sintering. This invention is simple to operate, the conditions are easy to control, the cost is low, it is non-toxic, harmless, and environmentally friendly. The low-temperature co-fired ceramic material prepared by this invention has a flexural strength in the range of 220-420 MPa, a thermal conductivity in the range of 5-11 W / (m·K), and a coefficient of thermal expansion that matches that of silicon components, showing great application potential in the field of electronic packaging materials and their manufacturing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of low-temperature co-fired ceramic materials, specifically relating to a high-strength low-temperature co-fired ceramic material and its water-based casting preparation method. Background Technology

[0002] Low-temperature co-fired ceramics (LTCC) are integrated multilayer ceramic materials created by printing interconnects, components, and circuits onto unsintered cast wafers, stacking these layers together, and sintering them. LTCC allows for the encapsulation of the three major passive components (resistors, capacitors, and inductors) and various other passive components such as filters and transformers within a multilayer wiring substrate, integrating them with active components to form a complete circuit system. Due to its excellent dielectric, thermal, and mechanical properties, LTCC meets the demands for miniaturization, high integration, and low cost in electronic components.

[0003] Low-temperature co-fired ceramics (LTCCs) employing glass / ceramic composite systems offer advantages such as easily tunable performance and simple fabrication processes. Their layered structure design can improve space utilization and achieve high integration in circuit systems. LTCC materials, with their excellent dielectric and thermal properties, have to some extent solved the miniaturization and integration problems of electronic components. However, a key factor currently limiting the miniaturization of electronic products is the mechanical strength of the packaging material itself. To ensure mechanical reliability and resist stress and drop impacts, when the mechanical strength of the device reaches its limit through structural design, it is necessary to increase the mechanical strength of the LTCC material itself to meet application requirements. Summary of the Invention

[0004] The purpose of this invention is to provide a water-based casting method for preparing high-strength low-temperature co-fired ceramic materials. This method uses water as the only solvent in the casting process. High-strength alumina ceramic powder, silicon nitride ceramic powder, alumina fiber and glass powder are mixed, water and dispersant are added and then ball-milled. Plasticizer, binder and defoamer are added and ball-milling is continued to prepare a uniform slurry suitable for casting. After defoaming, casting and drying, a uniform and smooth cast film is obtained. After vacuum hot pressing solid-state sintering, high-strength low-temperature co-fired ceramic materials can be obtained.

[0005] To achieve the above objectives, the present invention adopts the following technical solution: a water-based casting molding method for preparing high-strength low-temperature co-fired ceramic materials, comprising the following steps: S1. Weigh out bismuth trioxide, boron oxide, silicon dioxide, copper oxide and aluminum oxide in a molar ratio of 1:(0.1-1):(0.1-1):(0.4-1):(0.1-0.5), mix them and ball mill them evenly. Then place them at 600-800℃ for 1-4 hours. After natural cooling, ball mill them into powder to obtain BBSCA glass powder. S2. Mix BBSCA glass powder with alumina ceramic powder, silicon nitride ceramic powder, and alumina fiber at a mass ratio of 1:(0.6-1.5):(0-0.4):(0-0.1) to obtain a mixed powder. Take 100 parts by mass of the mixed powder, add 100-400 parts by mass of solvent and 2-4 parts by mass of dispersant and ball mill together. Then add 4-6 parts by mass of binder, 4-6 parts by mass of plasticizer and 0.5-1.5 parts by mass of defoamer, and continue ball milling to obtain a stable and uniform slurry. S3. After vacuum degassing the slurry obtained in step S2, cast it onto a PET film, dry it, and peel it off from the PET film to obtain the cast film. S4. After cutting the cast film and removing the organic additives, vacuum hot-press sinter it at 800-950℃ for 2-6 hours, and then cool it to obtain a high-strength low-temperature co-fired ceramic material.

[0006] Further improvements to the water-based tape casting preparation method for high-strength low-temperature co-fired ceramic materials: Preferably, the solvent in step S2 is deionized water.

[0007] Preferably, the dispersant in step S2 is one or a combination of two or more of polyvinylpyrrolidone, polyacrylic acid, and polyethyleneimine.

[0008] Preferably, the adhesive in step S2 is one or a combination of two or more of carboxymethyl cellulose, polyvinyl alcohol, and sodium carboxymethyl cellulose.

[0009] Preferably, the plasticizer in step S2 is one or a combination of two or more of polyvinyl alcohol and glycerin.

