Spline shaft deformation control method and apparatus
By combining steps such as gear hobbing, heat treatment, shot blasting, and straightening, the problems of long process length and high cost in spline shaft deformation control are solved, achieving efficient processing and cost savings for spline shafts.
Patent Information
- Application Number
- CN202411811725.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-12-10
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-12-10
AI Technical Summary
Existing spline shaft machining processes suffer from long procedures and high costs, especially in controlling spline deformation, where efficiency is low and expenses are high.
The process employs a combination of steps including gear shaping, heat treatment, shot blasting, straightening, and precision machining. This involves simultaneous carburizing and quenching, followed by straightening and precision machining after shot blasting, and dust removal using a specialized shot blasting device. This simplifies the process and reduces heat treatment costs.
This technology effectively controls spline shaft deformation, saves on machining and heat treatment costs, reduces unit costs, and improves production efficiency.
Smart Images

Figure CN119525938B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of machining technology, specifically to a method and equipment for controlling the deformation of a spline shaft. Background Technology
[0002] Splined shafts are a type of mechanical transmission, similar in function to parallel keys, semi-circular keys, and wedge keys—transmitting mechanical torque. They have longitudinal keyways on their outer surface, and rotating components fitted onto the shaft also have corresponding keyways to maintain synchronous rotation with the shaft. While rotating, some splined shafts can also slide longitudinally along the shaft, such as gearbox shift gears.
[0003] Spline machining methods: There are many methods for machining spline shafts. The main methods are cutting such as hobbing, milling, and grinding, and plastic deformation methods such as cold forging and cold rolling can also be used. The spline M-value refers to the spline pitch (MR) or common normal length, and it is an important parameter for measuring the spline tooth thickness. Measuring the spline M-value is crucial for ensuring the assembly accuracy and function of the spline.
[0004] Therefore, controlling the deformation of the spline shaft during the machining process is crucial. Traditional control processes generally include: machining → gear shaping → carburizing → machining → quenching → sandblasting → engraving → inspection → electrical pulse spline I → inspection → machining. This process has the problems of long processing steps and high cost. Summary of the Invention
[0005] To address the shortcomings of existing technologies, the technical problem to be solved by this invention is to provide a method and device for controlling spline shaft deformation, which can control spline deformation while saving costs.
[0006] To achieve the above objectives, the present invention provides a method for controlling spline shaft deformation, comprising:
[0007] (1) Gear shaping: The spline section of the spline shaft is machined by gear shaping, and the range of spline M value is tightened in the gear shaping process;
[0008] (2) Heat treatment, including carburizing and quenching, wherein the carburizing and quenching are performed simultaneously;
[0009] (3) Shot blasting: The entire surface of the spline shaft is shot blasted.
[0010] (4) Straightening;
[0011] (5) Precision machining: First, the spline runout is corrected to be less than 0.05 on the lathe. Then, the ejector hole is repaired. Next, the outer circle is ground, the internal thread is turned, the arc groove is turned, and the spline is ground, with the ejector hole as the positioning reference.
[0012] (6) Inspection.
[0013] Furthermore, in step (1), the product drawing requires the M value to be 103.065-103.132 / φ5, and the gear hobbing process is processed to 103.04-103.08 / φ5, tightening the tolerance range and reducing it by 0.02mm.
[0014] Furthermore, in step (2), the carburizing and quenching temperature is 890°C, and a quenching agent needs to be added to reduce the heat treatment temperature of the part while ensuring the required depth of the carburized layer.
[0015] Furthermore, in step (2), the heat treatment also includes stress-relieving tempering after carburizing and quenching.
[0016] Furthermore, the tempering temperature is 170±10 degrees Celsius, the holding time is 3 to 4 hours, and air cooling is used.
[0017] Furthermore, in step (4), the straightening requirements are: spline runout less than 0.05 mm, and runout in other positions less than 0.1 mm.
[0018] Further, in step (6), the inspection includes: checking the hardness, metallographic structure, layer depth, absence of residual steel shot on the surface, deformation of the parts, and ensuring that the spline pitch circle runout is less than 0.05, the other runouts are less than 0.1, and the spline M value is 103.065-103.132 / φ5.
[0019] Furthermore, all machining operations after heat treatment are based on splines.
[0020] An apparatus for implementing the spline shaft deformation control method as described in any one of the above claims, wherein the shot blasting process is performed by a shot blasting device of the spline shaft deformation control method apparatus, the shot blasting device comprising:
[0021] Shot blasting room;
[0022] A frame, located inside the shot blasting chamber, is used to install and fix the splined shaft to be shot blasted;
[0023] A shot blasting body, located above the frame, is used to perform shot blasting on the splined shaft; and
[0024] Dust removal equipment is used to treat the dust generated in the shot blasting chamber.
