Alternating current porcelain insulator and its manufacturing method

Through specific ratios and optimized processes, AC porcelain insulators have solved the problems of insufficient mechanical strength and insulation performance, achieving higher mechanical strength and insulation performance, and are suitable for the stable operation of power systems.

CN119613088BActive Publication Date: 2026-11-24JIANGXI LIHONG ELECTRIC PORCELAIN MFG CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411841803.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-12-13
Publication Date
2026-11-24
Estimated Expiration
2044-12-13

AI Technical Summary

Technical Problem

Traditional AC porcelain insulators have shortcomings in mechanical strength and insulation performance, making them susceptible to damage under external forces. Furthermore, the manufacturing process makes it difficult to ensure the uniformity of raw material mixing and molding quality, which affects product quality and the safety of power transmission.

Method used

Using a specific ratio of raw materials such as modified kaolin, nano-zirconium boride, and rare earth-doped zirconium silicate, combined with umbrella-skirt structure design and multi-stage magnetic field strength iron removal process, the crystal structure is optimized through electron beam irradiation treatment. Composite binders and fluxes are used to control the sintering temperature, ensuring uniform mixing of raw materials and molding quality.

Benefits of technology

It improves the mechanical strength and insulation performance of porcelain insulators, reduces the risk of breakage and damage, enhances insulation performance and power transmission safety under high voltage environments, and meets the high standards required by power systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005188133170000101
    Figure BDA0005188133170000101
  • Figure BDA0005188133170000111
    Figure BDA0005188133170000111
  • Figure BDA0005188133170000112
    Figure BDA0005188133170000112
Patent Text Reader

Abstract

This invention provides an AC porcelain insulator and its preparation method. A green body is prepared using raw materials in a specific ratio, including modified kaolin, nano-zirconium boride, hexagonal boron nitride, rare-earth-doped zirconium silicate, a composite binder, and a flux. The green body has an umbrella-skirt structure with 3-5 skirts, the height difference between adjacent skirts gradually increasing, and chamfered edges. The modified kaolin undergoes specific modification treatment, and the rare-earth-doped zirconium silicate is obtained through high-temperature calcination, enhancing insulation performance. The composite binder and flux optimize the green body's forming performance and lower the sintering temperature, respectively. The preparation method includes mixing and pulping, iron removal, granulation, and surface treatment steps. The mixing and pulping process uses ultrasonic vibration to promote uniform mixing; the iron removal process involves two magnetic separations; and the granulation process uses cold isostatic pressing. The final product has optimized mechanical strength and insulation performance, suitable for AC power systems, and can withstand harsh climatic conditions and mechanical stress.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of insulator manufacturing technology, and in particular to an AC porcelain insulator and its manufacturing method. Background Technology

[0002] In the field of power transmission and distribution, AC porcelain insulators play a crucial role, effectively supporting and insulating transmission lines to ensure the safe and stable transmission of electricity. With the continuous development of the power industry and the increasing demands for power supply reliability, higher standards are being set for the performance of AC porcelain insulators.

[0003] Traditional AC porcelain insulators have gradually revealed some shortcomings in practical applications. On the one hand, in terms of mechanical performance, some existing porcelain insulators have limited mechanical strength. Under long-term stress from conductor tension, wind loads, and other external forces, they are prone to cracking and damage. This not only affects the service life of the insulators themselves but may also lead to transmission line faults, threatening the normal operation of the power system. For example, some insulators cannot effectively resist external forces when encountering strong winds or changes in line tension during severe weather, resulting in structural damage and potentially causing power outages.

[0004] On the other hand, the insulation performance of traditional porcelain insulators needs improvement. Due to limitations in raw materials and manufacturing processes, their internal crystal structure is not ideal, and the control of impurity content is not precise enough. This can lead to problems such as partial discharge and decreased insulation performance under high-voltage environments, reducing the safety and stability of power transmission. Moreover, some existing manufacturing processes cannot guarantee the sufficient and uniform mixing of raw materials during production, which also affects the overall performance of the final product, resulting in inconsistent product quality.

[0005] In addition, the existing porcelain insulator production process is also lacking in terms of controlling the sintering temperature of the green blank and the molding quality. Either the sintering temperature is too high, which increases the production cost, or the green blank after molding is prone to defects, which affects the performance and appearance quality of the finished product. Summary of the Invention

[0006] In view of this, the present invention proposes an AC porcelain insulator and its preparation method to solve the above problems.