[0010] Preferably, the defoaming agent in step S2 is n-butanol.

[0011] Preferably, in step S3, the slurry is cast into a film and then naturally dried at 25°C-45°C.

[0012] Preferably, in step S4, after the cast film is cut, it is slowly heated to 500-650°C in a muffle furnace and held for 2-3 hours to remove organic additives.

[0013] Preferably, in step S2, after adding solvent and dispersant to the mixed powder, ball milling is performed for 8-16 hours, and then after adding binder, plasticizer and defoamer, ball milling is continued for 8-16 hours.

[0014] The second objective of this invention is to provide a water-based casting molding method for preparing high-strength low-temperature co-fired ceramic materials as described in any one of the above-mentioned methods, thereby obtaining high-strength low-temperature co-fired ceramic materials.

[0015] The advantages of this invention compared to the prior art are as follows: (1) This invention provides a water-based casting method for preparing high-strength low-temperature co-fired ceramic materials. The method involves mixing BBSCA glass powder and high-strength alumina ceramic powder (silicon nitride ceramic powder and alumina fiber can also be added), adding water as the sole solvent in the casting process, and adding dispersants, plasticizers, binders, and defoamers. The mixture is ball-milled to form a uniform slurry suitable for casting. After defoaming, casting, and drying, a uniform and smooth cast film is obtained. After vacuum hot-pressing solid-state sintering, a high-strength low-temperature co-fired ceramic material can be obtained. Since the solvent is only water, the production process is low-cost, environmentally friendly, and harmless to human health, making it suitable for large-scale factory production. This overcomes the problem that non-water-based casting processes typically require large amounts of toxic organic solvents, resulting in high production costs, environmental pollution, harm to human health, and hindering industrial production.

[0016] (2) The process of this invention is simple to operate and the conditions are easy to control. The cast film dries quickly, requiring only 0.5-1 hours of ventilation drying at 25℃-45℃ to achieve complete drying without cracking, making it suitable for continuous industrial production. The resulting cast film has good strength and flexibility, and can be cut and bent arbitrarily. The low-temperature co-fired ceramic material prepared by this invention has a flexural strength in the range of 220-420MPa and a thermal conductivity in the range of 5-11W / (m²). K), with a coefficient of thermal expansion that matches that of silicon components, has great application prospects in the field of electronic packaging materials and their manufacturing. Detailed Implementation

[0017] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.

[0018] Example 1

[0019] This embodiment provides a water-based casting method for preparing high-strength, low-temperature co-fired ceramic materials, specifically including the following steps: S1. Weigh out bismuth trioxide, boron oxide, silicon dioxide, copper oxide and aluminum oxide in a molar ratio of 1:0.1:0.1:0.4:0.1, mix them and ball mill them evenly. Place them at 600℃ for 2 hours and then cool them naturally. Ball mill them into powder to obtain BBSCA glass powder. S2. Mix BBSCA glass powder with alumina ceramic powder, silicon nitride ceramic powder, and alumina fiber at a mass ratio of 1:0.6:0.3:0.05 to obtain a mixed powder. Take 100 parts by mass of the mixed powder, add 100 parts by mass of solvent (deionized water) and 2 parts by mass of dispersant (polyvinylpyrrolidone), and ball mill together for 8 hours. Then add 4 parts by mass of binder (carboxymethyl cellulose), 4 parts by mass of plasticizer (polyethylene glycol), and 0.5 parts by mass of defoamer (n-butanol), and continue ball milling for 16 hours to obtain a stable and uniform slurry. S3. After vacuum degassing the slurry obtained in step S2, cast it onto a PET film. After the cast film is naturally dried at 45°C, it is peeled off from the PET film. S4. After cutting the cast film, place it in a muffle furnace and slowly heat it to 500°C and hold it for 2 hours to remove organic additives. Then, vacuum hot press sinter it at 800°C for 2 hours and cool it to obtain low-temperature co-fired ceramic sheet 1.