[0025] Furthermore, the dust removal equipment includes:
[0026] A dust collection hood, which is a flexible cover, covers the inner wall of the shot blasting chamber;
[0027] The vacuum pipe is located outside the shot blasting chamber and is connected to the vacuum hood; and
[0028] A wet scrubber, connected to the suction pipe, is used to spray and filter the dust drawn into the suction pipe.
[0029] The beneficial effects of this invention are:
[0030] The above-mentioned spline shaft deformation control method comprises the following steps: First, the spline section of the spline shaft is machined by gear shaping, and the spline M-value range is tightened during the gear shaping process; then, heat treatment is performed, which includes carburizing and quenching, and the carburizing and quenching are performed simultaneously; subsequently, the entire spline shaft surface is shot-blasted; then, straightening is performed; then, the spline runout is corrected to be less than 0.05 on a lathe, then the ejector pin hole is repaired, and then, using the ejector pin hole as the positioning reference, the outer diameter is ground, the internal thread is turned, the arc groove is turned, and the spline is ground; finally, inspection is performed. The spline shaft deformation control settings are used to achieve the above method.
[0031] The above method and equipment have the following advantages:
[0032] 1. Saves on transportation costs between carburizing and machining, and between machining and quenching;
[0033] 2. Saves on heat treatment costs. Previously, carburizing and quenching were separate processes requiring two heating cycles. Now, carburizing and quenching are completed in the same furnace, requiring only one heating cycle, thus saving on heating costs per piece.
[0034] 3. Eliminate the outsourced electrical pulse process for spline I, saving costs. Attached Figure Description
[0035] To more clearly illustrate the specific embodiments of the present invention, the accompanying drawings used in the specific embodiments will be briefly described below. In all the drawings, the elements or parts are not necessarily drawn to scale.
[0036] Figure 1 This is a flowchart illustrating a spline shaft deformation control method according to an embodiment of the present invention.
[0037] Figure 2 To achieve Figure 1 A schematic diagram of a shot blasting device for a method of controlling spline shaft deformation is shown.
[0038] Figure 3 for Figure 2 The diagram shows a dust removal device in a spline shaft deformation control device.
[0039] Figure 4 for Figure 2 A schematic diagram of a dust extraction hood in a spline shaft deformation control device is shown.
[0040] Figure 5 for Figure 2 A cross-sectional view of a dust extraction hood in a spline shaft deformation control device is shown.
[0041] Figure label:
[0042] 100. Shot blasting device; 110. Shot blasting chamber; 20. Frame; 130. Shot blasting body; 140. Dust removal equipment; 141. Dust suction hood; 1411. First mask; 1412. Second mask; 1413. Elastic support; 142. Dust suction pipe; 143. Wet dust collector; 144. Storage structure; 1441. Storage box; 1442. Winding spool; 1443. Handle. Detailed Implementation
[0043] To make the above-mentioned objects, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. Many specific details are set forth in the following description to provide a thorough understanding of the present invention. However, the present invention can be practiced in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of the invention; therefore, the invention is not limited to the specific embodiments disclosed below.
[0044] Please see Figure 1 This invention provides a method for controlling spline shaft deformation, the specific method of which is as follows:
[0045] S110, Gear shaping: Gear shaping is performed on the spline section of the spline shaft, and the range of spline M value is tightened during the gear shaping process.
[0046] S120, heat treatment, including carburizing and quenching, with carburizing and quenching performed simultaneously;
[0047] S130, shot blasting, shot blasting treatment is performed on the entire surface of the spline shaft;
[0048] S140, Straightening;
[0049] S150, precision machining: First, the spline runout is corrected to be less than 0.05 on the lathe. Then, the ejector hole is repaired. Next, the outer diameter is ground, the internal thread is turned, the arc groove is turned, and the spline is ground, using the ejector hole as the positioning reference.
[0050] S160, Inspection.
[0051] Specifically, the machining process involves the following steps:
[0052] First, the spline runout is corrected to be less than 0.05 on a lathe, then the ejector hole is repaired. Next, using the ejector hole as the positioning datum, the outer diameter is ground, the internal thread is turned, the arc groove is turned, and the spline is ground. Specific requirements for repairing the ejector hole are detailed below. Figure 1 The requirements for grinding the outer diameter are as follows: Figure 2 .
[0053] In this embodiment, the gear shaping process requires tightening the M-value range of the part. Specifically: the product drawing requires M-values of 103.065 and 103.132 / φ5, while the gear shaping process processes them to 103.04 and 103.08 / φ5, tightening the tolerance range and reducing it by 0.02mm. Specific requirements for the relevant gear shaping data can be found in [link to relevant documentation]. Figure 1 .
