Silica-zirconia synergistically modified polyurethane for use as a wall floor coating and method of making same

By preparing silicon-zirconium synergistic modified polyurethane, the problem of insufficient thermal stability of polyurethane materials under high temperature environment was solved, realizing high-temperature application on wall and floor coatings, while maintaining the toughness and service life of the material.

CN119592198BActive Publication Date: 2026-11-24CHANGZHOU VOCATIONAL INST OF ENG +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411925012.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-12-25
Publication Date
2026-11-24
Estimated Expiration
2044-12-25

AI Technical Summary

Technical Problem

Existing polyurethane materials are prone to degradation at high temperatures, making it difficult to maintain thermal stability in wall and floor coating applications in high-temperature industrial environments while ensuring that other properties remain unaffected.

Method used

A silicon-zirconium synergistic modified polyurethane was prepared by mixing zirconium-containing silicon polyurethane with amino polysilane. An interpenetrating polymer network was formed through covalent and hydrogen bonds, and the amount of curing agent was optimized to improve thermal stability and toughness.

Benefits of technology

While improving thermal stability, it avoids the coating embrittlement problem caused by excessive crosslinking density, thus maintaining the toughness and service life of polyurethane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention belongs to the field of polyurethane technology, specifically relating to a silicon-zirconium synergistic modified polyurethane for use as a wall and floor coating and its preparation method. The silicon-zirconium synergistic modified polyurethane for wall and floor coatings is prepared by mixing zirconium-containing silicon polyurethane and amino polysilane. The molecular backbones of both the zirconium-containing silicon polyurethane and the amino polysilane contain zirconium and silicon covalently bonded, improving the intrinsic thermal stability of the polyurethane. Simultaneously, the similar structures improve their compatibility. During the curing process, the silicon-zirconium synergistic modified polyurethane for wall and floor coatings can form an interpenetrating polymer network with the curing agent through hydrogen bonds and amino groups. By optimizing the amount of curing agent, the flexibility of the polymer network is improved. This enhances the thermal stability of the silicon-zirconium synergistic modified polyurethane for wall and floor coatings while avoiding the coating embrittlement problem caused by excessive crosslinking density, thus ensuring its toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polyurethane technology, and particularly relates to a silicon-zirconium synergistic modified polyurethane for use as a wall and floor coating and its preparation method. Background Technology

[0002] Polyurethane materials possess numerous advantages, including lightweight, wear resistance, oil resistance, low-temperature resistance, aging resistance, high hardness, and good elasticity. These properties enable their wide application in various fields, such as textiles, construction, aerospace, shipbuilding, transportation, medicine, and electronics. However, despite these excellent properties, polyurethane materials are prone to degradation at high temperatures, limiting their use in areas requiring high thermal stability, particularly for wall and floor coatings in high-temperature industrial environments.

[0003] Methods to improve the thermal stability of polyurethane include adding fillers with high thermal stability (such as flame retardants and carbon nanotubes), increasing the crosslinking degree of polyurethane, and silicone modification. However, adding fillers and silicone modification often face compatibility issues, affecting the modification effect and even causing adverse phenomena such as phase separation within the material. Increased crosslinking density reduces the material's flexibility and toughness, making it prone to cracking under impact, thus affecting its service life and protective effect. Currently, it is difficult to improve the thermal stability of polyurethane while ensuring that other properties remain unaffected. Summary of the Invention

[0004] To address the shortcomings of existing methods, the technical solution adopted in this invention is as follows: This invention provides a silicon-zirconium synergistic modified polyurethane for use as a wall and floor coating, wherein the polyurethane is composed of the following raw materials: zirconium-containing silicon polyurethane and amino polysilane.

[0005] Furthermore, the zirconium-containing silicon polyurethane is prepared by reacting polyethylene glycol, cyclopentadienyl zirconium trichloride, chlorosilane, and isocyanate compound.

[0006] Preferably, the molecular weight of the polyethylene glycol is 200-2000.

[0007] Preferably, the chlorosilane includes one or more of diphenyldichlorosilane, dimethyldichlorosilane, and dichlorodiethylsilane.

[0008] Preferably, the isocyanate compound includes one or more of o-phthalic diisocyanate, m-phthalic diisocyanate, isoflurone diisocyanate, hexamethylene diisocyanate, and triphenylmethane triisocyanate.

[0009] Furthermore, the aminopolysilane is prepared by reacting silane, aminosilane, zirconium oxychloride, and hexamethyldisiloxane.

[0010] Preferably, the silane includes one or more of methyldiethoxysilane and methyldimethoxysilane.

[0011] Preferably, the aminosilane includes one or more of N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane and aminopropylmethyldiethoxysilane.