[0007] The technical solution of this invention is implemented as follows: An AC porcelain insulator: The AC porcelain insulator is made by glazing, firing, and gluing a green blank. The green blank comprises the following raw materials in parts by weight: 40-50 parts modified kaolin, 10-15 parts nano-zirconium boride, 8-12 parts hexagonal boron nitride, 5-8 parts rare earth-doped zirconium silicate, 6-10 parts composite binder, and 3-5 parts flux; the average particle size of the nano-zirconium boride is 50-100 nm; the shape of the green blank is an umbrella-skirt structure, with 3-5 umbrella skirts. The height difference between adjacent umbrella skirts is distributed according to the rule of gradually increasing from top to bottom, with a height difference range of 5-10 mm, and the edges of the umbrella skirts are provided with a chamfer with a radius of 2-3 mm.

[0008] Furthermore, the green body comprises the following raw materials in parts by weight: 45 parts modified kaolin, 13 parts nano-zirconium boride, 10 parts hexagonal boron nitride, 7 parts rare earth-doped zirconium silicate, 8 parts composite binder, and 4 parts flux.

[0009] Furthermore, the modification method of the modified kaolin involves calcining the kaolin at 500-600℃ for 2-4 hours, then pulverizing and sieving it through a 200-300 mesh sieve to remove impurities and make the kaolin particles more uniform, thereby improving the irradiation modification effect. The kaolin is then placed in an electron beam irradiation device with an electron beam energy of 1.2-1.5 MeV, an electron beam current intensity of 3-5 mA, an irradiation dose of 50-80 kGy, and an irradiation time of 3-5 hours. After irradiation, the kaolin is placed in an oven at 80-100℃ for 1-2 hours. The treated kaolin exhibits directional lattice distortion in its crystal structure, improving the mechanical strength of the green body and enhancing its insulation properties.

[0010] Furthermore, the rare earth element in the rare earth-doped zirconium silicate is yttrium, and the doping amount, calculated as yttrium oxide, accounts for 3%-5% of the total mass of zirconium silicate. Specifically, zirconium silicate powder with a purity of not less than 95% and an average particle size of 1-5 μm is selected as the base raw material, and yttrium oxide powder with a particle size of 0.5-2 μm is taken. Both powders are dried in an oven at 120-150℃ for 3-4 hours. The two powders are then mixed and ground at a speed of 200-300 rpm for 2-4 hours. High-temperature calcination is then performed, with the temperature increased to 800-1000℃ at a rate of 5-8℃ / min, followed by a first holding time of 1-3 hours. The temperature is then increased to 1200-1300℃ at a rate of 3-5℃ / min and held at this temperature for 3-5 hours. After completion, the temperature is cooled to room temperature to obtain rare earth-doped zirconium silicate. This is used to refine the grain size and improve the insulation performance of the green blank.

[0011] Furthermore, during the calcination process, argon gas with a purity of 99.9% or higher is introduced as a protective gas, with the gas flow rate controlled at 10-20 L / min. This prevents the raw materials from being oxidized at high temperatures, which would affect the doping effect and the quality of the final product.

[0012] Furthermore, the composite binder is composed of polyvinyl butyral, sodium alginate and polyethylene glycol diacrylate in a mass ratio of 2-5:1-3:1 to ensure the molding performance of the green body.

[0013] Furthermore, the flux is a mixture of sodium fluorosilicate and zinc borate in a mass ratio of 1:1-3, which helps to reduce the sintering temperature of the green body.

[0014] Furthermore, a method for preparing an AC porcelain insulator includes the following steps:

[0015] S1. Mixing and pulping: Weigh the above raw materials according to the weight parts and add them to a high-speed mixer. At the same time, add deionized water and stir and mix at a speed of 800-1000 rpm for 30-45 minutes to obtain the pulp.

[0016] S2. Iron removal: Pour the slurry into a magnetic separator, set the magnetic field strength to 0.1-0.2T to obtain slurry I, and then continue to pour it into the magnetic separator, set the magnetic field strength to 0.8-1.2T to obtain slurry II. The flow rate of the slurry is 1-3cm / s. Filter and centrifuge to remove water from the slurry, and then dry it in an oven at 100-120℃ for 2-4 hours to reduce the moisture content to 5-10%.

[0017] S3. Granulation and Molding: Add ammonium bicarbonate to the iron-removed mixture and stir for 10-15 minutes. The amount added is 2.5-5% of the mixture mass. Transfer the mixture to a granulator for granulation, controlling the particle size to 0.5-1 mm. Then, place the granules into a mold and use a cold isostatic pressing process to form the green body. The molding pressure is 150-200 MPa, and the holding time is 5-8 minutes.

[0018] S4. Surface treatment: After the green body is demolded, it is glazed, fired, and glued to obtain the finished product.

[0019] Furthermore, the slurry concentration of S1 is 20-40%.

