Novel yellowing-resistant leather fatliquoring agent, preparation method and application thereof

A novel leather fatliquoring agent was prepared by using long-chain fatty alcohol polyoxypropylene ether, which solved the problem of yellowing of white and light-colored leather and achieved high resistance to yellowing, as well as good softness and oiliness.

CN119570991BActive Publication Date: 2026-11-24BROTHER ENTERPRISES HLDG CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411757821.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-12-03
Publication Date
2026-11-24
Estimated Expiration
2044-12-03

AI Technical Summary

Technical Problem

Existing leather fatliquoring agents are insufficient in resisting heat and light damage in white and light-colored leathers, leading to yellowing problems.

Method used

Using long-chain fatty alcohol polyoxypropylene ether as the main raw material, long-chain fatty alcohol polyoxypropylene ether sulfate and succinic acid monoester sulfonate are prepared through sulfonation and esterification reactions, and then mixed with nonionic emulsifier and mineral oil to form a novel leather fatliquoring agent resistant to yellowing.

Benefits of technology

It improves the softness and oiliness of the leather, while enhancing its resistance to ultraviolet rays and heat, and extending the leather's resistance to yellowing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119570991B_ABST
    Figure CN119570991B_ABST
Patent Text Reader

Abstract

This invention discloses a novel yellowing-resistant leather fatliquoring agent, its preparation method, and its application. The raw materials for preparing the novel yellowing-resistant leather fatliquoring agent provided by this invention include long-chain fatty alcohol polyoxypropylene ether. Sulfonates and esters are prepared using the long-chain fatty alcohol polyoxypropylene ether. Then, the sulfonates, esters, nonionic emulsifiers, mineral oil, and water are compounded to obtain a leather fatliquoring agent with a high yellowing resistance level. Long-chain fatty alcohol polyoxypropylene ether provides a good structural basis for fatliquoring softness from a molecular perspective. Simultaneously, the product molecule does not contain double bonds and has strong antioxidant stability. When used as a fatliquoring material, it can give leather excellent yellowing resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of leather technology, specifically to a novel yellowing-resistant leather fatliquoring agent, its preparation method, and its application. Background Technology

[0002] Fatliquoring agents are among the most widely used specialty chemicals in the leather industry. By fatliquoring, leather products gain softness and elasticity. Fatliquoring agents mainly consist of emulsifiers and emulsified components. Depending on the components, different leather fatliquoring agent products with varying properties can be derived, ultimately imparting different styles to leathers. With market changes, white and light-colored leather products are increasingly used in daily life and are very popular. To maintain the color of white and light-colored leather products, it is essential to improve the resistance of the oil components in the fatliquoring agent to heat and light damage, i.e., the yellowing resistance of the fatliquoring agent product.

[0003] Among the published patents in China, there are reports on leather fatliquoring agents with the advantage of yellowing resistance. Lü Bin et al. disclosed a succinate sulfonated pepper seed oil / nano-perovskite oxide composite yellowing-resistant fatliquoring agent and its preparation method (Lü Bin, Guo Xu, Gao Dangge, et al. A succinate sulfonated pepper seed oil / nano-perovskite oxide composite yellowing-resistant fatliquoring agent and its preparation method [P]. Shaanxi Province: CN201910920739.7, 2021-08-17). The zirconium-aluminum double-doped perovskite oxide used in this invention has excellent ultraviolet absorption capacity and certain tanning properties, increasing the absorption and binding of the fatliquoring agent while giving the leather high yellowing resistance. Zhang Yuehong et al. disclosed a yellowing-resistant titanium dioxide / fatty acid-based leather fatliquoring agent and its preparation method (Zhang Yuehong, Liu Chenyang, Ma Jianzhong. A yellowing-resistant titanium dioxide / fatty acid-based leather fatliquoring agent and its preparation method [P]. Shaanxi Province: CN202110797467.3, 2022-05-24). They introduced TiO2COOH ultraviolet shielding agent into the fatty acid-based fatliquoring agent by blending, thereby solving the problem of easy aging and yellowing of leather after fatliquoring. Huo Yueqing et al. disclosed a yellowing-resistant leather fatliquoring agent with modified sulfonated oil as the main agent and its preparation method (Huo Yueqing, Liu Xiaochen, Cao Shengti, et al. Yellowing-resistant leather fatliquoring agent with modified sulfonated oil as the main agent and its preparation method [P]. Shanxi Province: CN202311817349.X, 2024-04-05). They introduced polyoxyethylene (EO) groups into the modified sulfonated oil. The introduction of EO groups increases the molecular weight of the sulfonated oil, thereby reducing the active groups in the fatliquoring agent at the same addition amount, thus giving the fatliquoring agent good yellowing resistance and reducing the cost. Summary of the Invention

[0004] The purpose of this invention is to overcome the defects of the prior art and provide a novel anti-yellowing leather fatliquoring agent, its preparation method, and its application.

[0005] This invention provides a novel anti-yellowing leather fatliquoring agent, the raw material of which includes: long-chain fatty alcohol polyoxypropylene ether, the structural formula of which is shown below:

[0006]

[0007] In the above formula, R is a straight-chain C16 to C18 straight-chain alkane, and n is the degree of polymerization of propylene oxide, n = 5 to 10.

