Highly transparent pe / pa asymmetric film and method for preparing the same
By optimizing the layer structure and material ratio of the PE/PA asymmetric film, the problem of light scattering by microcrystals in the PA layer was solved, achieving high transparency and excellent mechanical properties, making it suitable for high-end packaging and optical applications.
Patent Information
- Application Number
- CN202411744112.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-30
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-11-30
AI Technical Summary
Traditional PE/PA asymmetric films suffer from poor transparency due to the scattering of light by the microcrystalline structure of the PA layer, which affects their performance in high-end packaging and optical applications.
A layered structure of PA/TIE/LLD/LLD/LD/TIE/PA/TIE/LLD is adopted. By rationally proportioning the materials of each layer, the TIE layer acts as a bonding layer to enhance adhesion. Combined with materials such as modified glass fiber and modified diatomaceous earth, the weight ratio and thickness range of each layer are optimized to reduce interface discontinuities and defects.
It improves the transparency, chemical stability, and mechanical strength of PE/PA asymmetric films, making them suitable for transparent protective layers and protective layers for optical sensors, and possessing excellent mechanical and barrier properties.
Smart Images

Figure BDA0005163221900000101
Abstract
Description
Technical Field
[0001] This application relates to the technical field of polymer materials, and in particular to a highly transparent PE / PA asymmetric film and its preparation method. Background Technology
[0002] PE / PA membranes are membrane materials composed of polyethylene (PE) and polyamide (PA, also known as nylon). Based on their structural characteristics, they can be divided into two main categories: symmetrical membranes and asymmetrical membranes. Symmetrical membranes have a symmetrical structure, such as a structure with PA in the middle and PE on both sides. Asymmetrical membranes, on the other hand, are characterized by asymmetry in their structure, such as an asymmetrical seven-layer co-extruded nylon membrane with a structure like PE / TIE / PE / PA / PE / TIE / PA.
[0003] Due to its excellent physical and processing properties, PE / PA asymmetric film has been widely used in the packaging and optical industries. PE / PA asymmetric film is a film co-extruded from different plastic materials. It has properties such as high barrier properties, oil resistance, moisture resistance, high temperature resistance, and low temperature resistance. It is suitable for packaging food, industrial and medical products. Its basic structure is PE / TIE / PE / PA / TIE / PE / PA, and the thickness ranges from 0.35 to 0.50 mm.
[0004] Traditional PE / PA asymmetric films tend to have PA that easily forms microcrystals. These microcrystal structures scatter light, thereby reducing the film's transparency and affecting its performance in high-end packaging and optical applications. Summary of the Invention
[0005] To improve the poor transparency of PE / PA asymmetric films, this application provides a highly transparent PE / PA asymmetric film and its preparation method.
[0006] This application provides a highly transparent PE / PA asymmetric film, employing the following technical solution: A highly transparent PE / PA asymmetric film has a structure of PA / TIE / LLD / LLD / LD / TIE / PA / TIE / LLD with an interlayer weight ratio of 0.125-0.131:0.064-0.070:0.073-0.079:0.073-0.079:0.218-0.224:0.064-0.070:0.103-0.109:0.064-0.070:0.189-0.195.
[0007] By adopting the above technical solution and using a reasonable ratio of PE and PA, high optical transparency of the film is achieved. The PA layer has excellent density, chemical resistance, and heat resistance, while the PE layer has excellent mechanical strength, stability, and transparency. The prepared PE / PA asymmetric film has good transparency, chemical stability, heat resistance, and mechanical strength, and is widely used in transparent protective layers, protective layers for optical sensors, and separation functions.
[0008] Further limiting the weight ratios of PA, TIE, LLD, LD, PA, and LLD ensures suitable thickness ranges for each layer. The coordinated structure of each layer reduces discontinuities and defects at the interfaces, thereby reducing light scattering and improving transparency. Additionally, the TIE layer acts as a bonding layer, enhancing adhesion between different polymer layers, reducing interlayer delamination, and thus improving the overall transparency of the film.
[0009] Preferably, the interlayer weight ratio of PA / TIE / LLD / LLD / LD / TIE / PA / TIE / LLD is 0.128:0.067:0.076:0.076:0.221:0.067:0.106:0.067:0.192.
[0010] By adopting the above technical solution, the weight ratio of each layer of PA / TIE / LLD / LLD / LD / TIE / PA / TIE / LLD is further defined as a point value. When the weight ratio between PA / TIE / LLD / LLD / LD / TIE / PA / TIE / LLD is this value ratio, the obtained PE / PA asymmetric film has the best mechanical properties, mechanical properties and transparency.
[0011] Preferably, the raw materials of the LD layer, by weight, include the following: 60-70 parts of low-density polyethylene, 15-20 parts of modified glass fiber, 10-13 parts of modified diatomaceous earth, 5-8 parts of polytetrafluoroethylene, 5-8 parts of maleic anhydride-grafted polyolefin elastomer, and 2-3 parts of disulfide phase.
