Process for the preparation of gasoline from plastics
By using a combination of mesoporous molecular sieves and microporous silica-alumina molecular sieve catalysts with tungsten, zirconium, aluminum, or niobium components, the high cost and environmental pollution problems of converting waste plastics into valuable products in existing technologies have been solved, achieving efficient and low-temperature gasoline production.
Patent Information
- Application Number
- CN202411560760.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2024-10-23
- Filing Date
- 2024-11-04
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-11-04
AI Technical Summary
Existing technologies rely heavily on organometallic complexes, precious metal catalysts, co-reactants, or complex downstream treatments when converting waste plastics into valuable products. This increases the difficulty and cost of treatment and may cause environmental pollution.
A combination of a first catalyst, which is a mesoporous molecular sieve containing tungsten, zirconium, aluminum or niobium components, and a second catalyst, is used to carry out a catalytic cracking reaction, avoiding the use of precious metals and co-reactants, and achieving low-temperature degradation of polyolefin plastics.
It significantly improves the conversion efficiency of polyolefin plastics, increases gasoline yield and selectivity, reduces reaction temperature and energy consumption, reduces the formation of small molecule alkanes, and the catalyst is stable in air and easy to synthesize.
Smart Images

Figure CN119529870B_ABST
Abstract
Description
[0001] Cross-references to related applications
[0002] This application claims the benefit of Chinese Patent Application No. 202411485451.9, filed on October 23, 2024, the contents of which are incorporated herein by reference. Technical Field
[0003] This invention relates to the field of plastic resource utilization technology, and specifically to a method for producing gasoline using plastics. Background Technology
[0004] Plastics are among the most widely used functional polymer materials, applied in almost all industrial and commercial sectors. Global plastic production surged to 8.3 billion tons in 2017 and is projected to exceed 34 billion tons by 2050. Polyolefins account for approximately 25% of global plastic production. As polymers with a C / C bond backbone, they are difficult to degrade in the environment, leading to a large accumulation of polyolefin waste in landfills and the natural environment, posing a threat to various ecosystems. While burning polyolefins can recover energy, it releases significant amounts of carbon dioxide. Pyrolysis and catalytic pyrolysis catalyze the degradation of polyolefin plastics at high temperatures (>400°C), but the high energy input of these catalytic reactions often results in the non-selective breaking of C / C bonds in polyolefin plastics, generating complex products and coke requiring cumbersome separation steps, leading to catalyst deactivation. Hydrogenolysis is a method for efficiently breaking C / C single bonds in polyolefins under milder conditions (<300°C), but it is prone to over-hydrogenolysis, resulting in the formation of large amounts of light C1-C3 hydrocarbons. Furthermore, the use of high-pressure hydrogen poses safety risks and increases equipment investment and operating costs.
[0005] In recent years, several methods have emerged for degrading polyolefins under milder conditions (<300℃), which, compared to pyrolysis and catalytic pyrolysis that directly break C=C single bonds, first activate the CH bonds in polyethylene (414 kJ / mol), then convert the C=C single bonds into olefin C=C double bonds, thereby promoting the catalytic cleavage of the polymer chain. In an ionic liquid environment, tert-butyl chloride can effectively activate the CH bonds in polyethylene (PE) to generate carbocations. The activated PE carbocations can be rapidly depolymerized and converted into C4-C bonds through isomerization, cleavage, and alkylation with isopentane. 36 Alkanes. Organometallic zirconium catalysts activate the CH bonds of polyolefins (PEs) via σ-bond exchange reactions, followed by β-alkyl elimination to form oligomers with C=C double bonds. These oligomers undergo heterobimetallic alkyl exchange with AlR3 to generate aliphatic alkylaluminum intermediates, which are then oxidized to fatty acids or alcohols. Noble metal iridium complexes, platinum, and ruthenium-based catalysts can also activate the CH bonds of polyolefins, allowing unsaturated polyolefins to be further converted into olefins, aromatics, or C4-C hydrocarbons.12 Alkanes.
[0006] However, these low-temperature conversion strategies for polyethylene degradation heavily rely on organometallic complexes (sensitive to air and water), precious metal catalysts, co-reactants (e.g., hydrogen and solvents), or complex downstream treatments. Therefore, there is an urgent need to develop cost-effective, efficient, and robust catalytic systems for converting waste plastics into valuable products. Summary of the Invention
[0007] The purpose of this invention is to overcome the problems of existing technologies that rely heavily on organometallic complexes, precious metal catalysts, co-reactants, or complex downstream treatments in the conversion of waste plastics into valuable products, which increases the difficulty and cost of treatment and easily causes environmental pollution. The invention provides a method for producing gasoline from plastics. The catalyst used in this technical solution can exist stably in the air and is inexpensive and easy to synthesize. It does not require the participation of co-reactants such as hydrogen, solvents, or olefins, and at the same time significantly enhances the conversion effect of polyolefin plastics.
[0008] To achieve the above objectives, the present invention provides a method for preparing gasoline using plastics. The method includes: catalytically cracking polyolefin plastics under an inert atmosphere in the presence of a first catalyst and a second catalyst, wherein the first catalyst contains an active component and an optional support, the active component being at least one selected from tungsten, zirconium, aluminum, and niobium, and the support being a mesoporous molecular sieve; the second catalyst being a microporous silica-alumina molecular sieve; and the mass ratio of the first catalyst to the second catalyst being 1:(0.25-20).
[0009] Preferably, the mass ratio of the first catalyst to the second catalyst is 1:(0.25-4).
[0010] Preferably, the mass ratio of the total mass of the first catalyst and the second catalyst to the amount of the polyolefin plastic is (0.1-1):1.
[0011] Preferably, the polyolefin plastic is polyethylene plastic and / or polypropylene plastic.
[0012] Preferably, the ratio of the average pore size of the first catalyst to that of the second catalyst is (1.75-3.2):1.
[0013] Preferably, in the first catalyst, the mesoporous molecular sieve is at least one of KIT-6, MCM-41 and SBA-15.
[0014] Preferably, the first catalyst contains an active component and a support, wherein the active component accounts for 1.15%-62.59% of the mass of the first catalyst.
[0015] Preferably, the first catalyst contains an active component and a support, wherein the active component is a tungsten component and a zirconium component, and the support is KIT-6.
[0016] Preferably, the active component accounts for 8.3%-51.62% of the mass of the first catalyst, more preferably 11%-39%, and even more preferably 16%-32%.
[0017] Preferably, the mass ratio of the tungsten component to the zirconium component is 1:(0.08-4).
[0018] Preferably, the method further includes preparing the first catalyst by the following steps: mixing and stirring a tungsten source, a zirconium source, a silicon source, a template agent, hydrochloric acid, n-butanol and water, followed by a hydrothermal reaction to obtain a mixture, separating the solid phase from the mixture and calcining it.