[0008] The present invention also provides a method for preparing the above-mentioned novel anti-yellowing leather fatliquoring agent, comprising the following steps: mixing and stirring long-chain fatty alcohol polyoxypropylene ether sulfate, long-chain fatty alcohol polyoxypropylene ether succinic acid monoester sulfonate, nonionic emulsifier and mineral oil at 50-60°C for 30 min, adding water until the solid content is 50-60%, and stirring for another 1 h to obtain the novel anti-yellowing leather fatliquoring agent;

[0009] Preferably, the amount of the long-chain fatty alcohol polyoxypropylene ether sulfate is 20-30 parts based on 100% solid content;

[0010] Preferably, the amount of the long-chain fatty alcohol polyoxypropylene ether succinate monoester sulfonate is 30-40 parts based on 100% solid content;

[0011] Preferably, the amount of the nonionic emulsifier is 10 to 20 parts;

[0012] Preferably, the amount of mineral oil used is 20 to 30 parts.

[0013] The present invention also provides the application of the above-mentioned novel yellowing-resistant leather fatliquoring agent in leather processing.

[0014] The present invention has the following beneficial effects:

[0015] This invention provides a novel anti-yellowing leather fatliquoring agent, its preparation method, and its application. The novel anti-yellowing leather fatliquoring agent provided by this invention uses long-chain fatty alcohol polyoxypropylene ether as its raw material. Compared with conventional long-chain fatty alcohol polyoxyethylene ether, it contains a certain amount of methyl groups in the polyether side chain, has a very low freezing point, and is in a liquid state at room temperature, thus facilitating sulfonation and esterification reactions. Simultaneously, due to the hydrophobicity of the polypropylene ether chain, it not only provides good softness and oiliness to the sulfonated and esterified products but also maintains good flowability. Furthermore, its molecule does not contain double bonds, exhibiting strong antioxidant stability, and when used as a fatliquoring material, it can give leather a high level of anti-yellowing performance. Attached Figure Description

[0016] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0017] Figure 1 A schematic diagram of the method for splitting the top layer of wet blue leather from cattle. Detailed Implementation

[0018] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0019] The following is a detailed description of a novel anti-yellowing leather fatliquoring agent, its preparation method, and its application, provided by embodiments of the present invention.

[0020] In a first aspect, embodiments of the present invention provide a novel anti-yellowing leather fatliquoring agent, the raw material for which includes: long-chain fatty alcohol polyoxypropylene ether, the structural formula of which is shown below:

[0021]

[0022] In the above formula, R is a straight-chain C16 to C18 straight-chain alkane, and n is the degree of polymerization of propylene oxide, n = 5 to 10.

[0023] This invention provides a novel anti-yellowing leather fatliquoring agent, the raw materials of which include long-chain fatty alcohol polyoxypropylene ether. This long-chain fatty alcohol polyoxypropylene ether is a hydrophobic material mainly composed of long alkane chains and polyoxypropylene (PO) groups. Its molecules do not contain double bonds and possess strong antioxidant properties, making it an excellent raw material for fatliquoring agents that can impart a high level of anti-yellowing to leather. Simultaneously, due to the -CH3 branched characteristics of the PO segments, the freezing point of the long-chain fatty alcohol polyoxypropylene ether molecules can be significantly reduced. As the main component of the fatliquoring agent, it not only improves the softness and oiliness of leather fibers but also increases the flowability of the fatliquoring agent product, facilitating its use in the leather tanning process.

[0024] In some alternative embodiments, the main components of the novel anti-yellowing leather fatliquoring agent include: long-chain fatty alcohol polyoxypropylene ether sulfate and long-chain fatty alcohol polyoxypropylene ether succinate monoester sulfonate prepared using long-chain fatty alcohol polyoxypropylene ether, as well as nonionic emulsifier, mineral oil and water.

[0025] In some alternative embodiments, long-chain fatty alcohol polyoxypropylene ether sulfate is prepared by sulfonating long-chain fatty alcohol polyoxypropylene ether and then neutralizing it, and long-chain fatty alcohol polyoxypropylene ether succinic acid monoester sulfonate is prepared by sulfonating long-chain fatty alcohol polyoxypropylene ether with succinic acid.

[0026] In some alternative embodiments, long-chain fatty alcohol polyoxypropylene ether sulfate is prepared by the following method: long-chain fatty alcohol polyoxypropylene ether is subjected to gas-liquid sulfonation reaction with SO3 component through a membrane sulfonation reactor, and then neutralized to obtain long-chain fatty alcohol polyoxypropylene ether sulfate.

[0027] Preferably, the structural formula of the long-chain fatty alcohol polyoxypropylene ether is as follows:

[0028]

[0029] In the above formula, R is a straight-chain C16 to C18 straight-chain alkane, and n is the degree of polymerization of propylene oxide, n = 5 to 10;

[0030] Preferably, the temperature at which the long-chain fatty alcohol polyoxypropylene ether enters the membrane sulfonation reactor is 10–50°C;

[0031] Preferably, the jacket water bath circulation temperature of the membrane sulfonation reactor is 30–80°C;

[0032] Preferably, the SO3 component is a mixture of SO3 and air, wherein the volume percentage of SO3 in the mixture is 3% to 7%, and the temperature at which the SO3 component enters the membrane sulfonation reactor is 40 to 60°C.