[0012] The preparation method of the silicon-zirconium synergistic modified polyurethane used as a wall and floor coating includes the following steps:

[0013] (1) Preparation of zirconium-containing silicon polyurethane: Polyethylene glycol and tetrahydrofuran were mixed, and then triethylamine was added and reacted at 0-8℃ for 10-12h. A mixture of cyclopentadienyl zirconium trichloride and chlorosilane was added dropwise and mixed evenly before being added dropwise to the reaction solution. Then an isocyanate compound was added and the reaction was continued at 55-80℃ for 8-13h. After the reaction was completed, the mixture was filtered and the filtrate was rotary evaporated to obtain zirconium-containing silicon polyurethane.

[0014] Preferably, the molar ratio of polyethylene glycol to triethylamine is 1:0.8-1.1.

[0015] Preferably, the molar ratio of polyethylene glycol, cyclopentadienyl zirconium trichloride, chlorosilane, and isocyanate compound is 1:0.01-0.04:0.01-0.04:0.2-0.3.

[0016] (2) Preparation of amino polysilane: First, mix silane and zirconium oxychloride evenly, then add amino silane; under magnetic stirring, add distilled water dropwise to the beaker to carry out hydrolysis-copolymerization reaction, stir for 30-50 min, add hexamethyldisiloxane, continue stirring reaction for 30 min, wash with water until neutral, distill off water and ethanol under reduced pressure to obtain amino polysilane.

[0017] Preferably, the molar ratio of the silane, zirconium oxychloride, aminosilane, and hexamethyldisiloxane is 1-3:0.1-0.3:0.7-1.0:0.1-0.4.

[0018] Preferably, the ratio of distilled water to silane is 0.8-1 mL: 0.01 mol.

[0019] (3) Preparation of silicon-zirconium synergistic modified polyurethane for use as wall and floor coating: Zirconium-containing silicon polyurethane and amino polysilane are mixed to prepare silicon-zirconium synergistic modified polyurethane for use as wall and floor coating.

[0020] Preferably, the mass ratio of the zirconium-containing silicon polyurethane to the amino polysilane is 1:0.1-0.4.

[0021] The silicon-zirconium synergistic modified polyurethane used as a wall and floor coating can be used to make coatings, which include the following raw materials: silicon-zirconium synergistic modified polyurethane used as a wall and floor coating and a curing agent; the mass ratio of the silicon-zirconium synergistic modified polyurethane used as a wall and floor coating and the curing agent is 100:4-8.

[0022] Preferably, the curing agent is a polyepoxy compound, including one or more of ethylene glycol diglycidyl ether, ethylene glycol diglycidyl ether, and glycidyl ether.

[0023] The beneficial effects of this invention are as follows:

[0024] The silicon-zirconium synergistic modified polyurethane used as a wall and floor coating of this invention is prepared by mixing zirconium-containing silicon polyurethane and amino polysilane. The main molecular chain of the zirconium-containing silicon polyurethane contains zirconium and silicon (Zr-OC, Zr-O-Si, Si-OC, etc.) bonded in the form of covalent bonds, improving the intrinsic thermal stability of the polyurethane. The amino polysilane molecular chain, similar to that of the zirconium-containing silicon polyurethane, contains zirconium and silicon bonded in the form of covalent bonds, giving it good compatibility with the zirconium-containing silicon polyurethane. During the curing process, the silicon-zirconium synergistic modified polyurethane used as a wall and floor coating can form an interpenetrating polymer network with the curing agent through hydrogen bonds and amino groups. By optimizing the amount of curing agent, the flexibility of the polymer network is improved. This enhances the thermal stability of the silicon-zirconium synergistic modified polyurethane used as a wall and floor coating while avoiding the coating embrittlement problem caused by excessive crosslinking density, thus ensuring its toughness. Detailed Implementation

[0025] The present invention will be further described below with reference to the embodiments.

[0026] Example 1:

[0027] (1) Preparation of zirconium-containing silicon polyurethane: 0.1 mol polyethylene glycol (PEG200) was mixed with 100 mL tetrahydrofuran, and then 0.1 mol triethylamine was added and reacted at 3-6 °C for 12 h. A mixture of 0.01 mol cyclopentadienyl zirconium trichloride and 0.04 mol dimethyl dichlorosilane was added dropwise and mixed evenly before being added dropwise to the reaction solution. Then 0.02 mol isoflurane diisocyanate was added and the reaction was continued at 60 °C for 12 h. After the reaction was completed, the mixture was filtered and the filtrate was rotary evaporated to obtain zirconium-containing silicon polyurethane.

