Metal composite plate and continuous production method thereof

By mechanically deforming and connecting metal composite plates using double-headed semi-hollow rivets, the problems of high cost and unstable quality in existing technologies are solved, and low-cost, safe and reliable metal composite plate production is achieved.

CN119526873BActive Publication Date: 2026-11-24YANGTZE UNIVERSITY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411777979.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-12-05
Publication Date
2026-11-24
Estimated Expiration
2044-12-05

AI Technical Summary

Technical Problem

Existing metal composite panel production processes suffer from high production costs, significant safety risks, and unstable quality, especially when thin plates are laminated, which is prone to quality defects such as delamination and debonding.

Method used

Double-headed semi-hollow rivets are used to connect the base plate and the composite plate through mechanical deformation. The insertion depth of the rivets is limited by the partition plate and the positioning flange. The extrusion process of the upper and lower rollers ensures the reliability of the connection and avoids the heating process.

Benefits of technology

It achieves low-cost and high-safety metal composite plate connection, is suitable for thin plates, avoids delamination and debonding defects, and reduces production energy consumption and costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119526873B_ABST
    Figure CN119526873B_ABST
Patent Text Reader

Abstract

This invention relates to a metal composite plate and its continuous manufacturing method, belonging to the technical field of metal sheet technology. The metal composite plate consists of stacked substrates and multiple layers of cladding plates, with the substrates and cladding plates connected, and the cladding plates themselves connected, via double-headed semi-hollow rivets. This metal composite plate and its continuous manufacturing method connect the plates using double-headed semi-hollow rivets, relying on the mechanical deformation between the rivets and the plates to firmly connect them, reducing the likelihood of delamination or detachment. The connection process does not require heating the plates, effectively reducing production costs. Because heating the plates is unnecessary, thin plates are less prone to deformation, ensuring uniform connection; simultaneously, thin plates do not require high strength or high toughness, significantly reducing the requirements for thin plates, and allowing for easy connection. This solves the problems of high production costs, susceptibility to quality defects, and unsuitability for thin-plate composites in existing metal composite plates.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a metal composite plate and its continuous preparation method, belonging to the field of metal sheet technology. Background Technology

[0002] With the rapid development of modern science and engineering technology, the limitations of single-metal materials can no longer meet the actual needs of engineering production. For example, in fields such as chemical engineering, oil and gas extraction, aerospace, and advanced weapons manufacturing, materials need to withstand harsh conditions such as high temperatures, heavy loads, and corrosion simultaneously. This places extremely stringent performance requirements on materials, and single-metal materials cannot meet multiple demands at the same time. To solve practical problems in engineering, metal composite plates have emerged.

[0003] Metal composite panels are sheets made by combining two or more different metal materials in the thickness direction through specific processing techniques. Metal composite panels combine the excellent properties of different metals. For example, in applications requiring both strength and corrosion resistance, a high-strength metal (such as carbon steel) serves as the base layer, providing the structural support strength to withstand significant pressure and tensile forces; while a corrosion-resistant metal (such as stainless steel or titanium) serves as the cladding, protecting the inner base metal from corrosive environments. Metal composite panels used in chemical containers and marine engineering equipment, for instance, combine the properties of different metals to ensure stable operation for extended periods in harsh chemical media or seawater environments. Furthermore, metal composite panels effectively reduce the consumption of expensive metals, lowering production costs. For example, pure titanium is expensive, but in some chemical equipment requiring extremely high corrosion resistance, using only titanium would be extremely costly. By using titanium-steel composite plates, titanium is used only on the surface that comes into contact with corrosive media, while the exterior is reinforced with relatively inexpensive steel as a base layer. This approach ensures corrosion resistance while reducing the consumption of titanium metal, thus significantly lowering material costs.

[0004] Currently, the main manufacturing processes for metal composite plates are explosive bonding and rolling bonding. Explosive bonding utilizes the impact force generated by an explosive detonation to cause high-speed collisions between different metal plates, resulting in plastic deformation, melting, and interatomic diffusion at the contact surface, thereby achieving a metallurgical bond between the metals (see the instruction manual appendix). Figure 1 ).

