Hemp fiber non-woven fabric, and preparation method and application thereof

By controlling the pore structure and porosity, and combining specific degumming and hydroentangling processes, a 100% virgin hemp fiber nonwoven fabric was prepared, solving the problems of insufficient air permeability, antibacterial properties and softness in existing technologies, and achieving excellent comprehensive performance.

CN119571535BActive Publication Date: 2026-11-24TIANZHICAO BIOPHARMACEUTICAL (HUNAN) CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411661388.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-11-20
Publication Date
2026-11-24
Estimated Expiration
2044-11-20

AI Technical Summary

Technical Problem

Existing technologies make it difficult to produce nonwoven fabrics with excellent breathability, antibacterial properties and softness from 100% virgin hemp fibers, and existing modification methods may affect the natural properties of hemp fibers.

Method used

Hemp fiber nonwoven fabric is prepared by controlling the pore structure and porosity of hemp fibers, using macropores, mesopores and micropores with specific pore size distributions, degumming with a compound bacterial solution of Bacillus alkalophilus and Pseudomonas fluorescens, and combining it with a multi-stage hydroentangling process.

Benefits of technology

It achieves excellent breathability, antibacterial properties and liquid evaporation rate of 100% virgin hemp fiber nonwoven fabric, improves softness, and maintains natural characteristics without chemical modification.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention discloses a hemp fiber nonwoven fabric, its preparation method, and its applications, belonging to the field of nonwoven fabric technology. The hemp fiber nonwoven fabric provided by this invention has good air permeability, antibacterial properties, and liquid evaporation rate; that is, it dries quickly after absorbing liquid, and its softness increases after liquid absorption. Therefore, it can be widely used in the preparation of hygiene products, especially as the surface layer of sanitary napkins. It is not only gentle and non-irritating, soft and quick-drying, but also has excellent antimicrobial properties and good breathability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of nonwoven fabric technology, and particularly relates to a hemp fiber nonwoven fabric, its preparation method, and its application. Background Technology

[0002] Hemp, originating in China, is one of the earliest textile raw materials used by humankind. It is a natural cellulose fiber that is biodegradable at the end of its lifespan, making hemp a resource-rich, renewable, and environmentally friendly raw material.

[0003] Hemp products are widely used in medical and civilian textile fields due to their cooling, breathable, UV-resistant, and naturally antibacterial properties. However, some unavoidable problems exist in the application of hemp. For example, hemp has a relatively high roughness, resulting in a poor user experience when made into materials that come into contact with the human body. Furthermore, existing technologies that reduce its roughness may affect its original breathability and antibacterial properties. Therefore, most current applications of hemp involve further modification or blending it with other fabrics. For instance, patent CN117211007A discloses a hemp fiber blended spunlace nonwoven fabric for disposable intimate apparel, which describes good antibacterial properties, no skin irritation, and softness and comfort. However, the proportion of hemp fiber in this solution is only 20-60%. Patent CN109576902A discloses a cotton-linen soft blended spunlace nonwoven fabric material, in which the proportion of hemp is only 5-50%. For example, although patent CN117338989A discloses a whole hemp fiber antibacterial sanitary napkin, analysis of its technical solution reveals that the surface layer does not use original hemp fiber, but rather modified hemp fiber, specifically ammonium oxalate-complex enzyme modified hemp fiber cloth. This helps to effectively remove clogging substances in the fiber network structure, increase oxygen content, and inhibit the growth of anaerobic bacteria while retaining the antibacterial properties of hemp fiber. Furthermore, while patent CN117569003A provides a whole hemp fiber antibacterial nonwoven fabric, its components are also not original hemp fiber, but rather products of original hemp fiber after a series of treatments, such as cottonized hemp fiber, hemp antibacterial microcapsules, and dicarboxylated hemp fiber.

[0004] Therefore, how to utilize hemp fiber to produce a product with excellent antibacterial and breathable properties, as well as good softness, has become a research hotspot. Summary of the Invention

[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a hemp fiber nonwoven fabric with excellent breathability, antibacterial properties and liquid evaporation rate, which is gentle, soft and non-irritating to human skin.

[0006] To achieve the above objectives, in a first aspect of the present invention, the present invention provides a hemp fiber nonwoven fabric, wherein the hemp fiber nonwoven fabric is composed of hemp fibers; the hemp fibers contain macropores with a pore size >10μm, mesopores with a pore size of 1-10μm and micropores with a pore size <1μm, and the total porosity of the hemp fibers is 30-50%.

[0007] In the hemp fiber, the porosity of macropores accounts for 48-65% of the total porosity, the porosity of mesopores accounts for 24-50% of the total porosity, and the porosity of micropores accounts for 2-12% of the total porosity.

[0008] When the moisture regain of the hemp fiber nonwoven fabric increases from 0% to 100%, the flexural stiffness decreases by ≥2%.

[0009] As an embodiment of the present invention, when the moisture regain of the hemp fiber nonwoven fabric increases from 0% to 100%, the bending stiffness decreases by 3-5%.

[0010] As an embodiment of the present invention, the total porosity of the hemp fiber is 36-48%.

[0011] As an embodiment of the present invention, in the hemp fiber, the porosity of macropores accounts for 51-60% of the total porosity.

[0012] As an embodiment of the present invention, in the hemp fiber, the porosity of the mesopores accounts for 36-44% of the total porosity.

[0013] As an embodiment of the present invention, in the hemp fiber, the porosity of small pores accounts for 3-6% of the total porosity.

[0014] As an embodiment of the present invention, the fineness of the hemp fiber is >2000Nm and the length is >28mm.

[0015] As an embodiment of the present invention, the fineness of the hemp fiber is 2240-2600 Nm and the length is 28.3-35 mm.

[0016] In a second aspect, the present invention provides a method for preparing the hemp fiber nonwoven fabric, the method comprising the following steps:

[0017] S1. Crush and pound the hemp stalks after rain and dew to obtain hemp bark;

[0018] S2. The hemp fiber is degummed once using a compound bacterial solution, wherein the compound bacterial solution contains alkalophilic Bacillus and fluorescent Pseudomonas in a mass ratio of 1:(1-2);

[0019] S3. Place the hemp fibers after the first degumming in step S2 into a secondary degumming solution for secondary degumming to obtain degummed hemp fibers; the pH value of the secondary degumming solution is 12-13.5, and the volume concentration of hydrogen peroxide in the secondary degumming solution is 9-10 mL / L.

[0020] S4. The degummed hemp fibers are soaked in oil, followed by deoiling and dehydration, and then subjected to humidification and curing treatment; the relative humidity of the humidification and curing treatment is 60-70%, and the temperature is ≥25℃.

[0021] S5. After humidification and conditioning treatment, open and comb the hemp fibers to obtain hemp fibers with a length >28mm and a residual glue rate of 5-20%.

[0022] S6. Hemp fibers are opened, cleaned, combed, and laid into a web to obtain a fiber web; wherein the basis weight of the fiber web is ≥33g / m³. 2 ;

[0023] S7. The fiber web is sequentially subjected to hydroentangling and post-hydroentangling treatment to obtain hemp fiber nonwoven fabric; wherein, the hydroentangling process includes four hydroentangling processes, and the hydroentangling pressures in the first to fourth hydroentangling processes are 35-45 bar, 60-70 bar, 75-85 bar, and 85-95 bar, respectively.

[0024] As an embodiment of the present invention, the concentration of bacteria in the compound bacterial solution is (0.1-10)×10⁻¹⁰. -8 CFU / mL.

[0025] As an embodiment of the present invention, the solid-liquid ratio of a single degumming step is 1g:(5-15)mL.

[0026] As an embodiment of the present invention, the temperature for degumming is 32-36°C and the time is 6-8 hours.

[0027] As an embodiment of the present invention, the solid-liquid ratio of the secondary degumming is 1g:(8-12)mL.

[0028] As an embodiment of the present invention, the temperature for secondary degumming is 98-100℃, and the time for secondary degumming is 60-120min.

[0029] In a third aspect, the present invention provides the application of the hemp fiber nonwoven fabric in the preparation of hygiene products.

[0030] As an embodiment of the present invention, the sanitary products include any one of sanitary napkins, panty liners, adhesive bandages, diapers, adult pull-up pants, and disposable underwear.

[0031] In a fourth aspect, the present invention provides a sanitary napkin, wherein the surface layer of the sanitary napkin is the hemp fiber nonwoven fabric described in the present invention.

[0032] As an embodiment of the present invention, the sanitary napkin further includes an absorbent layer and a bottom layer.

[0033] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0034] The hemp fiber nonwoven fabric provided by this invention exhibits a decrease in bending stiffness within a specific range when the moisture regain increases from 0% to 100%. Furthermore, the porosity of the hemp fibers and the proportion of porosity of pores within different pore size ranges to the total porosity in the hemp fiber nonwoven fabric provided by this invention are within a certain range, and the fineness of the hemp fibers is within a specific range. The resulting hemp fiber nonwoven fabric possesses excellent air permeability, antibacterial properties, and liquid evaporation rate, meaning it dries quickly after absorbing liquid, and its softness increases after liquid absorption. Therefore, it can be widely used in the preparation of hygiene products, especially as the surface layer of sanitary napkins, not only being gentle and non-irritating, soft and quick-drying, but also possessing excellent antimicrobial properties and good breathability. Attached Figure Description

[0035] Figure 1 These are photographs of hemp bark and hemp fibers taken at different steps in Example 1:

[0036] a - Photograph of hemp bark obtained after step S1 treatment; b - Photograph of hemp fiber obtained after degreasing and dehydration in step S4; c - Photograph of hemp fiber obtained after humidification and conditioning treatment in step S4.