[0012] By adopting the above technical solutions, low-density polyethylene (LD) exhibits good flexibility, high impact resistance, chemical stability, and good transparency, making the LD layer less prone to breakage under external forces and resistant to the erosion of various chemical substances. Modified glass fiber, with its high modulus and high strength, can form a reinforcing skeleton within the LD matrix, allowing the composite material to better distribute stress under load, thereby improving tensile strength, flexural strength, and compressive strength. The high hardness of modified glass fiber also enhances the wear resistance of the LD layer, reducing material loss during friction and wear. Modified diatomaceous earth, with its numerous, orderly arranged micropores, high porosity, and large specific surface area, combined with modified glass fiber, improves the modulus and flexural strength of the LD layer, enhancing the mechanical properties of the system. Furthermore, the microporous structure of modified diatomaceous earth can act as a barrier layer, improving the LD material's barrier performance against gases and moisture.
[0013] Polytetrafluoroethylene (PTFE) can improve the durability, weather resistance, and barrier properties of LD materials, ensuring stable performance in outdoor and harsh environments and reducing aging and degradation. Maleic anhydride-grafted polyolefin elastomers act as compatibilizers, promoting chemical bonding between different polymers, reducing phase separation, avoiding the formation of opaque phase interfaces, and improving the adhesion and mechanical properties of the LD layer. Maleic anhydride-grafted polyolefin elastomers also improve the dispersibility of other components in the LD layer, reducing the aggregation of opaque particles and thus increasing transparency. Furthermore, they can optimize the refractive index of the LD layer, control crystallinity and crystal morphology, and reduce light reflection and scattering at different phase interfaces, thereby improving transparency. The disulfide phase possesses excellent lubricating properties, significantly reducing the coefficient of friction of the LD layer, reducing wear, and improving the sliding properties of the material, which is beneficial for subsequent processing and application of the LD layer.
[0014] Preferably, the method for preparing the modified glass fiber includes the following steps: (1) Cut the glass fiber to a length of 1-2 mm, then disperse it in deionized water, add silane coupling agent, stir at 60-65℃ for 10-15 min, filter, dry, and obtain pretreated glass fiber; (2) Wash the straw powder with anhydrous ethanol 2-3 times, then disperse it in NaOH solution and soak for 20-25 minutes at a soaking temperature of 70-75℃. Wash with water, filter and dry to obtain pretreated straw powder. (3) Coat the surface of the pretreated glass fiber in step (1) with modified chitosan solution, then spray the pretreated straw powder in step (2) evenly onto the surface of the glass fiber, and dry it to obtain modified glass fiber.
[0015] By adopting the above technical solution, the glass fiber is first cut and then mixed with a silane coupling agent. The silicon-oxygen-silicon bonds formed after the silane coupling agent reacts with the surface of the glass fiber can firmly connect the glass fiber and other components, improve the interfacial bonding strength, and make the composite material have high mechanical properties.
[0016] Treating straw powder with NaOH solution alters the chemical properties of the straw surface, increases reaction sites, facilitates subsequent chemical modification, improves the interfacial bonding between straw powder and matrix materials, and thus improves the performance of composite materials.
[0017] A modified chitosan solution is coated onto the surface of pretreated glass fibers, forming a thin film of modified chitosan on the glass fibers. Then, pretreated straw powder is evenly sprayed onto the surface of the glass fibers. The straw powder can adhere to the surface of the glass fibers, improving the mechanical properties of the modified fibers. The high strength and high modulus of the glass fibers, combined with the biocompatibility of chitosan and the natural cellulose structure of the straw powder, produce a composite material with excellent mechanical properties. The resulting composite material has good biocompatibility, corrosion resistance, flame retardancy and thermal stability.
[0018] Preferably, the mass ratio of the glass fiber, modified chitosan solution, and pretreated straw powder is 1:0.04-0.06:0.1-0.3.
[0019] By adopting the above technical solution, the mass ratio of glass fiber, modified chitosan solution, and pretreated straw powder is further limited within a certain range, improving the mechanical properties, stability, and wear resistance of the glass fiber. The modified chitosan solution can coat the glass fiber, forming a thin film on its surface. The pretreated straw powder can adhere to the glass fiber surface. The modified chitosan solution has a certain viscosity, allowing the pretreated straw powder to adhere stably to the glass fiber surface, thus improving the mechanical properties of the glass fiber. When subsequently applied to PE films, this enhances the mechanical properties of the PE film, increasing its tensile strength and modulus, making it more robust under external forces. Furthermore, the addition of chitosan and glass fiber can improve the barrier properties of the PE film, reducing gas and moisture permeation and improving its thermal stability, allowing it to maintain good performance even at high temperatures.