[0019] Preferably, the tungsten source is ammonium metatungstate and / or tungsten chloride.
[0020] Preferably, the zirconium source is at least one of zirconium oxychloride, zirconium chloride, zirconium nitrate, and zirconium sulfate.
[0021] Preferably, the silicon source is ethyl silicate and / or methyl silicate.
[0022] Preferably, the template agent is P123 and / or F127.
[0023] Preferably, the ratio of the amount of the tungsten source, the zirconium source, the silicon source, the template agent, the hydrochloric acid, the n-butanol and the water is (0.2-1.8)g:(0.4-1.8)g:(6-10)g:(3.5-4)g:(5-8)g:(3.5-4)g:130mL.
[0024] Preferably, the concentration of the hydrochloric acid is 30wt%-38wt%.
[0025] Preferably, the conditions for the hydrothermal reaction include: a temperature of 90-110℃ and a time of 20-30h.
[0026] Preferably, the calcination conditions include a temperature of 550-750℃ and a time of 5-8h.
[0027] Preferably, the second catalyst is at least one of β molecular sieve, Mordenite molecular sieve, MCM-22 molecular sieve and HZSM-5 molecular sieve, and preferably HZSM-5 molecular sieve.
[0028] Preferably, the conditions for the catalytic cracking reaction include: a temperature of 220-280℃ and a time of 1-48h.
[0029] Preferably, the catalytic cracking reaction is carried out in a batch reactor.
[0030] Compared with the prior art, the present invention has the following technical effects:
[0031] (1) In the method for preparing gasoline using plastics described in this invention, the long chain of polyolefin is pre-fractured under the action of the first catalyst and generates short chain polymer substances with unsaturated carbon-carbon double bonds. This not only increases the mass and heat transfer efficiency of the reaction, but also allows for further hydrogen transfer, β-cracking and aromatization reactions under the action of the second catalyst at low temperature to generate hydrocarbons in the gasoline range. Through the synergistic effect of the first and second catalysts, the conversion effect of polyolefin plastics is significantly enhanced, and the plastic conversion rate and gasoline yield are improved. Under the condition of 240°C, the maximum yield of hydrocarbons in the gasoline range reaches 88%.
[0032] (2) The first and second catalysts described in this invention can exist stably in air and are inexpensive and easy to synthesize. They can catalyze the degradation of polyolefin plastics at low temperatures without the need for precious metals, hydrogen, solvents and olefins as co-reactants. At the same time, compared with a single catalyst system, the synergistic effect of the first and second catalysts significantly enhances the conversion effect of polyolefin plastics.
[0033] (3) The first catalyst and the second catalyst described in this invention have tunable structures and suitable acidic sites. They not only utilize the contact between the plastic degradation process and the catalytic active sites to increase the mass and heat transfer efficiency, but also improve the selectivity of gasoline products, reduce the amount of small molecule C1-C3 alkanes generated, and increase the octane number of gasoline.
[0034] (4) The method for preparing gasoline using plastics described in this invention has mild reaction conditions, is not prone to producing coke, and the catalyst can still maintain its initial performance after multiple reactions and recycling. Attached Figure Description
[0035] Figure 1 This is a TEM image of WZr-KIT-6 prepared in Example 1;
[0036] Figure 2 This is a TEM image of the HZSM-5 molecular sieve in the examples;
[0037] Figure 3 The images show the XRD patterns of WZr-KIT-6, HZSM-5, and mixtures of WZr-KIT-6 and HZSM-5 prepared in Example 1.
[0038] Figure 4The graph shows the low-temperature nitrogen adsorption-desorption curves of WZr-KIT-6, HZSM-5, and the mixture of WZr-KIT-6 and HZSM-5 prepared in Example 1.
[0039] Figure 5 The TPD diagrams of ammonia gas for WZr-KIT-6, HZSM-5, and mixtures of WZr-KIT-6 and HZSM-5 prepared in Example 1 are shown.
[0040] Figure 6 This is a catalytic cycle diagram of WZr-KIT-6 and HZSM-5 prepared in Example 1. Detailed Implementation
[0041] The following provides a detailed description of specific embodiments of the present invention. It should be understood that the specific embodiments described herein are for illustrative and explanatory purposes only and are not intended to limit the scope of the invention.
[0042] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0043] The method for preparing gasoline from plastics according to the present invention includes: catalytic cracking of polyolefin plastics under an inert atmosphere in the presence of a first catalyst and a second catalyst. The first catalyst contains an active component and an optional support. The active component is at least one selected from tungsten, zirconium, aluminum, and niobium. The support is a mesoporous molecular sieve. The second catalyst is a microporous silica-alumina molecular sieve. The mass ratio of the first catalyst to the second catalyst is 1:(0.25-20). According to the method of the present invention, the synergistic effect of the first and second catalysts not only facilitates the contact between the plastic degradation process and the catalytically active sites, increasing mass and heat transfer efficiency, but also significantly improves the selectivity of gasoline products. Furthermore, the first and second catalysts are stable in air, inexpensive, and easily synthesized, enabling low-temperature catalytic degradation of polyolefin plastics without the need for precious metals, hydrogen, solvents, and olefin co-reactants.
[0044] In the method described in this invention, in order to enhance the conversion effect of polyolefin plastics, the mass ratio of the first catalyst to the second catalyst is preferably 1:(0.25-4), more preferably 1:(2-4), and specifically, for example, 1:0.25, 1:0.5, 1:1, 1:2, 1:3 or 1:4.
[0045] In the method described in this invention, in order to increase the contact between the polyolefin plastic and the catalytic active sites and improve the mass transfer and heat transfer efficiency, the mass ratio of the total mass of the first catalyst and the second catalyst to the amount of the polyolefin plastic is preferably (0.1-1):1, more preferably (0.25-0.5):1, and specifically, for example, 1:4, 2:7, 1:3, 2:5 or 1:2.
[0046] In the method described in this invention, the polyolefin plastic can be polyethylene plastic and / or polypropylene plastic, preferably polyethylene plastic. The weight-average molecular weight of the polyethylene plastic can be 40,000-100,000. The weight-average molecular weight of the polypropylene plastic can be 80,000-100,000. Both the polyethylene plastic and the polypropylene plastic are commercially available.
[0047] In the method described in this invention, in order to improve the plastic conversion rate and gasoline yield, the ratio of the average pore size of the first catalyst to the second catalyst is preferably (1.75-3.2):1, more preferably (1.8-2.4):1. The average pore size of the first catalyst can be 4.2-7.7 nm, preferably 3.6-4.8 nm; the specific surface area can be 460-700 m². 2 / g, preferably 460-600m 2 / g. The average pore size of the second catalyst can be 2-2.4 nm, preferably 2-2.2 nm; the specific surface area can be 300-400 m². 2 / g, preferably 350-400m 2 / g.