[0033] Preferably, the molar ratio of SO3 component to long-chain fatty alcohol polyoxypropylene ether is 0.80–1.10:1, and the structural formula of the long-chain fatty alcohol polyoxypropylene ether sulfate obtained by the gas-liquid sulfonation reaction is shown below:

[0034]

[0035] Preferably, the alkaline solution used in the neutralization reaction includes one of the following: a 30% (w / w) NaOH solution, a 50% (w / w) KOH solution, and a 28% (w / w) NH4OH solution. The neutralization reaction temperature is 40–60°C, the time is 0.5–2 h, and the pH is 7.5–9.0. The structural formula of the long-chain fatty alcohol polyoxypropylene ether sulfate obtained by reacting the long-chain fatty alcohol polyoxypropylene ether sulfate with the alkaline solution is shown below:

[0036]

[0037] In the above formula, M is at least one of Na, K, and NH4;

[0038] Preferably, the long-chain fatty alcohol polyoxypropylene ether sulfate needs to be decolorized. The decolorization treatment is carried out under weakly alkaline conditions, wherein the pH of the decolorization treatment is 8.0-8.5, the temperature is 50-70℃, the time is 1-3h, and the decolorizing agent includes any one of hydrogen peroxide, thiourea dioxide, and sodium bisulfite.

[0039] This invention provides a novel anti-yellowing leather fatliquoring agent, comprising the following components: long-chain fatty alcohol polyoxypropylene ether sulfate, long-chain fatty alcohol polyoxypropylene ether succinic acid monoester sulfonate, nonionic emulsifier, and mineral oil. The preparation of the long-chain fatty alcohol polyoxypropylene ether sulfate includes the following steps: long-chain fatty alcohol polyoxypropylene ether enters from the top of a membrane sulfonation reactor, forming a thin liquid film along the inner wall of the sulfonation tube. Simultaneously, a component containing SO3 is filtered through a filter and enters the top of the membrane sulfonation reactor in a proportional manner. The two flow down in parallel, and the SO3 component rapidly completes a gas-liquid reaction on the liquid film. The membrane sulfonation reactor jacket is connected to circulating water to ensure a suitable reaction temperature. The sulfonic acid product flows out from the bottom of the sulfonation tube and is neutralized to a weakly alkaline state with an alkaline solution, then decolorized to obtain the long-chain fatty alcohol polyoxypropylene ether sulfate product.

[0040] The above process for preparing long-chain fatty alcohol polyoxypropylene ether sulfate does not employ sulfonyl chloride sulfonation, but rather SO3 sulfonation. This process allows for continuous and automated control, eliminates the need for hazardous chlorine gas, avoids the generation of large amounts of waste hydrogen chloride gas, and produces no organochlorine compounds in the product. The preparation reaction utilizes the gas-phase SO3 membrane sulfonation principle, resulting in a large contact area between reactants. The reaction can be completed through cyclical action under high SO3 concentrations, leading to high reaction efficiency and making it an "atom-economical reaction." It also avoids the generation of large amounts of waste, making it a synthesis method actively promoted in green industrial production.

[0041] In some alternative embodiments, long-chain fatty alcohol polyoxypropylene ether succinate monoester sulfonate is prepared by the following method: esterification of long-chain fatty alcohol polyoxypropylene ether with maleic anhydride to obtain long-chain fatty alcohol polyoxypropylene ether succinate monoester; and then sulfitization of long-chain fatty alcohol polyoxypropylene ether succinate monoester with sodium sulfite to obtain long-chain fatty alcohol polyoxypropylene ether succinate monoester sulfonate.

[0042] Preferably, the molar ratio of long-chain fatty alcohol polyoxypropylene ether to maleic anhydride is 1 to 1.2:1, the esterification reaction temperature is 90 to 105°C, and the esterification reaction time is 2.5 to 3.5 h.

[0043] Preferably, the molar ratio of long-chain fatty alcohol polyoxypropylene ether succinate monoester to sodium sulfite is 1 to 1.2:1, the sulfonation reaction temperature is 75 to 85°C, and the sulfonation reaction time is 2.5 to 3.5 h.

[0044] In some alternative embodiments, the nonionic emulsifier includes at least one of O-15 and O-20, and the mineral oil includes at least one of 32# white oil and 36# white oil.

[0045] Secondly, the present invention provides a method for preparing the above-mentioned novel anti-yellowing leather fatliquoring agent, comprising the following steps: mixing and stirring long-chain fatty alcohol polyoxypropylene ether sulfate, long-chain fatty alcohol polyoxypropylene ether succinic acid monoester sulfonate, nonionic emulsifier and mineral oil at 50-60°C for 30 min, adding water until the solid content is 50-60%, and stirring for another 1 h to obtain the novel anti-yellowing leather fatliquoring agent;

[0046] Preferably, the amount of long-chain fatty alcohol polyoxypropylene ether sulfate is 20-30 parts based on 100% solid content;

[0047] Preferably, the amount of long-chain fatty alcohol polyoxypropylene ether succinate monoester sulfonate is 30-40 parts, based on 100% content;

[0048] Preferably, the amount of nonionic emulsifier used is 10 to 20 parts;

[0049] Preferably, the amount of mineral oil used is 20 to 30 parts;

[0050] In some alternative embodiments, the pH value of the novel yellowing-resistant leather fatliquoring agent emulsion at a mass percentage of 10% is 6.0 to 7.0; the viscosity of the novel yellowing-resistant leather fatliquoring agent emulsion at 40°C is 0.2 to 0.4 Pa·s.

[0051] Thirdly, embodiments of the present invention provide the application of the above-mentioned novel yellowing-resistant leather fatliquoring agent or the novel yellowing-resistant leather fatliquoring agent prepared by the above-mentioned preparation method in leather processing.

[0052] The present invention will be further described below with reference to embodiments.