[0020] Preferably, the method for preparing the modified chitosan solution includes the following steps: dissolving chitosan in acetic acid solution, magnetically stirring at room temperature until the chitosan is completely dissolved, then adding sodium alginate and hydroxymethyl cellulose, stirring at 80-85℃ for 30-35 minutes, and allowing to stand to obtain the modified chitosan solution.
[0021] By employing the above technical solution, chitosan is dispersed in an acetic acid solution and stirred evenly. Sodium alginate and hydroxymethyl cellulose are then added. Electrostatic attraction occurs between the primary amino groups of chitosan and the carboxyl groups of sodium alginate. Sodium alginate forms a composite gel with chitosan through electrostatic interaction, enhancing the material's network structure and thus improving viscosity. Hydroxymethyl cellulose can physically crosslink with both chitosan and sodium alginate to form a composite gel. The hydroxyl groups of hydroxymethyl cellulose can form hydrogen bonds with the amino groups of chitosan, increasing the material's viscosity. The hydroxyl groups of hydroxymethyl cellulose can also form hydrogen bonds with the carboxylic acid groups of sodium alginate, enhancing intermolecular attraction and thus improving the mixture's viscosity. The mixture of chitosan, sodium alginate, and hydroxymethyl cellulose has a synergistic effect, increasing the system's stability, mechanical properties, and viscosity. This subsequently leads to tighter adhesion between glass fiber and straw powder, improving the overall performance of the glass fiber.
[0022] Preferably, the method for preparing the modified diatomaceous earth includes the following steps: (1) Calcine the diatomaceous earth at 300-320℃ for 50-60 min, grade and finely crush it, then disperse it in sodium oxalate solution, stir for 16-20 min, filter, and dry to obtain pretreated diatomaceous earth; (2) Disperse titanium dioxide in deionized water, add fatty alcohol polyoxyethylene ether and dispersant MF, stir evenly, filter, and dry to obtain pretreated titanium dioxide. (3) Disperse the pretreated diatomaceous earth from step (1) in deionized water, add the pretreated titanium dioxide and modified starch from step (2), stir at 80-85℃ for 1-2 hours, and dry to obtain modified diatomaceous earth.
[0023] By employing the above technical solutions, calcination of diatomaceous earth alters its particle structure and surface properties, making it more porous and improving its adsorption performance, purity, and stability. Mixing sodium oxalate with diatomaceous earth changes its surface properties, enhancing its adsorption capacity. The addition of sodium oxalate increases the negative charge on the diatomaceous earth surface, giving it a stronger adsorption capacity for positively charged pollutants.
[0024] Fatty alcohol polyoxyethylene ethers can adsorb onto the surface of titanium dioxide particles, forming a protective film to prevent particle re-agglomeration during processing and storage, thereby enhancing the stability of the system. Dispersant MF reduces the surface tension between titanium dioxide particles, preventing particle agglomeration and improving the dispersibility of titanium dioxide in the system. The synergistic effect of dispersant MF and fatty alcohol polyoxyethylene ethers can improve the processing performance of titanium dioxide in the polymer matrix, increase flowability, and make titanium dioxide easier to distribute uniformly in the matrix, exhibiting good dispersibility.
[0025] Pretreated titanium dioxide can be loaded onto the surface and pores of pretreated diatomaceous earth, improving its adsorption, covering power, and air permeability. Modified starch has certain viscosity and film-forming properties, which enables titanium dioxide to adhere to the surface of diatomaceous earth, improving the performance stability of modified diatomaceous earth. The resulting diatomaceous earth has excellent mechanical properties, adsorption, covering power, and air permeability.
[0026] Preferably, the mass ratio of diatomaceous earth, titanium dioxide and modified starch is 1:0.3-0.4:0.1-0.2.
[0027] By adopting the above technical solution, the mass ratio of diatomaceous earth, titanium dioxide, and modified starch is further limited within a certain range. Titanium dioxide has high hiding power and good optical properties, while diatomaceous earth has a porous structure and high adsorption capacity. Titanium dioxide can be loaded onto the surface and within the pores of diatomaceous earth, improving its hiding power, optical properties, adsorption capacity, and air permeability. Modified starch has excellent viscosity and adsorption properties, enabling titanium dioxide to be stably loaded into the diatomaceous earth structure, further improving the mechanical properties, stability, and mechanical strength of diatomaceous earth, and subsequently improving the corresponding properties of the PE layer.
[0028] Preferably, the method for preparing the modified starch includes the following steps: dispersing starch in sodium hydroxide solution, reacting at 40-45℃ for 4-5 hours, centrifuging, discarding the supernatant, adding water, shaking well, centrifuging again, filtering, and drying to obtain pretreated starch, then dispersing it in deionized water, adding nano-calcium carbonate and xanthan gum, stirring at 60-65℃, drying, and grinding to obtain modified starch.