[0048] In the method described in this invention, to improve the selectivity of gasoline products, the mesoporous molecular sieve in the first catalyst is preferably at least one of KIT-6, MCM-41, and SBA-15, more preferably KIT-6. The first catalyst may contain an active component and a support, wherein the mass percentage of the active component in the first catalyst can be 1.15%-62.59%, preferably 16%-32%. In some embodiments, the first catalyst contains an active component and a support, wherein the active component is a tungsten component and a zirconium component, the support is KIT-6, the mass percentage of the active component in the first catalyst is 8.3%-51.62%, and the mass ratio of the tungsten component to the zirconium component is 1:(0.08-4). In other embodiments, the first catalyst contains an active component and a support, wherein the active component is a tungsten component, the support is KIT-6, and the mass percentage of the active component in the first catalyst is 8.3%-51.62%. In some embodiments, the first catalyst contains an active component and a support, wherein the active component is a zirconium component and the support is KIT-6, and the active component accounts for 8.3%-51.62% of the mass of the first catalyst. In some embodiments, the first catalyst contains an active component and a support, wherein the active component is an aluminum component and the support is MCM-41, and the active component accounts for 1.15%-3% of the mass of the first catalyst. In some embodiments, the first catalyst contains an active component and a support, wherein the active component is an aluminum component and the support is SBA-15, and the active component accounts for 1.77%-54% of the mass of the first catalyst. In some embodiments, the first catalyst contains an active component and a support, wherein the active component is a niobium component and an aluminum component, the support is SBA-15, and the active component accounts for 5.8%-62.59% of the mass of the first catalyst, with a mass ratio of niobium to aluminum of 1:(0.14-12.48). In some embodiments, the first catalyst contains an active component, which is a zirconium component and an aluminum component, wherein the mass ratio of the zirconium component to the aluminum component is 1:(0.14-0.3). In some other embodiments, the first catalyst contains an active component, which is a tungsten component and an aluminum component, wherein the mass ratio of the tungsten component to the aluminum component is 1:(3.82-13.39).
[0049] In the method described in this invention, when the first catalyst contains an active component and a support, wherein the active component is a tungsten component and a zirconium component, and the support is KIT-6, the mass percentage of the active component in the first catalyst can be 8.3%-51.62%, preferably 11%-39%, more preferably 16%-32%; the mass ratio of the tungsten component to the zirconium component can be 1:(0.08-4), preferably 1:(0.2-4), more preferably 1:(0.4-3.6). The method may further include preparing the first catalyst according to the following steps: mixing and stirring a tungsten source, a zirconium source, a silicon source, a template agent, hydrochloric acid, n-butanol, and water, followed by a hydrothermal reaction to obtain a mixture; separating the solid phase from the mixture and calcining it. The tungsten source can be ammonium metatungstate and / or tungsten chloride, preferably ammonium metatungstate. The zirconium source can be at least one of zirconium oxychloride, zirconium chloride, zirconium nitrate, and zirconium sulfate, preferably zirconium oxychloride. The silicon source can be ethyl silicate and / or methyl silicate, preferably ethyl silicate. The template agent can be P123 (polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer) and / or F127 (polyethylene glycol-polypropylene glycol-polyethylene glycol triblock copolymer), preferably P123. The ratio of the amount of the tungsten source, the zirconium source, the silicon source, the template agent, the hydrochloric acid, the n-butanol, and the water can be (0.2-1.8) g:(0.4-1.8) g:(6-10) g:(3.5-4) g:(5-8) g:(3.5-4) g:130 mL, preferably (0.7-1) g:(0.7-1) g:(7-9) g:(3.6-3.8) g:(5-7) g:(3.6-3.8) g:130 mL. The concentration of the hydrochloric acid can be 30wt%-38wt%, preferably 36wt%-38wt%.
[0050] In the method described in this invention, the stirring conditions include: the temperature can be 20-30℃, preferably 23-28℃; the stirring rate can be 400-800rpm, preferably 500-700rpm; and the time can be 20-30h, preferably 22-26h.
[0051] In the method described in this invention, the conditions for the hydrothermal reaction include: a temperature of 90-110℃, preferably 95-105℃; and a time of 20-30h, preferably 22-26h.
[0052] In the method described in this invention, the specific process of separating the solid phase from the mixture may include: separating the solid phase from the mixture by filtration and then washing and drying it. The drying conditions include: a temperature of 100-120°C, preferably 105-115°C; and a time of 20-30 hours, preferably 22-26 hours.
[0053] In the method described in this invention, the calcination conditions include: a temperature of 550-750℃, preferably 550-650℃; and a time of 5-8 hours, preferably 6-7 hours. The calcination is carried out in a muffle furnace.
[0054] In the method described in this invention, when the first catalyst contains an active component and a support, wherein the active component is an aluminum component and the support is SBA-15, the mass percentage of the active component in the first catalyst is 1.77%-54%. The method may further include preparing the first catalyst according to the following steps: mixing P123, oxalic acid, and a first hydrochloric acid, then mixing with ethyl silicate, stirring at 20-30°C at a stirring rate of 400-800 rpm for 20-30 h to obtain SBA-15; then placing the prepared SBA-15 in an aqueous aluminum nitrate solution, adjusting the pH to 1.5-2.5 with a second hydrochloric acid, then placing it in a sealed autoclave, and performing a hydrothermal reaction at 110-130°C for 20-30 h; separating the solid phase from the resulting mixture by filtration, washing, and drying at 100-120°C for 20-30 h to obtain Al-SBA-15. The concentration of the first hydrochloric acid can be 1-3 mol / L. The ratio of the amount of P123, the oxalic acid, the first hydrochloric acid, and the ethyl silicate can be (2-3) g : (1-1.5) g : 40 mL : (4-5) g. The concentration of the aluminum nitrate aqueous solution can be 0.1-3 mol / L. The ratio of the amount of SBA-15 and the aluminum nitrate aqueous solution can be (0.8-1.5) g : 10 mL. The concentration of the second hydrochloric acid can be 0.5-2 mol / L.