[0037] Figure 2 A photograph of the hemp fiber nonwoven fabric prepared in Example 1:

[0038] a-Photo of single-layer hemp fiber nonwoven fabric; b-Photo of multi-layer hemp fiber nonwoven fabric;

[0039] Figure 3 This is a scanning electron microscope image of the hemp fiber obtained after step S1 in Example 1.

[0040] Figure 4 This is a scanning electron microscope (SEM) image of the hemp fibers obtained after step S5 in Example 1.

[0041] Figure 5 A photograph of the sanitary napkin product provided in Application Example 1:

[0042] a - Photo of the sanitary napkin product unfolded; b - Photo of the sanitary napkin product folded.

[0043] Figure 6A photograph of the adult pull-up diaper product provided in Application Example 2:

[0044] a - Photo of the outer side of an adult pull-up diaper; b - Photo of the inner side of an adult pull-up diaper. Detailed Implementation

[0045] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0046] In this invention, the technical features described in an open-ended manner include both closed-ended technical solutions composed of the listed features and open-ended technical solutions that include the listed features.

[0047] In this invention, numerical ranges are involved. Unless otherwise specified, the numerical ranges are considered continuous and include the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to integers, it includes every integer between the minimum and maximum values ​​of the range. Additionally, when multiple ranges are provided to describe features or characteristics, the ranges may be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are included.

[0048] Unless otherwise specified, all reagents or instruments used in this invention are commercially available products.

[0049] In one embodiment of the present invention, a hemp fiber nonwoven fabric is provided, wherein the hemp fiber nonwoven fabric is composed of hemp fibers; the hemp fibers contain macropores with a pore size >10μm, mesopores with a pore size of 1-10μm and micropores with a pore size <1μm, and the total porosity of the hemp fibers is 30-50%.

[0050] In the hemp fiber, the porosity of macropores accounts for 48-65% of the total porosity, the porosity of mesopores accounts for 24-50% of the total porosity, and the porosity of micropores accounts for 2-12% of the total porosity.

[0051] When the moisture regain of the hemp fiber nonwoven fabric increases from 0% to 100%, the flexural stiffness decreases by ≥2%.

[0052] The hemp fiber nonwoven fabric provided by this invention has good air permeability and antibacterial properties, as well as good liquid evaporation rate (liquids include water, blood, etc.) and softness.

[0053] Specifically, in the first aspect, the hemp fiber nonwoven fabric provided by this invention is composed of 100% virgin natural hemp fiber. Because existing methods of preparing hemp fiber fail to fundamentally solve the problems of coarseness and hardness, it is difficult to spin 100% virgin natural hemp fiber. Solving the coarseness and hardness problems would also result in excessive damage to the hemp fiber structure, leading to a significant decrease in the air permeability and antibacterial properties of the hemp fiber. Therefore, the all-hemp fiber nonwoven fabrics disclosed in the prior art are not composed of 100% natural virgin hemp fiber, but rather involve chemical modification of the virgin hemp fiber to improve the antibacterial properties of the product, or mixing the virgin hemp fiber with other fibers such as chemical fibers to reduce production difficulty. This invention, by controlling the specific pore structure and porosity of hemp fiber, can achieve the preparation of hemp fiber nonwoven fabric from 100% virgin natural hemp fiber without chemical modification, ensuring the raw material is natural and safe. Furthermore, it eliminates the need to consider the blending ratio with other fibers, making the raw material simple and the preparation convenient.

[0054] Secondly, the total porosity of hemp fibers in hemp fiber nonwoven fabric is 30-50%, with macropores (>10μm) accounting for 48-65%, mesopores (1-10μm) accounting for 24-50%, and micropores (<1μm) accounting for 2-12%. This range of total porosity and the proportion of macropores, mesopores, and micropores can better maintain the good natural properties of the original hemp fibers. It can even further improve the air permeability, antibacterial properties, and liquid evaporation rate of hemp fiber nonwoven fabric without modifying the hemp fibers, thus achieving superior comprehensive performance of hemp fiber nonwoven fabric prepared from original hemp fibers.

[0055] Thirdly, the hemp fiber nonwoven fabric provided by this invention uses 100% virgin hemp fiber and controls the pore structure and porosity of the hemp fiber within the range given in this invention. While maintaining the good natural properties of hemp fiber as much as possible, it can also effectively avoid the rigidity problem of hemp fiber. When the moisture regain of the prepared hemp fiber nonwoven fabric increases from 0% to 100%, the bending stiffness decreases by ≥2%. This decrease in bending stiffness can ensure that the hemp fiber fabric has good softness, is gentle and non-irritating, and has even better softness after absorbing liquid. Existing nonwoven fabrics made from hemp fiber blends or other fibers do not have the characteristic of being softer after absorbing liquid. Instead, they show an increase in hardness after absorbing liquid. That is, the hemp fiber nonwoven fabric prepared by this invention has a better user experience than nonwoven fabrics in the prior art.

[0056] For example, the total porosity of hemp fibers can be any point value or any two-point range between 30% and 50%, such as 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, etc.

[0057] For example, in the hemp fiber, the proportion of macropore porosity to total porosity can be any point value or any two points between 48% and 65%, such as 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, etc.

[0058] For example, in the hemp fiber, the porosity of the mesopores to the total porosity can be any point value or any two points between 24% and 50%, such as 24%, 26%, 28%, 30%, 32%, 34%, 36%, 38%, 40%, 42%, 44%, 46%, 48%, 50%, etc.

[0059] For example, in the hemp fiber, the porosity of the small pores to the total porosity can be any point value or any two points between 2% and 12%, such as 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, etc.

[0060] It should be noted that the total porosity of hemp fibers, as well as the porosities of macropores, mesopores, and micropores, were obtained through mercury porosimetry. Specifically, the mercury porosimetry method includes the following steps: drying hemp fibers at 50°C to constant weight (mass change rate less than 1% over 1 hour), then cutting them into 1cm segments with a mass <2g, and then placing the cut hemp fibers into a mercury porosimetry instrument for testing; the mercury porosimetry utilizes the conductivity of mercury, with a sensor collecting electrical information and converting it into a change in mercury, subsequently obtaining porosity information.

[0061] The pore radii of macropores, mesopores, and micropores are calculated using the Waschburn equation (Pr = -2γcosθ), where the interfacial tension γ between mercury and air is 0.485 N / m, the contact angle θ between mercury and the material is 130°, the pore radius r is in nm, and P is the applied external pressure in Psia.

[0062] For example, when the moisture regain of the hemp fiber nonwoven fabric increases from 0% to 100%, the decrease in bending stiffness can be any point value or any two-point range value of ≥2%, such as 2-6%, 2-4%, 4-6%, 3-5%, etc., or 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0%, 5.5%, 6.0%, etc.

[0063] It should be noted that when the moisture regain of hemp fiber nonwoven fabric increases from 0% to 100%, the decrease in bending stiffness is equal to (bending stiffness at 0% moisture regain - bending stiffness at 100% moisture regain) / bending stiffness at 0% moisture regain × 100%.

[0064] The bending stiffness of the hemp fiber nonwoven fabric at 0% or 100% moisture regain was tested using a YG207N automatic fabric stiffness tester, specifically as follows:

[0065] (1) Determine and calculate the mass per unit area of ​​the sample according to GB / T4669;

[0066] (2) Randomly cut 12 samples with a sample size of (25±1)mm×(250+1)mm; the long side of 6 samples is parallel to the longitudinal direction of the hemp fiber nonwoven fabric, and the long side of 6 samples is parallel to the transverse direction of the hemp fiber nonwoven fabric; the samples are taken at least 100mm away from the edge of the hemp fiber nonwoven fabric.

[0067] (3) Place the sample on the platform, with one end of the sample coinciding with the front edge of the platform. Place the upper pressure plate on the sample and align it.

[0068] (4) Press the start button and push the sample forward at a certain speed so that the sample extends beyond the front edge of the platform and bends under its own weight until the extended end of the sample contacts the inclined plane. Record the extension length of the sample.

[0069] (5) Take half of the extension length as the bending length, record four bending lengths for each specimen, and calculate the average bending length of each specimen accordingly; calculate the average bending length C of each specimen in both directions, in centimeters; calculate the average bending stiffness per unit width in both directions according to Equation I, and retain three significant figures.

[0070] Equation I: G = m × C 3 ×10 -3 ;

[0071] Where G is the bending stiffness per unit width, measured in millinewtons per centimeter (mN·cm); and m is the mass per unit area of ​​the specimen, measured in grams per square meter (g / m²). 2 C is the average bending length of the sample, in centimeters (cm).

[0072] In addition, a moisture regain of 0% means the hemp fiber nonwoven fabric is in its dry state; a moisture regain of 100% means the hemp fiber nonwoven fabric has absorbed water and its weight is twice its dry weight; to achieve a moisture regain of 100%, water is sprayed onto the surface of the hemp fiber nonwoven fabric using a sprayer, combed, and left to stand in a sealed bag for more than 4 hours, then the hemp fiber nonwoven fabric is taken out, weighed, and the moisture regain is calculated to 100%.

[0073] In one embodiment, when the moisture regain of the hemp fiber nonwoven fabric increases from 0% to 100%, the flexural stiffness decreases by 3-5%.