[0053] The preparation method of long-chain fatty alcohol polyoxypropylene ether sulfate is as follows:

[0054] Experimental Example 1:

[0055] (1) Sulfonation reaction

[0056] Take 1 kg of long-chain fatty alcohol polyoxypropylene ether RO(CH(CH3)CH2) n OH (n=5, R is a straight-chain C16~C18 straight-chain alkane), the feed temperature is set to 20℃, the SO3 component is prepared by sulfur combustion method, and the temperature of SO3 / air mixed gas is 50℃ and the volume percentage is 4%. The molar ratio of SO3 component to long-chain fatty alcohol polyoxypropylene ether is 1.05:1. Long-chain fatty alcohol polyoxypropylene ether and SO3 component enter the sulfonator from the top of the sulfonator to undergo sulfonation reaction. The water bath temperature of the sulfonation tube jacket is 65℃. Long-chain fatty alcohol polyoxypropylene ether sulfate is discharged, followed by neutralization and decolorization reaction.

[0057] (2) Neutralization reaction

[0058] Long-chain fatty alcohol polyoxypropylene ether sulfate was neutralized with a 30% NaOH solution (30% of the sulfate content) at 50°C for 1 hour, and the pH was adjusted to 8.5.

[0059] (3) Decolorization reaction

[0060] 2% (based on sulfate) of hydrogen peroxide was added to the neutralized long-chain fatty alcohol polyoxypropylene ether sulfate solution. The temperature was controlled at 55℃ and pH at 8.5. The reaction was carried out for 1.5 hours. Then, citric acid monohydrate was added to adjust the pH of the final product (10%) to 7.5. The solid content of the product was 75%. The sulfonation degree of the long-chain fatty alcohol polyoxypropylene ether sulfate was tested and found to be 60% (the sulfonation degree of the product was determined in accordance with the national standard GB / T 5173-2018).

[0061] Experimental Example 2:

[0062] (1) Sulfonation reaction

[0063] Take 2 kg of long-chain fatty alcohol polyoxypropylene ether RO(CH(CH3)CH2). nOH (n=8, R is a straight-chain C16~C18 straight-chain alkane), the feed temperature is set to 35℃, the SO3 component is prepared by sulfur combustion method, and the temperature of SO3 / air mixture is 60℃ and the volume percentage is 5%. The molar ratio of SO3 component to long-chain fatty alcohol polyoxypropylene ether is 1:1. The long-chain fatty alcohol polyoxypropylene ether and SO3 / process air mixture enter the sulfonator from the top of the sulfonator to undergo sulfonation reaction. The water bath temperature of the sulfonation tube jacket is 45℃. The long-chain fatty alcohol polyoxypropylene ether sulfate is discharged, followed by neutralization and decolorization reaction.

[0064] (2) Neutralization reaction

[0065] Long-chain fatty alcohol polyoxypropylene ether sulfate was neutralized with 50% KOH solution (25% of the sulfate) at 40°C for 2 hours, and the pH was adjusted to 9.0.

[0066] (3) Decolorization reaction

[0067] 0.5% (based on sulfate) of thiourea dioxide was added to the neutralized long-chain fatty alcohol polyoxypropylene ether sulfate solution. The temperature was controlled at 60℃ and pH at 8.2, and the reaction was carried out for 3 hours. Then, citric acid monohydrate was added to adjust the pH of the final product (10%) to 7.5. The solid content of the product was 75%, and the sulfonation degree of the long-chain fatty alcohol polyoxypropylene ether sulfate was 71%.

[0068] Experimental Example 3:

[0069] (1) Sulfonation reaction

[0070] Take 1.5 kg of long-chain fatty alcohol polyoxypropylene ether RO(CH(CH3)CH2). n OH (n=10, R is a straight-chain C16~C18 straight-chain alkane), the feed temperature is 45℃, the SO3 component is prepared by liquid SO3 evaporation, and the SO3 / air mixture is obtained at 45℃ and 7% by volume. The molar ratio of SO3 component to long-chain fatty alcohol polyoxypropylene ether is 0.85:1. Long-chain fatty alcohol polyoxypropylene ether and SO3 component enter the sulfonator from the top of the sulfonator to undergo sulfonation reaction. The water bath temperature of the sulfonation tube jacket is 55℃. Long-chain fatty alcohol polyoxypropylene ether sulfate is discharged, followed by neutralization and decolorization reaction.

[0071] (2) Neutralization reaction

[0072] Long-chain fatty alcohol polyoxypropylene ether sulfate was neutralized with 28% NH4OH solution (30% of the sulfate) at 50°C for 1.5 h, and the pH was adjusted to 8.0.

[0073] (3) Decolorization reaction

[0074] 1% sodium bisulfite (calculated as sulfate) was added to the neutralized long-chain fatty alcohol polyoxypropylene ether sulfate solution. The temperature was controlled at 65℃ and pH at 8.5. The reaction was carried out for 2 hours. Then, citric acid monohydrate was added to adjust the pH of the final product (10%) to 7.5. The solid content of the product was 75%. The sulfonation degree of the long-chain fatty alcohol polyoxypropylene ether sulfate was 64%.

[0075] The preparation method of long-chain fatty alcohol polyoxypropylene ether succinic acid monoester sulfonate is as follows:

[0076] Experimental Example 4:

[0077] (1) Esterification reaction

[0078] Add 254g of long-chain fatty alcohol polyoxypropylene ether RO(CH(CH3)CH2) to a 1000mL four-necked flask equipped with a stirrer. n OH (n=5, R is a straight-chain C16~C18 straight-chain alkane) and 49g of maleic anhydride (the molar ratio of long-chain fatty alcohol polyoxypropylene ether to maleic anhydride was controlled at 1.1:1) were reacted at 95℃ for 3h to obtain long-chain fatty alcohol polyoxypropylene ether succinic acid monoester.