[0020] Example 2

[0021] This embodiment provides a water-based casting method for preparing high-strength, low-temperature co-fired ceramic materials, specifically including the following steps: S1. Weigh out bismuth trioxide, boron oxide, silicon dioxide, copper oxide and aluminum oxide in a molar ratio of 1:0.2:0.2:0.5:0.2, mix them and ball mill them evenly. Place them at 650℃ for 2 hours and then cool them naturally. Ball mill them into powder to obtain BBSCA glass powder. S2. Mix BBSCA glass powder with alumina ceramic powder and silicon nitride ceramic powder at a mass ratio of 1:1.5:0.3 to obtain a mixed powder. Take 100 parts by mass of the mixed powder, add 200 parts by mass of solvent (deionized water) and 3 parts by mass of dispersant (polyacrylic acid), and ball mill for 16 hours. Then add 5 parts by mass of binder (polyvinyl alcohol), 5 parts by mass of plasticizer (glycerin) and 1.0 part by mass of defoamer (n-butanol), and continue ball milling for 8 hours to obtain a stable and uniform slurry. S3. After vacuum degassing the slurry obtained in step S2, cast it onto a PET film. After the cast film dries naturally at 35°C, it is peeled off from the PET film. S4. After cutting the cast film, place it in a muffle furnace and slowly heat it to 550°C and hold it for 2 hours to remove organic additives. Then, vacuum hot press sinter it at 850°C for 2 hours and cool it to obtain low-temperature co-fired ceramic sheet 2.

[0022] Example 3

[0023] This embodiment provides a water-based casting method for preparing high-strength, low-temperature co-fired ceramic materials, specifically including the following steps: S1. Weigh out bismuth trioxide, boron oxide, silicon dioxide, copper oxide and aluminum oxide in a molar ratio of 1:0.5:0.5:0.7:0.3, mix them and ball mill them evenly. Place them at 700℃ for 2 hours and then cool them naturally. Ball mill them into powder to obtain BBSCA glass powder. S2. Mix BBSCA glass powder and alumina ceramic powder at a mass ratio of 1:0.6 to obtain a mixed powder. Take 100 parts by mass of the mixed powder, add 300 parts by mass of solvent (deionized water) and 3.5 parts by mass of dispersant (polyethyleneimine), and ball mill for 10 hours. Then add 5 parts by mass of binder (sodium carboxymethyl cellulose), 5 parts by mass of plasticizer (glycerol), and 1.2 parts by mass of defoamer (n-butanol), and continue ball milling for 10 hours to obtain a stable and uniform slurry. S3. After vacuum degassing the slurry obtained in step S2, cast it onto a PET film. After the cast film dries naturally at 30°C, it is peeled off from the PET film. S4. After cutting the cast film, place it in a muffle furnace and slowly heat it to 600°C and hold it for 2 hours to remove organic additives. Then, vacuum hot press sinter it at 900°C for 2 hours and cool it to obtain low-temperature co-fired ceramic sheet 3.

[0024] Example 4

[0025] This embodiment provides a water-based casting method for preparing high-strength low-temperature co-fired ceramic materials, specifically including the following steps: S1. Weigh out bismuth trioxide, boron oxide, silicon dioxide, copper oxide and aluminum oxide in a molar ratio of 1:1:1:1:0.5, mix them and ball mill them evenly, place them at 800℃ for 2 h and then cool them naturally, ball mill them into powder to obtain BBSCA glass powder. S2, BBSCA glass powder, alumina ceramic powder, silicon nitride ceramic powder, and alumina fiber were mixed in a mass ratio of 1:0.6:0.3:0.1 to obtain a mixed powder. 100 parts by mass of the mixed powder were taken, and 400 parts by mass of solvent (deionized water) and 4 parts by mass of dispersant (polyethyleneimine) were added and ball-milled for 12 hours. Then, 6 parts by mass of binder (polyvinyl alcohol), 6 parts by mass of plasticizer (polyethylene glycol), and 1.5 parts by mass of defoamer (n-butanol) were added, and ball milling was continued for 12 hours to obtain a stable and uniform slurry. S3. After vacuum degassing the slurry obtained in step S2, cast it onto a PET film. After the cast film dries naturally at 25°C, it is peeled off from the PET film. S4. After cutting the cast film, place it in a muffle furnace and slowly heat it to 650°C and hold it for 2 hours to remove organic additives. Then, vacuum hot press sinter it at 950°C for 2 hours and cool it to obtain low-temperature co-fired ceramic sheet 4.