[0055] In the method described in this invention, when the first catalyst contains an active component and a support, wherein the active component is a niobium component and an aluminum component, and the support is SBA-15, the mass percentage of the active component in the first catalyst is 5.8%-62.59%, and the mass ratio of the niobium component to the aluminum component is 1:(0.14-12.48). The method may further include preparing the first catalyst according to the following steps: mixing P123, oxalic acid, and hydrochloric acid, then mixing with ethyl silicate, and stirring at 20-30°C at a stirring rate of 400-800 rpm for 20-30 hours to obtain SBA-15; then placing the prepared SBA-15 in an aqueous aluminum nitrate solution, adjusting the pH to 1.5-2.5 with a second hydrochloric acid, then placing it in a sealed autoclave, and performing a hydrothermal reaction at 110-130°C for 20-30 hours, filtering the resulting mixture... The solid phase is separated from the compound, washed, and dried at 100-120℃ for 20-30 h to obtain Al-SBA-15 (the active component is aluminum, and the support is SBA-15). Al-SBA-15, niobic acid, second oxalic acid, and water are mixed and stirred at 20-30℃ with a stirring rate of 400-800 rpm for 14-20 h. The solid phase is separated from the mixture by filtration, washed, and dried at 100-120℃ for 20-30 h, then calcined at 400-550℃ for 5-8 h. The concentration of the first hydrochloric acid can be 1-3 mol / L. The ratio of P123, the first oxalic acid, the first hydrochloric acid, and the ethyl silicate can be (2-3) g: (1-1.5) g: 40 mL: (4-5) g. The concentration of the aluminum nitrate aqueous solution can be 0.1-3 mol / L. The ratio of SBA-15 to the aluminum nitrate aqueous solution can be (0.8-1.5) g: 10 mL. The concentration of the second hydrochloric acid can be 0.5-2 mol / L. The ratio of Al-SBA-15, niobic acid, the second oxalic acid, and water can be (1.5-2.5) g: (0.3-0.6) g: (0.6-0.9) g: 20 mL.
[0056] In the method described in this invention, when the first catalyst contains an active component and a support, wherein the active component is an aluminum component and the support is MCM-41, the mass percentage of the active component in the first catalyst is 1.15%-3%. The method may further include preparing the first catalyst according to the following steps: mixing tetradecyltrimethylammonium bromide aqueous solution, sodium aluminate, sodium silicate, sulfuric acid, and water, and stirring at 20-30°C at a stirring rate of 400-800 rpm for 2-5 hours, followed by reacting at 95-110°C for 5-8 days, separating the solid phase from the resulting mixture by filtration, washing, and drying at 100-120°C for 20-30 hours. The concentration of the tetradecyltrimethylammonium bromide aqueous solution may be 0.1-0.2 g / mL. The concentration of the sulfuric acid may be 8 wt%-15 wt%. The ratio of the amount of the tetradecyltrimethylammonium bromide aqueous solution, the sodium aluminate, the sodium silicate, the sulfuric acid and the water can be (90-100) mL: (0.15-0.3) g: (15-20) g: (4-8) g: 15 mL.
[0057] In the method described in this invention, when the first catalyst contains an active component, and the active component is a zirconium component and an aluminum component, the mass ratio of the zirconium component to the aluminum component is 1:(0.14-0.3). The method may further include preparing the first catalyst according to the following steps: mixing F127, hydrochloric acid, aluminum nitrate, zirconium oxychloride, and ethanol, stirring at 30-35°C at a stirring rate of 400-800 rpm for 20-30 h, followed by hydrothermal treatment at 90-110°C for 20-30 h, then separating the solid phase by filtration and drying at 50-80°C for 45-60 h, and finally calcining at 500-650°C for 4-7 h. The concentration of the hydrochloric acid can be 30-38 wt%. The ratio of the amounts of F127, hydrochloric acid, aluminum nitrate, zirconium oxychloride, and ethanol can be (3-4) g:(2-3) g:(2.5-3.5) g:(2-3.5) g:25 mL.
[0058] In the method described in this invention, when the first catalyst contains an active component, and the active component is a tungsten component and an aluminum component, the mass ratio of the tungsten component to the aluminum component is 1:(3.82-13.39). The method may further include preparing the first catalyst according to the following steps: mixing an aqueous solution of ammonium metatungstate and γ-Al₂O₃ and stirring at 38-45°C at a stirring rate of 400-800 rpm for 15-20 h; then separating the solid phase by filtration; and then drying successively at 100-120°C for 10-15 h and calcining at 420-500°C for 4-7 h. The concentration of the aqueous solution of ammonium metatungstate can be 8-15 g / L. The mass ratio of the aqueous solution of ammonium metatungstate to γ-Al₂O₃ can be 10 mL:(0.8-1.5) g.
[0059] In the method described in this invention, in order to improve the plastic conversion rate and gasoline yield, the second catalyst is preferably at least one of β molecular sieve, Mordenite molecular sieve, MCM-22 molecular sieve and HZSM-5 molecular sieve, more preferably HZSM-5 molecular sieve.
[0060] In the method described in this invention, in order to ensure the occurrence of the catalytic cracking reaction, the inert atmosphere is preferably argon and / or nitrogen, more preferably argon, and in a preferred case, the purity of the argon is 99.0 wt%-99.9 wt%.
[0061] In the method described in this invention, the conditions for the catalytic cracking reaction include: a temperature of 220-280°C, preferably 230-250°C; and a time of 1-48 hours, preferably 36-48 hours. The catalytic cracking reaction can be carried out in a batch reactor.
[0062] In the method described in this invention, the method may specifically include: mixing the first catalyst and the second catalyst, then mixing and grinding them with the polyolefin plastic, then placing the resulting mixture in the batch reactor, introducing an inert atmosphere, heating to 220-280°C, and carrying out the catalytic cracking reaction for 1-48 hours.
[0063] In some embodiments, the method for preparing gasoline using plastics according to the present invention includes: mixing a first catalyst and a second catalyst, then mixing and grinding them with polyolefin plastic, and then placing the resulting mixture in the batch reactor, introducing an inert atmosphere, heating to 220-280°C, and carrying out the catalytic cracking reaction for 1-48 hours. The first catalyst contains an active component and a support; the active component is at least one selected from tungsten, zirconium, aluminum, and niobium; the support is at least one selected from KIT-6, MCM-41, and SBA-15; and the active component accounts for 1.15%-62.59% of the mass of the first catalyst. The second catalyst is at least one selected from β-zeolite, Mordenite, MCM-22, and HZSM-5 molecular sieves. The average pore size ratio of the first catalyst to the second catalyst is (1.75-3.2):1; the average pore size of the first catalyst is 4.2-7.7 nm; and the specific surface area is 460-700 m². 2 / g; the second catalyst has an average pore size of 2.0-2.4 nm and a specific surface area of 180-530 m². 2 / g; the mass ratio of the first catalyst to the second catalyst is 1:(0.25-4); the mass ratio of the total mass of the first catalyst and the second catalyst to the mass of the polyolefin plastic is (0.1-1):1.