[0079] (2) Sulphurization reaction

[0080] First, prepare the sodium sulfite solution: Dissolve 57.3g of sodium sulfite in 210g of water in a 500mL four-necked flask equipped with a stirrer (controlling the molar ratio of ester to sodium sulfite to be 1.1:1), stir at 33℃ for 20min, then adjust the pH of the solution to 7.5 with monoethanolamine, stir at 33℃ for 10min and set aside.

[0081] Sodium sulfite solution was slowly added to a four-necked flask containing long-chain fatty alcohol polyoxypropylene ether succinate monoester. The temperature was controlled at 80°C and the addition time was 30 min. After the addition was completed, the reaction was carried out for 3 h. Water was added until the solid content was 60% and the mixture was stirred evenly to obtain long-chain fatty alcohol polyoxypropylene ether succinate monoester sulfonate.

[0082] Experimental Example 5:

[0083] (1) Esterification reaction

[0084] Add 348.5 g of long-chain fatty alcohol polyoxypropylene ether RO(CH(CH3)CH2) to a 1000 mL four-necked flask equipped with a stirrer. n OH (n=8, R is a straight-chain C16-C18 straight-chain alkane) and 49g of maleic anhydride (the molar ratio of long-chain fatty alcohol polyoxypropylene ether to maleic anhydride was controlled at 1.15:1) were reacted at 105℃ for 2.5h to obtain long-chain fatty alcohol polyoxypropylene ether succinic acid monoester.

[0085] (2) Sulphurization reaction

[0086] First, prepare the sodium sulfite solution: Dissolve 63g of sodium sulfite in 285g of water in a 500mL four-necked flask equipped with a stirrer (controlling the molar ratio of ester to sodium sulfite to be 1:1), stir at 33℃ for 20min, then adjust the pH of the solution to 7.5 with monoethanolamine, stir at 33℃ for 10min and set aside.

[0087] Sodium sulfite solution was slowly added to a four-necked flask containing long-chain fatty alcohol polyoxypropylene ether succinate monoester. The temperature was controlled at 75°C and the addition time was 30 min. After the addition was completed, the reaction was carried out for 3.5 h. Water was added until the solid content was 60% and the mixture was stirred evenly to obtain long-chain fatty alcohol polyoxypropylene ether succinate monoester sulfonate.

[0088] Experimental Example 6:

[0089] (1) Esterification reaction

[0090] Add 351g of long-chain fatty alcohol polyoxypropylene ether RO(CH(CH3)CH2) to a 1000mL four-necked flask equipped with a stirrer. n OH (n=10, R is a straight-chain C16~C18 straight-chain alkane) and 49g of maleic anhydride (controlling the molar ratio of long-chain fatty alcohol polyoxypropylene ether to maleic anhydride to 1:1) were reacted at 90℃ for 3.5h to obtain long-chain fatty alcohol polyoxypropylene ether succinic acid monoester.

[0091] (2) Sulphurization reaction

[0092] First, prepare the sodium sulfite solution: Dissolve 54.8g of sodium sulfite in 200g of water in a 500mL four-necked flask equipped with a stirrer (controlling the molar ratio of ester to sodium sulfite to be 1.15:1), stir at 33℃ for 20min, then adjust the pH of the solution to 7.5 with monoethanolamine, stir at 33℃ for 10min and set aside.

[0093] Sodium sulfite solution was slowly added to a four-necked flask containing long-chain fatty alcohol polyoxypropylene ether succinate monoester. The temperature was controlled at 85°C and the addition time was 30 min. After the addition was completed, the reaction was carried out for 2.5 h. Water was added until the solid content was 60% and the mixture was stirred evenly to obtain long-chain fatty alcohol polyoxypropylene ether succinate monoester sulfonate.

[0094] The preparation method of the novel anti-yellowing fatliquoring agent is as follows:

[0095] Example 1:

[0096] In a mixing reactor, 20 parts of long-chain fatty alcohol polyoxypropylene ether (n=5) sulfate prepared in Example 1, 40 parts of long-chain fatty alcohol polyoxypropylene ether (n=8) succinic acid monoester sulfonate prepared in Example 5, 15 parts of O-15 emulsifier, and 25 parts of 32# white oil (all by mass fraction) were added. The mixing temperature was controlled at 50℃, and after stirring for 30 min, water was added to bring the solid content to 50%, and then stirring was continued for 1 h. After uniform mixing, a novel anti-yellowing fatliquoring agent was obtained. The appearance was a yellow transparent liquid with a viscosity of 0.31 Pa·s at 40℃. The pH of a 10% (by mass) emulsion of the novel anti-yellowing fatliquoring agent was 6.4.

[0097] Example 2:

[0098] In a reaction vessel, 30 parts of long-chain fatty alcohol polyoxypropylene ether (n=10) sulfate prepared in Example 3, 35 parts of long-chain fatty alcohol polyoxypropylene ether (n=5) succinic acid monoester sulfonate prepared in Example 4, 12 parts of O-20 emulsifier, and 23 parts of 36# white oil (all by mass fraction) were added. The mixing temperature was controlled at 55℃, and after stirring for 30 min, water was added until the solid content reached 55%, and then stirring was continued for 1 h. After uniform mixing, a novel anti-yellowing fatliquoring agent was obtained. The appearance was a yellow transparent liquid with a viscosity of 0.34 Pa·s at 40℃. The pH of a 10% (by mass) emulsion of the novel anti-yellowing fatliquoring agent was 6.5.