[0054] In this embodiment, carburizing and quenching are performed simultaneously. This operation can save the transfer costs between carburizing and machining, and between machining and quenching. In specific implementation, a carburizing and quenching temperature of 890° is selected, and a carburizing agent is added at the same time. While ensuring the required depth of carburized layer of the part, the heat treatment temperature of the part is reduced, and the deformation of the part is reduced.
[0055] In this embodiment, the specific calibration process is as follows:
[0056] When calibrating parts in a press, the calibration requirements are: spline runout less than 0.05mm, runout in other positions less than 0.1mm, and further correction of axial deformation of the parts.
[0057] In a preferred embodiment, the heat treatment also includes stress-relieving tempering after carburizing and quenching.
[0058] Specifically, the tempering temperature is 170±10 degrees Celsius, the holding time is 3 to 4 hours, and air cooling is used.
[0059] In this embodiment, during precision machining, the spline runout is first corrected on a lathe to be less than 0.05 mm. Then, the ejector hole is repaired. Next, using the ejector hole as a positioning reference, the outer diameter is ground, the internal thread is turned, the arc groove is turned, and the spline is ground. Specific requirements for repairing the ejector hole are detailed below. Figure 2 For specific requirements of the grinding of the outer diameter, please refer to [link / reference]. Figure 3 .
[0060] In this embodiment, the inspection process includes: checking the hardness, metallographic structure, layer depth, absence of residual steel shot on the surface, deformation of the parts, and ensuring that the spline pitch circle runout is less than 0.05, the other runouts are less than 0.1, and the spline M value is 103.065, 103.132 / φ5.
[0061] It should be noted that the positions processed after heat treatment are all based on the spline, ensuring the positional relationship between the outer circle, spline, arc groove, and internal thread, thus achieving the purpose of controlling spline deformation and meeting the requirements of the product drawings.
[0062] Please see Figures 2 to 5 In addition, the present invention also provides an apparatus for implementing the above-mentioned spline shaft deformation control method. This apparatus includes a shot blasting device 100. The shot blasting process is completed by the shot blasting device 100. The shot blasting device 100 includes a shot blasting chamber 110, a frame 200, a shot blasting body 130, and a dust removal device 140.
[0063] Specifically, the frame 200 is set inside the shot blasting chamber 110 for installing and fixing the splined shaft to be shot blasted; the shot blasting body 130 is located above the frame 200 for shot blasting the splined shaft; and the dust removal equipment 140 is used to remove the dust generated inside the shot blasting chamber 110.
[0064] When in use, first fix the spline on the frame 200, then start the shot blasting body 130 and the dust removal equipment 140 to perform shot blasting on the spline shaft. During the shot blasting process, the dust removal equipment 140 sucks out the dust generated in the shot blasting chamber 110 to prevent excessive dust from causing flammable and explosive reactions.
[0065] Specifically, the dust removal equipment 140 includes a dust suction hood 141, a dust suction pipe 142, and a wet scrubber 143. The dust suction hood 141 is a flexible hood that covers the inner wall of the shot blasting chamber 110. The dust suction pipe 142 is located outside the shot blasting chamber 110 and is connected to the dust suction hood 141. The wet scrubber 143 is connected to the dust suction pipe 142 and is used to spray and filter the dust sucked into the dust suction pipe 142.
[0066] By using the dust removal equipment 140, the dust collection effect can be improved because the dust collection hood 141 covers the inner wall of the shot blasting chamber 110.
[0067] Specifically, the dust suction hood 141 is a long strip, with one end connected to the suction pipe 142. Multiple suction holes are spaced along the length of the dust suction hood 141. In use, the long strip dust suction hood 141 is sequentially fixed along the shot blasting chamber 110 until it completely covers the inner wall of the chamber. The fixing method can be adhesive, screw fixing, etc. Using this method, the dust suction hood 141 can be used with shot blasting chambers 110 of different sizes, thereby improving ease of use.
[0068] Specifically, the dust collection hood 141 includes a first mask 1411 and a second mask 1412 disposed opposite to each other. The edges of the first mask 1411 and the second mask 1412 are sealed together to form a sealed bag. The dust collection hole is opened on the first mask 1411, and the second mask 1412 is disposed against the inner wall of the shot blasting chamber 110.
[0069] In a preferred embodiment, a plurality of elastic support members 1413 are arranged at intervals inside the dust collection hood 141. The elastic support members 1413 allow the first mask 1411 and the second mask 1412 to be in a separate state when the dust collection hood 141 is in the unfolded state, thereby further improving the dust collection effect.
[0070] As a preferred embodiment, the dust removal equipment 140 also includes a storage structure 144 for storing the dust collection hood 141.
