A pretreatment method of nickel oxide powder for preparing an SOFC anode

By subjecting nickel oxide powder to high-temperature calcination and crushing, the problem of surface protrusion of nickel oxide powder during the preparation of NiO/YSZ membranes was solved, ensuring the integrity of the electrolyte layer and improving the performance of solid oxide fuel cells.

CN119613089BActive Publication Date: 2026-11-20ANHUI ESTONE MATERIAL TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411738954.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-11-29
Publication Date
2026-11-20
Estimated Expiration
2044-11-29

AI Technical Summary

Technical Problem

In the prior art, when nickel oxide powder is used to prepare NiO/YSZ membranes, black spots and protrusions are easily formed on the surface, which can damage the electrolyte layer and lead to leakage in solid oxide fuel cells.

Method used

A pretreatment method of high-temperature calcination and crushing of nickel oxide powder was adopted, with the calcination temperature controlled at 1200-1400℃ and the time at 0.5-10h. The powder was then subjected to dry ball milling to prepare nickel oxide powder with uniform particle size, which was used to prepare NiO/YSZ film materials.

Benefits of technology

It effectively reduces the black spot protrusions on the surface of the NiO/YSZ film material, avoids damage to the electrolyte layer, and improves the battery's sealing and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119613089B_ABST
    Figure CN119613089B_ABST
Patent Text Reader

Abstract

The application discloses a pretreatment method of nickel oxide powder for SOFC anode preparation, and relates to the technical field of solid oxide fuel cells, wherein the pretreatment of the nickel oxide powder can be completed by high-temperature calcination and crushing of the nickel oxide powder; the nickel oxide powder is pretreated by high-temperature calcination and crushing, and the nickel oxide in the powder can be reacted with impurities through the calcination; the pretreated nickel oxide powder is applied to the preparation of the SOFC anode, and the problem that the surface of the NiO / YSZ film material and the Ni / YSZ film material has black spots and protrusions due to the local abnormal growth of the nickel oxide particles during high-temperature sintering of the green body can be avoided, and the existence of the black spots and protrusions can be avoided to damage the electrolyte layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of solid oxide fuel cell technology, and more specifically to a pretreatment method for nickel oxide powder used in SOFC anode preparation. Background Technology

[0002] Solid oxide fuel cells (SOFCs) are the third generation of fuel cells, following phosphate fuel cells and molten carbonate fuel cells. They are highly efficient and environmentally friendly energy conversion devices. SOFCs are not limited by the Carnot cycle and can directly convert energy from fossil fuels into electrical energy. With the increasing severity of energy and environmental issues, SOFC research has become a hot research topic in the energy and materials fields.

[0003] SOFC consists of three parts: a porous anode layer, a dense electrolyte layer, and a porous cathode layer. The anode material of SOFC should have a porous structure to ensure the transport of reactant gases, increase the three-phase reaction interface of the electrode, electrolyte, and fuel gas, and make the anode reaction easier to proceed.

[0004] The most commonly used anode material is a composite metal ceramic of metallic nickel (Ni) and yttrium-stabilized zirconium oxide (YSZ). This is mainly achieved by pre-preparing a NiO / YSZ film and then reducing NiO in a reducing environment to obtain the Ni / YSZ anode.

[0005] In the fabrication of single cells, the electrolyte is typically coated onto a NiO / YSZ film and then co-sintered. Since the electrolyte layer is only 4–10 μm thick, the flatness of the NiO / YSZ film is extremely important; there must be no abnormal protrusions on the surface, otherwise the electrolyte layer will be damaged, leading to battery leakage.

[0006] When researchers used commercially available industrial-grade nickel oxide to prepare NiO / YSZ films, they found numerous black spots and protrusions on the sintered films. These protrusions on the surface of the NiO / YSZ films could damage the electrolyte layer during co-sintering, leading to leakage in the single cell. Summary of the Invention

[0007] The technical problem to be solved by the present invention is to provide a pretreatment method for nickel oxide powder for SOFC anode preparation. The pretreated nickel oxide powder is used to prepare NiO / YSZ membrane material, which can effectively reduce the protrusions of black spots on the surface of the membrane material and avoid damage to the electrolyte layer.

[0008] The technical problem to be solved by this invention is achieved by the following technical solution:

[0009] One of the objectives of this invention is to provide a pretreatment method for nickel oxide powder used in SOFC anode preparation, wherein the nickel oxide powder is calcined and crushed at high temperature to complete the pretreatment of nickel oxide powder.

[0010] The second objective of this invention is to provide a method for preparing NiO / YSZ film material for SOFC anodes, comprising the following steps:

[0011] (1) Add YSZ powder, nickel oxide powder treated by the aforementioned pretreatment method and binder to solvent, mix evenly to obtain slurry;

[0012] (2) The slurry is cast and dried to obtain a raw blank;

[0013] (3) The green blank is sintered at high temperature to obtain NiO / YSZ film material.