[0099] Example 3:

[0100] In a reaction vessel, 22 parts of long-chain fatty alcohol polyoxypropylene ether (n=8) sulfate prepared in Example 2, 32 parts of long-chain fatty alcohol polyoxypropylene ether (n=10) succinic acid monoester sulfonate prepared in Example 6, 20 parts of O-15 emulsifier, and 26 parts of 36# white oil (all by mass fraction) were added. The mixing temperature was controlled at 60℃, and after stirring for 30 min, water was added until the solid content reached 60%, and then stirring was continued for 1 h. After uniform mixing, the novel anti-yellowing fatliquoring agent was obtained. It was a yellow transparent liquid with a viscosity of 0.35 Pa·s at 40℃. The pH of the 10% (by mass) novel anti-yellowing fatliquoring agent emulsion was 6.8.

[0101] Example 4:

[0102] In a reaction vessel, 25 parts of long-chain fatty alcohol polyoxypropylene ether (n=5) sulfate prepared in Example 1, 38 parts of long-chain fatty alcohol polyoxypropylene ether (n=10) succinic acid monoester sulfonate prepared in Example 6, 17 parts of O-20 emulsifier, and 20 parts of 32# white oil (all by mass fraction) were added. The mixing temperature was controlled at 60℃, and after stirring for 30 min, water was added to bring the solid content to 55%, and then stirring was continued for 1 h. After uniform mixing, the novel anti-yellowing fatliquoring agent was obtained. It was a yellow transparent liquid with a viscosity of 0.27 Pa·s at 40℃, and the pH of a 10% (by mass) novel anti-yellowing fatliquoring agent emulsion was 6.7.

[0103] Comparative Example 1

[0104] The product uses HFK-N fatliquoring agent, manufactured by Brother Technology Co., Ltd.

[0105] Comparative Example 2

[0106] Similar to the steps in Example 1, the only difference is that the sulfate of the long-chain fatty alcohol polyoxypropylene ether (n=5, R is a straight-chain C16-C18 straight-chain alkane) prepared in Example 1 was adjusted to 10 parts, and the succinic acid monoester sulfonate of the long-chain fatty alcohol polyoxypropylene ether (n=8) prepared in Example 5 was adjusted to 50 parts. A novel anti-yellowing fatliquoring agent was obtained, which was a yellow, semi-transparent liquid with a viscosity of 0.66 Pa·s at 40°C. The pH of a 10% (w / w) emulsion of the novel anti-yellowing fatliquoring agent was 6.5.

[0107] Comparative Example 3

[0108] Similar to the steps in Example 1, the only difference is that the sulfate of the long-chain fatty alcohol polyoxypropylene ether (n=5, R is a straight-chain C16-C18 straight-chain alkane) prepared in Example 1 was adjusted to 40 parts, and the succinic acid monoester sulfonate of the long-chain fatty alcohol polyoxypropylene ether (n=8) prepared in Example 5 was adjusted to 20 parts. A novel anti-yellowing fatliquoring agent was obtained, which appeared as a yellow, semi-transparent liquid with a viscosity of 0.58 Pa·s at 40°C. The pH of a 10% (w / w) emulsion of the novel anti-yellowing fatliquoring agent was 6.4.

[0109] Comparative Example 4

[0110] Similar to the steps in Example 1, except that the O-15 emulsifier was adjusted to 5 parts and the 32# white oil to 35 parts. A novel anti-yellowing fatliquoring agent was obtained, which appeared as a pale yellow paste with a viscosity of 2.42 Pa·s at 40°C. The pH of a 10% (w / w) emulsion of the novel anti-yellowing fatliquoring agent was 6.5.

[0111] Comparative Example 5

[0112] Similar to the steps in Example 1, except that the O-15 emulsifier was adjusted to 30 parts and the 32# white oil to 10 parts. A novel anti-yellowing fatliquoring agent was obtained, which appeared as a pale yellow paste with a viscosity of 1.47 Pa·s at 40°C. The pH of the 10% (w / w) emulsion of the novel anti-yellowing fatliquoring agent was 6.3.

[0113] Comparative Example 6

[0114] Similar to the steps in Example 1, the only difference being that the mixing temperature was controlled at 80°C. A novel anti-yellowing fatliquoring agent was obtained, appearing as a yellow transparent liquid with a viscosity of 0.29 Pa·s at 40°C. The pH of a 10% (w / w) emulsion of this novel anti-yellowing fatliquoring agent was 6.4. However, after a period of time, a small amount of floating oil appeared on the surface of the product, possibly due to the decomposition of some materials caused by excessively high compounding temperatures.

[0115] Comparative Example 7

[0116] Similar to the steps in Example 1, the only difference is that the mixing temperature is controlled at 30°C. A novel anti-yellowing fatliquoring agent is obtained, which is a yellow transparent liquid with a viscosity of 0.32 Pa·s at 40°C. The pH of a 10% (w / w) emulsion of this novel anti-yellowing fatliquoring agent is 6.4. However, this product requires a longer mixing time when compounding; otherwise, the materials are difficult to fully dissolve and mix evenly, and the emulsification of the system may be insufficient.

[0117] Comparative Example 8

[0118] Similar to the steps in Example 1, except that the solid content was adjusted to 30% during water replenishment. A pale yellow gel-like product was obtained, which is not suitable for use as a finished fatliquoring agent.