[0020] Furthermore, the temperature inside the S1 high-speed mixer is controlled at 30-40℃, and during the mixing process, ultrasonic vibration is performed every 10-15 minutes with an ultrasonic power of 500-800W and a vibration time of 2-4 minutes to promote more thorough and uniform mixing of the raw materials.

[0021] Compared with the prior art, the beneficial effects of the present invention are:

[0022] Firstly, in terms of mechanical properties, the use of specially modified kaolin with a specific ratio of raw materials and a rational skirt structure design results in excellent mechanical properties, reducing the risk of breakage and extending service life, thus effectively ensuring the stability of power system operation. Secondly, irradiation treatment helps optimize the internal microstructure of kaolin, reducing the impact of crystal defects and impurities on electron conduction. When applied to the production of AC porcelain insulators, this structural optimization can effectively suppress electron migration, enabling the insulator to better block current under high voltage conditions, reducing the probability of leakage and partial discharge, thereby improving the insulation performance of the insulator. Simultaneously, the rare earth-doped zirconium silicate in the raw material is prepared through a rigorous process, refining the grain size and improving the insulation performance of the green blank, allowing the insulator to maintain good insulation under high voltage conditions, reducing partial discharge, and enhancing the safety of power transmission. Furthermore, the composite binder ensures good green blank forming results, and the flux lowers the sintering temperature, saving energy, controlling costs, and preventing the deterioration of raw material properties, which is conducive to improving the overall quality of the product. Meanwhile, during the mixing and pulping process, the rotation speed, concentration, and temperature are controlled, and ultrasonic vibration is used to ensure that all raw materials are fully and uniformly mixed, thereby improving the consistency and stability of product performance. In addition, the iron removal process involves setting the magnetic field strength and controlling the flow rate in stages to efficiently remove iron. During granulation and molding, each parameter is precisely controlled to ensure molding quality and dimensional accuracy. The synergistic effect of multiple processes effectively improves the overall performance of the product and better meets the high standards required by the power system for AC porcelain insulators. Detailed Implementation

[0023] To better understand the technical content of this invention, specific embodiments are provided below to further illustrate the invention.

[0024] Unless otherwise specified, the experimental methods used in the embodiments of this invention are all conventional methods.

[0025] Unless otherwise specified, all materials and reagents used in the embodiments of this invention are commercially available.

[0026] Example 1

[0027] An AC porcelain insulator: The AC porcelain insulator is made by glazing, firing, and gluing a green blank. The green blank includes the following raw materials in parts by weight: 40 parts modified kaolin, 10 parts nano zirconium boride, 8 parts hexagonal boron nitride, 5 parts rare earth doped zirconium silicate, 6 parts composite binder, and 3 parts flux.

[0028] The modification method for the kaolin involves calcining the kaolin at 500℃ for 2 hours, then pulverizing and sieving it through a 200-mesh sieve to remove impurities and make the kaolin particles more uniform, thus improving the irradiation modification effect. The kaolin is then placed in an electron beam irradiation device with an electron beam energy of 1.2 MeV, an electron beam current intensity of 3 mA, an irradiation dose of 50 kGy, and an irradiation time of 3 hours. After irradiation, the kaolin is placed in an oven at 80℃ for 1 hour. The treated kaolin exhibits directional lattice distortion in its crystal structure, improving the mechanical strength and insulation properties of the green body.

[0029] The average particle size of the nano-zirconium boride is 50 nm.

[0030] The rare earth element in the rare earth-doped zirconium silicate is yttrium, and the doping amount, calculated as yttrium oxide, accounts for 3% of the total mass of zirconium silicate. Specifically, zirconium silicate powder with a purity of not less than 95% and an average particle size of 1 μm is selected as the base raw material, and yttrium oxide powder with a particle size of 0.5 μm is taken. Both powders are dried in an oven at 120°C for 3 hours. The two powders are then mixed and ground at 200 rpm for 2 hours, followed by high-temperature calcination. The temperature is increased to 800°C at a rate of 5°C / min, and held for 1 hour. The temperature is then increased to 1200°C at a rate of 3°C / min and held at this temperature for 3 hours. During the calcination process, argon gas with a purity of 99.9% or higher is introduced as a protective gas, and the gas flow rate is controlled at 10 L / min. After completion, the mixture is cooled to room temperature to obtain rare earth-doped zirconium silicate.

[0031] The composite binder is composed of polyvinyl butyral, sodium alginate and polyethylene glycol diacrylate in a mass ratio of 2:1:1 to ensure the molding performance of the green body.

[0032] The flux is a mixture of sodium fluorosilicate and zinc borate in a mass ratio of 1:1-3, which helps to reduce the sintering temperature of the green body.