[0014] The beneficial effects of this invention are as follows: This invention pre-treats nickel oxide powder by first calcining it at high temperature and then crushing it. Calcination allows the nickel oxide in the powder to react with impurities. When the pre-treated nickel oxide powder is used to prepare SOFC anodes, the problem of black spot protrusions on the surface of NiO / YSZ film material and Ni / YSZ film material due to abnormal local growth of nickel oxide particles will not occur during the high-temperature sintering of the blank, thus avoiding the damage to the electrolyte layer caused by the presence of black spot protrusions. Attached Figure Description

[0015] Figure 1 Image of the sample prepared in Example 1;

[0016] Figure 2 Images of the samples prepared in Example 2;

[0017] Figure 3 Image of the sample prepared in Example 3;

[0018] Figure 4 Image of the sample prepared for Comparative Example 1;

[0019] Figure 5 Image of the sample prepared in Example 4;

[0020] Figure 6 Image of the sample prepared in Example 5;

[0021] Figure 7 Image of the sample prepared in Example 6;

[0022] Figure 8 Image of the sample prepared for Comparative Example 2;

[0023] Figure 9 Image of the sample prepared for Comparative Example 3;

[0024] Figure 10 The EDS test results for the black spots in the sample prepared in Comparative Example 3;

[0025] Figure 11 Image of the sample prepared for Comparative Example 4. Detailed Implementation

[0026] To make the technical means, creative features, objectives and effects of this invention easier to understand, the invention will be further described below with reference to specific embodiments and illustrations.

[0027] This invention provides a pretreatment method for nickel oxide powder used in SOFC anode preparation, which involves calcining and crushing the nickel oxide powder at high temperature to complete the pretreatment.

[0028] Furthermore, the particle size D50 of the nickel oxide powder before pretreatment is 1–5 μm.

[0029] Furthermore, the high-temperature calcination temperature is 1200–1400℃, and the time is 0.5–10 hours. A calcination temperature above 1400℃ will result in excessive energy consumption for pretreatment; a calcination temperature below 1200℃ cannot solve the technical problem to be solved by this invention.

[0030] Furthermore, the crushing method is dry ball milling. Dry ball milling has the advantages of simple operation, high processing efficiency, low energy consumption, and easy large-scale production. It can also obtain powders with good particle size uniformity and controllable particle size range.

[0031] Furthermore, the particle size D50 of the pretreated nickel oxide powder is 1–5 μm.

[0032] This invention also provides a method for preparing NiO / YSZ film material for SOFC anodes, comprising the following steps:

[0033] (1) Add YSZ powder, nickel oxide powder treated by the aforementioned pretreatment method and binder to solvent, mix evenly to obtain slurry;

[0034] (2) The slurry is cast and dried to obtain a raw blank;

[0035] (3) The green blank is sintered at high temperature to obtain NiO / YSZ film material.

[0036] Furthermore, the adhesive includes, but is not limited to, one or more of polyvinyl butyral (PVB), carboxymethyl cellulose (CMC), polyvinyl alcohol (PVA), polyethersulfone (PESf), and polyvinylpyrrolidone (PVP).

[0037] Furthermore, the solvent includes, but is not limited to, one or more of ethanol, water, ethylene glycol, and methyl ethyl ketone. Ball milling can be used during slurry preparation to improve the dispersion uniformity of YSZ powder, nickel oxide powder, and binder in the solvent, increase the specific surface area of ​​the particles, reduce the resistivity of the slurry, and thus improve battery performance.

[0038] Furthermore, the mass ratio of the YSZ powder to the pretreated nickel oxide powder and the binder is (30-40):(60-70):(1-5).

[0039] Furthermore, the mixing method is wet ball milling. On the one hand, wet ball milling breaks down the solid particles in the slurry; on the other hand, it makes the slurry composition uniform.

[0040] Furthermore, the high-temperature sintering temperature is 1300–1450°C, and the time is 1–2 hours.

[0041] Furthermore, the surface of the NiO / YSZ film material is free of black spots or protrusions.

[0042] Furthermore, the NiO / YSZ film material can be prepared by reducing the NiO / YSZ film material in a hydrogen atmosphere.

[0043] Example 1

[0044] Step 1: Weigh 100g of nickel oxide powder (particle size D50 = 2μm) and calcine it in a muffle furnace at 1200℃ for 2h; add the calcined solid to a 500mL ball mill jar, and add 500g of zirconium beads with a diameter of 2mm to the ball mill jar. Ball mill at a speed of 500r / min until the particle size D50 is 2μm, and dry it in an oven at 150℃ until the moisture content is less than 0.3wt%. This completes the pretreatment of nickel oxide powder.

[0045] Step 2: Add 2g PVB, 67g ethanol, 40g YSZ powder (particle size D50 = 0.5μm), 60g of pretreated nickel oxide (particle size D50 = 2μm), and 500g zirconium beads with a diameter of 2mm to a 500mL ball mill jar. Ball mill at 500r / min for 24h to obtain a slurry. Cast the slurry into a shape and dry it at 105℃ for 24h to obtain a green blank. Cut the green blank into 118mm×118mm square pieces and sinter them in a muffle furnace at 1450℃ for 2h to obtain a sample.