[0028] (2) Preparation of amino polysilane: First, mix 0.1 mol methyl dimethoxysilane and 0.02 zirconium oxychloride evenly, then add 0.07 mol aminopropylmethyl diethoxysilane; under magnetic stirring, add 8 mL distilled water dropwise to the beaker to carry out hydrolysis-copolymerization reaction, stir for 30 min, add 0.02 mol hexamethyldisiloxane, continue stirring reaction for 30 min, wash with water until neutral, distill off water and ethanol under reduced pressure to obtain amino polysilane.

[0029] (3) Preparation of silicon-zirconium synergistic modified polyurethane for use as wall and floor coating: Zirconium-containing silicon polyurethane and amino polysilane are mixed at a mass ratio of 1:0.3 to obtain silicon-zirconium synergistic modified polyurethane for use as wall and floor coating.

[0030] Example 2:

[0031] The difference between Example 2 and Example 1 is that in step (3), zirconium-containing silicon polyurethane and amino polysilane are in a mass ratio of 1:0.1, while the rest is the same as in Example 1.

[0032] Example 3:

[0033] The difference between Example 3 and Example 1 is that in step (3), the zirconium-containing silicon polyurethane and amino polysilane are in a mass ratio of 1:0.2, while the rest is the same as in Example 1.

[0034] Example 4:

[0035] The difference between Example 4 and Example 1 is that in step (1), a mixture of 0.02 mol cyclopentadienyl zirconium trichloride and 0.03 mol dimethyl dichlorosilane is added, while the rest is the same as in Example 1.

[0036] Example 5:

[0037] The difference between Example 5 and Example 1 is that in step (1), a mixture of 0.03 mol cyclopentadienyl zirconium trichloride and 0.02 mol dimethyl dichlorosilane is added, while the rest is the same as in Example 1.

[0038] Example 6:

[0039] The difference between Example 5 and Example 1 is that in step (1), a mixture of 0.04 mol cyclopentadienyl zirconium trichloride and 0.01 mol dimethyl dichlorosilane is added, while the rest is the same as in Example 1.

[0040] Example 7

[0041] The difference between Example 7 and Example 1 is that in step (3), the zirconium-containing silicon polyurethane and amino polysilane are in a mass ratio of 1:0.4, while the rest is the same as in Example 1.

[0042] Comparative Example 1

[0043] The difference between Comparative Example 1 and Example 1 is that in step (3), zirconium-containing silicon polyurethane and amino polysilane are in a mass ratio of 1:0, and the rest is the same as in Example 1.

[0044] Comparative Example 2

[0045] The difference between Comparative Example 2 and Example 1 is that in step (1), a mixture of 0 mol cyclopentadienyl zirconium trichloride and 0.05 mol dimethyl dichlorosilane is added, while the rest is the same as in Example 1.

[0046] Example of effect 1

[0047] The polyurethane prepared in the above examples and comparative examples was mixed with ethylene glycol diglycidyl ether, poured into a mold, and cured at 100℃ / 4h + 130℃ / 4h. Impact strength (original sample, after 300℃ / 2h pretreatment) and fracture toughness were tested according to ASTM D256-10 and GB / T2567-2021. The test results are shown in Table 1. The mass ratio of polyurethane to ethylene glycol diglycidyl ether was 100:6.

[0048] Table 1

[0049]

[0050] Example 2

[0051] The polyurethane prepared in Example 5 was mixed with ethylene glycol diglycidyl ether amino at a mass ratio of 100:4-8, poured into a mold, and cured at 100℃ / 4h + 130℃ / 4h. The impact strength and hardness were tested according to ASTM D256-10 and ASTM D2240, and the results are shown in Table 2.

[0052] Table 2

[0053] Mass ratio of polyurethane to ethylene glycol diglycidyl ether amino Surface hardness <![CDATA[Impact Strength (KJ / m -2 )]]> 100:4 63 72 100:6 71 79 100:8 77 67 100:10 82 56

[0054] Based on the above-described preferred embodiments of the present invention, and through the foregoing description, those skilled in the art can make various changes and modifications without departing from the inventive concept. The technical scope of this invention is not limited to the contents of the specification, but must be determined according to the scope of the claims.