[0005] Explosive welding composite plates have many advantages. First, they have a wide range of applications, capable of rapidly and strongly welding together various metal materials, especially metals with significant differences in melting point, coefficient of thermal expansion, and hardness. Second, they can be welded to a wide range of sizes; the size and specifications of explosively welded metal plates are not limited by equipment conditions, and the applicable plate thickness is wide. Third, the welded components have excellent performance; explosively welded components have high bonding strength, excellent performance, and good machinability. However, explosive welding also has disadvantages: First, explosive welding requires directional blasting technology, necessitating the deployment of a large amount of explosives on the plate (the larger the composite area, the more explosives are required). This places extremely high demands on both technology and safety, and the explosives and buffer layers are consumables, leading to extremely high production costs. Furthermore, because production is done through explosions, to ensure safety, the process is generally carried out outdoors, subject to weather and climate limitations, resulting in low production efficiency and further increasing production costs. Second, the metals to be welded must have sufficient toughness and impact resistance to withstand the explosive force and impact. Thin plates that cannot withstand the impact of explosives cannot be welded. In addition, during the composite process of large-size panels, the detonation wave travels a long distance and its stability decreases, which can lead to quality problems such as non-adhesion at the edges.

[0006] Rolling composite refers to a metallurgical process in which two or more metal sheets are pressed together under certain temperature and pressure conditions using a heavy rolling mill, causing atomic diffusion between the interfaces of the sheets and thus achieving a strong bond (see the instruction manual appendix). Figure 2 Roll lamination is not limited by site or weather conditions and does not use explosives, buffer layers, or other consumables. Compared to explosive lamination, it significantly reduces production costs, technical requirements, and safety risks. Furthermore, roll lamination does not suffer from pressure decay, ensuring adhesion between edge plates and thus guaranteeing product quality. However, to ensure rapid atomic diffusion and bonding between plates, the plates need to be heated before rolling. Firstly, the energy consumption during heating increases production costs; secondly, for thin plates, heating easily causes deformation, which is random and uncontrollable, potentially leading to uneven bonding during rolling and affecting product quality. Additionally, because the rolling process only applies force briefly to the plates, atomic diffusion is not deep enough, resulting in weak bonding at the lamination interface and defects such as delamination and detachment.

[0007] Therefore, it is necessary to design a metal composite plate and its continuous preparation method to solve the above problems. Summary of the Invention

[0008] The purpose of this invention is to address the shortcomings of existing technologies by providing a metal composite plate that can achieve uniform bonding, ensure product quality, and reduce production costs, as well as a continuous preparation method thereof.

[0009] The technical solution of this invention is: A metal composite plate, comprising a stacked substrate and multiple (at least one) cladding plates, characterized in that the substrate and cladding plates are connected, and the cladding plates are connected to each other, by double-headed semi-hollow rivets.

[0010] The double-headed semi-hollow rivet consists of a partition plate, an upper riveting leg, and a lower riveting leg. The upper riveting leg is provided at the top of the partition plate, and the lower riveting leg is provided at the bottom of the partition plate.

[0011] The riveted upper leg and the riveted lower leg are both annular cavities with uniform wall thickness.

[0012] The riveted upper leg and riveted lower leg are respectively annular cavities with a wall thickness on one side greater than that on the other side.

[0013] The partition plate is provided with a positioning flange on its outer side.