[0074] For example, when the moisture regain of the hemp fiber nonwoven fabric increases from 0% to 100%, the decrease in bending stiffness can be any point value or any two points between 3 and 5%, such as 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5.0%, etc.

[0075] This invention has found that when the moisture regain of the hemp fiber nonwoven fabric increases from 0% to 100%, the decrease in bending stiffness not only affects the softness of the hemp fiber nonwoven fabric, but also has a certain impact on the liquid evaporation rate and antibacterial properties of the product. When the decrease in bending stiffness is further selected to be 3-5%, the resulting product has better softness after absorbing liquid and a higher liquid evaporation rate, meaning that the liquid can evaporate quickly after absorption, maintaining a dry user experience, and also has better antibacterial properties.

[0076] In one embodiment, the total porosity of the hemp fibers is 36-48%.

[0077] This invention has found that hemp fiber has a loose and porous structure, but the porosity range of hemp fiber obtained by different treatment methods is different. The porosity of hemp fiber not only affects the air permeability of hemp fiber nonwoven fabric, but also its antibacterial effect and softness. When the porosity of hemp fiber is further selected to be 36-48%, the resulting hemp fiber nonwoven fabric has better air permeability and antibacterial properties, a larger liquid evaporation rate, and excellent softness.

[0078] In one embodiment, the macropores in the hemp fibers account for 51-60% of the total porosity.

[0079] In one embodiment, the porosity of mesopores in the hemp fibers accounts for 36-44% of the total porosity.

[0080] In one embodiment, the porosity of the hemp fibers is 3-6% of the total porosity.

[0081] The present invention has found that when the porosity of the macropores, mesopores and micropores of hemp fibers is further selected to be within the above-mentioned ranges, the resulting hemp fiber nonwoven fabric has better overall performance.

[0082] In one embodiment, the fineness of the hemp fiber is >2000 Nm and the length is >28 mm.

[0083] In one embodiment, the hemp fiber has a fineness of 2240-2600 Nm and a length of 28.3-35 mm.

[0084] It should be noted that the fineness of the hemp fiber was obtained by mid-section weighing method according to GB / T 18147.4-2015, and the length was obtained by hand-group weighing method according to GB / T 18147.3-2015.

[0085] For example, the fineness of hemp fiber can be any point value or any two points between 2240-2600 Nm, such as 2240 Nm, 2260 Nm, 2280 Nm, 2300 Nm, 2320 Nm, 2340 Nm, 2360 Nm, 2380 Nm, 2400 Nm, 2420 Nm, 2440 Nm, 2460 Nm, 2480 Nm, 2500 Nm, 2520 Nm, 2540 Nm, 2560 Nm, 2580 Nm, 2600 Nm, etc. The length of hemp fibers can be any point value or any two points between 28.3-35mm, such as 28.3mm, 28.5mm, 28.8mm, 29.0mm, 29.3mm, 29.5mm, 29.8mm, 30.0mm, 30.3mm, 30.5mm, 30.8mm, 31.0mm, 31.3mm, 31.5mm, 31.8mm, 32.0mm, 32.3mm, 32.5mm, 32.8mm, 33.0mm, 33.3mm, 33.5mm, 33.8mm, 34.0mm, 34.3mm, 34.5mm, 34.8mm, 35.0mm, etc.

[0086] The present invention has found that the fineness and length of hemp fibers can affect the softness and liquid evaporation rate of hemp fibers to a certain extent. When the fineness and length of hemp fibers are further selected within the above range, the resulting product has better softness and faster liquid evaporation.

[0087] In one embodiment of the present invention, the present invention provides a method for preparing the hemp fiber nonwoven fabric, the method comprising the following steps:

[0088] S1. Crush and pound the hemp stalks after rain and dew to obtain hemp bark;

[0089] S2. The hemp fiber is degummed once using a compound bacterial solution, wherein the compound bacterial solution contains alkalophilic Bacillus and fluorescent Pseudomonas in a mass ratio of 1:(1-2);

[0090] S3. Place the hemp fibers after the first degumming in step S2 into a secondary degumming solution for secondary degumming to obtain degummed hemp fibers; the pH value of the secondary degumming solution is 12-13.5, and the volume concentration of hydrogen peroxide in the secondary degumming solution is 9-10 mL / L.

[0091] S4. The degummed hemp fibers are soaked in oil, followed by deoiling and dehydration, and then subjected to humidification and curing treatment; the relative humidity of the humidification and curing treatment is 60-70%, and the temperature is ≥25℃.

[0092] S5. After humidification and conditioning treatment, open and comb the hemp fibers to obtain hemp fibers with a length >28mm and a residual glue rate of 5-20%.

[0093] S6. Hemp fibers are opened, cleaned, combed, and laid into a web to obtain a fiber web; wherein the basis weight of the fiber web is ≥33g / m³. 2 ;

[0094] S7. The fiber web is sequentially subjected to hydroentangling and post-hydroentangling treatment to obtain hemp fiber nonwoven fabric; wherein, the hydroentangling process includes four hydroentangling processes, and the hydroentangling pressures in the first to fourth hydroentangling processes are 35-45 bar, 60-70 bar, 75-85 bar, and 85-95 bar, respectively.

[0095] The method for preparing hemp fiber nonwoven fabric provided by this invention does not introduce special equipment, is easy to operate, can efficiently produce hemp fiber nonwoven fabric, and is beneficial to actual production.

[0096] It should be noted that the residual gum rate of hemp fiber was obtained by referring to Part 2 of GB / T 18147.2-2008, which describes the test method for residual gum rate.

[0097] For example, the residual gum content of hemp fiber can be any point value or any two points between 5% and 20%, such as 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, etc.

[0098] The present invention has found that the sequential first and second degumming processes have a certain impact on the porosity of hemp fibers and the proportion of different pore sizes. When the first and second degumming processes of the present invention are selected, the pore structure characteristics of the hemp fibers prepared are within the scope of the present invention, thereby enabling the preparation of hemp fiber nonwoven fabrics with excellent comprehensive performance.

[0099] Specifically, this invention specifies that the compound bacterial solution used in the primary degumming process contains *Bacillus alkalophilus* and *Pseudomonas fluorescens* in a mass ratio of 1:(1-2). That is, *Bacillus alkalophilus* and *Pseudomonas fluorescens* are selected for their combination. On the one hand, *Bacillus alkalophilus* and *Pseudomonas fluorescens* are naturally abundant and easily obtained; on the other hand, *Bacillus alkalophilus* can produce alkaline β-mannanase effectively, while *Pseudomonas fluorescens* can stably produce pectinase and hemicellulase. The combination of these two in a certain proportion forms a compound bacterial solution. Under the combined action of the aforementioned enzymes and other enzymes produced, it can not only improve the degumming process but also... The combined effect of the two degumming processes achieves excellent degumming results and can balance the content of cellulose, hemicellulose, and lignin in hemp fibers within a suitable degumming rate range. This results in suitable cohesion of the hemp fibers during subsequent carding and web laying, enabling successful carding and web laying to produce hemp fiber nonwoven fabrics. Furthermore, the primary degumming process of the aforementioned specific types of microorganisms is relatively mild, and the enzymes produced have excellent synergistic effects, effectively and gently enzymatically hydrolyzing the gum components in hemp bark without damaging the basic supporting structure of the hemp fibers, thereby altering the pore structure and porosity of the hemp fibers. The secondary degumming process specified in this invention involves placing the hemp fibers, after primary degumming, in a secondary degumming solution with a pH of 12-13.5 and a hydrogen peroxide concentration of 9-10 mL / L. This secondary degumming, performed after the primary degumming, within a specific pH range and with a specific hydrogen peroxide concentration, further removes the gum, maintains the balance of vitamin, lignin, and hemicellulose content, thereby altering the pore structure and porosity of the hemp fibers and maintaining suitable bonding between them. This lays the foundation for achieving the excellent overall performance of hemp fiber nonwoven fabrics.

[0100] In one embodiment, the pH value of the secondary degumming solution is achieved by adding sodium hydroxide to achieve a pH value of 12-13.5.

[0101] This invention achieves a pH value of 12-13.5 for the secondary degumming solution by selecting natural, non-toxic, and harmless sodium hydroxide. This not only ensures good environmental protection but also leaves no residue. As a result, the hemp fiber nonwoven fabric prepared from hemp fibers obtained by adjusting the pH value with sodium hydroxide is mild, non-irritating, and highly safe.

[0102] In one embodiment, the concentration of bacteria in the compound bacterial solution is (0.1-10)×10⁻⁶. -8 CFU / mL.

[0103] In one embodiment, the solvent for the composite bacterial solution is water. The composite bacterial solution is prepared by adding *Bacillus alkalophilus* and *Pseudomonas fluorescens* to water at a mass ratio of 1:(1-2) to obtain the composite bacterial solution.

[0104] In one embodiment, the solid-liquid ratio for a single degumming step is 1 g: (5-15) mL.

[0105] In one embodiment, the temperature for degumming is 32-36°C and the time is 6-8 hours.

[0106] In one embodiment, the solid-liquid ratio of the secondary degumming is 1g:(8-12)mL.

[0107] In one embodiment, the temperature for the secondary degumming is 98-100°C, and the time for the secondary degumming is 60-120 minutes.

[0108] This invention has found that the combination of specific types of microorganisms, as well as the pH value of the secondary degumming solution and the volume concentration of hydrogen peroxide, can affect the pore structure characteristics of hemp fibers during primary and secondary degumming processes. Further optimization of parameters for primary and secondary degumming processes can effectively improve degumming efficiency.