[0064] In other embodiments, the method for preparing gasoline using plastics according to the present invention includes: mixing a tungsten source, a zirconium source, a silicon source, a template agent, hydrochloric acid, n-butanol, and water, and stirring at 20-30°C and a stirring rate of 400-800 rpm for 20-30 hours; then carrying out a hydrothermal reaction at 90-110°C for 20-30 hours to obtain a mixture; separating the solid phase from the mixture by filtration, washing, and drying at 100-120°C for 20-30 hours; then calcining at 550-750°C for 5-8 hours to obtain a first catalyst; mixing the first catalyst and the second catalyst; then mixing and grinding the mixture with polyolefin plastic; and finally placing the resulting mixture in the reactor. The reactor is purged with an inert atmosphere and heated to 220-280℃ for 1-48 hours to carry out the catalytic cracking reaction. The ratio of the amounts of the tungsten source, zirconium source, silicon source, template agent, hydrochloric acid, n-butanol, and water is (0.2-1.8) g : (0.4-1.8) g : (6-10) g : (3.5-4) g : (5-8) g : (3.5-4) g : 130 mL. The second catalyst is HZSM-5 molecular sieve, and the ratio of the average pore size of the first catalyst to the second catalyst is (1.75-3.2):1. The average pore size of the first catalyst is 4.2-7.7 nm, and its specific surface area is 460-700 m².2 / g; the second catalyst has an average pore size of 2.0-2.4 nm and a specific surface area of 180-530 m². 2 / g; the mass ratio of the first catalyst to the second catalyst is 1:(0.25-4); the mass ratio of the total mass of the first catalyst and the second catalyst to the mass of the polyolefin plastic is (0.1-1):1.
[0065] The following examples further illustrate the method for preparing gasoline using plastics according to the present invention. These examples are implemented based on the technical solution of the present invention, providing detailed implementation methods and specific operating procedures; however, the scope of protection of the present invention is not limited to the following examples.
[0066] Unless otherwise specified, the experimental methods used in the following examples are conventional methods in the art. Unless otherwise specified, the experimental materials used in the following examples are commercially available. Polyethylene plastic was purchased from Macklin Company, brand name Macklin, with a weight-average molecular weight of 80,000; polypropylene plastic was purchased from Ruixiang Plastics Company, with a weight-average molecular weight of 80,000; HZSM-5 molecular sieve was purchased from Tianjin Nanhua Catalyst Co., Ltd.; the molar ratio of silica to alumina was 25; β-molecular sieve, Mordenite molecular sieve, and MCM-22 molecular sieve were all purchased from Tianjin Nanhua Catalyst Co., Ltd.
[0067] Example 1
[0068] 0.9 g ammonium metatungstate, 0.8 g zirconium oxychloride, 8 g ethyl silicate, 3.7 g P123, 6 g 37 wt% hydrochloric acid, and 3.7 g n-butanol were added to a conical flask containing 130 mL deionized water and mixed. The mixture was stirred at 25 °C at 600 rpm for 24 h, followed by a hydrothermal reaction at 100 °C for 24 h to obtain a mixture. The solid phase was separated from the mixture by filtration, washed, and dried at 110 °C for 24 h. Then, it was calcined at 550 °C for 5 h to obtain WZr-KIT-6 (the active components are tungsten and zirconium, the support is KIT-6, the mass percentage of the active component in WZr-KIT-6 is 32%, and the mass ratio of the tungsten component to the zirconium component is 1:0.5). 0.02 g of WZr-KIT-6 and 0.08 g of... The mixture was mixed with HZSM-5 molecular sieve, then mixed with 0.3g of polyethylene plastic and ground. The resulting mixture was then placed in a batch reactor, argon gas was introduced, the temperature was raised to 240℃ and the catalytic cracking reaction was carried out for 48h. After the reaction was completed, the mixture was naturally cooled to 25℃.
[0069] Example 2
[0070] 0.4 g ammonium metatungstate, 0.4 g zirconium oxychloride, 6 g ethyl silicate, 3.5 g P123, 5 g 30 wt% hydrochloric acid, and 3.5 g n-butanol were added to a conical flask containing 130 mL of deionized water and mixed. The mixture was stirred at 20 °C and 400 rpm for 20 h, followed by a hydrothermal reaction at 90 °C for 20 h to obtain a mixture. The solid phase was separated from the mixture by filtration, washed, and dried at 100 °C for 20 h. Then, it was calcined at 550 °C for 5 h to obtain WZr-KIT-6 (the active components are tungsten and zirconium, the support is KIT-6, the mass percentage of the active component in WZr-KIT-6 is 21%, and the mass ratio of the tungsten component to the zirconium component is 1:0.52). 0.05 g of WZr-KIT-6 and 0.05 g of... The mixture was mixed with HZSM-5 molecular sieve, then mixed with 0.4g of polyethylene plastic and ground. The resulting mixture was then placed in a batch reactor, argon gas was introduced, the temperature was raised to 220℃ and the catalytic cracking reaction was carried out for 24h. After the reaction was completed, the mixture was naturally cooled to 25℃.
[0071] Example 3
[0072] 1.8 g ammonium metatungstate, 1.8 g zirconium sulfate, 10 g ethyl silicate, 4 g P123, 8 g 38 wt% hydrochloric acid, and 4 g n-butanol were added to a conical flask containing 130 mL deionized water and mixed. The mixture was stirred at 30 °C and 800 rpm for 30 h, followed by a hydrothermal reaction at 110 °C for 30 h to obtain a mixture. The solid phase was separated from the mixture by filtration, washed, and dried at 120 °C for 30 h. Then, it was calcined at 750 °C for 8 h to obtain WZr-KIT-6 (the active components are tungsten and zirconium, the support is KIT-6, the mass percentage of the active component in WZr-KIT-6 is 39%, and the mass ratio of the tungsten component to the zirconium component is 1:0.4). 0.08 g of WZr-KIT-6 and 0.02 g of... The mixture was mixed with HZSM-5 molecular sieve, then mixed with 0.1g of polyethylene plastic and ground. The resulting mixture was then placed in a batch reactor, argon gas was introduced, the temperature was raised to 240℃ and the catalytic cracking reaction was carried out for 1 hour. After the reaction was completed, the mixture was naturally cooled to 25℃.
[0073] Example 4
[0074] 0.2 g tungsten chloride, 0.8 g zirconium chloride, 8 g methyl silicate, 3.7 g F127, 6 g 37 wt% hydrochloric acid, and 3.7 g n-butanol were added to a conical flask containing 130 mL deionized water and mixed. The mixture was stirred at 25 °C at 600 rpm for 24 h, followed by a hydrothermal reaction at 100 °C for 24 h to obtain a mixture. The solid phase was separated from the mixture by filtration, washed, and dried at 110 °C for 24 h. Then, it was calcined at 550 °C for 6 h to obtain WZr-KIT-6 (the active components are tungsten and zirconium components, the support is KIT-6, the mass percentage of the active component in WZr-KIT-6 is 11%, and the mass ratio of the tungsten component to the zirconium component is 1:3.6). 0.02 g WZr-KIT-6 and 0.08 g... The mixture was mixed with HZSM-5 molecular sieve, then mixed with 1g of polypropylene plastic and ground. The resulting mixture was then placed in a batch reactor, argon gas was introduced, the temperature was raised to 280℃ and the catalytic cracking reaction was carried out for 48h. After the reaction was completed, the mixture was naturally cooled to 25℃.