[0014] A continuous preparation method for a metal composite plate, characterized by comprising the following steps: (1) Select connection points evenly on the substrate according to the width of the substrate and the connection strength requirements between the plates; (2) Unwind the rolled substrate and transport it to the lower die of the stamping machine; with the connection point as the center, insert and fix the riveting lower leg of the double-headed semi-hollow rivet onto the substrate through the stamping machine; when the riveting lower leg is connected to the substrate, the stamping machine is reset. (3) Repeat step 2) to continuously rivet double-headed semi-hollow rivets onto the substrate; (4) Continue to convey the substrate with double-headed semi-hollow rivets between the upper and lower rollers; during the continued conveying of the substrate, unwind the rolled composite board and convey it between the upper and lower rollers. (5) The substrate and the cladding plate enter the upper roller and the lower roller. The upper roller and the lower roller squeeze the substrate and the cladding plate against each other, inserting the upper leg of the double-headed semi-hollow rivet on the substrate and fixing it on the cladding plate, thereby connecting the substrate and the cladding plate through the double-headed semi-hollow rivet. (6) For multi-layer metal composite plates (at least two layers of composite plates), the connected substrate and composite plates are treated as a whole as a new substrate, and steps 1)-5) are repeated to rivet the multi-layer composite plates respectively.

[0015] The lower roller is equipped with an adjustment wheel at its front end to adjust the conveying angle of the substrate.

[0016] The press includes an upper die and a lower die. The cross-section of the upper die is shaped like an inverted "mountain". A die post is set in the center of the upper die to straighten and limit the upper leg of the rivet during the riveting process of the double-headed semi-hollow rivet to the substrate.

[0017] A continuous preparation method for a metal composite plate, characterized by comprising the following steps: (1) Select connection points evenly on the substrate according to the width of the substrate and the connection strength requirements between the plates; (2) Unwind the rolled substrate and transport the substrate to the lower die of the stamping machine; with the connection point as the center, align the thicker side of the riveting lower leg of the double-headed semi-hollow rivet with the front end of the substrate transport direction, and insert and fix the riveting lower leg onto the substrate through the stamping machine; when the riveting lower leg is connected to the substrate, the stamping machine is reset. (3) Repeat step 2) to continuously rivet double-headed semi-hollow rivets onto the substrate; (4) Continue to convey the substrate with double-headed semi-hollow rivets between the upper and lower rollers; during the continued conveying of the substrate, unwind the rolled composite board and convey it between the upper and lower rollers. (5) The substrate and the cladding plate enter the upper roller and the lower roller. The upper roller and the lower roller squeeze the substrate and the cladding plate against each other, inserting the upper leg of the double-headed semi-hollow rivet on the substrate and fixing it on the cladding plate, thereby connecting the substrate and the cladding plate through the double-headed semi-hollow rivet. (6) For multi-layer metal composite plates (at least two layers of composite plates), the connected substrate and composite plates are treated as a whole as a new substrate, and steps 1)-5) are repeated to rivet the multi-layer composite plates respectively.

[0018] The press includes an upper die and a lower die. The cross-section of the upper die is in the shape of an inverted "mountain". The die post of the upper die is eccentrically set so as to straighten and limit the upper leg of the riveting during the riveting process of the double-headed semi-hollow rivet and the substrate.

[0019] The beneficial effects of this invention are as follows: This metal composite plate and its continuous manufacturing method connect the plates using double-headed semi-hollow rivets. The connection relies on the mechanical deformation between the rivets and the plates, ensuring a strong bond and minimizing defects such as delamination and detachment. The connection process does not require heating the plates, effectively reducing production costs. Because heating is unnecessary, thin plates are less prone to deformation, ensuring uniform connection. Furthermore, since thin plates do not require high strength or high toughness, the requirements are significantly reduced, and thin plates can be easily connected. This solves the problems of high production costs, susceptibility to quality defects, and unsuitability for thin-plate composites in existing metal composite plates. Attached Figure Description

[0020] Figure 1 This is a schematic diagram illustrating the principle of explosive recombination; Figure 2 This is a schematic diagram illustrating the principle of rolling composite; Figure 3 This is a schematic diagram of the structure of the metal composite plate (single-layer composite plate) of Embodiment 1 of the present invention; Figure 4 This is a schematic diagram of the structure of the metal composite plate (single-layer composite plate) in Embodiment 2 of the present invention; Figure 5 This is a production schematic diagram of the metal composite plate (single-layer composite plate) of Embodiment 1 of the present invention; Figure 6 yes Figure 5 Enlarged view of point A in the middle; Figure 7 This is a production schematic diagram of the metal composite plate (single-layer composite plate) of Embodiment 2 of the present invention; Figure 8 yes Figure 7 Enlarged diagram of point A in the middle.