[0119] Comparative Example 9

[0120] Similar to the steps in Example 1, the only difference is that the solid content is adjusted to 80% during water replenishment. A novel anti-yellowing fatliquoring agent is obtained, which is a pale yellow viscous paste with virtually no fluidity, and is not suitable for use as a finished fatliquoring agent.

[0121] Analysis of anti-yellowing fatliquoring agents:

[0122] Using 1.8mm thick, evenly shaved blue wet leather from the top layer of cattle as the test material, according to... Figure 1 The products from Examples 1, 2, 3, and 4 of the preparation of the anti-yellowing fatliquoring agent and the products from Comparative Examples 1, 2, 3, 4, and 5 were divided and subjected to fatliquoring performance tests according to the application process in Table 1, and sensory evaluations were performed.

[0123] Table 1

[0124]

[0125]

[0126]

[0127] The yellowing resistance (sunlight resistance, UV resistance) of fat-treated leather blanks was analyzed according to the national standard HG / T3689-2001.

[0128] The heat resistance and damp heat resistance of fat-cured leather blanks to yellowing were analyzed using the following methods:

[0129] (1) Heat resistance test method:

[0130] ① Sample preparation

[0131] Sample shape and specifications: Cut a rectangular blank with dimensions of 62±2mm*12±2mm using scissors. The thickness of the sample should not exceed 50±2mm (the shape and specifications of special samples can be determined according to the actual situation). Sample quantity: Determined according to the number of testing items, with no less than three valid samples for each item and each test.

[0132] ② Setting parameters and installing the sample

[0133] Set the temperature inside the test chamber to 120±2℃. Cover the two ends of the sample with a light-shielding sheet for 20mm and place the sample on the tray.

[0134] ③Detection

[0135] Place the tray into the test chamber, turn on the switch, and allow the test piece to dry for 4 hours. After the specified time has elapsed, remove the test piece from the test chamber and remove the light-shielding sheet from the test piece.

[0136] ④ Result determination

[0137] Under a standard multi-light source color matching light box, the yellowing level of the obscured part of the sample is directly evaluated by visual inspection using a gray sample card, and the worst result is selected as the final result.

[0138] (2) Test method for resistance to damp heat:

[0139] ① Sample preparation

[0140] Sample shape and specifications: Cut a rectangular blank with dimensions of 62±2mm*12±2mm using scissors. The thickness of the sample should not exceed 50±2mm (the shape and specifications of special samples can be determined according to the actual situation). Sample quantity: Determined according to the number of testing items, with no less than three valid samples for each item and each test.

[0141] ② Setting parameters and installing the sample

[0142] Using a constant temperature and humidity chamber, set the humidity to 95% RH, cover the two ends of the sample with a light shield for 20mm, and place the sample on a tray.

[0143] ③Detection

[0144] Place the desiccator in a constant temperature and humidity chamber, turn on the switch (temperature set to 60℃), and allow the sample to stand for 36 hours. After the specified time has elapsed, remove the sample from the chamber.

[0145] ④ Result determination

[0146] Under a standard multi-light source color matching light box, the yellowing level of the obscured part of the sample is directly evaluated by visual inspection using a gray sample card, and the worst result is selected as the final result.

[0147] The application performance evaluation results of the novel yellowing-resistant leather fatliquoring agent emulsion are shown in Table 2 below.

[0148] Table 2

[0149]

[0150]

[0151] The results above show that selecting an appropriate compounding ratio can better coordinate the state, stability, and application performance of the fatliquoring agent. The fatliquoring agent compounded using the scheme provided in this invention is transparent and stable, exhibits excellent application performance, and also has good resistance to yellowing. When applied to leather fatliquoring, it can not only make the leather softer and fuller but also give it a higher level of resistance to yellowing. In contrast, proportional fatliquoring agents are difficult to maintain synergy among appearance, stability, and application performance.

[0152] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A leather fatliquoring agent resistant to yellowing, characterized in that, The main components of the anti-yellowing leather fatliquoring agent include: long-chain fatty alcohol polyoxypropylene ether sulfate and long-chain fatty alcohol polyoxypropylene ether succinate monosulfonate prepared using long-chain fatty alcohol polyoxypropylene ether, as well as nonionic emulsifier, mineral oil, and water. The long-chain fatty alcohol polyoxypropylene ether sulfate, long-chain fatty alcohol polyoxypropylene ether succinate monosulfonate, nonionic emulsifier, and mineral oil are mixed and stirred at 50-60°C for 30 minutes, water is added until the solid content is 50-60%, and then stirred for another hour to obtain the anti-yellowing leather fatliquoring agent. The structural formula of the long-chain fatty alcohol polyoxypropylene ether is shown below: In the above formula, R is a straight-chain C16~C18 straight-chain alkane, and n is the degree of polymerization of propylene oxide, n=5~10; The amount of the long-chain fatty alcohol polyoxypropylene ether sulfate is 20-30 parts, based on 100% solid content; The amount of the long-chain fatty alcohol polyoxypropylene ether succinate monoester sulfonate is 30-40 parts based on 100% solid content. The amount of the nonionic emulsifier used is 10-20 parts; The amount of mineral oil used is 20-30 parts.

2. The leather fatliquoring agent for yellowing resistance according to claim 1, characterized in that, The long-chain fatty alcohol polyoxypropylene ether sulfate is prepared by sulfonating the long-chain fatty alcohol polyoxypropylene ether and then neutralizing it.