Claims

1. A silicon-zirconium synergistic modified polyurethane for use as a wall and floor coating, characterized in that, The polyurethane is composed of zirconium-containing silicon polyurethane and amino polysilane; The method for preparing the zirconium-containing silicon polyurethane is as follows: polyethylene glycol is mixed with tetrahydrofuran, followed by the addition of triethylamine and the reaction is carried out at 0-8°C for 10-12 h. A uniform mixture of cyclopentadienyl zirconium trichloride and chlorosilane is then added dropwise. An isocyanate compound is then added, and the reaction is continued at 55-80°C for 8-13 h. After the reaction is completed, the mixture is filtered, and the filtrate is rotary evaporated to obtain the zirconium-containing silicon polyurethane. The preparation method of the aminopolysilane is as follows: First, mix silane and zirconium oxychloride evenly, then add aminosilane; under magnetic stirring, add distilled water dropwise to the beaker to carry out hydrolysis-copolymerization reaction, stir for 30-50 min, add hexamethyldisiloxane, continue stirring reaction for 30 min, wash with water until neutral, and distill off water and ethanol under reduced pressure to obtain aminopolysilane. The silane includes one or more of methyldiethoxysilane and methyldimethoxysilane; The aminosilane includes one or more of N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane and aminopropylmethyldiethoxysilane.

2. The silicon-zirconium synergistic modified polyurethane used as a wall and floor coating according to claim 1, characterized in that, The mass ratio of zirconium-containing silicon polyurethane to amino polysilane in the polyurethane is 1:0.1-0.

4.

3. The silicon-zirconium synergistic modified polyurethane used as a wall and floor coating according to claim 1, characterized in that, The chlorosilanes include one or more of diphenyl dichlorosilane, dimethyl dichlorosilane, and dichlorodiethylsilane; The isocyanate compound includes one or more of the following: phthalic diisocyanate, isophthalic diisocyanate, isoflurone diisocyanate, hexamethylene diisocyanate, and triphenylmethane triisocyanate.

4. A method for preparing a silicon-zirconium synergistic modified polyurethane for use as a wall and floor coating according to claim 1, characterized in that, Includes the following steps: (1) Preparation of zirconium-containing silicon polyurethane: Polyethylene glycol and tetrahydrofuran were mixed, and then triethylamine was added and reacted at 0-8℃ for 10-12 h. A uniform mixture of cyclopentadienyl zirconium trichloride and chlorosilane was added dropwise. Then isocyanate compound was added and the reaction was continued at 55-80℃ for 8-13 h. After the reaction was completed, the mixture was filtered and the filtrate was rotary evaporated to obtain zirconium-containing silicon polyurethane. (2) Preparation of amino polysilane: First, mix silane and zirconium oxychloride evenly, then add amino silane; under magnetic stirring, add distilled water dropwise to the beaker to carry out hydrolysis-copolymerization reaction, stir for 30-50 min, add hexamethyldisiloxane, continue stirring reaction for 30 min, wash with water until neutral, distill off water and ethanol under reduced pressure to obtain amino polysilane; (3) Preparation of silicon-zirconium synergistic modified polyurethane for use as wall and floor coating: Zirconium-containing silicon polyurethane and amino polysilane are mixed to prepare silicon-zirconium synergistic modified polyurethane for use as wall and floor coating.

5. The method for preparing silicon-zirconium synergistic modified polyurethane for use as a wall and floor coating according to claim 4, characterized in that, The molar ratio of polyethylene glycol to triethylamine in step (1) is 1:0.8-1.1; The molar ratio of polyethylene glycol, cyclopentadienyl zirconium trichloride, chlorosilane, and isocyanate compound is 1:0.01-0.04:0.01-0.04:0.2-0.

3.

6. The method for preparing silicon-zirconium synergistic modified polyurethane for use as a wall and floor coating according to claim 4, characterized in that, The molar ratio of silane, zirconium oxychloride, aminosilane, and hexamethyldisiloxane in step (2) is 1-3:0.1-0.3:0.7-1.0:0.1-0.4; The ratio of distilled water to silane is 0.8-1 mL: 0.01 mol.

7. The method for preparing silicon-zirconium synergistic modified polyurethane for use as a wall and floor coating according to claim 4, characterized in that, The mass ratio of zirconium-containing silicon polyurethane and amino polysilane in step (3) is 1:0.1-0.

4.

8. An application of the silicon-zirconium synergistic modified polyurethane as a wall and floor coating according to claim 1, characterized in that, For use in making coatings; the coatings include the following raw materials: silicon-zirconium synergistic modified polyurethane used as a wall and floor coating, and a curing agent; the mass ratio of the silicon-zirconium synergistic modified polyurethane used as a wall and floor coating to the curing agent is 100:4-8.

9. The application according to claim 8, characterized in that, The curing agent is ethylene glycol diglycidyl ether.

Citation Information

Patent Citations

  • Process for the preparation of silylated polyurethane polymers using titanium-containing and zirconium-containing catalysts

    CN105829377A

  • Temperature-resistant and shear-resistant organic boron and zirconium composite cross-linking agent for oil field fracturing and preparation method thereof

    CN118620598A