[0033] Example 2

[0034] An AC porcelain insulator: The AC porcelain insulator is made by glazing, firing, and gluing a green blank. The green blank includes the following raw materials in parts by weight: 50 parts modified kaolin, 15 parts nano zirconium boride, 12 parts hexagonal boron nitride, 8 parts rare earth doped zirconium silicate, 10 parts composite binder, and 5 parts flux.

[0035] The modification method of the kaolin involves calcining the kaolin at 600℃ for 4 hours, then pulverizing and sieving it through a 300-mesh sieve to remove impurities and make the kaolin particles more uniform, thereby improving the irradiation modification effect. The kaolin is then placed in an electron beam irradiation device with an electron beam energy of 1.5 MeV, an electron beam current intensity of 5 mA, an irradiation dose of 80 kGy, and an irradiation time of 5 hours. After irradiation, the kaolin is placed in an oven at 100℃ for 2 hours. The treated kaolin exhibits directional lattice distortion in its crystal structure, improving the mechanical strength and insulation properties of the green body.

[0036] The average particle size of the nano-zirconium boride is 100 nm.

[0037] The rare earth element in the rare earth-doped zirconium silicate is yttrium, and the doping amount, calculated as yttrium oxide, accounts for 5% of the total mass of zirconium silicate. Specifically, zirconium silicate powder with a purity of not less than 95% and an average particle size of 5 μm is selected as the base raw material, and yttrium oxide powder with a particle size of 2 μm is taken. Both powders are dried in an oven at 120-150℃ for 4 hours. The two powders are then mixed and ground at 300 rpm for 4 hours, followed by high-temperature calcination. The temperature is increased to 1000℃ at a rate of 8℃ / min, and held for 3 hours. The temperature is then increased to 1300℃ at a rate of 5℃ / min and held at this temperature for 5 hours. During the calcination process, argon gas with a purity of 99.9% or higher is introduced as a protective gas, and the gas flow rate is controlled at 20 L / min. After completion, the mixture is cooled to room temperature to obtain rare earth-doped zirconium silicate.

[0038] The composite binder is composed of polyvinyl butyral, sodium alginate and polyethylene glycol diacrylate in a mass ratio of 5:3:1 to ensure the molding performance of the green body.

[0039] The flux is a mixture of sodium fluorosilicate and zinc borate in a mass ratio of 1:3, which helps to reduce the sintering temperature of the green body.

[0040] Example 3

[0041] An AC porcelain insulator: The AC porcelain insulator is made by glazing, firing, and gluing a green blank. The green blank includes the following raw materials in parts by weight: 45 parts modified kaolin, 13 parts nano zirconium boride, 10 parts hexagonal boron nitride, 7 parts rare earth doped zirconium silicate, 8 parts composite binder, and 4 parts flux.

[0042] The modification method of the kaolin involves calcining the kaolin at 550℃ for 3 hours, then pulverizing and sieving it through a 250-mesh sieve to remove impurities and make the kaolin particles more uniform, thus improving the irradiation modification effect. The kaolin is then placed in an electron beam irradiation device with an electron beam energy of 1.3 MeV, an electron beam current intensity of 4 mA, an irradiation dose of 70 kGy, and an irradiation time of 4 hours. After irradiation, the kaolin is placed in an oven at 80-100℃ for 1-2 hours. The treated kaolin exhibits directional lattice distortion in its crystal structure, improving the mechanical strength and insulation properties of the green body.

[0043] The average particle size of the nano-zirconium boride is 80 nm.

[0044] The rare earth element in the rare earth-doped zirconium silicate is yttrium, and the doping amount, calculated as yttrium oxide, accounts for 4% of the total mass of zirconium silicate. Specifically, zirconium silicate powder with a purity of not less than 95% and an average particle size of 3 μm is selected as the base material, and yttrium oxide powder with a particle size of 1.5 μm is taken. Both powders are dried in an oven at 135°C for 3 hours. The two powders are then mixed and ground at 250 rpm for 3 hours, followed by high-temperature calcination. The temperature is increased to 900°C at a rate of 7°C / min, and held for 2 hours. The temperature is then increased to 1200°C at a rate of 4°C / min and held at this temperature for 4 hours. During the calcination process, argon gas with a purity of 99.9% or higher is introduced as a protective gas, and the gas flow rate is controlled at 15 L / min. After completion, the mixture is cooled to room temperature to obtain rare earth-doped zirconium silicate.

[0045] The composite binder is composed of polyvinyl butyral, sodium alginate and polyethylene glycol diacrylate in a mass ratio of 2-5:1-3:1 to ensure the molding performance of the green body.

[0046] The flux is a mixture of sodium fluorosilicate and zinc borate in a mass ratio of 1:2, which helps to reduce the sintering temperature of the green body.