[0029] By employing the above technical solution, starch is mixed with sodium hydroxide solution to obtain pretreated starch. Sodium hydroxide can induce internal breakage and cross-linking of starch molecules, transforming the starch molecules from a granular structure to a homogeneous gel-like structure, thus increasing the viscosity of the pretreated starch. Nano-calcium carbonate can be uniformly dispersed in the starch system, forming heterogeneous nucleation, improving the crystallinity of the system, and enhancing its resistance to thermal decomposition and heat distortion. The interaction between xanthan gum and starch molecules can alter the microstructure of the starch paste, forming hydrogen bonds or chain entanglements, thereby increasing the viscosity of the starch system. The mixed use of xanthan gum and nano-calcium carbonate can promote the dispersion of nano-calcium carbonate in the matrix, improving the stability of the system. The viscosity of xanthan gum can prevent the agglomeration of nano-calcium carbonate, ensuring its uniform distribution in the matrix, thereby optimizing the material's performance and significantly improving the mechanical properties of the composite material, such as impact strength and flexural strength. The mixture of starch, nano-calcium carbonate, and xanthan gum has a synergistic effect, resulting in modified starch with good mechanical properties, viscosity, and processing performance, which in turn helps to improve the properties of diatomaceous earth and titanium dioxide, and subsequently modify the corresponding properties of the PE layer.
[0030] Secondly, this application also provides a method for preparing a high-transparency PE / PA asymmetric film, comprising the following steps: melting and plasticizing PA resin, TIE resin, LLD resin, LLD resin, LD resin, TIE resin, PA resin, TIE resin, and LLD resin in different extruders respectively; extruding the molten resin into the same die head; uniformly distributing the resin in the die head according to a certain interlayer structure; and obtaining an asymmetric nine-layer co-extruded nylon film by blowing, cooling, shaping, and winding through a nine-layer blown film equipment.
[0031] By adopting the above technical solution and preparation method, the operation is simple and the process time is short, which helps to improve the production efficiency of preparing high-transparency PE / PA asymmetric films. The obtained high-transparency PE / PA asymmetric films have good mechanical properties.
[0032] In summary, this application has the following beneficial effects: 1. In this application, a high optical transparency of the film is achieved by using a reasonable ratio of PE and PA. The PA layer has excellent density, chemical resistance, and heat resistance, while the PE layer has excellent mechanical strength, stability, and transparency. The prepared PE / PA asymmetric film has good transparency, chemical stability, heat resistance, and mechanical strength.
[0033] 2. This application specifies the weight ratio between PA, TIE, LLD, LD, PA, and LLD to ensure that each layer has a suitable thickness range. The combination of the structure of each layer can reduce discontinuities and defects at the interface, thereby reducing light scattering and improving transparency.
[0034] 3. In this application, the TIE layer serves as an adhesive layer, which enhances the adhesion between different polymer layers, reduces interlayer peeling, and thus improves the overall transparency of the film. Detailed Implementation
[0035] The present application will be further described in detail below with reference to the embodiments.
[0036] The raw materials used in the examples and comparative examples are all commercially available.
[0037] Preparation example of modified glass fiber Preparation Example 1-1 The preparation method of modified glass fiber includes the following steps: (1) Cut 1.2 kg of glass fiber to a length of 1-2 mm, then disperse it in 2 L of deionized water, add silane coupling agent KH-550, stir at 65℃ for 12 min, filter, dry, and obtain pretreated glass fiber; (2) Wash 0.8 kg of straw powder three times with anhydrous ethanol, then disperse it in 1.5 L of 30% NaOH solution and soak for 25 min at a soaking temperature of 75 °C. Wash with water, filter and dry to obtain pretreated straw powder. (3) Coat the surface of the pretreated glass fiber in step (1) with modified chitosan solution, then spray the pretreated straw powder in step (2) evenly onto the surface of the glass fiber, and dry it to obtain modified glass fiber.
[0038] The mass ratio of glass fiber, modified chitosan solution, and pretreated straw powder was 1:0.04:0.1.
[0039] The preparation method of modified chitosan solution includes the following steps: dissolve 1 kg of chitosan in 2 L of 5% acetic acid solution, stir magnetically at room temperature until the chitosan is completely dissolved, then add 0.3 kg of sodium alginate and 0.1 kg of hydroxymethyl cellulose, stir at 85℃ for 35 min, and let stand to obtain modified chitosan solution.
[0040] Preparation Examples 1-2 The difference from preparation example 1-1 is that straw powder is not added in step (2).
[0041] Preparation Examples 1-3 The difference from Preparation Example 1-1 is that in step (3), no modified chitosan solution is added.
[0042] Preparation Examples 1-4 The difference from Preparation Example 1-1 is that the mass ratio of glass fiber, modified chitosan solution and pretreated straw powder is 1:0.06:0.3.