3. The leather fatliquoring agent for yellowing resistance according to claim 2, characterized in that, The long-chain fatty alcohol polyoxypropylene ether sulfate is prepared by the following method: long-chain fatty alcohol polyoxypropylene ether is subjected to gas-liquid sulfonation reaction with SO3 component through a membrane sulfonation reactor, and then neutralized to obtain long-chain fatty alcohol polyoxypropylene ether sulfate.

4. The leather fatliquoring agent for yellowing resistance according to claim 3, characterized in that, The long-chain fatty alcohol polyoxypropylene ether enters the membrane sulfonation reactor at a temperature of 10~50℃.

5. The leather fatliquoring agent for yellowing resistance according to claim 3, characterized in that, The jacketed water bath circulation temperature of the membrane sulfonation reactor is 30~80℃.

6. The leather fatliquoring agent for yellowing resistance according to claim 3, characterized in that, The SO3 component is a mixture of SO3 and air, wherein the SO3 accounts for 3% to 7% of the volume percentage of the mixture, and the SO3 component enters the membrane sulfonation reactor at a temperature of 40 to 60°C.

7. The leather fatliquoring agent for resisting yellowing according to claim 3, characterized in that, The molar ratio of the SO3 component to the long-chain fatty alcohol polyoxypropylene ether is 0.80~1.10:1, and the structural formula of the long-chain fatty alcohol polyoxypropylene ether sulfate obtained by the gas-liquid sulfonation reaction is shown below: 。 8. The leather fatliquoring agent for yellowing resistance according to claim 7, characterized in that, The alkaline solution used in the neutralization reaction includes one of the following: a 30% NaOH solution, a 50% KOH solution, or a 28% NH4OH solution. The neutralization reaction temperature is 40–60°C, the time is 0.5–2 hours, and the pH is 7.5–9.

0. The structural formula of the long-chain fatty alcohol polyoxypropylene ether sulfate obtained by reacting the long-chain fatty alcohol polyoxypropylene ether sulfate with the alkaline solution is shown below: In the above formula, M is at least one of Na, K, and NH4.

9. The leather fatliquoring agent for resisting yellowing according to claim 3, characterized in that, The long-chain fatty alcohol polyoxypropylene ether sulfate needs to be decolorized. The decolorization treatment is carried out under weakly alkaline conditions, wherein the pH of the decolorization treatment is 8.0~8.5, the temperature is 50~70℃, and the time is 1~3h. The decolorizing agent includes any one of hydrogen peroxide, thiourea dioxide, and sodium bisulfite.

10. The leather fatliquoring agent for resisting yellowing according to claim 1, characterized in that, The long-chain fatty alcohol polyoxypropylene ether succinic acid monoester sulfonate is prepared by sulfonating long-chain fatty alcohol polyoxypropylene ether with succinic acid.

11. The leather fatliquoring agent for resisting yellowing according to claim 10, characterized in that, The long-chain fatty alcohol polyoxypropylene ether succinate monoester sulfonate is prepared by the following method: long-chain fatty alcohol polyoxypropylene ether is subjected to esterification reaction with maleic anhydride to obtain long-chain fatty alcohol polyoxypropylene ether succinate monoester; then, the long-chain fatty alcohol polyoxypropylene ether succinate monoester is subjected to sulfite reaction with sodium sulfite to obtain long-chain fatty alcohol polyoxypropylene ether succinate monoester sulfonate.

12. The leather fatliquoring agent for resisting yellowing according to claim 11, characterized in that, The molar ratio of long-chain fatty alcohol polyoxypropylene ether to maleic anhydride is 1~1.2:1, the esterification reaction temperature is 90~105℃, and the esterification reaction time is 2.5~3.5h.

13. The leather fatliquoring agent for resisting yellowing according to claim 11, characterized in that, The molar ratio of long-chain fatty alcohol polyoxypropylene ether succinate monoester to sodium sulfite is 1~1.2:1, the sulfonation reaction temperature is 75~85℃, and the sulfonation reaction time is 2.5~3.5h.

14. The leather fatliquoring agent for resisting yellowing according to claim 1, characterized in that, The nonionic emulsifier includes at least one of O-15 and O-20, and the mineral oil includes at least one of 32# white oil and 36# white oil.

15. A method for preparing a leather fatliquoring agent resistant to yellowing according to any one of claims 1-14, characterized in that, Includes the following steps: Long-chain fatty alcohol polyoxypropylene ether sulfate, long-chain fatty alcohol polyoxypropylene ether succinic acid monoester sulfonate, nonionic emulsifier and mineral oil are mixed and stirred at 50~60℃ for 30min, water is added until the solid content is 50~60%, and then stirred for 1h to obtain the yellowing-resistant leather fatliquoring agent. The amount of the long-chain fatty alcohol polyoxypropylene ether sulfate is 20-30 parts, based on 100% solid content; The amount of the long-chain fatty alcohol polyoxypropylene ether succinate monoester sulfonate is 30-40 parts based on 100% solid content. The amount of the nonionic emulsifier used is 10-20 parts; The amount of mineral oil used is 20-30 parts.

16. The preparation method according to claim 15, characterized in that, The viscosity of the yellowing-resistant leather fatliquoring agent at 40°C is 0.2-0.4 Pa·s; the pH value of a 10% (by mass) yellowing-resistant leather fatliquoring agent is 6.0-7.

0.

17. The application of the anti-yellowing leather fatliquoring agent according to any one of claims 1-14 or the anti-yellowing leather fatliquoring agent prepared by the preparation method according to any one of claims 15-16 in leather processing.

Citation Information

Patent Citations

  • Synthetic fatliquor for low fogging upholstery leather

    EP1319723A1