[0109] In one embodiment, during the secondary degumming process, additives and penetrants may also be added to the secondary degumming solution.

[0110] This invention does not have specific requirements for the selection of additives and penetrants, and can select substances that are conventionally selectable in the art. For example, the additives include at least one of sodium metabisulfite and trisodium phosphate, and the penetrants include at least one of penetrants JFC series, penetrant OE-35, penetrant SF, penetrant T, penetrant OEP-70, and penetrant AEP; the mass concentration of the additives and penetrants can be 0.8-1 g / mL.

[0111] This invention has found that humidification and conditioning treatment can prevent damage to hemp fibers during subsequent opening, carding, and web-laying stages, thereby better preserving the structural and functional characteristics of hemp fibers and achieving good overall performance. For example, the relative humidity during humidification and conditioning treatment can be any point value or any two points within a range of 60-70%, such as 60%, 62%, 64%, 66%, 68%, 70%, etc.; the temperature can be any point value or any two points within a range of ≥25℃, such as 25-30℃, 25-35℃, 25-40℃, etc.

[0112] In one embodiment, the length of the hemp fiber is 28.3-35 mm.

[0113] The present invention has found that the length of hemp fibers has a significant impact on the success of web laying. When the length of hemp fibers is selected within the range given in this invention, especially 28.3-35 mm, web laying and preparation of hemp fiber nonwoven fabric can be successfully achieved. For example, the length of hemp fibers can be any point value or any two points within the range of 28.3-35mm, such as 28.3mm, 28.5mm, 28.8mm, 29.0mm, 29.3mm, 29.5mm, 29.8mm, 30.0mm, 30.3mm, 30.5mm, 30.8mm, 31.0mm, 31.3mm, 31.5mm, 31.8mm, 32.0mm, 32.3mm, 32.5mm, 32.8mm, 33.0mm, 33.3mm, 33.5mm, 33.8mm, 34.0mm, 34.3mm, 34.5mm, 34.8mm, 35.0mm, etc.

[0114] This invention reveals that the web-laying method and the quantitative range of the fiber web during the nonwoven fabric preparation process affect the uniformity of hemp fiber arrangement and the interaction between hemp fibers. It also influences the pore structure of the prepared hemp fibers, thus affecting the overall performance of the nonwoven fabric. Using the cross-laying method and the quantitative range of the fiber web within the parameters provided in this invention can ensure uniform stress distribution in the prepared hemp fiber nonwoven fabric, avoiding problems such as localized stress concentration. Furthermore, it can further improve the pore structure of the hemp fibers used in the web-laying process. This, in turn, helps achieve good air permeability, antibacterial properties, softness, and low liquid evaporation rate in the hemp fiber nonwoven fabric.

[0115] In one embodiment, the basis weight of the fiber web in the web laying is 33-38 g / m². 2 .

[0116] For example, the basis weight of the fiber web in the web laying can be 33-38 g / m². 2 The value can be any point or any range between two points, for example, 33g / m 2 34g / m 2 35g / m 2 36g / m 2 37g / m 2 37g / m 2 wait.

[0117] This invention has discovered that the hydroentangling process affects the entanglement effect of the hemp fiber web formed after web laying, and the parameters in the hydroentangling process also affect the pore structure of the hemp fibers in the web. By selecting the multi-stage hydroentangling process of this invention, specifically a four-stage hydroentangling process to hydroentangle the hemp fiber web after web laying, and limiting the hydroentangling pressure range of the first to fourth stages, the entanglement effect of the hemp fiber web can be effectively enhanced, and the pore structure of the hemp fibers in the web can be further improved. This results in the subsequent preparation of hemp fiber nonwoven fabric with good air permeability and antibacterial properties, as well as excellent softness and excellent liquid evaporation rate.

[0118] For example, the hydroentangling pressure in the first hydroentangling process can be any point value or any two-point range between 35 and 45 bar, such as 35 bar, 37 bar, 39 bar, 40 bar, 42 bar, 45 bar, etc.; the hydroentangling pressure in the second hydroentangling process can be any point value or any two-point range between 60 and 70 bar, such as 60 bar, 62 bar, 64 bar, 66 bar, 68 bar, 70 bar, etc.; the hydroentangling pressure in the third hydroentangling process can be any point value or any two-point range between 75 and 85 bar, such as 75 bar, 77 bar, 79 bar, 80 bar, 82 bar, 85 bar, etc.; the hydroentangling pressure in the fourth hydroentangling process can be any point value or any two-point range between 85 and 95 bar, such as 85 bar, 87 bar, 89 bar, 90 bar, 92 bar, 95 bar, etc.

[0119] This invention does not require specific methods for processing hemp under rain and dew; conventional methods can be used, which involve spreading the hemp stems flat in the field and allowing them to degummed under sunlight and rain. Factors affecting hemp processing under rain and dew include temperature, time, moisture, light, and the type of microorganisms.

[0120] In one embodiment, the degumming process further includes inactivation, filtration, collection of filter residue, and washing.

[0121] In one embodiment, the inactivation temperature is 95-100°C.

[0122] In one embodiment, the cleaning is performed by washing with water.

[0123] In one embodiment, the secondary degumming process further includes oxygen bleaching and acid washing.

[0124] Oxygen bleaching involves immersing hemp fibers, after secondary degumming, in an oxygen bleaching agent. This invention does not impose any particular limitation on the selection of the oxygen bleaching agent; a stabilizer may also be added to the oxygen bleaching agent. The stabilizer can be conventionally selected, such as at least one of sodium silicate, non-silicone stabilizers, polyhydroxycarboxylate salts, magnesium salts, and nitride stabilizers, with a stabilizer mass percentage of 0.3-0.6%.

[0125] The present invention does not have special requirements for the temperature and time of immersion during oxygen bleaching; the effects of the present invention can be achieved within the conventional immersion temperature and time range in the art.

[0126] For example, the impregnation temperature is 98-100°C and the time is 60-90 minutes.

[0127] This invention does not have special requirements for acid washing. The pH value of the system after acid washing is 7, which can completely neutralize the natural alkaline substances added during the secondary degumming process, ensuring the mildness, non-irritation and safety of hemp fibers.

[0128] For example, pickling can be performed using acetic acid, with the acetic acid added at a ratio of 0.01-0.02%.

[0129] In one embodiment, in step S4, the oil used in the oil immersion treatment is a mixture of vegetable oil, mineral oil and water, and the treatment time is 10-14 hours.

[0130] This invention has found that oil impregnation can increase the lubricity between hemp fibers and reduce the damage to hemp fibers caused by opening, combing, and web laying during the subsequent preparation of hemp fiber nonwoven fabric. This can better maintain or even improve the structural characteristics of the prepared hemp fibers, and achieve the preparation of hemp fiber nonwoven fabric with excellent overall performance.

[0131] This invention does not have special requirements on the type of vegetable oil and mineral oil; any vegetable oil and mineral oil that can be conventionally used for fiber impregnation can be used. For example, the vegetable oil includes at least one of palm oil, soybean oil, rapeseed oil, peanut oil, corn oil, and olive oil; the mineral oil includes at least one of mineral oil, petrolatum, mineral wax, paraffin wax, microcrystalline wax, ceresin wax, and lignite wax.

[0132] In one embodiment, the mass ratio of vegetable oil to mineral oil is (0.8-1.2):1.

[0133] The present invention has found that when the mass ratio of vegetable oil to mineral oil in the oil immersion treatment is (0.8-1.2):1, the oil immersion effect is better.

[0134] For example, the oil immersion time can be any point value or any two-point range value between 50 and 70 minutes, such as 50 minutes, 55 minutes, 60 minutes, 65 minutes, 70 minutes, etc.

[0135] In one embodiment, the oil immersion treatment is followed by a 10-14 hour period of rest before deoiling and dehydration.

[0136] In one embodiment, the humidification and conditioning treatment in step S4 takes 12-48 hours.

[0137] This invention does not have special requirements for the loosening and combing after humidification and conditioning treatment; conventional operations in the field can be used.

[0138] In one embodiment, in step S6, the cleaning process involves pressing the hemp fibers and then opening, removing impurities, and mixing them using a carding machine.

[0139] In one embodiment, in step S6, combing involves further loosening and combing the hemp fibers after they have been opened and cleaned to form a fiber web.

[0140] This invention does not have special requirements for opening and cleaning, and can use conventional equipment and conventional operating methods in this field.

[0141] In one embodiment, step S7, the post-hydroentanglement treatment includes oxygen bleaching, drying, and impurity removal. Oxygen bleaching involves impregnating the hydroentangled hemp fibers in an oxygen bleaching agent.

[0142] This invention does not have special requirements for the selection of oxygen bleaching agents; any conventional oxygen bleaching agent that can be used for nonwoven fabrics can be used.

[0143] For example, the oxygen bleaching agent may be an aqueous solution of hydrogen peroxide and sodium hydroxide, wherein the mass percentage of hydrogen peroxide and the mass percentage of sodium hydroxide in the oxygen bleaching agent are 1.5-2%.

[0144] The present invention does not have special requirements for the temperature and time of immersion during oxygen bleaching; the effects of the present invention can be achieved within the conventional immersion temperature and time range in the art.

[0145] For example, the impregnation temperature is 98-100°C and the time is 60-90 minutes.

[0146] The present invention does not have special requirements for the drying process and the impurity removal process. Conventional drying methods and impurity removal methods in the field can be used to achieve the purpose of the present invention.

[0147] In one embodiment of the present invention, the present invention provides the application of hemp fiber nonwoven fabric in the preparation of hygiene products.