[0043] Preparation Examples 1-5 The difference from Preparation Example 1-1 is that the mass ratio of glass fiber, modified chitosan solution and pretreated straw powder is 1:0.01:0.6.
[0044] Preparation Examples 1-6 The difference from Preparation Example 1-1 is that sodium alginate is not added in the preparation method of the modified chitosan solution.
[0045] Preparation Examples 1-7 The difference from Preparation Example 1-1 is that hydroxymethyl cellulose is not added in the preparation method of the modified chitosan solution.
[0046] Preparation example of modified diatomaceous earth Preparation Example 2-1 The preparation method of modified diatomaceous earth includes the following steps: (1) 1.8 kg of diatomaceous earth was calcined at 320℃ for 55 min, then put into an air jet mill for classification and fine crushing, and then dispersed in 2.5 L of sodium oxalate solution with a mass fraction of 55%, stirred for 20 min, filtered, and dried to obtain pretreated diatomaceous earth. (2) Disperse titanium dioxide in 1.2L of deionized water, add 0.05kg of fatty alcohol polyoxyethylene ether and 0.04kg of dispersant MF, stir evenly, filter, and dry to obtain pretreated titanium dioxide; (3) Disperse the pretreated diatomaceous earth from step (1) in 4.5L of deionized water, add the pretreated titanium dioxide and modified starch from step (2), stir at 85℃ for 1.5h, and dry to obtain modified diatomaceous earth.
[0047] The mass ratio of diatomaceous earth, titanium dioxide, and modified starch is 1:0.3:0.2.
[0048] The method for preparing modified starch includes the following steps: 0.9 kg of starch is dispersed in 1.5 L of 0.8% sodium hydroxide solution, reacted at 45 °C for 5 h, centrifuged, the supernatant is discarded, water is added and shaken well, centrifuged again, filtered and dried to obtain pretreated starch, which is then dispersed in 3 L of deionized water, 0.1 kg of nano-calcium carbonate and 0.08 kg of xanthan gum are added, stirred at 65 °C, dried, and ground to obtain modified starch.
[0049] Preparation Example 2-2 The difference from preparation example 2-1 is that titanium dioxide is not added in step (2).
[0050] Preparation Examples 2-3 The difference from preparation example 2-1 is that no modified starch is added in step (3).
[0051] Preparation Examples 2-4 The difference from Preparation Example 2-1 is that the mass ratio of diatomaceous earth, titanium dioxide and modified starch is 1:0.4:0.1.
[0052] Preparation Examples 2-5 The difference from Preparation Example 2-1 is that the mass ratio of diatomaceous earth, titanium dioxide and modified starch is 1:0.1:0.5.
[0053] Preparation Examples 2-6 The difference from Preparation Example 2-1 is that nano-calcium carbonate is not added in the preparation method of modified starch.
[0054] Preparation Examples 2-7 The difference from Preparation Example 2-1 is that xanthan gum is not added in the preparation method of the modified starch. Example
[0055] Example 1 A highly transparent PE / PA asymmetric film with the structure PA / TIE / LLD / LLD / LD / TIE / PA / TIE / LLD; The interlayer weight ratio of PA / TIE / LLD / LLD / LD / TIE / PA / TIE / LLD is 0.128:0.067:0.076:0.076:0.221:0.067:0.106:0.067:0.192, where the weight of LD is 1 kg.
[0056] The preparation method of the above-mentioned high-transparency PE / PA asymmetric film includes the following steps: 1.5 kg PA resin, 0.5 kg TIE resin, 1.2 kg LLD resin, 1.2 kg LLD resin, 1.3 kg LD resin, 0.5 kg TIE resin, 1.5 kg PA resin, 0.5 kg TIE resin, and 1.2 kg LLD resin are melted and plasticized in different extruders. The molten resin is extruded into the same die and evenly distributed in the die according to a certain interlayer structure. The film is then blown, cooled, shaped, and wound up using a nine-layer blown film equipment to obtain an asymmetric nine-layer co-extruded nylon film. Among them, the blown film temperature is 210°C, the longitudinal stretching is 3 times, the transverse stretching is 4 times, the stretching temperature is 80°C, and the blow-up ratio is 1.5.
[0057] PA resin was purchased from Dongguan Baojia Plastics Co., Ltd.; TIE resin, which is EVA modified adhesive resin, was purchased from Dongguan Taotao Plastic Raw Materials Co., Ltd.; LLD resin, which is linear low-density polyethylene, was purchased from Shanghai Youcheng International Trade Co., Ltd.; and LD resin, which is low-density polyethylene, was purchased from Yuyao Deyi Plastics Co., Ltd.
[0058] The interlayer thicknesses of PA / TIE / LLD / LLD / LD / TIE / PA / TIE / LLD are 4μm, 3μm, 4μm, 4μm, 5μm, 3μm, 4μm, 3μm, and 4μm, respectively.