[0026] Example 5

[0027] This embodiment provides a water-based casting method for preparing high-strength low-temperature co-fired ceramic materials, specifically including the following steps: S1. Weigh out bismuth trioxide, boron oxide, silicon dioxide, copper oxide and aluminum oxide in a molar ratio of 1:0.3:0.5:0.6:0.25, mix them and ball mill them evenly. Place them at 700℃ for 2 h and then cool them naturally. Ball mill them into powder to obtain BBSCA glass powder. S2, BBSCA glass powder, alumina ceramic powder, and alumina fiber are mixed at a mass ratio of 1:0.6:0.05 to obtain a mixed powder. Take 100 parts by mass of the mixed powder, add 200 parts by mass of solvent (deionized water) and 3 parts by mass of dispersant (polyethyleneimine), and ball mill for 12 hours. Then add 5 parts by mass of binder (polyvinyl alcohol), 5 parts by mass of plasticizer (polyethylene glycol), and 1 part by mass of defoamer (n-butanol), and continue ball milling for 12 hours to obtain a stable and uniform slurry. S3. After vacuum degassing the slurry obtained in step S2, cast it onto a PET film. After the cast film dries naturally at 25°C, it is peeled off from the PET film. S4. After cutting the cast film, place it in a muffle furnace and slowly heat it to 600℃ and hold it for 2.5h to remove organic additives. Then, vacuum hot press sinter it at 900℃ for 4h and cool it to obtain low-temperature co-fired ceramic sheet 5.

[0028] The prepared low-temperature co-fired ceramic sheets 1-5 were tested for bending resistance, thermal conductivity, thermal expansion, and density. The specific testing methods are as follows: (1) Bending strength: The three-point bending strength of the sintered sheet was measured using a universal testing machine (INSTRON 5960, Instron, USA). The sintered sheet was cut into long strips, and its maximum load was tested. The bending strength was calculated using the formula:

[0029] In the formula, F is the maximum load (N), L is the support span, and b and d are the width and thickness of the specimen (mm), respectively. Each sample is tested 5 times and the average value is taken. (2) Thermal conductivity: The thermal conductivity of the sintered sheet was measured using a HotDisk thermal constant analyzer (TPS2200, HotDisk AB, Sweden). The sintered sheet was sandwiched between two foams, and a probe was placed under the sample. Each sample was measured three times at room temperature, and the average value was taken. (3) Thermal expansion properties: The change in size of the sintered sheet with temperature was measured using a thermomechanical analyzer (TMA). The sample size was 4 mm × 4 mm, and the sample surface was polished smooth. The temperature range was 25~200°C. o C, heating rate is 5 oThe formula for calculating the coefficient of thermal expansion (CTE) is as follows: C / min CTE =

[0030] In the formula, L 0 ΔT represents the initial thickness of the sample, ΔT represents the temperature change, and ΔL represents the thickness change of the sample within the temperature ΔT.

[0031] (4) Density analysis: The density of the sintered sheet was tested using a densitometer (AR-150PM, Guangdong Dahong, China). Each sample was tested 5 times and the average value was taken.

[0032] The test results for low-temperature co-fired ceramic sheet 1 are as follows: flexural strength of 331.13 MPa, thermal conductivity of 10.61 W / mK, coefficient of thermal expansion of 6.21 ppm / ℃, and density of 4.23 g / cm³. 3 The test results show that this example produced a material with high mechanical properties, good thermal conductivity, and a thermal expansion coefficient that matches well with silicon semiconductor material.

[0033] The test results for the low-temperature co-fired ceramic sheet 2 are as follows: flexural strength of 266.75 MPa, thermal conductivity of 9.76 W / mK, coefficient of thermal expansion of 5.95 ppm / ℃, and density of 3.95 g / cm³. 3 The test results show that this example produced a material with high mechanical properties, good thermal conductivity, and a thermal expansion coefficient that matches well with silicon semiconductor material.

[0034] The test results for low-temperature co-fired ceramic sheet 3 are as follows: flexural strength of 226.13 MPa, thermal conductivity of 9.49 W / mK, coefficient of thermal expansion of 5.46 ppm / ℃, and density of 3.54 g / cm³. 3 The test results show that this example produced a material with high mechanical properties, good thermal conductivity, and a thermal expansion coefficient that matches well with silicon semiconductor material.

[0035] The test results for low-temperature co-fired ceramic sheet 4 are as follows: flexural strength of 288.63 MPa, thermal conductivity of 8.64 W / mK, coefficient of thermal expansion of 5.12 ppm / ℃, and density of 4.14 g / cm³. 3 The test results show that this example produced a material with high mechanical properties, good thermal conductivity, and a thermal expansion coefficient that matches well with silicon semiconductor material.