[0075] Example 5
[0076] 0.9 g ammonium metatungstate, 8 g ethyl silicate, 3.7 g P123, 6 g 37 wt% hydrochloric acid, and 3.7 g n-butanol were added to an Erlenmeyer flask containing 130 mL deionized water and mixed. The mixture was stirred at 25 °C at 600 rpm for 24 h, followed by a hydrothermal reaction at 100 °C for 24 h to obtain a mixture. The solid phase was separated from the mixture by filtration, washed, and dried at 110 °C for 24 h. Then, it was calcined at 550 °C for 7 h to obtain W-KIT-6 (the active component is tungsten, the support is KIT-6, and the mass percentage of the active component in W-KIT-6 is 22%). 0.025 g W-KIT-6 and 0.075 g... The mixture was mixed with HZSM-5 molecular sieve, then mixed with 0.3g of polyethylene plastic and ground. The resulting mixture was then placed in a batch reactor, argon gas was introduced, the temperature was raised to 240℃ and the catalytic cracking reaction was carried out for 48h. After the reaction was completed, the mixture was naturally cooled to 25℃.
[0077] Example 6
[0078] 0.9 g zirconium oxychloride, 8 g ethyl silicate, 3.7 g P123, 6 g 37 wt% hydrochloric acid, and 3.7 g n-butanol were added to an Erlenmeyer flask containing 130 mL of deionized water and mixed. The mixture was stirred at 25 °C at 600 rpm for 24 h, followed by a hydrothermal reaction at 100 °C for 24 h to obtain a mixture. The solid phase was separated from the mixture by filtration, washed, and dried at 110 °C for 24 h. Then, it was calcined at 550 °C for 5 h to obtain Zr-KIT-6 (the active component is zirconium, the support is KIT-6, and the mass percentage of the active component in Zr-KIT-6 is 13%). 0.02 g Zr-KIT-6 and 0.08 g... The mixture was mixed with HZSM-5 molecular sieve, then mixed with 0.3g of polyethylene plastic and ground. The resulting mixture was then placed in a batch reactor, argon gas was introduced, the temperature was raised to 240℃ and the catalytic cracking reaction was carried out for 48h. After the reaction was completed, the mixture was naturally cooled to 25℃.
[0079] Example 7
[0080] 2.2 g of P123 and 1.2 g of oxalic acid were added to 40 mL of 2 mol / L hydrochloric acid solution, followed by the addition of 4.58 g of ethyl silicate. The mixture was stirred at 600 rpm for 24 h at 25 °C to obtain SBA-15. Then, 1 g of SBA-15 was placed in 10 mL of 2 mol / L aluminum nitrate aqueous solution, and the pH was adjusted to 2 with 1 mol / L hydrochloric acid. The mixture was then placed in a sealed autoclave and subjected to a hydrothermal reaction at 120 °C for 24 h. The solid phase was separated from the resulting mixture by filtration, washed, and dried at 100 °C for 24 h to obtain Al-SBA-15 (the active component is aluminum, the support is SBA-15, and the mass percentage of the active component in Al-SBA-15 is 54%). 0.02 g of Al-SBA-15 and 0.08 g of... The mixture was mixed with HZSM-5 molecular sieve, then mixed with 0.3g of polyethylene plastic and ground. The resulting mixture was then placed in a batch reactor, argon gas was introduced, the temperature was raised to 240℃ and the catalytic cracking reaction was carried out for 48h. After the reaction was completed, the mixture was naturally cooled to 25℃.
[0081] Example 8
[0082] 2.2 g of P123 and 1.2 g of oxalic acid were added to 40 mL of 2 mol / L hydrochloric acid solution, followed by the addition of 4.58 g of ethyl silicate. The mixture was stirred at 600 rpm for 24 h at 25 °C to obtain SBA-15. Then, 1 g of SBA-15 was placed in 10 mL of 2 mol / L aluminum nitrate aqueous solution, and the pH was adjusted to 2 with 1 mol / L hydrochloric acid. The mixture was then placed in a sealed autoclave and subjected to a hydrothermal reaction at 120 °C for 24 h. The solid phase was separated from the resulting mixture by filtration, washed, and dried at 100 °C for 24 h to obtain Al-SBA-15. 1 g of... Al-SBA-15, 0.2 g niobic acid, 0.36 g oxalic acid, and 20 mL of water were mixed and stirred at 25 °C at 600 rpm for 16 h. The solid phase was separated from the mixture by filtration, washed, and dried at 100 °C for 24 h. Then, it was calcined at 450 °C for 5 h to obtain Nb-Al-SBA-15 (the active components are niobium and aluminum components, the support is SBA-15, the mass percentage of the active components in Nb-Al-SBA-15 is 61%, and the mass ratio of the niobium component to the aluminum component is 1:7.7). 0.02 g of Nb-Al-SBA-15 and 0.08 g of HZSM-5 molecular sieve were mixed, followed by mixing with 0.3 g of polyethylene plastic and grinding. The resulting mixture was then placed in a batch reactor, argon gas was introduced, the temperature was raised to 240 °C, and the catalytic cracking reaction was carried out for 48 h. After the reaction was completed, it was naturally cooled to 25 °C.
[0083] Example 9
[0084] 95 mL of a 0.158 g / mL tetradecyltrimethylammonium bromide aqueous solution, 2.1 g sodium aluminate, 18.7 g sodium silicate, 5.6 g 10 wt% sulfuric acid, and 15 mL of water were mixed and stirred at 600 rpm for 3 h at 25 °C. The mixture was then reacted at 100 °C for 6 days. The solid phase was separated from the resulting mixture by filtration, washed, and dried at 100 °C for 24 h to obtain Al-MCM-41 (the active component is aluminum, the support is MCM-41, and the mass percentage of the active component in Al-MCM-41 is 3%). 0.02 g of Al-MCM-41 and 0.08 g of HZSM-5 molecular sieve were mixed, followed by mixing with 0.3 g of polyethylene plastic and grinding. The resulting mixture was then placed in a batch reactor, argon gas was introduced, the temperature was raised to 240 °C, and the catalytic cracking reaction was carried out for 48 h. After the reaction, the mixture was naturally cooled to 25 °C.
[0085] Example 10
[0086] The method was implemented according to Example 1, except that the HZSM-5 molecular sieve was replaced with a β molecular sieve.
[0087] Example 11
[0088] The method of Example 1 was implemented, except that HZSM-5 molecular sieve was replaced with Mordenite molecular sieve.