[0059] Example 2 A highly transparent PE / PA asymmetric film differs from Example 1 in that the interlayer weight ratio is 0.125:0.064:0.073:0.073:0.218:0.070:0.109:0.064:0.195.
[0060] Example 3 A highly transparent PE / PA asymmetric film differs from Example 1 in that the interlayer weight ratio is 0.131:0.070:0.079:0.079:0.224:0.064:0.103:0.070:0.189.
[0061] Example 4 A highly transparent PE / PA asymmetric film differs from Example 1 in that the raw materials of the LD layer, by weight, include the following: 60 kg of low-density polyethylene, 15 kg of modified glass fiber, 10 kg of modified diatomaceous earth, 5 kg of polytetrafluoroethylene, 5 kg of maleic anhydride-grafted polyolefin elastomer, and 3 kg of disulfide phase.
[0062] The modified glass fiber was prepared using Preparation Example 1-1; the modified diatomaceous earth was prepared using Preparation Example 2-1.
[0063] Example 5 A highly transparent PE / PA asymmetric film differs from Example 4 in that the raw materials of the LD layer, by weight, include the following: 70 kg of low-density polyethylene, 20 kg of modified glass fiber, 13 kg of modified diatomaceous earth, 8 kg of polytetrafluoroethylene, 8 kg of maleic anhydride-grafted polyolefin elastomer, and 2 kg of disulfide phase.
[0064] Example 6 A highly transparent PE / PA asymmetric film, which differs from Example 4 in that the modified glass fiber is prepared using Preparation Examples 1-2.
[0065] Example 7 A highly transparent PE / PA asymmetric film, which differs from Example 4 in that the modified glass fiber is prepared using Preparation Examples 1-3.
[0066] Example 8 A highly transparent PE / PA asymmetric film, which differs from Example 4 in that the modified glass fiber is prepared using Preparation Examples 1-4.
[0067] Example 9 A highly transparent PE / PA asymmetric film, which differs from Example 4 in that the modified glass fiber is prepared using Preparation Examples 1-5.
[0068] Example 10 A highly transparent PE / PA asymmetric film, which differs from Example 4 in that the modified glass fiber is prepared using Preparation Examples 1-6.
[0069] Example 11 A highly transparent PE / PA asymmetric film, which differs from Example 4 in that the modified glass fiber is prepared using Preparation Examples 1-7.
[0070] Example 12 A highly transparent PE / PA asymmetric film, which differs from Example 4 in that the modified diatomaceous earth is prepared using Preparation Example 2-2.
[0071] Example 13 A highly transparent PE / PA asymmetric film, which differs from Example 4 in that the modified diatomaceous earth is prepared using Preparation Examples 2-3.
[0072] Example 14 A highly transparent PE / PA asymmetric film, which differs from Example 4 in that the modified diatomaceous earth is prepared using Preparation Examples 2-4.
[0073] Example 15 A highly transparent PE / PA asymmetric film, which differs from Example 4 in that the modified diatomaceous earth is prepared using Preparation Examples 2-5.
[0074] Example 16 A highly transparent PE / PA asymmetric film, which differs from Example 4 in that the modified diatomaceous earth is prepared using Preparation Examples 2-6.
[0075] Example 17 A highly transparent PE / PA asymmetric film, which differs from Example 4 in that the modified diatomaceous earth is prepared using Preparation Examples 2-7.
[0076] Comparative Example Comparative Example 1 A highly transparent PE / PA asymmetric film differs from Example 1 in that the interlayer weight ratio is 0.115:0.053:0.071:0.071:0.202:0.053:0.100:0.053:0.180.
[0077] Comparative Example 2 A highly transparent PE / PA asymmetric film differs from Example 1 in that the interlayer weight ratio is 0.138:0.085:0.082:0.082:0.229:0.085:0.111:0.085:0.199.
[0078] Performance testing The high-transparency PE / PA asymmetric films prepared in Examples 1-17 and Comparative Examples 1-2 were subjected to performance tests. Tensile strength and elongation at break were tested according to GB / T1040.3-2006; puncture force and dart impact tests were conducted according to GB / T9639.1-2008 and GB / T10004-2008; and the average mixed gas permeability (the main components of the mixed gas are oxygen and nitrogen) was tested according to GB / T1038-2000 (unit: 10 μm (g / m²)). 2 • 24h); The absorption performance of the thin film in the visible light region was tested using a UV-2600I UV spectrophotometer (SHIMADZU Japan) at a wavelength of 600nm. The test results are shown in Table 1.