[0047] The above Examples 1-3 were prepared using the following methods:

[0048] S1. Mixing and pulping: Weigh the above raw materials according to the weight parts and add them to a high-speed mixer. At the same time, add deionized water. Control the temperature at 35℃ and stir at 900 rpm for 40 minutes. During the stirring and mixing process, perform ultrasonic vibration treatment every 12 minutes. The ultrasonic power is 700W and the vibration time is 3 minutes to obtain a pulp with a mass concentration of 30%.

[0049] S2. Iron removal: Pour the slurry into a magnetic separator and set the magnetic field strength to 0.15T to obtain slurry I. Then pour it into the magnetic separator again and set the magnetic field strength to 1.0T to obtain slurry II. The flow rate of the slurry is 2cm / s. Filter and centrifuge to remove water from the slurry. Then dry it in an oven at 110℃ for 3 hours to reduce the moisture content to 8%.

[0050] S3. Granulation and Molding: Add ammonium bicarbonate to the iron-removed mixture and stir for 12 minutes. The amount added is 4% of the mixture mass. Transfer the mixture to a granulator for granulation, controlling the particle size to 0.8 mm. Then place the granules into a mold and use a cold isostatic pressing process to form the green body. The molding pressure is 180 MPa, and the holding time is 7 minutes.

[0051] S4. Surface treatment: After the green body is demolded, it is glazed, fired, and glued to obtain the finished product.

[0052] Example 4

[0053] An AC porcelain insulator: The AC porcelain insulator is made by glazing, firing, and gluing a green blank. The green blank includes the following raw materials in parts by weight: 45 parts modified kaolin, 13 parts nano zirconium boride, 10 parts hexagonal boron nitride, 7 parts rare earth doped zirconium silicate, 8 parts composite binder, and 4 parts flux.

[0054] The modification method of the kaolin involves calcining the kaolin at 550℃ for 3 hours, then pulverizing and sieving it through a 250-mesh sieve to remove impurities and make the kaolin particles more uniform, thus improving the irradiation modification effect. The kaolin is then placed in an electron beam irradiation device with an electron beam energy of 1.3 MeV, an electron beam current intensity of 4 mA, an irradiation dose of 70 kGy, and an irradiation time of 4 hours. After irradiation, the kaolin is placed in an oven at 80-100℃ for 1-2 hours. The treated kaolin exhibits directional lattice distortion in its crystal structure, improving the mechanical strength and insulation properties of the green body.

[0055] The average particle size of the nano-zirconium boride is 80 nm.

[0056] The rare earth element in the rare earth-doped zirconium silicate is yttrium, and the doping amount, calculated as yttrium oxide, accounts for 4% of the total mass of zirconium silicate. Specifically, zirconium silicate powder with a purity of not less than 95% and an average particle size of 3 μm is selected as the base material, and yttrium oxide powder with a particle size of 1.5 μm is taken. Both powders are dried in an oven at 135°C for 3 hours. The two powders are then mixed and ground at 250 rpm for 3 hours, followed by high-temperature calcination. The temperature is increased to 900°C at a rate of 7°C / min, and held for 2 hours. The temperature is then increased to 1200°C at a rate of 4°C / min and held at this temperature for 4 hours. During the calcination process, argon gas with a purity of 99.9% or higher is introduced as a protective gas, and the gas flow rate is controlled at 15 L / min. After completion, the mixture is cooled to room temperature to obtain rare earth-doped zirconium silicate.

[0057] The composite binder is composed of polyvinyl butyral, sodium alginate and polyethylene glycol diacrylate in a mass ratio of 2-5:1-3:1 to ensure the molding performance of the green body.

[0058] The flux is a mixture of sodium fluorosilicate and zinc borate in a mass ratio of 1:2, which helps to reduce the sintering temperature of the green body.

[0059] The preparation method used in Example 4 above is as follows:

[0060] S1. Mixing and pulping: Weigh the above raw materials according to the weight parts and add them to a high-speed mixer. At the same time, add deionized water and stir at 800 rpm for 30 minutes to obtain the pulp.

[0061] S2. Iron removal: Pour the slurry into a magnetic separator, control the temperature at 30℃, and set the magnetic field strength to 0.1T to obtain slurry I. Then continue to pour it into the magnetic separator, and set the magnetic field strength to 0.8T to obtain slurry II. The flow rate of the slurry is 1cm / s. Ultrasonic vibration is performed every 10 minutes, with an ultrasonic power of 500W and a vibration time of 2 minutes. Filter and centrifuge to remove water from the slurry, and then dry it in an oven at 100℃ for 2 hours to reduce the moisture content to 5%.