[0089] Example 12
[0090] The method of Example 1 was implemented, except that HZSM-5 molecular sieve was replaced with MCM-22 molecular sieve.
[0091] Example 13
[0092] The method of Example 1 was implemented, except that polyethylene plastic was replaced with recycled powder of polyolefin plastic (PE gloves and plastic bags were dried at 80°C and then ground).
[0093] Example 14
[0094] The method was implemented according to Example 1, except that 0.02g WZr-KIT-6 and 0.08g HZSM-5 molecular sieves were replaced with 0.005g WZr-KIT-6 and 0.095g HZSM-5 molecular sieves.
[0095] Example 15
[0096] 3.2g F127, 2g 37wt% hydrochloric acid, 3g aluminum nitrate, and 2.6g zirconium oxychloride were added to 25mL anhydrous ethanol and stirred at 32℃ for 24h at a stirring rate of 600rpm. The mixed solvent was placed in a hydrothermal reactor and hydrothermally treated at 100℃ for 24h. The solid phase was then separated by filtration and dried in an oven at 60℃ for 48h. Subsequently, it was calcined at 550℃ for 5h to obtain ZrO2-Al2O3. 0.02g ZrO2-Al2O3 (the mass ratio of zirconium component to aluminum component was 1:0.29) and 0.08g HZSM-5 molecular sieve were mixed, then mixed with 0.3g polyethylene plastic and ground. The resulting mixture was then placed in a batch reactor, argon gas was introduced, the temperature was raised to 240℃, and the catalytic cracking reaction was carried out for 48h. After the reaction was completed, it was naturally cooled to 25℃.
[0097] Example 16
[0098] 0.1 g of ammonium metatungstate was dissolved in 10 mL of deionized water, and 1 g of γ-Al2O3 was added. The resulting mixture was stirred at 40 °C at a stirring rate of 600 rpm for 16 h. The solid phase was then separated by filtration and subsequently dried at 110 °C for 12 h and calcined at 450 °C for 5 h to obtain WO3-Al2O3. 0.02 g of WO3-Al2O3 (the mass ratio of tungsten component to aluminum component was 1:7.16) and 0.08 g of HZSM-5 molecular sieve were mixed, followed by mixing with 0.3 g of polyethylene plastic and grinding. The resulting mixture was then placed in a batch reactor, argon gas was introduced, the temperature was raised to 240 °C, and the catalytic cracking reaction was carried out for 48 h. After the reaction was completed, the mixture was naturally cooled to 25 °C.
[0099] Comparative Example 1
[0100] The method was implemented according to Example 1, except that 0.02g WZr-KIT-6 and 0.08g HZSM-5 molecular sieves were replaced with 0.095g WZr-KIT-6 and 0.005g HZSM-5 molecular sieves.
[0101] Comparative Example 2
[0102] The method described in Example 1 is followed, except that WZr-KIT-6 is not added, as follows:
[0103] 0.1g of HZSM-5 molecular sieve was mixed, then mixed with 0.3g of polyethylene plastic and ground. The resulting mixture was then placed in a batch reactor, argon gas was introduced, the temperature was raised to 240℃ and the catalytic cracking reaction was carried out for 48h. After the reaction was completed, it was naturally cooled to 25℃.
[0104] Comparative Example 3
[0105] The method described in Example 1 was followed, except that HZSM-5 molecular sieve was not added, as follows:
[0106] 0.1g of WZr-KIT-6 was mixed, then mixed with 0.3g of polyethylene plastic and ground. The resulting mixture was then placed in a batch reactor, argon gas was introduced, the temperature was raised to 240°C and the catalytic cracking reaction was carried out for 48 hours. After the reaction was completed, it was naturally cooled to 25°C.
[0107] Test Example 1
[0108] The WZr-KIT-6 and HZSM-5 prepared in Example 1 were characterized by transmission electron microscopy. The test methods were in accordance with the national standard GB / T 17507, as follows: Figure 1 and Figure 2 As shown, WZr-KIT-6 material has a distinct mesoporous structure, while HZSM-5 molecular sieve is a microporous material.
[0109] The WZr-KIT-6, HZSM-5, and mixtures of WZr-KIT-6 and HZSM-5 prepared in Example 1 were characterized by XRD using an X-ray diffractometer. The test methods were performed in accordance with the national standard GB / T30904-2014. Figure 3 As shown, the tungsten and zirconium components are highly dispersed on the KIT-6 support, and the crystal structure of HZSM-5 is not changed after WZr-KIT-6 is mixed with HZSM-5 molecular sieve catalyst.
[0110] The WZr-KIT-6, HZSM-5, and mixtures of WZr-KIT-6 and HZSM-5 prepared in Example 1 were subjected to low-temperature nitrogen adsorption-desorption tests. The test method referred to the national standard GB / T 5211-2008. Figure 4 As shown, WZr-KIT-6 is a mesoporous material, while HZSM-5 molecular sieve is a microporous material. The measured average pore size and specific surface area of WZr-KIT-6 and HZSM-5 are recorded in Table 1.
[0111] The WZr-KIT-6, HZSM-5, and mixtures of WZr-KIT-6 and HZSM-5 prepared in Example 1 were subjected to ammonia TPD testing. Before adsorption, 100 mg of the sample was activated in flowing helium at 300 °C for 2 h, followed by ammonia adsorption at 100 °C for 30 min, and then purged with helium for 1 h. Finally, the temperature was increased from 100 °C to 700 °C at a rate of 10 °C / min, and the TCD signal was recorded. Figure 5 As shown, the mixed catalyst has fewer strong acid sites compared to the HZSM-5 molecular sieve.
[0112] The catalysts prepared in Examples 2-16 were also characterized by transmission electron microscopy, XRD, low-temperature nitrogen adsorption-desorption test and ammonia TPD test. The results were similar to those in Example 1 and will not be repeated here. The average pore size and specific surface area of the catalysts were recorded in Table 1.
[0113] Test Example 2
[0114] The gaseous products from the reactions of Examples 1-16 and Comparative Examples 1-3 were collected using gas bags and subjected to qualitative and quantitative analysis by gas chromatography. Simultaneously, 2 mL of dichloromethane was added to a batch reactor, and the mixture was centrifuged at 10,000 rpm for solid-liquid separation. The separated liquid products were subjected to qualitative and quantitative analysis by gas chromatography-mass spectrometry and gas chromatography, following the national standard GB / T 30431-2020. The separated solid products were dried at 120°C for 12 hours. The plastic conversion rate and gasoline yield were calculated and recorded in Table 2. The calculation formulas are: Plastic conversion rate = ((initial plastic mass - remaining plastic mass) / initial plastic mass), Gasoline yield = (gasoline mass / (initial plastic mass - remaining plastic mass)).