[0021] In the diagram: 1. Base plate, 2. Composite plate, 3. Separator plate, 4. Riveted upper leg, 5. Riveted lower leg, 6. Positioning flange, 7. Upper mold, 8. Upper roller, 9. Lower roller, 10. Adjusting wheel, 11. Mold column, 12. Buffer layer, 13. Explosive, 14. Support block, 15. Welding platform, 16. Roller. Detailed Implementation Example 1

[0022] This metal composite plate consists of a stacked substrate 1 and multiple (at least one) cladding plates 2. The substrate 1 and cladding plates 2 are connected to each other, as are the cladding plates 2 to each other, by double-headed semi-hollow rivets. The substrate 1 and cladding plates 2 are firmly connected through mechanical deformation between the substrate 1 and the double-headed semi-hollow rivets, and between the cladding plates 2 and the double-headed semi-hollow rivets. Because it is connected through mechanical deformation, explosives are not required, thus effectively reducing technical requirements and safety risks. Furthermore, since it is not connected through interatomic diffusion at the interface, heating of the plate is not required, effectively reducing energy consumption and thus production costs.

[0023] The double-headed semi-hollow rivet consists of a partition plate 3, an upper riveting leg 4, and a lower riveting leg 5. The upper riveting leg 4 is located at the top of the partition plate 3 for riveting to the composite plate 2. The lower riveting leg 5 is located at the bottom of the partition plate 3 for riveting to the base plate 1. The function of the partition plate 3 is to push the double-headed semi-hollow rivet downward through the punching force applied to the partition plate 3, thereby inserting and fixing the double-headed semi-hollow rivet into the base plate 1; at the same time, the interaction between the partition plate 3 and the base plate 1 limits the insertion depth of the double-headed semi-hollow rivet, preventing the double-headed semi-hollow rivet from inserting too deeply and puncturing the base plate 1 or the composite plate 2.

[0024] The upper riveting leg 4 and the lower riveting leg 5 are both annular cavities with uniform wall thickness. The inner side of the port of the upper riveting leg 4 and the lower riveting leg 5 is provided with a conical surface, which guides the deformation direction of the upper riveting leg 4 and the lower riveting leg 5 through the conical surface, so that the upper riveting leg 4 and the lower riveting leg 5 deform outward instead of collapsing inward, ensuring that the mechanical deformation of the upper riveting leg 4 and the lower riveting leg 5 with the plate can firmly connect the double-headed semi-hollow rivet with the plate.

[0025] A positioning flange 6 is provided on the outer side of the partition plate 3. The function of the positioning flange 6 is to further limit the double-headed semi-hollow rivet, and in conjunction with the partition plate 3, prevent the double-headed semi-hollow rivet from penetrating too deeply and piercing the plate.

[0026] The continuous preparation method of this metal composite plate includes the following steps: According to the width of substrate 1 and the connection strength requirements between the plates, connection points are evenly selected on the substrate.

[0027] Unwind the rolled substrate 1 and feed it to the lower die of the stamping machine. Centered on the connection point, insert and fix the riveting lower leg 5 of the double-headed semi-hollow rivet onto the substrate 1 through the stamping machine. When the riveting lower leg 5 is connected to the substrate 1, the stamping machine resets. Repeat the above process to continuously rivet double-headed semi-hollow rivets onto the substrate 1.

[0028] The substrate 1, which is riveted with double-headed semi-hollow rivets, continues to be conveyed between the upper roller 8 and the lower roller 9; during the continued conveying of the substrate 1, the rolled-up composite plate 2 is unwound and conveyed between the upper roller 8 and the lower roller 9.