[0148] The hemp fiber nonwoven fabric provided by this invention possesses excellent air permeability, antibacterial properties, and good softness. In particular, its bending stiffness shows a significant decreasing trend after liquid absorption, indicating a tendency to become softer with use, resulting in a superior user experience. Simultaneously, the hemp fiber nonwoven fabric also exhibits a good liquid evaporation rate, allowing liquid to evaporate quickly after absorption, thus maintaining good dryness and further preventing microbial growth, thereby enhancing its antibacterial properties. Therefore, it can be widely used in the preparation of hygiene products.

[0149] In one embodiment, the sanitary products include any one of sanitary napkins, panty liners, adhesive bandages, diapers, adult pull-up pants, and disposable underwear.

[0150] In one embodiment of the present invention, a sanitary napkin is provided, wherein the surface layer of the sanitary napkin is the hemp fiber nonwoven fabric described in the present invention.

[0151] The sanitary napkin surface layer provided by this invention uses the hemp fiber nonwoven fabric of this invention. Firstly, the hemp fiber nonwoven fabric has high breathability, ensuring good breathability when applied to the preparation of the sanitary napkin surface layer. Secondly, the hemp fiber nonwoven fabric has good antibacterial properties, inhibiting the growth of microorganisms and achieving excellent antibacterial effects when applied to the surface layer. Thirdly, hemp fiber has excellent softness, which increases after absorbing liquid, preventing friction and irritation to the skin when applied to the sanitary napkin surface layer, providing a gentle and comfortable user experience. Fourthly, hemp fiber has a good liquid evaporation rate, allowing for rapid evaporation after liquid absorption when used as a surface layer in the preparation of sanitary napkins, improving dryness during use, enhancing the user experience, and avoiding the problem of microbial growth caused by slow liquid evaporation, thus ensuring a long-lasting antibacterial effect.

[0152] In one embodiment, the sanitary napkin further includes an absorbent layer and a bottom layer.

[0153] This invention does not impose any particular restrictions on the materials used for the absorbent layer and the bottom layer of sanitary napkins; any materials that can be conventionally used for the absorbent layer and the bottom layer of sanitary napkins can be used.

[0154] For example, the material of the absorbent layer may be a polymer absorbent material, fiber, etc., wherein the polymer absorbent material includes at least one of polyethylene and polypropylene, and the fiber includes at least one of cotton fiber and bamboo pulp paper.

[0155] For example, the underlying layer may be a PE film, a non-fabric composite film, etc.

[0156] Example 1

[0157] This invention provides a hemp fiber nonwoven fabric, the preparation method of which includes the following steps:

[0158] S1. Place hemp stalks in a field for dew reflux to obtain dew-fed hemp. The dew reflux temperature is 18-30℃, and the time is 25 days. After dew reflux, collect the hemp stalks and break them up. Then remove the woody parts and impurities from the broken hemp stalks to obtain hemp fiber. A photograph of the obtained hemp fiber is shown below. Figure 1 As shown in Figure a;

[0159] S2. Place the hemp fiber in a biological degumming pot, and add a compound bacterial solution at 35℃ according to a solid-liquid ratio of 1g:10mL (the solvent in the compound bacterial solution is water, and the total concentration of Bacillus alkalophilus and Pseudomonas fluorescens in the compound bacterial solution is 10). -8 The concentration of CFU / mL was 1:1 (the preservation number of Bacillus alkalophilus and Pseudomonas fluorescens was CCTCC M2016316 and the preservation number of Pseudomonas fluorescens was CGMCC No. 3839). The bacteria were subjected to biological degumming at 35°C for 7 hours. After the biological degumming process, the bacteria were heated to 95°C for inactivation, then filtered, and the filter residue was collected and washed with water.

[0160] S3. Add the filter residue washed in step S2 and the secondary degumming solution to the secondary degumming pot at a solid-liquid ratio of 1g:10mL, and degumme at 98℃ for 90min. After the secondary degumming is completed, take out the hemp fiber, wash it three times with water, and then add it to the oxygen bleaching agent at a solid-liquid ratio of 1g:10mL. Oxy-bleach at 98℃ for 60min. After the oxygen bleaching is completed, wash it three times with water, and then add an acetic acid aqueous solution (the mass percentage of acetic acid in the acetic acid aqueous solution is 0.02%) to wash until the pH value of the system is 7. Finally, wash with water and spin dry.

[0161] The secondary degumming solution has a pH of 12.4 and contains sodium hydroxide, hydrogen peroxide, sodium metabisulfite, trisodium phosphate, and penetrant JFC as the solvent. The volume concentration of hydrogen peroxide in the secondary degumming solution is 10 mL / L, the mass concentration of sodium metabisulfite is 0.9 g / L, the mass concentration of trisodium phosphate is 0.9 g / L, and the mass concentration of penetrant JFC is 0.9 g / L.

[0162] The solutes in the oxygen bleaching agent include hydrogen peroxide, sodium hydroxide, and sodium silicate, and the solvent is water; in the oxygen bleaching agent, the mass percentage of hydrogen peroxide is 2%, the mass percentage of sodium hydroxide is 0.5%, and the mass percentage of sodium silicate is 0.5%.

[0163] S4. Immerse the hemp fibers spun dry in step S3 in the oil-impregnating agent and keep them for 60 minutes. After the oil impregnation is completed, drain the oil-impregnating agent and let them stand for 12 hours. Then, remove the oil and water. Next, humidify and cure the hemp fibers after the oil and water removal. Place them in an environment with a relative humidity of 65% and a temperature of 30°C for 24 hours.

[0164] The solutes in the oil extractant are soybean oil and mineral oil in a mass ratio of 1:1, and the solvent is water, with the mass ratio of soybean oil and mineral oil to water being 1:10.

[0165] A photograph of hemp fibers after the oil and water removal process is shown below. Figure 1 As shown in Figure b, the photograph of hemp fibers after the humidification and conditioning treatment is as follows. Figure 1 As shown in c;

[0166] S5. Loosen, comb, and compact the hemp fibers after the humidification and conditioning treatment in step S4 to obtain hemp fibers;

[0167] S6. The hemp fibers prepared in step S5 are opened, cleaned, and mixed using a carding machine. Then, they are fed into a hemp bin via a hemp suction machine, followed by carding into a fiber web by multiple carding machines. The fiber webs formed by the multiple carding machines are then combined, stacked, and cross-laid, with the web-laying parameters controlled to achieve a fiber basis weight of 36 g / m². 2 ;

[0168] S7. The fiber web after cross-laying in step S6 is hydroentangled using a rotary drum hydroentanglement machine. A total of four hydroentanglement processes are performed. The hydroentanglement pressures in the first to fourth hydroentanglement processes are 40 bar, 65 bar, 80 bar, and 90 bar, respectively. After hydroentanglement, a hydroentangled hemp fiber nonwoven fabric is obtained. Then, the hydroentangled hemp fiber nonwoven fabric is added to an oxygen bleaching agent at a solid-liquid ratio of 1g:10mL and oxygen bleached at 98℃ for 75 minutes. After oxygen bleaching, it is washed three times with water and spun dry. Finally, it is dried and impurities are removed to obtain a hemp fiber nonwoven fabric.

[0169] The oxygen bleaching agent contains hydrogen peroxide and sodium hydroxide as solutes and water as solvent; the mass percentage of hydrogen peroxide in the oxygen bleaching agent is 2%, and the mass percentage of sodium hydroxide is 1.5%.

[0170] A photograph of the prepared hemp fiber nonwoven fabric is shown below. Figure 2 As shown in Figure a, where Figure 2 The image in Figure 'b' represents a photograph taken when hemp fiber nonwoven fabric is further processed into multiple layers.

[0171] Examples 2-6 and Comparative Examples 1-3

[0172] Examples 2-6 and Comparative Examples 1-3 each provide a hemp fiber nonwoven fabric. The parameters of the hemp fiber nonwoven fabrics described in each example and comparative example are shown in Table 1 below.

[0173] Through experiments, the pH value of the secondary degumming solution and the humidity of the humidification curing treatment in the secondary degumming process were adjusted based on Example 1 to achieve the parameters of the hemp fiber nonwoven fabrics in Examples 2-3 in Table 1.

[0174] Through experimentation, the parameters of the hemp fiber nonwoven fabrics in Examples 4-5 in Table 1 were achieved by adjusting the temperatures of the first and second degumming processes based on Example 1.

[0175] Through experiments, the parameters of the hemp fiber nonwoven fabric in Example 6 in Table 1 were achieved by adjusting the mass ratio of alkalophilic Bacillus and fluorescent Pseudomonas in the compound bacterial solution during the first degumming and the volume concentration of hydrogen peroxide in the second degumming solution during the second degumming, based on Example 1.

[0176] Through experiments, the temperature and time of the first and second degumming processes were adjusted based on Example 1 to achieve the parameters of the hemp fiber nonwoven fabric in Comparative Example 1 in Table 1.

[0177] Through experiments, the parameters of the fiber web and the hydroentanglement were adjusted based on Example 1 to achieve the parameters of the hemp fiber nonwoven fabrics in Comparative Examples 2-3 in Table 1.

[0178] It should be noted that Examples 2-6 and Comparative Examples 1-3 include, but are not limited to, the methods by which the inventors, through experimentation, adjusted the parameters in Table 1 as described above. The methods selected and adjusted through experimentation are given only as illustrative examples.