[0115] Stability test
[0116] The WZr-KIT-6 and HZSM-5 molecular sieves prepared in Example 1 were mixed, then mixed with 0.3g of polyethylene plastic and ground. The resulting mixture was then placed in a batch reactor, argon gas was introduced, the temperature was raised to 240℃, and the catalytic cracking reaction was carried out for 12 hours. After the reaction, it was naturally cooled to 25℃. The gaseous products after the reaction were collected using gas bags and subjected to gas chromatography for qualitative and quantitative analysis. At the same time, 2mL of dichloromethane was added to the batch reactor, and then the liquid was removed and centrifuged at 10000rpm for solid-liquid separation. The separated liquid products were subjected to gas chromatography-mass spectrometry and gas chromatography for qualitative and quantitative analysis, and the test methods were in accordance with the national standard GB / T 30431-2020. The separated solid products were dried at 120℃ for 12 hours, and the plastic conversion rate was calculated. The above operation was repeated 4 times for catalytic cracking of polyethylene plastic after calcining the separated solid products at 550℃ for 5 hours, and the plastic conversion rate was recorded. Figure 6 .
[0117] from Figure 6 As can be seen, according to the method for preparing gasoline using plastics as described in this invention, the catalyst can still maintain its initial performance after multiple reactions, recycling, and regeneration.
[0118] In this paper, the content of active components in the catalysts in Examples 1-16 was determined by inductively coupled plasma (ICP) testing, and the testing method was based on the national standard GB / T 13747.26-2022.
[0119] Table 1
[0120] catalyst Average pore size (nm) <![CDATA[Specific surface area (m 2 / g)]]> WZr-KIT-6 in Example 1 4.6 460 WZr-KIT-6 in Example 2 5.0 480 WZr-KIT-6 in Example 3 5.4 490 WZr-KIT-6 in Example 4 7.7 500 W-KIT-6 in Example 5 5.8 540 Zr-KIT-6 in Example 6 4.2 670 Al-SBA-15 in Example 7 5.6 700 Nb-Al-SBA-15 in Example 8 5.8 680 Al-MCM-41 in Example 9 6.0 650 HZSM-5 molecular sieve 2.4 350 β-molecular sieve 2.2 530 Mordenite molecular sieve 2.2 440 MCM-22 molecular sieve 2.3 490 <![CDATA[ZrO2-Al2O3 in Example 15]]> 4.6 130 <![CDATA[WO3-Al2O3 in Example 16]]> 4.7 200
[0121] Table 2
[0122] serial number Gasoline production rate (%) Plastic conversion rate (%) Example 1 88.0 95.2 Example 2 60.7 69.8 Example 3 56.0 63.0 Example 4 69.8 76.1 Example 5 70.2 78.6 Example 6 72.0 79.6 Example 7 59.8 70.4 Example 8 60.2 71.0 Example 9 59.8 65.0 Example 10 77.2 87.8 Example 11 57.8 68.0 Example 12 56.4 69.1 Example 13 82.2 90.0 Example 14 85.7 96.5 Example 15 50.5 60.4 Example 16 45.0 54.0
[0123] As can be seen from the results in Table 2, Examples 1-16 of the method for preparing gasoline using plastics according to the present invention have high gasoline yield and plastic conversion rate.
[0124] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A method for preparing gasoline using plastic, characterized in that, The method includes: catalytically cracking polyolefin plastics under an inert atmosphere in the presence of a first catalyst and a second catalyst. The first catalyst contains an active component and a support, wherein the active component is at least one selected from tungsten, zirconium, aluminum and niobium, and the support is a mesoporous molecular sieve. The second catalyst is a microporous silica-alumina molecular sieve; The mass ratio of the first catalyst to the second catalyst is 1:(0.25-20); The mesoporous molecular sieve is at least one of KIT-6, MCM-41 and SBA-15; The second catalyst is at least one of β-zeolite, Mordenite, MCM-22, and HZSM-5. The conditions for the catalytic cracking reaction include: a temperature of 220-280℃ and a time of 1-48h.
2. The method according to claim 1, characterized in that, The mass ratio of the first catalyst to the second catalyst is 1:(0.25-4).
3. The method according to claim 1 or 2, characterized in that, The mass ratio of the total mass of the first catalyst and the second catalyst to the amount of the polyolefin plastic is (0.1-1):
1.
4. The method according to claim 1 or 2, characterized in that, The polyolefin plastic is polyethylene plastic and / or polypropylene plastic.
5. The method according to claim 1 or 2, characterized in that, The ratio of the average pore size of the first catalyst to that of the second catalyst is (1.75-3.2):
1.
6. The method according to claim 1, characterized in that, The first catalyst contains an active component and a support, wherein the active component accounts for 1.15%-62.59% of the mass of the first catalyst.
7. The method according to claim 1, characterized in that, The first catalyst contains an active component and a support, wherein the active component is a tungsten component and a zirconium component, and the support is KIT-6.
8. The method according to claim 7, characterized in that, The active component accounts for 8.3%-51.62% of the mass of the first catalyst; and / or, The mass ratio of the tungsten component to the zirconium component is 1:(0.08-4).
9. The method according to claim 7 or 8, characterized in that, The method further includes preparing the first catalyst by following these steps: mixing and stirring a tungsten source, a zirconium source, a silicon source, a template agent, hydrochloric acid, n-butanol, and water, followed by a hydrothermal reaction to obtain a mixture, separating the solid phase from the mixture, and calcining it.
10. The method according to claim 9, characterized in that, The tungsten source is ammonium metatungstate and / or tungsten chloride; and / or, The zirconium source is at least one selected from zirconium oxychloride, zirconium chloride, zirconium nitrate, and zirconium sulfate; and / or, The silicon source is ethyl silicate and / or methyl silicate; and / or, The template agent is P123 and / or F127; and / or, The ratio of the amounts of the tungsten source, the zirconium source, the silicon source, the template agent, the hydrochloric acid, the n-butanol, and the water is (0.2-1.8) g : (0.4-1.8) g : (6-10) g : (3.5-4) g : (5-8) g : (3.5-4) g : 130 mL; and / or, The concentration of the hydrochloric acid is 30wt%-38wt%; and / or, The conditions for the hydrothermal reaction include: a temperature of 90-110℃ and a time of 20-30 hours; and / or, The calcination conditions include a temperature of 550-750℃ and a time of 5-8 hours.
11. The method according to claim 1, 2, 6, 7 or 8, characterized in that, The second catalyst is HZSM-5 molecular sieve.
12. The method according to claim 1, 2, 6, 7 or 8, characterized in that, The catalytic cracking reaction is carried out in a batch reactor.
Citation Information
Patent Citations
Waste plastic cracking catalyst as well as preparation method and application thereof
CN115672391A
Method for preparing aromatic hydrocarbon-rich bio-oil through synergistic pyrolysis of biomass and waste plastics
CN116179234A