[0029] The substrate 1 and the cladding plate 2 enter the upper roller 8 and the lower roller 9. The upper roller 8 and the lower roller 9 press against the substrate 1 and the cladding plate 2, inserting and fixing the riveting upper leg 4 of the double-headed semi-hollow rivet on the substrate 1 onto the cladding plate 2, thereby connecting the substrate 1 and the cladding plate 2 through the double-headed semi-hollow rivet. Because the upper roller 8 and the lower roller 9 press the plate from front to back, rather than from top to bottom, there is a sequence to the pressing of the plate by the upper roller 8 and the lower roller 9. During the pressing process of the upper roller 8 and the lower roller 9, the pressing force will first act on the front end of the double-headed semi-hollow rivet. At the same time, due to the forward movement of the plate, the front end of the riveting upper leg of the double-headed semi-hollow rivet is prone to collapse backward and be pulled upward out of the plate, which can easily lead to connection failure. The solution in this embodiment is as follows: An adjusting wheel 10 is provided at the front end of the lower roller 9 to adjust the conveying angle of the substrate 1, so that the substrate 1 with double-headed semi-hollow rivets is attached to the composite plate 2. Then, through the tension between the plates, the upper leg 4 of the double-headed semi-hollow rivet is pre-inserted into the composite plate 2, thereby reducing the interaction force between the plate and the double-headed semi-hollow rivet during the pressing process of the upper roller 8 and the lower roller 9, ensuring that the upper leg 4 is not easy to collapse to the rear end, and the lower leg 5 is not easy to be pulled out from the substrate 1, thereby ensuring that the connection between the double-headed semi-hollow rivet and the plate is reliable, thus ensuring a firm connection between the substrate 1 and the composite plate 2.

[0030] For multi-layer metal composite panels (at least two layers of composite panels), the already connected substrate 1 and composite panel 2 are treated as a whole as a new substrate, and the above process is repeated to rivet the multi-layer composite panels 2 respectively.

[0031] The stamping machine includes an upper die 7 and a lower die. The cross-section of the upper die 7 is shaped like an inverted "mountain". A die post 11 is provided in the center of the upper die 7 to straighten and limit the riveting upper leg 4 during the riveting process of the double-headed semi-hollow rivet to the base plate 1. Example 2

[0032] This metal composite plate consists of a stacked substrate 1 and multiple (at least one) cladding plates 2. The substrate 1 and cladding plates 2 are connected to each other, as are the cladding plates 2 to each other, by double-headed semi-hollow rivets. The substrate 1 and cladding plates 2 are firmly connected through mechanical deformation between the substrate 1 and the double-headed semi-hollow rivets, and between the cladding plates 2 and the double-headed semi-hollow rivets. Because it is connected through mechanical deformation, explosives are not required, thus effectively reducing technical requirements and safety risks. Furthermore, since it is not connected through interatomic diffusion at the interface, heating of the plate is not required, effectively reducing energy consumption and thus production costs.

[0033] The double-headed semi-hollow rivet consists of a partition plate 3, an upper riveting leg 4, and a lower riveting leg 5. The upper riveting leg 4 is located at the top of the partition plate 3 for riveting to the composite plate 2. The lower riveting leg 5 is located at the bottom of the partition plate 3 for riveting to the base plate 1. The function of the partition plate 3 is to push the double-headed semi-hollow rivet downward through the punching force applied to the partition plate 3, thereby inserting and fixing the double-headed semi-hollow rivet into the base plate 1; at the same time, the interaction between the partition plate 3 and the base plate 1 limits the insertion depth of the double-headed semi-hollow rivet, preventing the double-headed semi-hollow rivet from inserting too deeply and puncturing the base plate 1 or the composite plate 2.