[0062] S3. Granulation and Molding: Add ammonium bicarbonate to the iron-removed mixture and stir for 10 minutes. The amount added is 2.5% of the mixture mass. Transfer the mixture to a granulator for granulation, controlling the particle size to 0.5 mm. Then place the granules into a mold and use a cold isostatic pressing process to form the green body. The molding pressure is 150 MPa, and the holding time is 5 minutes.

[0063] S4. Surface treatment: After the green body is demolded, it is glazed, fired, and glued to obtain the finished product.

[0064] Example 5

[0065] An AC porcelain insulator: The AC porcelain insulator is made by glazing, firing, and gluing a green blank. The green blank includes the following raw materials in parts by weight: 45 parts modified kaolin, 13 parts nano zirconium boride, 10 parts hexagonal boron nitride, 7 parts rare earth doped zirconium silicate, 8 parts composite binder, and 4 parts flux.

[0066] The modification method of the kaolin involves calcining the kaolin at 550℃ for 3 hours, then pulverizing and sieving it through a 250-mesh sieve to remove impurities and make the kaolin particles more uniform, thus improving the irradiation modification effect. The kaolin is then placed in an electron beam irradiation device with an electron beam energy of 1.3 MeV, an electron beam current intensity of 4 mA, an irradiation dose of 70 kGy, and an irradiation time of 4 hours. After irradiation, the kaolin is placed in an oven at 80-100℃ for 1-2 hours. The treated kaolin exhibits directional lattice distortion in its crystal structure, improving the mechanical strength and insulation properties of the green body.

[0067] The average particle size of the nano-zirconium boride is 80 nm.

[0068] The rare earth element in the rare earth-doped zirconium silicate is yttrium, and the doping amount, calculated as yttrium oxide, accounts for 4% of the total mass of zirconium silicate. Specifically, zirconium silicate powder with a purity of not less than 95% and an average particle size of 3 μm is selected as the base material, and yttrium oxide powder with a particle size of 1.5 μm is taken. Both powders are dried in an oven at 135°C for 3 hours. The two powders are then mixed and ground at 250 rpm for 3 hours, followed by high-temperature calcination. The temperature is increased to 900°C at a rate of 7°C / min, and held for 2 hours. The temperature is then increased to 1200°C at a rate of 4°C / min and held at this temperature for 4 hours. During the calcination process, argon gas with a purity of 99.9% or higher is introduced as a protective gas, and the gas flow rate is controlled at 15 L / min. After completion, the mixture is cooled to room temperature to obtain rare earth-doped zirconium silicate.

[0069] The composite binder is composed of polyvinyl butyral, sodium alginate and polyethylene glycol diacrylate in a mass ratio of 2-5:1-3:1 to ensure the molding performance of the green body.

[0070] The flux is a mixture of sodium fluorosilicate and zinc borate in a mass ratio of 1:2, which helps to reduce the sintering temperature of the green body.

[0071] The preparation method used in Example 5 above is as follows:

[0072] S1. Mixing and pulping: Weigh the above raw materials according to the weight parts and add them to a high-speed mixer. At the same time, add deionized water and stir at 1000 rpm for 45 minutes to obtain the pulp.

[0073] S2. Iron removal: Pour the slurry into a magnetic separator, control the temperature at 40℃, and set the magnetic field strength to 0.2T to obtain slurry I. Then continue to pour it into the magnetic separator, and set the magnetic field strength to 1.2T to obtain slurry II. The flow rate of the slurry is 3cm / s. Ultrasonic vibration is performed every 15 minutes, with an ultrasonic power of 800W and a vibration time of 4 minutes. Filter and centrifuge to remove water from the slurry, and then dry it in an oven at 120℃ for 4 hours to reduce the moisture content to 5-10%.

[0074] S3. Granulation and Molding: Add ammonium bicarbonate to the iron-removed mixture and stir for 15 minutes. The amount added is 5% of the mixture mass. Transfer the mixture to a granulator for granulation, controlling the particle size to 1 mm. Then, place the granules into a mold and use a cold isostatic pressing process to form the green body. The molding pressure is 200 MPa, and the holding time is 8 minutes.

[0075] S4. Surface treatment: After the green body is demolded, it is glazed, fired, and glued to obtain the finished product.

[0076] Comparative Example 1

[0077] The difference between this comparative example and Example 3 is that the green blank includes the following raw materials in parts by weight: 35 parts modified kaolin, 20 parts nano zirconium boride, 5 parts hexagonal boron nitride, 3 parts rare earth-doped zirconium silicate, 12 parts composite binder, and 8 parts flux.