[0179] Table 1

[0180]

[0181]

[0182] The test methods for each parameter in Table 1 above are as follows:

[0183] 1. The total porosity of hemp fibers, the proportion of macropores (pore size > 10 μm), mesopores (pore size 1-10 μm), and micropores (pore size < 1 μm): obtained by mercury porosimetry, specifically as follows:

[0184] After drying hemp fibers at 50°C to constant weight (mass change rate less than 1% in 1 hour), they were cut into 1cm segments with a mass of less than 2g. The cut hemp fibers were then placed in a mercury porosimeter for testing.

[0185] The pore radii of macropores, mesopores, and micropores are calculated using the Waschburn equation (Pr = -2γcosθ), where the interfacial tension γ between mercury and air is 0.485 N / m, the contact angle θ between mercury and the material is 130°, the pore radius r is in nm, and P is the applied external pressure in Psia.

[0186] 2. Length of hemp fibers: The length was determined by the manual grouping and weighing method according to GB / T 18147.3-2015.

[0187] 3. Fineness of hemp fiber: The fineness was obtained by mid-section weighing method according to GB / T 18147.4-2015.

[0188] 4. The test method for the decrease in bending stiffness (ΔG) of hemp fiber nonwoven fabric when the moisture regain increases from 0% to 100% includes the following steps:

[0189] (1) Sample preparation: Take two hemp nonwoven fabric samples. One sample is dried at 50℃ to constant weight (mass change rate of less than 1% in 1 hour) to obtain hemp fiber nonwoven fabric with 0% moisture regain. The other sample is sprayed with water on the surface of hemp fiber nonwoven fabric, combed and left to stand in a sealed bag for more than 4 hours until the mass is twice the mass of hemp fiber nonwoven fabric with 0% moisture regain, which is hemp fiber nonwoven fabric with 100% moisture regain.

[0190] (2) Determine and calculate the mass per unit area of ​​the sample according to GB / T4669;

[0191] (3) Randomly cut 12 samples with a sample size of (25±1)mm×(250+1)mm; the long side of 6 samples is parallel to the longitudinal direction of the hemp fiber nonwoven fabric, and the long side of 6 samples is parallel to the transverse direction of the hemp fiber nonwoven fabric; the samples are taken at least 100mm away from the edge of the hemp fiber nonwoven fabric.

[0192] (4) Place the sample on the platform of the YG207N automatic fabric stiffness tester, with one end of the sample coinciding with the front edge of the platform. Place the upper pressure plate on the sample and align it.

[0193] (5) Press the start button and push the sample forward at a certain speed so that the sample extends beyond the front edge of the platform and bends under its own weight until the extended end of the sample contacts the inclined plane. Record the extension length of the sample.

[0194] (6) Take half of the extension length as the bending length, record four bending lengths for each specimen, and calculate the average bending length of each specimen accordingly; calculate the average bending length C of each specimen in both directions, in centimeters; calculate the average bending stiffness per unit width in both directions according to Equation I, and retain three significant figures.

[0195] Equation I: G = m × C 3 ×10 -3 ;

[0196] Where G is the bending stiffness per unit width, measured in millinewtons per centimeter (mN·cm); and m is the mass per unit area of ​​the specimen, measured in grams per square meter (g / m²). 2 C represents the average bending length of the specimen, in centimeters (cm).

[0197] (7) Calculate the change range through bending stiffness. The decrease range of bending stiffness △G = (bending stiffness at 0% moisture regain - bending stiffness at 100% moisture regain) / bending stiffness at 0% moisture regain × 100.

[0198] Comparative Example 4

[0199] The present invention provides a hemp fiber nonwoven fabric as a comparative example. The only difference between the hemp fiber nonwoven fabric and Example 1 is that the carding parameters were adjusted through experiments to make the length of the hemp fiber 15mm.

[0200] Subsequent processing revealed that the hemp fibers were too short to be successfully cross-laid, thus preventing the formation of hemp nonwoven fabric.

[0201] Comparative Example 5

[0202] This invention provides a hemp fiber nonwoven fabric as a comparative example. The only difference between this hemp fiber nonwoven fabric and Example 1 is that the basis weight of the fiber web in the web laying is 25 g / m². 2 ;

[0203] Subsequent processing revealed that the spunlace fiber web had holes due to the low basis weight of the web during the fabrication process, making it impossible to produce hemp nonwoven fabric.

[0204] Comparative Example 6

[0205] The present invention provides a hemp fiber nonwoven fabric as a comparative example. The only difference between the hemp fiber nonwoven fabric and Example 1 is that the hydroentangling process includes two hydroentangling processes. The hydroentangling pressure in the first hydroentangling process is 40 bar, and the hydroentangling pressure in the second hydroentangling process is 65 bar.

[0206] In subsequent preparation, due to the insufficient number of hydroentanglement processes in the hydroentanglement step, the fiber web could not be completely entangled, thus preventing the formation of hemp nonwoven fabric.

[0207] Comparative Example 7

[0208] The present invention provides a hemp fiber nonwoven fabric as a comparative example. The only difference between the hemp fiber nonwoven fabric and Example 1 is that the hydroentangling process includes four hydroentangling processes, and the hydroentangling pressures in the first to fourth hydroentangling processes are 20 bar, 50 bar, 60 bar and 75 bar respectively.

[0209] In subsequent preparation, the hydroentanglement pressure during the hydroentanglement process was too low, resulting in the inability to completely entangle the fiber web, thus preventing the formation of hemp nonwoven fabric.

[0210] Comparative Example 8

[0211] The present invention provides a hemp fiber nonwoven fabric as a comparative example. The only difference between the hemp fiber nonwoven fabric and Example 1 is that the hydroentangling process includes four hydroentangling processes, and the hydroentangling pressures in the first to fourth hydroentangling processes are 50 bar, 80 bar, 95 bar, and 105 bar, respectively.

[0212] In subsequent processing, the excessively high hydroentangling pressure during the hydroentangling process caused holes in the fiber web, making it impossible to produce hemp nonwoven fabric.

[0213] Comparative Example 9

[0214] The present invention provides a hemp fiber nonwoven fabric as a comparative example. The only difference between the hemp fiber nonwoven fabric and Example 1 is that the hydroentangling process includes four hydroentangling processes, and the hydroentangling pressures in the first to fourth hydroentangling processes are 40 bar, 80 bar, 95 bar and 65 bar, respectively.

[0215] In subsequent preparation, due to the excessive gradient of hydroentanglement pressure during the hydroentanglement process, holes appeared in the fiber web, and some parts could not be completely entangled, so it was impossible to prepare hemp nonwoven fabric.

[0216] Comparative Example 10

[0217] The present invention provides a hemp fiber nonwoven fabric as a comparative example. The only difference between the hemp fiber nonwoven fabric and Example 1 is that the hemp fiber nonwoven fabric is first degummed twice and then degummed once.

[0218] Subsequent processing revealed that the hemp fibers, after undergoing a second degumming process followed by a third degumming process, had a low degree of degumming and a high residual glue rate. This resulted in uneven fiber combing and an inability to successfully cross-lay the web, thus preventing the formation of hemp nonwoven fabric.

[0219] Comparative Example 11

[0220] The present invention provides a hemp fiber nonwoven fabric as a comparative example. The only difference between the hemp fiber nonwoven fabric and Example 1 is that the mass ratio of Bacillus alkalophilus and Pseudomonas fluorescens in the compound bacterial solution is 1:6.

[0221] Subsequent processing revealed that the hemp fibers, due to their bonding strength, experienced significant resistance during carding, leading to breakage and preventing successful web formation. Consequently, hemp nonwoven fabric could not be produced.

[0222] Comparative Example 12

[0223] The present invention provides a hemp fiber nonwoven fabric as a comparative example. The only difference between the hemp fiber nonwoven fabric and Example 1 is that the mass ratio of Bacillus alkalophilus and Pseudomonas fluorescens in the compound bacterial solution is 6:1.

[0224] Subsequent processing revealed that the hemp fibers, due to their bonding strength, experienced significant resistance during carding, leading to breakage and preventing successful web formation. Consequently, hemp nonwoven fabric could not be produced.

[0225] Comparative Example 13

[0226] The present invention provides a hemp fiber nonwoven fabric as a comparative example. The only difference between the hemp fiber nonwoven fabric and Example 1 is that Bacillus subtilis (commonly available, purchased from Beijing Bio-Tech Biotechnology Co., Ltd.) is used instead of Bacillus alkalophilus.

[0227] Subsequent processing revealed that the hemp fibers, due to their bonding strength, experienced significant resistance during carding, leading to breakage and preventing successful web formation. Consequently, hemp nonwoven fabric could not be produced.

[0228] Comparative Example 14

[0229] The present invention provides a hemp fiber nonwoven fabric as a comparative example. The only difference between the hemp fiber nonwoven fabric and Example 1 is that Bacillus subtilis (commonly available commercially, purchased from Beijing Bio-Biotechnology Co., Ltd.) is used instead of Pseudomonas fluorescens.

[0230] Subsequent processing revealed that the hemp fibers, due to their bonding strength, experienced significant resistance during carding, leading to breakage and preventing successful web formation. Consequently, hemp nonwoven fabric could not be produced.

[0231] Comparative Example 15

[0232] The present invention provides a hemp fiber nonwoven fabric as a comparative example. The only difference between the hemp fiber nonwoven fabric and Example 1 is that the pH value of the secondary degumming solution is 10 and the volume concentration of hydrogen peroxide in the secondary degumming solution is 7 mL / L.