[0034] The upper riveting leg 4 and the lower riveting leg 5 are annular cavities with a wall thickness on one side greater than that on the other side. The inner side of the port of the upper riveting leg 4 and the lower riveting leg 5 is provided with a conical surface to guide the deformation direction of the upper riveting leg 4 and the lower riveting leg 5, so that the upper riveting leg 4 and the lower riveting leg 5 deform outward instead of collapsing inward. This ensures that the mechanical deformation of the upper riveting leg 4 and the lower riveting leg 5 with the plate allows the double-headed semi-hollow rivet to be firmly connected to the plate.

[0035] A positioning flange 6 is provided on the outer side of the partition plate 3. The function of the positioning flange 6 is to further limit the double-headed semi-hollow rivet, and in conjunction with the partition plate 3, prevent the double-headed semi-hollow rivet from penetrating too deeply and piercing the plate.

[0036] The continuous preparation method of this metal composite plate includes the following steps: According to the width of substrate 1 and the connection strength requirements between the plates, connection points are evenly selected on substrate 1.

[0037] Unwind the rolled substrate 1 and feed it into the lower die of the stamping machine. With the connection point as the center, align the thicker side of the riveting leg 5 of the double-headed semi-hollow rivet towards the front end of the substrate 1 in the feeding direction, and insert and fix the riveting leg 5 onto the substrate 1 using the stamping machine. Once the riveting leg 5 is in place with the substrate 1, the stamping machine resets. Repeat the above process to continuously rivet double-headed semi-hollow rivets onto the substrate 1.

[0038] The substrate 1, riveted with double-headed semi-hollow rivets, continues to be conveyed between the upper roller 8 and the lower roller 9. During the continued conveying of the substrate 1, the rolled-up composite plate 2 is unwound and conveyed between the upper roller 8 and the lower roller 9.

[0039] The substrate 1 and the cladding plate 2 enter the upper roller 8 and the lower roller 9. The upper roller 8 and the lower roller 9 press against the substrate 1 and the cladding plate 2, inserting and fixing the riveting upper leg 4 of the double-headed semi-hollow rivet on the substrate 1 onto the cladding plate 2, thereby connecting the substrate 1 and the cladding plate 2 through the double-headed semi-hollow rivet. Because the upper roller 8 and the lower roller 9 press the plate from front to back, rather than from top to bottom, there is a sequence to the pressing of the plate by the upper roller 8 and the lower roller 9. During the pressing process of the upper roller 8 and the lower roller 9, the pressing force will first act on the front end of the double-headed semi-hollow rivet. At the same time, due to the forward movement of the plate, the front end of the riveting upper leg of the double-headed semi-hollow rivet is prone to collapse backward and be pulled upward out of the plate, which can easily lead to connection failure. The solution in this embodiment is to increase the wall thickness on one side of the riveted upper leg 4 and the riveted lower leg 5, and to position the riveted upper leg 4 and the riveted lower leg 5 on the side with the larger wall thickness toward the front end of the substrate 1 in the conveying direction, thereby placing the riveted upper leg 4 and the riveted lower leg 5 on the side with the larger wall thickness under stress first. Due to the increased wall thickness, the strength of the side of the riveted upper leg 4 and the riveted lower leg 5 that is subjected to stress first is enhanced, making it less likely to collapse backward when the riveted upper leg 4 is under stress, and making it less likely for the riveted lower leg 5 to be pulled out of the substrate 1, thereby ensuring the reliability of the connection and ensuring a firm connection between the substrate 1 and the composite plate 2.

[0040] For multi-layer metal composite panels (at least two layers of composite panels), the already connected substrate 1 and composite panel 2 are treated as a whole as a new substrate, and the above process is repeated to rivet the multi-layer composite panels 2 respectively.

[0041] The stamping machine includes an upper die 7 and a lower die. The cross-section of the upper die 7 is shaped like an inverted "mountain". The die column 11 of the upper die 7 is eccentrically set so as to straighten and limit the riveting upper leg 4 through the upper die 7 during the riveting process of the double-headed semi-hollow rivet and the base plate 1.