[0078] Comparative Example 2

[0079] The difference between this comparative example and Example 3 is that the kaolin used as the raw material for the green body was not modified.

[0080] Comparative Example 3

[0081] The difference between this comparative example and Example 3 is that the zirconium silicate raw material of the green blank was not doped with rare earth elements.

[0082] Comparative Example 4

[0083] The difference between this comparative example and Example 3 is that the iron removal step was not performed in the preparation method described herein.

[0084] I. Electrical Performance Testing

[0085] 1. Insulation resistance test: Test standard GB / T1001.1-2021;

[0086] 2. AC withstand voltage test: GB / T16927.1-2011; expressed as the maximum passable test voltage, and the test time is set according to the standard;

[0087] 3. Distributed voltage test: GB / T16927.1-2011; take the example value of the average distributed voltage of a single insulator in the insulator string;

[0088] 4. Leakage current detection: GB / T1001.2-2021; Measured under the same operating voltage of 110kV;

[0089] Test results:

[0090] Table 1:

[0091]

[0092]

[0093] The AC porcelain insulators prepared in the example group showed superior performance to the comparative group in all aspects, indicating that the insulators of the examples have certain advantages in terms of design, raw material selection or manufacturing process, making them more reliable and stable in electrical performance and more suitable for applications such as power transmission lines with high electrical insulation requirements.

[0094] II. Mechanical Performance Testing

[0095] 1. Tensile Strength Test: Mount both ends of the AC insulator specimens from Examples 1-5 and Comparative Examples 1-4 onto the upper and lower clamps of the tensile testing machine. Ensure the clamps firmly hold the specimen and that the tensile force is applied evenly along the insulator's axis, avoiding eccentric loading. Start the tensile testing machine and slowly apply the tensile force at a specified rate until the insulator specimen fails. During the test, the testing machine automatically records data such as the magnitude of the tensile force and the elongation of the specimen.

[0096] 2. Bending Strength Test: Place the specimen on the support blades, adjust the distance between the blades so that the length of the specimen beyond the blades is 10mm, and ensure that the two support blades are in the same plane and parallel to each other. Simultaneously, position the loading blade in the center of the two support blades. Turn on the insulator ceramic bending test machine and apply a constant load at an average speed of 10-50 N / s until the specimen fails. During the loading process, care must be taken to avoid impact when the loading blade contacts the specimen to prevent additional damage to the specimen and affecting the test results. Record the maximum load at which the specimen fails.

[0097] 3. Torsional Strength Test: The AC porcelain insulator specimen is mounted on the clamps of the torsion testing machine. Suitable torsion fixtures, such as a three-jaw chuck or a two-way clamping type, are typically used to ensure the specimen is securely fixed and will not loosen or slip during torsion. The torsion testing machine is started, and the torque is applied to the specimen at a specified torsion speed via the servo motor and reduction system. The torsion speed is controlled within the range of 1 R / min.

[0098] Test results:

[0099] Table 2:

[0100]

[0101]

[0102] Based on the above analysis of tensile strength, bending strength and torsional strength, it can be seen that the AC porcelain insulator represented by the example is superior to the comparative example in terms of mechanical performance. Moreover, Example 3 stands out with its excellent performance in these three key indicators and has superior mechanical performance.

[0103] Compared with Comparative Example 1, Example 3 shows that the raw materials for insulator blanks can improve various mechanical performance indicators under a specific ratio, enabling them to better cope with complex mechanical stress conditions in actual operation.

[0104] Compared with Comparative Example 2, Example 3 uses kaolin irradiated with a high-energy electron beam with a specific irradiation dose to induce directional lattice distortion in its crystal structure. Compared with traditional untreated kaolin, this can better improve the performance of porcelain insulator green bodies, laying the foundation for improving the mechanical strength and insulation performance of the green bodies.

[0105] Compared with Comparative Example 3, Example 3 uses rare earth yttrium-doped zirconium silicate and precisely controls the doping amount, which can refine the grains and further improve the insulation performance of the green blank. This is an optimization of the performance of traditional zirconium silicate materials, making them more suitable for the production of high-performance ceramic insulators.

[0106] Compared with Comparative Example 4, Example 3 shows that iron removal treatment can significantly reduce the iron content in porcelain insulators, improve their insulation performance, and at the same time, reduce the number of stress concentration points formed by iron impurities in porcelain insulators, thereby improving the mechanical strength and durability of porcelain insulators.