[0071] Specifically, the storage structure 144 includes a storage box 1441, a winding shaft 1442, and a handle 1443. The inner cavity of the storage box 1441 is hollow. The winding shaft 1442 can rotate and is located inside the inner cavity of the storage box 1441. The handle 1443 is located inside the storage box 1441 and is connected to one end of the storage box 1441. The side wall of the storage box 1441 has a through hole that communicates with the inner cavity of the storage box 1441. The end of the dust hood 141 away from the dust suction pipe 142 passes through the through hole and is wound around the winding shaft 1442.
[0072] During installation, first fix the position of the suction pipe 142. Then, along the inner wall of the shot blasting chamber 110, from top to bottom in a spiral downward direction, fixing the suction hood 141 to the inner wall of the shot blasting chamber 110 while releasing the wire. When vacuuming is not needed, disconnect the connection between the suction hood 141 and the inner wall of the shot blasting chamber 110 by rotating the winding shaft 1442 using the handle 1443, and then store the suction hood 141 into the storage structure 144.
[0073] The processing using the above methods and equipment has the following advantages:
[0074] 1. Saves on transportation costs between carburizing and machining, and between machining and quenching, saving 100 yuan per piece;
[0075] 2. Saves heat treatment costs. Previously, carburizing and quenching were separate processes, requiring two heating cycles. Now, carburizing and quenching are completed in the same furnace, requiring only one heating cycle, saving 120 yuan per piece.
[0076] 3. Eliminate the outsourced electrical pulse process for spline I, saving costs. Savings are 460 yuan per piece.
[0077] In summary, the new process saves 680 yuan per piece.
[0078] Based on an annual production of 6,000 units, the savings and value creation amount to approximately 4.08 million yuan per year.
[0079] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be covered within the scope of the claims and specification of the present invention.
Claims
1. A method for controlling the deformation of a splined shaft, characterized in that, include: (1) Gear shaping: The spline section of the spline shaft is machined by gear shaping, and the range of spline M value is tightened in the gear shaping process. The product drawing requires the spline M value to be 103.065-103.132 / φ5. The gear shaping process is processed to 103.04-103.08 / φ5, tightening the tolerance range and reducing it by 0.02mm. The spline M value refers to the spline pitch (MR) or common normal length. (2) Heat treatment, including carburizing and quenching, wherein the carburizing and quenching are performed simultaneously; (3) Shot blasting: The entire surface of the spline shaft is shot blasted. (4) Straightening; (5) Precision machining: First, the spline runout is corrected to be less than 0.05 on the lathe. Then, the ejector hole is repaired. Next, the outer circle is ground, the internal thread is turned, the arc groove is turned, and the spline is ground, with the ejector hole as the positioning reference. (6) Inspection.
2. The spline shaft deformation control method according to claim 1, characterized in that, In step (2), the carburizing and quenching temperature is 890°C, and a quenching agent needs to be added to reduce the heat treatment temperature of the part while ensuring the required depth of the carburized layer.
3. The spline shaft deformation control method according to claim 1, characterized in that, In step (2), the heat treatment also includes stress-relieving tempering after carburizing and quenching.
4. The spline shaft deformation control method according to claim 3, characterized in that, The tempering temperature is 170±10 degrees Celsius, and the holding time is 3 to 4 hours, with air cooling as the method.
5. The spline shaft deformation control method according to claim 1, characterized in that, In step (4), the straightening requirements are: spline runout less than 0.05 mm, and runout in other positions less than 0.1 mm.
6. The spline shaft deformation control method according to claim 1, characterized in that, In step (6), the inspection includes: checking the hardness, metallographic structure, layer depth, absence of residual steel shot on the surface, deformation of the parts, and ensuring that the spline pitch circle runout is less than 0.05, the other runouts are less than 0.1, and the spline M value is 103.065-103.132 / φ5.
7. The spline shaft deformation control method according to claim 1, characterized in that, All machining operations after heat treatment are based on splines.
8. The spline shaft deformation control method according to any one of claims 1-7, characterized in that, The shot blasting process is completed by the shot blasting device of the spline shaft deformation control method equipment, and the shot blasting device includes: Shot blasting room; A frame, located inside the shot blasting chamber, is used to install and fix the splined shaft to be shot blasted; A shot blasting body, located above the frame, is used to perform shot blasting on the splined shaft; and Dust removal equipment is used to treat the dust generated in the shot blasting chamber.
9. The spline shaft deformation control method according to claim 8, characterized in that, The dust removal equipment includes: A dust collection hood, which is a flexible cover, covers the inner wall of the shot blasting chamber; The vacuum pipe is located outside the shot blasting chamber and is connected to the vacuum hood; and A wet scrubber, connected to the suction pipe, is used to spray and filter the dust drawn into the suction pipe.
Citation Information
Patent Citations
Machining method of spline gear shaft
CN108115372A
Gear cutting method and system for bidirectional slotting herringbone gear and medium
CN116921777A