[0042] This metal composite plate and its continuous manufacturing method connect the plates using double-headed semi-hollow rivets. The connection relies on the mechanical deformation between the rivets and the plates, ensuring a strong bond and minimizing defects such as delamination and detachment. The connection process does not require heating the plates, effectively reducing production costs. Because heating is unnecessary, thin plates are less prone to deformation, ensuring uniform connection. Furthermore, since thin plates do not require high strength or high toughness, the requirements are significantly reduced, and thin plates can be easily connected. This solves the problems of high production costs, susceptibility to quality defects, and unsuitability for thin-plate composites in existing metal composite plates.

Claims

1. A continuous preparation method for a metal composite plate, characterized in that: It includes the following steps: 1) According to the width of the substrate (1) and the connection strength requirements between the plates, select connection points evenly on the substrate; 2) Unwind the rolled substrate (1) and transport the substrate (1) to the lower die of the stamping machine; with the connection point as the center, insert and fix the riveting lower leg (5) of the double-headed semi-hollow rivet onto the substrate (1) through the stamping machine; when the riveting lower leg (5) is connected to the substrate (1) in place, the stamping machine is reset. 3) Repeat step 2) continuously rivet double-headed semi-hollow rivets onto the substrate (1); 4) Continue to convey the substrate (1) with double-headed semi-hollow rivets between the upper roller (8) and the lower roller (9); during the continued conveying of the substrate (1), unwind the rolled composite plate (2) and convey the composite plate (2) between the upper roller (8) and the lower roller (9); 5) The substrate (1) and the cladding plate (2) enter the upper roller (8) and the lower roller (9). The upper roller (8) and the lower roller (9) squeeze the substrate (1) and the cladding plate (2) together, inserting and fixing the upper leg (4) of the double-headed semi-hollow rivet on the substrate (1) onto the cladding plate (2), thereby connecting the substrate (1) and the cladding plate (2) through the double-headed semi-hollow rivet. 6) For multilayer metal composite plates, take the connected substrate (1) and composite plate (2) as a whole as a new substrate, and repeat steps 1)-5) to rivet the multilayer composite plate (2) respectively; The lower roller (9) is provided with an adjustment wheel (10) at its front end, so as to adjust the conveying angle of the substrate (1) by means of the adjustment wheel (10); The metal composite plate is composed of a stacked base plate (1) and multiple layers of composite plates (2). The base plate (1) and the composite plates (2) are connected to each other and to each other by double-headed semi-hollow rivets. The double-headed semi-hollow rivet is composed of a partition plate (3), an upper riveting leg (4), and a lower riveting leg (5). The upper riveting leg (4) is provided at the top of the partition plate (3), and the lower riveting leg (5) is provided at the bottom of the partition plate (3). The upper riveting leg (4) and the lower riveting leg (5) on the side with the larger wall thickness are directed toward the front end of the substrate (1) in the conveying direction, so that the upper riveting leg (4) and the lower riveting leg (5) on the side with the larger wall thickness are subjected to force first. The riveted upper leg (4) and riveted lower leg (5) are respectively annular cavities with a wall thickness on one side greater than that on the other side; The partition plate (3) is provided with a positioning flange (6) on its outer side.

2. The continuous preparation method of a metal composite plate according to claim 1, characterized in that: The press includes an upper die (7) and a lower die. The cross-section of the upper die (7) is in the shape of an inverted "mountain". A die post (11) is provided in the center of the upper die (7) to straighten and limit the riveted upper leg (4) during the riveting process of the double-headed semi-hollow rivet and the substrate (1).

3. The continuous preparation method of a metal composite plate according to claim 1, characterized in that: The press includes an upper die (7) and a lower die. The cross-section of the upper die (7) is in the shape of an inverted "mountain". The die column (11) of the upper die (7) is eccentrically set so as to straighten and limit the riveted upper leg (4) through the upper die (7) during the riveting process of the double-headed semi-hollow rivet and the substrate (1).

Citation Information

Patent Citations

  • Bidirectional semi-hollow self-punching rivet riveting method

    CN118513494A