[0233] Subsequent processing revealed that the residual glue content of the hemp fibers was too high at 30%, resulting in uneven fiber combing and failure to successfully cross-lay the web, thus preventing the formation of hemp nonwoven fabric.

[0234] Comparative Example 16

[0235] The present invention provides a hemp fiber nonwoven fabric as a comparative example. The only difference between the hemp fiber nonwoven fabric and Example 1 is that the pH value of the secondary degumming solution is 14 and the volume concentration of hydrogen peroxide in the secondary degumming solution is 12 mL / L.

[0236] Subsequent processing revealed that the residual glue content of the hemp fibers was too low at 3%, resulting in excessive fiber combing and failure to successfully cross-lay the web, thus preventing the formation of hemp nonwoven fabric.

[0237] Example 1

[0238] Since comparative examples 4-16 could not produce the corresponding hemp nonwoven fabric, they were not investigated.

[0239] The properties of the hemp fiber nonwoven fabrics prepared in Examples 1-6 and Comparative Examples 1-3 were tested respectively, specifically in the following aspects:

[0240] 1. Breathability

[0241] The test was conducted in accordance with GB / T5453, using a YG(B)461D digital fabric air permeability meter; the air permeability was recorded.

[0242] 2. Softness

[0243] The bending stiffness of hemp fiber nonwoven fabric was tested at 0% and 100% according to the test method for the decrease in bending stiffness when the moisture regain of hemp fiber nonwoven fabric increases from 0% to 100%.

[0244] 3. Liquid evaporation rate

[0245] The liquids included water and blood, and the testing methods remained consistent. The blood used was commercially available artificial blood, specifically:

[0246] (1) Cut 5 pieces of hemp fiber nonwoven fabric, each piece measuring 10cm×10cm, and mark them to distinguish them. The sample should be flat and without wrinkles.

[0247] (2) Condition the cut sample to equilibrium under standard atmospheric conditions;

[0248] (3) Weigh the original weight of the sample, accurate to 0.001g;

[0249] (4) Use a pipette to accurately measure 0.2 mL of liquid and gently drop it onto the sample, keeping the pipette tip no more than 1 cm away from the sample surface;

[0250] (5) When the droplet comes into contact with the sample surface and spreads completely, immediately remove it with tweezers and weigh it, accurate to 0.001g;

[0251] (6) After weighing the sample, hang it vertically in the standard atmosphere and weigh it every (1±0.5) min, accurate to 0.001g.

[0252] (7) The experiment can be ended when the change rate of mass between two consecutive weighings does not exceed 1%, and the time when the mass remains unchanged is recorded.

[0253] 4. Antibacterial properties

[0254] 1) Test method for antibacterial performance of soluble antibacterial (inhibitory) products: The test was conducted in accordance with Appendix C4 of GB 15979-2002; the strains used were Staphylococcus aureus ATCC 6538, Escherichia coli 8099, and Candida albicans ATCC 10231; the test was repeated three times, and the antibacterial rate at 2 min and 20 min was recorded;

[0255] 2) Test method for antibacterial performance of non-leaching antibacterial (inhibitory) products: The test was conducted according to Appendix C5 of GB 15979-2002; the strains used were Staphylococcus aureus ATCC 6538, Escherichia coli 8099, and Candida albicans ATCC 10231; the test was repeated three times, and the average antibacterial rate was recorded; commercially available pure cotton nonwoven fabric was used as a control sample;

[0256] 5. Mildness test

[0257] 1) Skin allergy test:

[0258] (1) Preparation before the experiment: Cut hemp fiber nonwoven fabric into 2.5×2.5cm pieces. 2 The test specimens of various sizes are moistened with physiological saline during the test and used for skin allergy testing.

[0259] (2) The test sample group consisted of 16 healthy white guinea pigs with intact skin. 24 hours before the experiment, the left side of the guinea pig's back was 3×3cm 2 Hair removal was performed within the designated area. The following day, the test sample was moistened and applied directly to the left side of the hair removal area, then covered with a non-irritating plastic film and secured with non-irritating adhesive tape for induced contact, which lasted for 6 hours. Induction was repeated on days 7 and 14 using the same method. On day 28, the test sample was moistened and applied to the right side in a 3×3cm area. 2 Hair removal was performed on the hair-free area (hair removed the day before the experiment), and stimulation was initiated 6 hours later. A negative control group was also included, where the test sample was applied only during stimulation contact. The positive control group underwent the same procedure as the test sample group, but 2,4-dinitrochlorobenzene was used instead of the test sample. The induction concentration was 1%, and the stimulation concentration was 0.2%. Skin reactions were observed 24 and 48 hours after stimulation contact, and the skin reactions were scored according to Table 2.

[0260] Table 2

[0261]

[0262] According to the criteria in Table 2, the number of animals that showed skin reactions (reaction ≥1) was divided by the number of experimental animals in the group to obtain the sensitization rate (%). The sensitization intensity was assessed according to Table 3. When the sensitization rate was 0%, it was judged that no skin allergic reaction was observed.

[0263] Table 3

[0264] Sensitization rate / % 0-8 9-28 29-64 65-80 81-100 Sensitization intensity Very mild Mild moderate strength Extreme strength

[0265] 2) Vaginal mucosal stimulation (single time):

[0266] (1) Take a sample of hemp fiber nonwoven fabric, add sterile physiological saline, and after 24 hours, extract the sample solution for vaginal mucosal irritation test.

[0267] (2) Healthy, young female rabbits were selected and divided into an experimental group and a control group, with 3 rabbits in each group. The sample solution was used as the test sample, and physiological saline was used as the control sample. The animals were fixed supine, exposing the perineum and vaginal opening. The catheter was moistened and gently inserted into the vagina. 2 mL of the test solution or control solution was slowly injected with a syringe. The catheter was then withdrawn, completing the treatment. The animals were euthanized 24 hours later, and the intact vagina was removed. The vagina was visually inspected for signs of congestion, edema, etc. The vagina was fixed in 10% formalin solution for 24 hours. Tissue sections were prepared from the two ends and the center of the vagina for histopathological examination. The irritation response of the vaginal mucosa was scored according to Table 4.

[0268] Table 4

[0269]

[0270] Stimulus response integral = A + B + C + D. According to the standards in Table 4, the stimulation response integrals of the three sites of the three animals in the experimental group are added together and then divided by the total number of observations (number of animals × 3) to obtain the average score of the vaginal mucosal stimulation response of the experimental group. The scoring method for the control group is the same as above. After subtracting the average score of the control group from the average score of the experimental group to obtain the stimulation index, the stimulation intensity is graded according to Table 5.

[0271] Table 5

[0272] Vaginal mucosal irritation index <1 1~<5 5~<9 9~<12 ≥12 Intensity of vaginal mucosal irritation response none Extremely light Mild moderate Severe

[0273] The results of the above effect tests are shown in Table 6-7;

[0274] Table 6

[0275]

[0276] Table 7

[0277]

[0278]

[0279] As can be seen from Example 1 and Comparative Examples 4-16, the inventors of this application have explored a method for preparing nonwoven fabric using 100% hemp fiber as raw material, and have solved the current problem that nonwoven fabric cannot be prepared using 100% hemp fiber, and have successfully prepared a nonwoven fabric made entirely of hemp fiber.

[0280] Furthermore, as shown in Tables 6 and 7, the microstructure and parameters of the hemp fiber nonwoven fabric have a significant impact on its air permeability, antibacterial properties, softness, and liquid evaporation rate. Through research on the microstructure and parameters of the prepared hemp fiber nonwoven fabric, the inventors of this application ultimately obtained a hemp fiber nonwoven fabric with excellent comprehensive performance. Further, as can be seen from Examples 1-6 and Comparative Examples 1-3, the micropore structure and bending stiffness changes of the hemp fiber nonwoven fabric have a significant impact on its air permeability, antibacterial properties, softness, and liquid evaporation rate. When the total porosity of the hemp fibers in the hemp fiber nonwoven fabric provided by this invention, as well as the proportions of macropores, mesopores, and micropores to the total porosity, are within the range given by this invention, and when the moisture regain of the hemp fiber nonwoven fabric increases from 0% to 100%, and the decrease in bending stiffness is within the range given by this invention, the obtained hemp fiber nonwoven fabric exhibits good air permeability, antibacterial properties, softness, and liquid evaporation rate. Specifically, the hemp fiber nonwoven fabrics obtained in Examples 1-6 have an air permeability of over 621.2 mm / s, a flexural stiffness of less than 0.860 mN·cm at 0% moisture regain, a flexural stiffness of less than 0.827 mN·cm at 100% moisture regain, a water evaporation time of less than 30 min, a blood evaporation time of less than 49 min, and show no irritation in irritation tests. In terms of antibacterial tests, the inhibition rates against Escherichia coli, Staphylococcus aureus, and Candida albicans at 20 min are 87.3-96.4%, 75%, and 100%, respectively, in the dissolution antibacterial test. The antibacterial rates against Escherichia coli, Staphylococcus aureus, and Candida albicans in the non-dissolving antibacterial test are between 0-84.6% and 62.4-71.6%, respectively, ranging from 35-49%, 42-61%, and 74-86%. In particular, when the total porosity of hemp fibers and the proportions of macropores, mesopores, and micropores to the total porosity are further selected within the preferred range given in this invention, and when the moisture regain of the hemp fiber nonwoven fabric increases from 0% to 100%, the decrease in bending stiffness is also within the preferred range given in this invention, the overall performance of the obtained hemp fiber nonwoven fabric is even better. Specifically, the hemp fiber nonwoven fabrics obtained in Examples 1-3 have an air permeability of over 678.8 mm / s, a bending stiffness of less than 0.780 mN·cm at 0% moisture regain, a bending stiffness of less than 0.743 mN·cm at 100% moisture regain, a water evaporation time of less than 27 min, a blood evaporation time of less than 45 min, and show no irritation in irritation tests. In terms of antibacterial tests, the inhibition rates against Escherichia coli, Staphylococcus aureus, and Candida albicans at 20 min in the leaching antibacterial test are between 92.5-96.4%, 80.7-84.6%, and 69.8-71.6%, respectively, while the inhibition rates against Escherichia coli, Staphylococcus aureus, and Candida albicans in the non-leaching antibacterial test are between 43-49%, 57-61%, and 84-86%, respectively.