[0079] Table 1 Test data for the examples and comparative examples As shown in Table 1, the highly transparent PE / PA asymmetric films prepared in Examples 1-3 of this application possess good mechanical properties, barrier properties, transparency, and mechanical strength. Specifically, Example 1 exhibits a longitudinal tensile strength of 42.5 MPa, a transverse tensile strength of 34.2 MPa, a longitudinal elongation at break of 397.2%, a transverse elongation at break of 521.3%, a film puncture force of 1.781 N, a dart impact mass of 689 g, a mixed gas transmittance of 312.5 ± 2.3 10 μm (g / m²·24h), and a light transmittance of 92%. This indicates that the prepared highly transparent PE / PA asymmetric films possess good mechanical properties and strength. The coordinated structure of each layer reduces discontinuities and defects at the interface, thereby reducing light scattering and improving transparency. Furthermore, the PE / PA asymmetric films exhibit good barrier properties, effectively blocking oxygen, nitrogen, and other gases from the environment.
[0080] The raw materials for the PE layer in Examples 4-5 were prepared in-house according to this application. Compared with Example 1, the obtained PE / PA asymmetric film has better mechanical properties, barrier properties and transparency, indicating that the modified glass fiber and modified diatomaceous earth used in this application improve the mechanical properties of the PE layer, while still maintaining high transparency.
[0081] In Examples 6-7, the modified glass fiber preparation methods did not include straw powder and modified chitosan solution. In Examples 8-9, the mass ratio of glass fiber, modified chitosan solution, and pretreated straw powder was changed. As shown in Table 1, the performance test results of tensile strength, elongation at break, film puncture force, dart impact mass, and mixed gas permeability of Examples 6-7 were significantly worse than those of Examples 4-5. The performance test results of tensile strength, elongation at break, film puncture force, dart impact mass, and mixed gas permeability of Example 9 were better than those of Examples 5-7, but worse than those of Examples 4-5 and Example 8. This indicates that the modified chitosan solution can coat the glass fiber, and the pretreated straw powder can adhere to the surface of the glass fiber. The modified chitosan solution enables the pretreated straw powder to adhere stably to the surface of the glass fiber, improving the mechanical properties of the glass fiber. When subsequently applied to PE film, it enhances the mechanical properties of the PE film. Moreover, the addition of chitosan and glass fiber can improve the barrier properties of the PE film, reduce the permeation of gas and moisture, and improve the barrier properties of the PE film.
[0082] In the preparation methods of the modified chitosan solutions in Examples 10-11, sodium alginate and hydroxymethyl cellulose were not added. As shown in Table 1, the performance test results of tensile strength, elongation at break, film puncture force, dart impact mass, and mixed gas permeability of Examples 10-11 were significantly worse than those of Examples 4-5, but better than those of Example 7. This indicates that the mixture of chitosan, sodium alginate, and hydroxymethyl cellulose has a synergistic effect, which increases the stability, mechanical properties, and viscosity of the system. Subsequently, it makes the glass fiber and straw powder adhere tightly, thereby increasing the comprehensive performance of the glass fiber.
[0083] In Examples 12-13, the preparation methods of modified diatomaceous earth did not include titanium dioxide or modified starch. In Examples 14-15, the mass ratio of diatomaceous earth, titanium dioxide, and modified starch was changed. As shown in Table 1, the performance test results of tensile strength, elongation at break, film puncture force, dart impact mass, and mixed gas permeability of Examples 12-13 were significantly worse than those of Examples 4-5. The performance test results of tensile strength, elongation at break, film puncture force, dart impact mass, and mixed gas permeability of Example 15 were better than those of Examples 12-13, but worse than those of Examples 4-5 and Example 14. This indicates that titanium dioxide can be loaded on the surface and in the pores of diatomaceous earth, improving the covering power, barrier properties, adsorption properties, and air permeability of diatomaceous earth. Modified starch has excellent viscosity and adsorption properties, which allows titanium dioxide to be stably loaded in the diatomaceous earth structure, further improving the mechanical properties, stability, and mechanical strength of diatomaceous earth, and subsequently improving the corresponding properties of the PE layer.
[0084] In the preparation methods of modified starch in Examples 16-17, neither nano-calcium carbonate nor xanthan gum was added. As shown in Table 1, the performance test results of tensile strength, elongation at break, film puncture force, dart impact mass, and mixed gas permeability of Examples 16-17 were better than those of Example 13, but worse than those of Examples 4-5. This indicates that the mixture of starch, nano-calcium carbonate, and xanthan gum has a synergistic effect, and the resulting modified starch has good mechanical properties, viscosity, and processing properties, which in turn helps to improve the properties between diatomaceous earth and titanium dioxide, and subsequently change the corresponding properties of the PE layer.