[0107] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. An AC porcelain insulator, characterized in that: The AC porcelain insulator is made by glazing, firing, and gluing a green blank. The green blank comprises the following raw materials in parts by weight: 40-50 parts modified kaolin, 10-15 parts nano-zirconium boride, 8-12 parts hexagonal boron nitride, 5-8 parts rare earth-doped zirconium silicate, 6-10 parts composite binder, and 3-5 parts flux. The average particle size of the nano-zirconium boride is 50-100 nm. The green blank has an umbrella-skirt structure with 3-5 umbrella skirts. The height difference between adjacent umbrella skirts gradually increases from top to bottom, with a height difference range of 5-10 mm. The edges of the umbrella skirts are chamfered with a radius of 2-3 mm. The modification method of the modified kaolin is to calcine the kaolin at 500-600℃ for 2-4 hours, then crush and sieve it with a mesh size of 200-300 to remove impurities, and then place it in an electron beam irradiation device with an electron beam energy of 1.2-1.5MeV, an electron beam current intensity of 3-5mA, an irradiation dose of 50-80kGy, and an irradiation time of 3-5h. After irradiation, it is placed in an oven at 80-100℃ and kept warm for 1-2 hours.

2. An AC porcelain insulator as described in claim 1, characterized in that: The green body comprises the following raw materials in parts by weight: 45 parts modified kaolin, 13 parts nano-zirconium boride, 10 parts hexagonal boron nitride, 7 parts rare earth-doped zirconium silicate, 8 parts composite binder, and 4 parts flux.

3. An AC porcelain insulator as described in claim 1, characterized in that: The rare earth element in the rare earth-doped zirconium silicate is yttrium, and the doping amount, calculated as yttrium oxide, accounts for 3%-5% of the total mass of zirconium silicate. Specifically, zirconium silicate powder with a purity of not less than 95% and an average particle size of 1-5 μm is selected as the base raw material, and yttrium oxide powder with a particle size of 0.5-2 μm is taken. Both powders are dried in an oven at 120-150℃ for 3-4 hours. The two powders are mixed and ground at a speed of 200-300 rpm for 2-4 hours. Then, high-temperature calcination is carried out. The temperature is raised to 800-1000℃ at a rate of 5-8℃ / min, and held for 1-3 hours. The temperature is then raised to 1200-1300℃ at a rate of 3-5℃ / min and held at this temperature for 3-5 hours. After completion, the temperature is cooled to room temperature to obtain rare earth-doped zirconium silicate.

4. An AC porcelain insulator as described in claim 3, characterized in that: During the calcination process, argon gas with a purity of 99.9% or higher is introduced as a protective gas, and the gas flow rate is controlled at 10-20 L / min.

5. An AC porcelain insulator as described in claim 1, characterized in that: The composite adhesive is composed of polyvinyl butyral, sodium alginate and polyethylene glycol diacrylate in a mass ratio of 2-5:1-3:

1.

6. An AC porcelain insulator as described in claim 1, characterized in that: The flux is a mixture of sodium fluorosilicate and zinc borate in a mass ratio of 1:1-3.

7. The method for preparing an AC porcelain insulator as described in claim 1, characterized in that: Includes the following steps: S1. Mixing and pulping: Weigh the above raw materials according to the weight parts and add them to a high-speed mixer. At the same time, add deionized water and stir and mix at a speed of 800-1000 rpm for 30-45 minutes to obtain the pulp. S2. Iron removal: Pour the slurry into a magnetic separator, set the magnetic field strength to 0.1-0.2T to obtain slurry I. Then continue to pour it into the magnetic separator, set the magnetic field strength to 0.8-1.2T to obtain slurry II. The flow rate of the slurry is 1-3cm / s. Filter and centrifuge to remove water from the slurry, and then dry it in an oven at 100-120℃ for 2-4 hours to reduce the moisture content to 5-10%. S3. Granulation and molding: Add ammonium bicarbonate to the iron-removed mixture and stir for 10-15 minutes. The amount added is 2.5-5% of the mass of the mixture. Transfer to a granulator for granulation. The particle size is controlled at 0.5-1 mm. Then put it into a mold and use cold isostatic pressing to form the green body. The forming pressure is 150-200 MPa and the holding time is 5-8 minutes. S4. Surface treatment: After the green body is demolded, it is glazed, fired, and glued to obtain the finished product.

8. The method for preparing an AC porcelain insulator as described in claim 7, characterized in that: The slurry concentration of S1 is 20-40%.

9. The method for preparing an AC porcelain insulator as described in claim 7, characterized in that: The temperature inside the S1 high-speed mixer is controlled at 30-40℃, and during the mixing process, ultrasonic vibration is performed every 10-15 minutes, with an ultrasonic power of 500-800W and a vibration time of 2-4 minutes.

Citation Information

Patent Citations

  • Preparation method of thermoplastic inorganic powder

    CN105482162A

  • Coal gangue baking-free brick with mouldproof and antibacterial effects

    CN106082821A