[0281] As can be seen from Examples 1 and Comparative Examples 1-3, when the total porosity of the hemp fibers used to prepare the hemp fiber nonwoven fabric is too low, or the proportions of macropores, mesopores, and micropores in the total porosity are outside the specific range described in this invention, or when the moisture regain of the hemp fiber nonwoven fabric increases from 0% to 100%, and the decrease in bending stiffness is outside the range given in this invention, the overall performance of the obtained hemp fiber nonwoven fabric shows a significant downward trend, especially its antibacterial properties. The different total porosity of the hemp fibers and the different proportions of macropores, mesopores, and micropores not only affect the air permeability of the hemp fiber nonwoven fabric, thus affecting the antibacterial properties of the product, but also affect the distribution and content of antibacterial groups on the hemp fibers in the hemp fiber nonwoven fabric, thereby affecting the antibacterial properties of the product. In other words, the antibacterial properties of the obtained hemp fiber nonwoven fabric are affected by many factors, including the total porosity of the hemp fibers, the proportions of macropores, mesopores, and micropores in the hemp fibers, and the distribution and content of antibacterial groups in the hemp fibers. Therefore, although the total porosity of Comparative Example 3 is within the scope of this invention, its antibacterial rate was found to be low in multiple parallel tests. It is speculated that this is because the proportion of macropores, mesopores and micropores in the total porosity changes, which leads to changes in the distribution and content of antibacterial groups on hemp fibers, thereby affecting the antibacterial properties of the product.

[0282] In addition, scanning electron microscopy (SEM) was performed on the hemp fibers involved in the preparation of the hemp fiber nonwoven fabric in Example 1. Specifically, a cross-section of the fiber was cut using a Hastelloy slicer, attached to conductive adhesive, and dried. The cross-section of the fiber was then observed using a cold field scanning electron microscope (SEM) with an accelerating voltage of 10 kV. Gold sputtering was performed on the fiber before observation under the cold field SEM. The observation results are as follows: Figure 3 and Figure 4 As shown; where, Figure 3 These are scanning electron microscope (SEM) images of hemp fiber obtained after step S1 in the preparation process of hemp fiber in Example 1, at different magnifications. Figure 3 It can be seen that the proportion of small pores in hemp bark is relatively large, while the proportion of large pores is relatively small. Figure 4 These are scanning electron microscope (SEM) images of hemp fibers treated in step S4 of Example 1 at different magnifications. Figure 4 As can be seen, after treatment, the proportion of small pores in hemp fibers decreased significantly, while the proportion of large pores increased, and the porosity of hemp fibers also showed a significant increasing trend after treatment.

[0283] Application Example 1

[0284] This invention provides a sanitary napkin, which includes a sanitary napkin body and protective wings. The protective wings are disposed on both sides of the sanitary napkin body. The sanitary napkin body consists of a top layer, a wrapping layer, a bottom film, and an outer wrapping film from top to bottom. An absorbent layer is provided inside the wrapping layer.

[0285] The surface layer is made of hemp fiber nonwoven fabric as described in this invention.

[0286] The photograph of the sanitary napkin product is as follows: Figure 5 As shown, where Figure 5 In the image, 'a' represents the unfolded photograph. Figure 5 Image b is a folded photograph.

[0287] Application Example 2

[0288] An application example of this invention provides an adult pull-up trouser, which includes an adult pull-up trouser body. The adult pull-up trouser body consists of a top layer, an absorbent core, and a bottom film, arranged sequentially from the skin-contacting side downwards. The absorbent core includes a first absorbent core and a second absorbent core, with the second absorbent core located below the first absorbent core. The top layer is made of hemp fiber nonwoven fabric as described in this invention.

[0289] The photograph of the adult pull-up pants product is as follows: Figure 6 As shown, where Figure 6 Image 'a' is a photograph of the outer side view. Figure 6 Image b is an internal view photograph.

[0290] Finally, it should be noted that the above embodiments are used to illustrate the technical solutions of the present invention and not to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the essence and scope of the technical solutions of the present invention.

Claims

1. A hemp fiber nonwoven fabric, characterized in that, The hemp fiber nonwoven fabric is composed of 100% virgin natural hemp fiber; the hemp fiber contains macropores with a pore size >10μm, mesopores with a pore size of 1-10μm, and micropores with a pore size <1μm, and the total porosity of the hemp fiber is 30-50%; In the hemp fiber, macropores account for 48-65% of the total porosity, mesopores account for 24-50% of the total porosity, and micropores account for 2-12% of the total porosity. When the moisture regain of the hemp fiber nonwoven fabric increases from 0% to 100%, the flexural stiffness decreases by ≥2%; The preparation method of the hemp fiber nonwoven fabric includes the following steps: S1. Crush and pound the hemp stalks after rain and dew to obtain hemp bark; S2. The hemp fiber is degummed once using a compound bacterial solution, wherein the compound bacterial solution contains alkalophilic Bacillus and fluorescent Pseudomonas in a mass ratio of 1:(1-2); S3. Place the hemp fibers after the first degumming in step S2 into a secondary degumming solution for secondary degumming to obtain degummed hemp fibers; the pH value of the secondary degumming solution is 12-13.5, and the volume concentration of hydrogen peroxide in the secondary degumming solution is 9-10 mL / L. S4. The degummed hemp fibers are soaked in oil, then de-oiled and dehydrated and subjected to humidification curing treatment; the relative humidity of the humidification curing treatment is 60-70%, the temperature is 25-40℃, and the humidification curing treatment time is 12-48h. S5. After humidification and conditioning treatment, the hemp fibers are opened and combed to obtain hemp fibers with a length of 28.3-35mm and a residual glue rate of 5-20%. S6. Hemp fibers are opened, cleaned, combed, and laid into a web to obtain a fiber web; wherein the basis weight of the fiber web is 33-38 g / m². 2 ; S7. The fiber web is sequentially subjected to hydroentangling and post-hydroentangling treatment to obtain hemp fiber nonwoven fabric; wherein, the hydroentangling process includes four hydroentangling processes, and the hydroentangling pressures in the first to fourth hydroentangling processes are 35-45 bar, 60-70 bar, 75-85 bar, and 85-95 bar, respectively. The concentration of bacteria in the compound bacterial solution is (0.1-10)×10⁻¹⁰. -8 CFU / mL; The solid-liquid ratio of the first degumming step is 1g:(5-15)mL, the temperature of the first degumming step is 32-36℃, and the time is 6-8h; The solid-liquid ratio of the secondary degumming is 1g:(8-12)mL, the temperature of the secondary degumming is 98-100℃, and the time of the secondary degumming is 60-120min; In step S4, the oil used in the oil immersion treatment is a mixture of vegetable oil, mineral oil and water, and the treatment time is 50-70 minutes.

2. The hemp fiber nonwoven fabric according to claim 1, characterized in that, When the moisture regain of the hemp fiber nonwoven fabric increases from 0% to 100%, the bending stiffness decreases by 3-5%.

3. The hemp fiber nonwoven fabric according to claim 1, characterized in that, The total porosity of the hemp fiber is 36-48%; And / or, in the hemp fibers, the porosity of macropores accounts for 51-60% of the total porosity; And / or, in the hemp fibers, the porosity of mesopores accounts for 36-44% of the total porosity; And / or, in the hemp fibers, the porosity of small pores accounts for 3-6% of the total porosity.

4. The hemp fiber nonwoven fabric according to claim 1, characterized in that, The fineness of the hemp fiber is >2000 Nm and the length is >28 mm.

5. The hemp fiber nonwoven fabric according to claim 4, characterized in that, The fineness of the hemp fiber is 2240-2600 Nm, and the length is 28.3-35 mm.

6. The use of hemp fiber nonwoven fabric as described in any one of claims 1-5 in the preparation of hygiene products.

7. The application according to claim 6, characterized in that, The sanitary products include any one of sanitary napkins, panty liners, adhesive bandages, diapers, and adult pull-up pants.

8. A sanitary napkin, characterized in that, The surface layer of the sanitary napkin is a hemp fiber nonwoven fabric as described in any one of claims 1-5.

9. The sanitary napkin according to claim 8, characterized in that, The sanitary napkin also includes an absorbent layer and a bottom layer.

Citation Information

Patent Citations

  • Blended spunlace non-woven material for cotton and linen wipe and preparation method thereof

    CN109576902A

  • All-hemp fiber antibacterial non-woven fabric and preparation method thereof

    CN117569003A

  • Technological process of ramie bast fiber

    CN101824658A

  • Hemp fiber blended spunlace non-woven fabric for disposable underwear and preparation method

    CN117211007A

  • All-hemp fiber antibacterial sanitary towel and preparation method thereof

    CN117338989A