[0085] Comparative Examples 1-2 varied the interlayer weight ratios of PA / TIE / LLD / LLD / LD / TIE / PE / TIE / LL+LD. Compared to Examples 1-3, the performance test results of the membrane in terms of tensile strength, elongation at break, membrane puncture force, dart impact mass, and mixed gas permeability were significantly worse than those in Examples 1-3. This indicates that the interlayer weight ratios of each membrane specified in this application have a significant impact on the overall performance of the membrane. Setting appropriate weight ratios for each membrane layer allows for suitable thickness ranges between layers. The coordinated structure of each layer can reduce discontinuities and defects at the interface, thereby reducing light scattering and improving transparency and mechanical properties.
[0086] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.
Claims
1. A highly transparent PE / PA asymmetric film, characterized in that, The structure is PA / TIE / LLD / LLD / LD / TIE / PA / TIE / LLD, with an interlayer weight ratio of 0.125-0.131:0.064-0.070:0.073-0.079:0.073-0.079:0.218-0.224:0.064-0.070:0.103-0.109:0.064-0.070:0.189-0.195; The raw materials of the LD layer, by weight, include the following: 60-70 parts of low-density polyethylene, 15-20 parts of modified glass fiber, 10-13 parts of modified diatomaceous earth, 5-8 parts of polytetrafluoroethylene, 5-8 parts of maleic anhydride-grafted polyolefin elastomer, and 2-3 parts of disulfide phase. The method for preparing the modified glass fiber includes the following steps: (1) Cut the glass fiber to a length of 1-2 mm, then disperse it in deionized water, add silane coupling agent, stir at 60-65℃ for 10-15 min, filter, dry, and obtain pretreated glass fiber; (2) Wash the straw powder with anhydrous ethanol 2-3 times, then disperse it in NaOH solution and soak for 20-25 minutes at a soaking temperature of 70-75℃. Wash with water, filter and dry to obtain pretreated straw powder; (3) Coat the surface of the pretreated glass fiber in step (1) with modified chitosan solution, then spray the pretreated straw powder in step (2) evenly onto the surface of the glass fiber, and dry it to obtain modified glass fiber.
2. The highly transparent PE / PA asymmetric film according to claim 1, characterized in that, The interlayer weight ratio of PA / TIE / LLD / LLD / LD / TIE / PA / TIE / LLD is 0.128:0.067:0.076:0.076:0.221:0.067:0.106:0.067:0.
192.
3. The highly transparent PE / PA asymmetric film according to claim 1, characterized in that, The mass ratio of the glass fiber, modified chitosan solution, and pretreated straw powder is 1:0.04-0.06:0.1-0.
3.
4. A highly transparent PE / PA asymmetric film according to claim 1, characterized in that, The method for preparing the modified chitosan solution includes the following steps: dissolving chitosan in acetic acid solution, stirring magnetically at room temperature until the chitosan is completely dissolved, then adding sodium alginate and hydroxymethyl cellulose, stirring at 80-85℃ for 30-35 minutes, and allowing to stand to obtain the modified chitosan solution.
5. A highly transparent PE / PA asymmetric film according to claim 1, characterized in that, The method for preparing the modified diatomaceous earth includes the following steps: (1) Calcine the diatomaceous earth at 300-320℃ for 50-60 min, then classify and finely crush it, disperse it in sodium oxalate solution, stir for 16-20 min, filter, and dry to obtain pretreated diatomaceous earth; (2) Disperse titanium dioxide in deionized water, add fatty alcohol polyoxyethylene ether and dispersant MF, stir evenly, filter, and dry to obtain pretreated titanium dioxide; (3) Disperse the pretreated diatomaceous earth from step (1) in deionized water, add the pretreated titanium dioxide and modified starch from step (2), stir at 80-85℃ for 1-2 hours, and dry to obtain modified diatomaceous earth.
6. A highly transparent PE / PA asymmetric film according to claim 5, characterized in that, The mass ratio of diatomaceous earth, titanium dioxide, and modified starch is 1:0.3-0.4:0.1-0.
2.
7. A highly transparent PE / PA asymmetric film according to claim 5, characterized in that, The method for preparing the modified starch includes the following steps: dispersing starch in sodium hydroxide solution, reacting at 40-45℃ for 4-5 hours, centrifuging, discarding the supernatant, adding water, shaking well, centrifuging again, filtering, and drying to obtain pretreated starch, then dispersing it in deionized water, adding nano-calcium carbonate and xanthan gum, stirring at 60-65℃, drying, and grinding to obtain modified starch.
8. A method for preparing a highly transparent PE / PA asymmetric film according to claim 1, characterized in that, The process includes the following steps: PA resin, TIE resin, LLD resin, LLD resin, LD resin, TIE resin, PA resin, TIE resin, and LLD resin are melted and plasticized in different extruders. The molten resin is then extruded into the same die and evenly distributed in the die according to a certain interlayer structure. The film is then blown, cooled, shaped, and wound up using a nine-layer blown film equipment to obtain an asymmetric nine-layer co-extruded nylon film.
Citation Information
Patent Citations
Asymmetric seven-layer co-extruded nylon membrane
CN104669737A