[0036] The test results for low-temperature co-fired ceramic sheet 5 were as follows: flexural strength of 254.36 MPa, thermal conductivity of 9.35 W / mK, coefficient of thermal expansion of 5.57 ppm / ℃, and density of 3.86 g / cm³. 3The test results show that this example produced a material with high mechanical properties, good thermal conductivity, and a thermal expansion coefficient that matches well with silicon semiconductor material.

[0037] Those skilled in the art should understand that the above descriptions are merely several specific embodiments of the present invention, and not all embodiments. It should be noted that many modifications and improvements can be made by those skilled in the art, and all modifications or improvements not exceeding the scope of the claims should be considered within the protection scope of the present invention.

Claims

1. A water-based casting method for preparing high-strength, low-temperature co-fired ceramic materials, characterized in that, Includes the following steps: S1. Weigh out bismuth trioxide, boron oxide, silicon dioxide, copper oxide and aluminum oxide in a molar ratio of 1:(0.1-1):(0.1-1):(0.4-1):(0.1-0.5), mix them and ball mill them evenly. Then place them at 600-800℃ for 1-4 hours. After natural cooling, ball mill them into powder to obtain BBSCA glass powder. S2. Mix BBSCA glass powder with alumina ceramic powder, silicon nitride ceramic powder, and alumina fiber at a mass ratio of 1:(0.6-1.5):(0-0.4):(0-0.1) to obtain a mixed powder. Take 100 parts by mass of the mixed powder, add 100-400 parts by mass of solvent and 2-4 parts by mass of dispersant and ball mill together. Then add 4-6 parts by mass of binder, 4-6 parts by mass of plasticizer and 0.5-1.5 parts by mass of defoamer, and continue ball milling to obtain a stable and uniform slurry. S3. After vacuum degassing the slurry obtained in step S2, cast it onto a PET film, dry it, and peel it off from the PET film to obtain the cast film. S4. After cutting the cast film and removing the organic additives, vacuum hot-press sinter it at 800-950℃ for 2-6 hours, and then cool it to obtain a high-strength low-temperature co-fired ceramic material.

2. The water-based casting method for preparing high-strength low-temperature co-fired ceramic materials according to claim 1, characterized in that, The solvent mentioned in step S2 is deionized water.

3. The water-based casting method for preparing high-strength low-temperature co-fired ceramic materials according to claim 1, characterized in that, The dispersant mentioned in step S2 is one or a combination of two or more of polyvinylpyrrolidone, polyacrylic acid, and polyethyleneimine.

4. The water-based casting method for preparing high-strength low-temperature co-fired ceramic materials according to claim 1 or 2, characterized in that, The adhesive mentioned in step S2 is one or a combination of two or more of carboxymethyl cellulose, polyvinyl alcohol, and sodium carboxymethyl cellulose.

5. The water-based casting method for preparing high-strength low-temperature co-fired ceramic materials according to claim 1 or 2, characterized in that, The plasticizer mentioned in step S2 is one or a combination of two of polyvinyl alcohol and glycerin.

6. The water-based casting method for preparing high-strength low-temperature co-fired ceramic materials according to claim 1, characterized in that, The defoaming agent mentioned in step S2 is n-butanol.

7. The water-based casting method for preparing high-strength low-temperature co-fired ceramic materials according to claim 1, characterized in that, In step S3, the slurry is cast into a film and then naturally dried at 25℃-45℃.

8. The water-based casting method for preparing high-strength low-temperature co-fired ceramic materials according to claim 1, characterized in that, In step S4, after the cast film is cut, it is slowly heated to 500-650℃ in a muffle furnace and held for 2-3 hours to remove organic additives.

9. The water-based casting method for preparing high-strength low-temperature co-fired ceramic materials according to claim 1, characterized in that, In step S2, after adding solvent and dispersant to the mixed powder, ball milling is performed for 8-16 hours. Then, binder, plasticizer and defoamer are added and ball milling is continued for another 8-16 hours.

10. A high-strength low-temperature co-fired ceramic material prepared by a water-based casting method according to any one of claims 1-9.

Citation Information

Patent Citations

  • Heat-conducting low-temperature co-fired ceramic material and preparation method thereof

    CN110683837A

  • High-thermal-conductivity low-temperature co-fired ceramic material and preparation method thereof

    CN115385666A