[0046] Examples 2-6 and Comparative Examples 1-2

[0047] The method of Example 1 was followed, except that the calcination temperature or calcination time of the nickel oxide powder during pretreatment was adjusted, as shown in Table 1. The presence of black raised spots on the surface of the samples prepared in Examples 1-3 and Comparative Examples 1-2 was observed, and the results are shown in Table 1.

[0048] Table 1

[0049]

[0050]

[0051] Combination Figures 1-4 It is known that when the calcination temperature of nickel oxide powder is controlled at 1200–1400℃ during pretreatment, the prepared sample surface has no black spots or protrusions. When the calcination temperature is below 1200℃, more black spots and protrusions appear on the prepared sample surface. Of course, the calcination temperature can be higher than 1400℃, but this will increase energy consumption. Therefore, it is recommended to control the calcination temperature of nickel oxide powder during pretreatment at 1200–1400℃.

[0052] Combination Figures 5-8 It is known that when the calcination time of nickel oxide powder is controlled within 0.5–10 h during pretreatment, the prepared sample surface has no black spot protrusions. When the calcination time is less than 0.5 h, more black spot protrusions appear on the prepared sample surface because the nickel oxide in the nickel oxide powder does not react completely with the impurities. Of course, the calcination time can be greater than 10 h, but this will increase energy consumption. Therefore, it is recommended to control the calcination time of nickel oxide powder within 0.5–10 h during pretreatment.

[0053] Comparative Example 3

[0054] The method of Example 1 was followed, except that the nickel oxide powder was not pretreated; instead, the sample was prepared directly using nickel oxide powder (particle size D50 = 2 μm). Observation of the sample prepared in Comparative Example 3 revealed numerous black raised dots on its surface, such as... Figure 9 As shown.

[0055] Combination Figure 9 It is known that if nickel oxide powder is used to prepare samples directly without pretreatment, many black spots will appear on the surface of the prepared samples. This is because the nickel oxide in the blank reacts with impurities in the nickel oxide during high-temperature sintering.

[0056] right Figure 9 X-ray energy dispersive spectroscopy (EDS) was performed on the black spots in the image, and the results are shown in [Figure number missing]. Figure 10 .Depend on Figure 10 It can be seen that in addition to nickel (the main element), the black spots also contain impurity elements such as Al and Fe. This suggests that impurity elements such as Al and Fe may cause abnormal local growth of nickel oxide particles, forming the raised black spots.

[0057] Comparative Example 4

[0058] The method of Example 2 was followed, except that a small amount of iron oxide was added to the surface of the green blank before high-temperature sintering. Observation of the sample prepared in Comparative Example 4 revealed numerous black raised spots on its surface, such as... Figure 11 As shown.

[0059] Combination Figure 11 It is known that adding a small amount of iron oxide to the surface of the green blank before high-temperature sintering results in numerous black raised spots on the surface of the prepared sample. This is due to the reaction between iron oxide and nickel oxide during high-temperature sintering.

[0060] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the present invention as claimed. The scope of protection of this invention is defined by the appended claims and their equivalents.

Claims

1. A pretreatment method for nickel oxide powder used in SOFC anode preparation, characterized in that: The nickel oxide powder is pretreated by calcining and crushing at high temperature to obtain pretreated nickel oxide powder. The high temperature calcination is 1200~1400℃ and the time is 0.5~10 h. The nickel oxide powder contains Al and Fe impurity elements. The surface of the NiO / YSZ film material prepared from the pretreated nickel oxide powder is free of black spots and protrusions.

2. The pretreatment method according to claim 1, characterized in that: The particle size D50 of the nickel oxide powder before pretreatment is 1~5μm.

3. The pretreatment method according to claim 1, characterized in that: The crushing method is dry ball milling.

4. The pretreatment method according to claim 1, characterized in that: The particle size D50 of the pretreated nickel oxide powder is 1~5μm.

5. A method for preparing a NiO / YSZ film material for SOFC anodes, characterized in that, Includes the following steps: (1) Add YSZ powder, nickel oxide powder pretreated by any one of the pretreatment methods described in claims 1 to 4, and binder to a solvent and mix them evenly to obtain a slurry; (2) The slurry is cast and dried to obtain a raw blank; (3) The green blank is sintered at high temperature to obtain NiO / YSZ film material; The surface of the NiO / YSZ film material is free of black spots or protrusions.

6. The preparation method according to claim 5, characterized in that: The adhesive is one or more of PVB, CMC, PVA, PESf, and PVP.

7. The preparation method according to claim 5, characterized in that: The solvent is one or more of ethanol, water, ethylene glycol, and methyl ethyl ketone.

8. The preparation method according to claim 5, characterized in that: The mass ratio of YSZ powder to pretreated nickel oxide powder and binder is (30~40): (60~70): (1~5).

9. The preparation method according to claim 5, characterized in that: The high-temperature sintering temperature is 1300~1450℃, and the time is 1~2h.

Citation Information

Patent Citations

  • Nickel oxide particles and method for producing nickel oxide particles

    CN117397070A